A thermoelectric material, its preparation method, and a thermoelectric device

By doping the thermoelectric material AgCuSe with S and Ce or Zn, its electrical transport properties are improved, the problem of low power factor is solved, higher conductivity and power factor are achieved, and its application range is expanded.

CN123061920APending Publication Date: 2026-11-10SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611578289.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The low power factor of the existing thermoelectric material AgCuSe limits its application.

Method used

By co-doping the thermoelectric material AgCuSe with S and Ce or with S and Zn, its electrical transport properties can be improved, and its electrical conductivity and power factor can be enhanced.

Benefits of technology

It significantly improves the electrical conductivity and power factor of thermoelectric materials, enhancing their performance in specific application scenarios, especially their potential applications in low-power energy harvesting and flexible thermoelectric devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061920A_ABST
    Figure CN123061920A_ABST
Patent Text Reader

Abstract

This invention discloses a thermoelectric material, its preparation method, and a thermoelectric device, relating to the field of thermoelectric material technology. The chemical formula of the thermoelectric material is AgCu. 1‑x Se 1‑γ S γ M x M is either Zn or Ce; when M is Zn, 0.01 ≤ x ≤ 0.04, 0.01 ≤ γ ≤ 0.04; when M is Ce, 0.02 ≤ x ≤ 0.04, 0.01 ≤ γ ≤ 0.04. Compared to the thermoelectric material AgCuSe, the thermoelectric material provided by this invention has higher conductivity and power factor. Specifically, this invention improves the electrical transport properties of the thermoelectric material AgCuSe by co-doping with S and Ce or co-doping with S and Zn, thereby enhancing its conductivity and power factor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermoelectric materials technology, and in particular to a thermoelectric material, its preparation method, and a thermoelectric device. Background Technology

[0002] Thermoelectric materials are materials capable of converting heat energy into electrical energy, and they have wide applications in power generation and refrigeration. Among them, AgCuSe thermoelectric material has attracted the attention of researchers because it combines the advantages of Cu2Se and Ag2Se thermoelectric materials. However, AgCuSe has a low power factor, which limits its application to some extent.

[0003] Therefore, existing technologies still need to be improved and developed. Summary of the Invention

[0004] Based on the shortcomings of the prior art, the purpose of this invention is to provide a thermoelectric material, its preparation method, and a thermoelectric device, aiming to solve the problem that the power factor of the thermoelectric material AgCuSe still needs to be further improved.

[0005] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a thermoelectric material, wherein the chemical formula of the thermoelectric material is AgCu. 1- x Se 1-γ S γ M x M is Zn or Ce; When M is Zn, 0.01≤x≤0.04, 0.01≤γ≤0.04; When M is Ce, 0.02≤x≤0.04, 0.01≤γ≤0.04.

[0006] Optionally, the thermoelectric material has the chemical formula AgCu. 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 AgCu 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu0.97 Se 0.98 S 0.02 Ce 0.03 or AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 .

[0007] A second aspect of the present invention provides a method for preparing the thermoelectric material as described above, comprising the following steps: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, then melting and cooling them to obtain a block-shaped thermoelectric material.

[0008] A third aspect of the present invention provides another method for preparing the thermoelectric material as described above, comprising the following steps: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder and M particles, melting them, and cooling them to obtain a block-shaped thermoelectric material. The block-shaped thermoelectric material is subjected to deformation heat treatment to extend the block-shaped thermoelectric material and obtain a thin film-shaped thermoelectric material.

[0009] Optionally, the deformation heat treatment is performed at a temperature of 323~470 K and at a pressure of 10~1000 MPa.

[0010] Optionally, according to AgCu 1-x Se 1-γ S γ M x The specific steps for smelting Ag particles, Cu particles, Se particles, sulfur powder, and M particles, based on the stoichiometric ratio of each element, include: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, placing them in a first container, and then sealing the first container after evacuating it. The sealed first container was placed in a muffle furnace for melting.

[0011] Optionally, according to AgCu 1-x Se 1-γS γ M x The specific steps for smelting Ag particles, Cu particles, Se particles, sulfur powder, and M particles, based on the stoichiometric ratio of each element, include: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, placing them in a first container, and then sealing the first container after evacuating it. Place the sealed first container into the second container, and then evacuate and seal the second container. The sealed second container was placed in a muffle furnace for melting.

[0012] Optionally, the inner wall of the first container is coated with a carbon film.

[0013] Optionally, the process parameters for smelting are as follows: First, heat the material to 200-400 ℃ at a rate of 1-10 ℃ / min, and hold it at 200-400 ℃ for 240 min. Then, heat the material to 1100-1300 ℃ at a rate of 0.1-20 ℃ / min, and hold it at 1100-1300 ℃ for 720 min. Next, cool the material to 450-550 ℃ at a rate of 0.1-10 ℃ / min, and hold it at 450-550 ℃ for 2 days. Finally, cool the material to room temperature at a rate of 1-20 ℃ / min.

[0014] In a fourth aspect, the present invention provides a thermoelectric device comprising alternating N-type thermoelectric elements and P-type thermoelectric elements, wherein the N-type thermoelectric elements comprise the thermoelectric material described above.

[0015] Beneficial effects: Compared to the thermoelectric material AgCuSe, the thermoelectric material provided by this invention has higher electrical conductivity and power factor. Specifically, this invention improves the electrical transport properties of the thermoelectric material AgCuSe and enhances its electrical conductivity and power factor by co-doping it with S and Ce or with S and Zn. Attached Figure Description

[0016] Figure 1 This is a diagram illustrating the synthesis process of the thermoelectric material AgCuSe.

[0017] Figure 2 The graphs show the performance of the thermoelectric material AgCuSe prepared by different synthesis processes. In the graphs, a is the electrical conductivity as a function of temperature, b is the Seebeck coefficient as a function of temperature, c is the power factor as a function of temperature, and d is the thermal conductivity as a function of temperature.

[0018] Figure 3 The XRD patterns of the various block thermoelectric materials in Comparative Example 1 are shown.

[0019] Figure 4 The images show the XRD patterns of the various block thermoelectric materials in Example 1.

[0020] Figure 5 The images show the XRD patterns of the block thermoelectric materials in Example 2 and the block thermoelectric materials in Comparative Example 2.

[0021] Figure 6 For the bulk thermoelectric materials AgCuSe and AgCuSe in Comparative Example 1 0.98 S 0.02 and the bulk thermoelectric material AgCu in Example 1 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 and AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 The performance graphs are shown, where a is the electrical conductivity as a function of temperature, b is the Seebeck coefficient as a function of temperature, c is the power factor as a function of temperature, d is the thermal conductivity as a function of temperature, e is the lattice thermal conductivity as a function of temperature, and f is the thermoelectric figure of merit as a function of temperature.

[0022] Figure 7 For the bulk thermoelectric materials AgCuSe and AgCuSe in Comparative Example 1 0.98 S 0.02 Comparative Example 2: Bulk thermoelectric material AgCu 0.99 Se 0.98 S 0.02 Ce 0.01 In Example 1, the bulk thermoelectric material AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 and the bulk thermoelectric material AgCu in Example 2 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 and AgCu 0.96 Se0.98 S 0.02 Ce 0.04 The performance graphs are shown, where a is the electrical conductivity as a function of temperature, b is the Seebeck coefficient as a function of temperature, c is the power factor as a function of temperature, d is the thermal conductivity as a function of temperature, e is the lattice thermal conductivity as a function of temperature, and f is the thermoelectric figure of merit as a function of temperature.

[0023] Figure 8 The thin-film thermoelectric material AgCu in Example 4 0.97 Se 0.98 S 0.02 Ce 0.03 SEM image.

[0024] Figure 9 The figures show the performance of each thin-film thermoelectric material in Example 3, where a is the conductivity versus temperature, b is the Seebeck coefficient versus temperature, and c is the power factor versus temperature.

[0025] Figure 10 The figures show the performance of each thin-film thermoelectric material in Example 4, where a is the conductivity versus temperature, b is the Seebeck coefficient versus temperature, and c is the power factor versus temperature.

[0026] Figure 11 This is a schematic diagram of the out-of-plane flexible thermoelectric device structure in Example 5.

[0027] Figure 12 The diagram shows the performance of the out-of-plane flexible thermoelectric device in Example 5, where a is the relationship between output voltage and output current under different temperature differences, and b is the relationship between output power and output current under different temperature differences.

[0028] in, Figure 2 b, c, and d in the text adopt the same as Figure 2 The same legend as 'a' in the diagram; Figure 6 b, c, d, e, and f in the formula adopt the same as... Figure 6 The same legend as 'a' in the diagram; Figure 7 b, c, d, e, and f in the formula adopt the same as... Figure 7 The same legend as 'a' in the diagram; Figure 9 b and c in the text adopt the same as Figure 9 The same legend as 'a' in the diagram; Figure 10 b and c in the text adopt the same as Figure 10 The same legend as 'a' in the diagram. Detailed Implementation

[0029] This invention provides a thermoelectric material, its preparation method, and a thermoelectric device. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0031] If the embodiments of the present invention involve descriptions such as "first" or "second", such descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated.

[0032] For some application scenarios, such as transient thermoelectric power generation, wearable human body heat power generation, and low-power energy harvesting scenarios from infinitely large ambient heat sources (surfaces of industrial equipment), the power factor of thermoelectric materials is a core indicator. Therefore, in these scenarios, either the operating time is short and the heat conduction process has not yet fully occurred, or the heat source supply is sufficient and heat loss due to thermal conductivity does not affect system operation. Thus, the impact of thermal conductivity on performance is negligible, and there is no need to deliberately pursue low thermal conductivity in pursuit of high thermoelectric figure of merit. Therefore, it is necessary to further improve the power factor of the thermoelectric material AgCuSe to enable its better application in these scenarios. Based on this, this invention provides a thermoelectric material, wherein the chemical formula of the thermoelectric material is AgCu. 1-x Se 1-γ S γ M x M is Zn or Ce; when M is Zn, 0.01≤x≤0.04, 0.01≤γ≤0.04; when M is Ce, 0.02≤x≤0.04, 0.01≤γ≤0.04.

[0033] Compared to the thermoelectric material AgCuSe, the thermoelectric material provided in this embodiment of the invention has higher electrical conductivity and power factor. Specifically, this embodiment of the invention improves the carrier mobility, enhances its electrical transport performance, and increases its electrical conductivity and power factor by co-doping the thermoelectric material AgCuSe with S and Ce or with S and Zn.

[0034] In this embodiment, as an example, when M is Zn, x can be 0.01, 0.02, 0.03 or 0.04, etc.; γ can be 0.01, 0.02, 0.03 or 0.04, etc.

[0035] When M is Ce, x can be 0.02, 0.03, or 0.04, etc.; γ can be 0.01, 0.02, 0.03, or 0.04, etc.

[0036] In some embodiments, γ = 0.02. That is, the chemical formula of the thermoelectric material is AgCu. 1-x Se 0.98 S 0.02 M x M is either Ce or Zn; when M is Zn, 0.01 ≤ x ≤ 0.04; when M is Ce, 0.02 ≤ x ≤ 0.04.

[0037] In some embodiments, the thermoelectric material has the chemical formula AgCu. 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 AgCu 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 or AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 .

[0038] Among them, the thermoelectric material AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 The power factor can reach 28 μWcm at 300 K (near room temperature). -1 K -2 Compared to the undoped thermoelectric material AgCuSe, it improved by approximately 86%. The thermoelectric material AgCu... 0.98 Se 0.98 S 0.02 Zn 0.02 The power factor can reach 22 μWcm at 300 K (near room temperature). -1 K -2Compared to undoped AgCuSe, this represents an improvement of approximately 46%. Furthermore, compared to the undoped thermoelectric material AgCuSe, the thermoelectric material AgCu... 0.97 Se 0.98 S 0.02 Ce 0.03 The thermoelectric figure of merit has also been improved, and it has a wider range of application prospects.

[0039] This invention also provides a method for preparing the thermoelectric material as described above, comprising the following steps: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element is determined by mixing Ag particles (silver particles), Cu particles (copper particles), Se particles (selenium particles), sulfur powder, and M particles (Ce particles or Zn particles, i.e., cerium particles or zinc particles), smelting, and cooling to obtain a block-shaped thermoelectric material.

[0040] In this embodiment, AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of Ag, Cu, Se, S, and M is 1:(1-x):(1-γ):γ:x. For example, when γ=0.02, x=0.02, and M is Zn, Ag particles, Cu particles, Se particles, sulfur powder, and Zn particles are mixed and smelted according to a molar ratio of 1:0.98:0.98:0.02:0.02.

[0041] When γ=0.02, x=0.03, and M is Ce, Ag particles, Cu particles, Se particles, sulfur powder, and Ce particles are mixed and smelted according to a molar ratio of 1:0.97:0.98:0.02:0.03.

[0042] This invention also provides a method for preparing the thermoelectric material as described above, comprising the following steps: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder and M particles, melting them, and cooling them to obtain a block-shaped thermoelectric material. The block-shaped thermoelectric material is subjected to deformation heat treatment to extend the block-shaped thermoelectric material and obtain a thin film-shaped thermoelectric material.

[0043] This invention discovers that blocky thermoelectric materials have thermoplasticity at certain temperatures, and therefore can be stretched after deformation heat treatment to form thin-film thermoelectric materials. These thin-film thermoelectric materials have multiple slip band micro-features, good mechanical flexibility and thermoelectric properties, and good deformation and bending ability. They can achieve bending deformation with a bending radius of less than 1 cm at room temperature without breaking, and have great practical application value. They can be used for the preparation of flexible thermoelectric devices.

[0044] In some embodiments, the temperature used for the deformation heat treatment is 323~470 K, specifically 323~450 K (e.g., 323 K, 350 K, 380 K, 400 K, 410 K, 420 K, 430 K, 440 K or 450 K, etc.), that is, a temperature range not higher than the AgCuSe phase transition temperature (450 K) is selected, and the pressure used for the deformation heat treatment is 10~1000 MPa (e.g., 10 MPa, 100 MPa, 200 MPa, 500 MPa, 800 MPa or 1000 MPa, etc.).

[0045] Specifically, within this temperature range, the Ag and Cu cation sublattices undergo intense disordering and high migration, resulting in significant lattice softening. Under external force, the thermoelectric material can exhibit considerable plastic / viscoplastic flow and freeze upon cooling.

[0046] In some embodiments, the deformation heat treatment methods include, but are not limited to, hot pressing, hot rolling, hot forging, or hot rolling.

[0047] In some embodiments, the deformation heat treatment is carried out by hot rolling. The hot rolling temperature is 323~470K, the pressure is 100 MPa, and the rolling speed is 0.3~0.5 cm / s (e.g., 0.3 cm / s, 0.4 cm / s, or 0.5 cm / s). After 1~10 times (e.g., 1, 2, 3, 5, 8, or 10 times), the block thermoelectric material is processed into a thin film thermoelectric material with a thickness of 30~60 μm (e.g., 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, or 60 μm).

[0048] In some implementations, according to AgCu 1-x Se 1-γ S γ M x The specific steps for smelting Ag particles, Cu particles, Se particles, sulfur powder, and M particles, based on the stoichiometric ratio of each element, include: According to AgCu 1-x Se 1-γ Sγ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, placing them in a first container, and then sealing the first container after evacuating it. The sealed first container was placed in a muffle furnace for melting.

[0049] In some implementations, according to AgCu 1-x Se 1-γ S γ M x The specific steps for smelting Ag particles, Cu particles, Se particles, sulfur powder, and M particles, based on the stoichiometric ratio of each element, include: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, placing them in a first container, and then sealing the first container after evacuating it. Place the sealed first container into the second container, and then evacuate and seal the second container. The sealed second container was placed in a muffle furnace for melting.

[0050] In this embodiment, the purpose of using two nested containers is that the process of cooling the mixed raw materials from a high-temperature molten state to room temperature involves a phase transition, changing from a high-temperature disordered superionic phase to a low-temperature ordered phase. Due to the drastic phase transition, the volume of the ingot inside the first container will change significantly, which may cause the inner first container to crack. To reduce the risk of the ingot being exposed to air and oxidized, a second container is used.

[0051] For example, the total mass of Ag particles, Cu particles, Se particles, sulfur powder, and M particles can be 5~50 g (e.g., 5 g, 10 g, 15 g, 20 g, 25 g, 30 g, 35 g, 40 g, 45 g, or 50 g, etc.); the first container is evacuated to 1×10 - 4 After sealing, the second container is evacuated to 1×10⁻⁶. -4 After Pa, seal.

[0052] In some embodiments, the inner wall of the first container is coated with a carbon film. This prevents the mixed raw materials from reacting with the inner wall of the first container and facilitates the complete removal of the sintered product. The carbon film acts as an inert insulating layer, effectively suppressing interfacial reactions and cross-contamination between the mixed raw materials and the first container. Furthermore, it reduces the adhesion of the mixed raw materials to the inner wall of the first container, which is beneficial for the complete removal of the sintered product and the reuse of the first container. In addition, the carbon film has a certain absorption and reduction effect on residual oxygen at high temperatures, helping to maintain a low oxygen partial pressure inside the first container and preventing accidental oxidation of the target product.

[0053] In some implementations, the process parameters for smelting are as follows: First, heat the material to 200-400 ℃ at a rate of 1-10 ℃ / min, and hold it at 200-400 ℃ for 240 min. Then, heat the material to 1100-1300 ℃ at a rate of 0.1-20 ℃ / min, and hold it at 1100-1300 ℃ for 720 min. Next, cool the material to 450-550 ℃ at a rate of 0.1-10 ℃ / min, and hold it at 450-550 ℃ for 2 days. Finally, cool the material to room temperature at a rate of 1-20 ℃ / min.

[0054] In some specific implementations, the temperature is first increased from room temperature to 400 °C at a rate of 1 °C / min, and held at 400 °C for 240 min (for pre-reaction, since the melting point of Se is around 220 °C, this avoids excessively rapid Se volatilization and helps suppress the growth of other impurity phases). Then, the temperature is increased to 1100 °C at a rate of 0.7 °C / min and held at 1100 °C for 720 min. After that, the temperature is decreased to 550 °C at a rate of 0.333 °C / min and held at 550 °C for 2 days. Finally, the temperature is decreased to room temperature (25 °C) at a rate of 1.3125 °C / min.

[0055] This invention also provides a thermoelectric device comprising alternating N-type thermoelectric elements and P-type thermoelectric elements, wherein the N-type thermoelectric elements comprise the thermoelectric material described above in this invention embodiment.

[0056] When the N-type thermoelectric element uses the thin-film thermoelectric material described in the embodiments of the present invention, the thermoelectric device can be a flexible thermoelectric device. This flexible thermoelectric device, with an actual temperature difference of 3.93 K, can achieve an open-circuit voltage of 5.66 mV, an open-circuit current exceeding 30 mA, a maximum power of 43.5 μW, and a maximum normalized power density of 0.8 μWcm³. -1 K -2 It has very promising application prospects.

[0057] The present invention will be further described below through specific embodiments.

[0058] First, AgCuSe thermoelectric materials were prepared using two different processes, and the preparation processes were studied.

[0059] Process 1: such as Figure 1 As shown, the temperature was first increased from room temperature (25 °C) to 400 °C at a rate of 1 °C / min and held at 400 °C for 240 min. Then, the temperature was increased to 1100 °C at a rate of 0.7 °C / min and held at 1100 °C for 720 min. After that, the temperature was decreased to 550 °C at a rate of 0.333 °C / min and held at 550 °C (i.e., annealing) for 2 days. Finally, the temperature was decreased to room temperature (25 °C) at a rate of 1.3125 °C / min.

[0060] Process 2: such as Figure 1 As shown, the temperature was first increased from room temperature (25 °C) to 400 °C at a rate of 2 °C / min and held at 400 °C for 240 min. Then, the temperature was increased to 1100 °C at a rate of 1.458 °C / min and held at 1100 °C for 720 min. After that, the temperature was decreased to 550 °C at a rate of 0.333 °C / min and held at 550 °C (i.e., annealing) for 2 days. Finally, the temperature was decreased to room temperature (25 °C) at a rate of 1.3125 °C / min.

[0061] The performance of the thermoelectric material AgCuSe obtained by two different processes was tested, and the results are as follows: Figure 2 As shown, compared to process one, the rapid heating of process two leads to poor thermoelectric properties of the material. Therefore, in the following examples and comparative examples, process one with slow heating and long heat preservation is used.

[0062] Unless otherwise specified, the raw materials and equipment used in the following examples are all commercially available products. The purity of the silver, copper, and selenium granules is 99.999%; the purity of the cerium, zinc, and sulfur powder is above 99.9%.

[0063] Example 1 This embodiment provides a bulk thermoelectric material and its preparation method. The chemical formula of the bulk thermoelectric material is AgCu. 1- x Se 0.98 S 0.02 Zn x x is 0.01, 0.02, 0.03 and 0.04 respectively.

[0064] The preparation method of bulk thermoelectric materials includes the following steps: According to AgCu1-x Se 0.98 S 0.02 Zn x To determine the stoichiometric ratio of each element, 15 g of silver, copper, selenium, sulfur, and zinc granules were weighed, mixed, and placed in a fine quartz tube with an inner diameter of 10 mm (the inner wall of the fine quartz tube was pre-coated with a carbon film twice using acetone). The fine quartz tube was then evacuated to a vacuum level of 1 × 10⁻⁶ using a vacuum pump. -4 After Pa, flame sealing is performed. Then, the sealed thin quartz tube is placed into a coarse quartz tube with an inner diameter of 20 mm. The coarse quartz tube is then evacuated to 1×10⁻⁶. - 4 After Pa, the tube was sealed. Then, the sealed coarse quartz tube was placed in a muffle furnace for melting. Specifically, the temperature was first increased from room temperature to 400 °C at a rate of 1 °C / min, and then held at 400 °C for 240 min for pre-reaction. Subsequently, the temperature was increased to 1100 °C at a rate of 0.7 °C / min and held for 720 min to allow the raw materials to react fully. Then, the temperature was decreased to 550 °C at a rate of 0.333 °C / min and annealed at 550 °C for 2 days to optimize the crystal structure of the material. Finally, the temperature was decreased to room temperature at a rate of 1.3125 °C / min to prepare the bulk thermoelectric material AgCu. 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 and AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 .

[0065] Example 2 This embodiment provides a bulk thermoelectric material and its preparation method. The chemical formula of the bulk thermoelectric material is AgCu. 1- x Se 0.98 S 0.02 Ce x x is 0.02, 0.03 and 0.04 respectively.

[0066] The preparation method of the bulk thermoelectric material is basically the same as that in Example 1, the only difference being: according to AgCu 1-x Se 0.98 S 0.02 Ce xBased on the stoichiometric ratio of each element, 15 g of silver, copper, selenium, sulfur powder, and cerium granules were weighed out, and the final product was a blocky thermoelectric material AgCu. 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 and AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 .

[0067] Comparative Example 1 This comparative example provides a bulk thermoelectric material and its preparation method. The chemical formula of the bulk thermoelectric material is AgCuSe. 1-γ S γ γ is 0, 0.01, 0.02, 0.03 and 0.04 respectively.

[0068] The preparation method of the bulk thermoelectric material is basically the same as that in Example 1, except that: according to AgCuSe 1-γ S γ Based on the stoichiometric ratio of each element, 15 g of silver granules, copper granules, selenium granules, and sulfur powder were weighed out, and the final product was a blocky thermoelectric material AgCuSe. 0.99 S 0.01 AgCuSe 0.98 S 0.02 AgCuSe 0.97 S 0.03 and AgCuSe 0.96 S 0.04 .

[0069] Comparative Example 2 This comparative example provides a bulk thermoelectric material and its preparation method. The chemical formula of the bulk thermoelectric material is AgCu. 1- x Se 0.98 S 0.02 Ce x x=0.01.

[0070] The preparation method of the bulk thermoelectric material is basically the same as that in Example 1, the only difference being: according to AgCu 1-x Se 0.98 S 0.02 Ce x Based on the stoichiometric ratio of each element, 15 g of silver granules, copper granules, selenium granules, sulfur powder, and cerium granules were weighed out, and the final product was a bulk thermoelectric material AgCu. 0.99 Se 0.98S 0.02 Ce 0.01 .

[0071] The block thermoelectric materials in Examples 1, 2, 1, and 2 were tested: (1) X-ray diffraction (XRD) tests were performed on each bulk thermoelectric material in Example 1, Example 2, Comparative Example 1 and Comparative Example 2, wherein the bulk thermoelectric material in Comparative Example 1 (i.e. bulk thermoelectric material AgCuSe, AgCuSe) 0.99 S 0.01 AgCuSe 0.98 S 0.02 AgCuSe 0.97 S 0.03 and AgCuSe 0.96 S 0.04 The XRD pattern of ) is as follows Figure 3 As shown; the bulk thermoelectric materials in Example 1 (i.e., bulk thermoelectric material AgCu) 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 and AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 The XRD pattern of ) is as follows Figure 4 As shown; the bulk thermoelectric materials in Example 2 (i.e., bulk thermoelectric material AgCu) 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 and AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 ), and the bulk thermoelectric material in Comparative Example 2 (i.e., the bulk thermoelectric material AgCu) 0.99 Se 0.98 S 0.02 Ce 0.01 The XRD pattern of ) is as follows Figure 5 As shown.

[0072] As can be seen, there are no impurity peaks in the XRD pattern, which indicates that each block thermoelectric material is a pure phase.

[0073] (2) Performance tests were conducted on the bulk thermoelectric materials in Examples 1, 2, Comparative Example 1, and Comparative Example 2 at different temperatures. Among them, the bulk thermoelectric materials AgCuSe and AgCuSe in Comparative Example 1 were tested. 0.98 S 0.02 and the bulk thermoelectric material AgCu in Example 1 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 and AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 Performance results as follows Figure 6 As shown.

[0074] Comparative Example 1: Bulk thermoelectric materials AgCuSe and AgCuSe 0.98 S 0.02 Comparative Example 2: Bulk thermoelectric material AgCu 0.99 Se 0.98 S 0.02 Ce 0.01 In Example 1, the bulk thermoelectric material AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 and the bulk thermoelectric material AgCu in Example 2 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 and AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 Performance results as follows Figure 7 As shown.

[0075] Depend on Figure 6 and Figure 7The results show that all thermoelectric materials are n-type thermoelectric materials. For the bulk thermoelectric material AgCuSe, doping with S atoms only slightly improves its conductivity and power factor, while further doping with Zn or Ce atoms (at specific doping amounts) can significantly improve its conductivity and power factor. Bulk thermoelectric material AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 and AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 The highest power factor in the room temperature region can reach 22 μWcm. -1 K -2 and 28 μWcm -1 K -2 Compared to the undoped bulk thermoelectric material AgCuSe, the improvements were 46% and 86%, respectively.

[0076] Furthermore, compared to the undoped bulk thermoelectric material AgCuSe, the bulk thermoelectric material AgCu... 0.97 Se 0.98 S 0.02 Ce 0.03 It not only has a high power factor, but also a high thermoelectric figure of merit, making it more widely applicable.

[0077] Example 3 This embodiment provides a thin-film thermoelectric material and its preparation method. The chemical formula of the thin-film thermoelectric material is the same as that in Example 1.

[0078] The preparation method of thin-film thermoelectric materials includes the following steps: The block thermoelectric material prepared in Example 1 was cut into cubes and then placed in a hot roller press. The temperature was set to 353 K, the pressure to 100 MPa, the rolling speed to 0.3 cm / s, and the rolling cycle to 5 times, resulting in a thin film with a thickness of 30 μm. This yielded the final thin-film thermoelectric material AgCu. 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 and AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 .

[0079] Example 4 This embodiment provides a thin-film thermoelectric material and its preparation method. The chemical formula of the thin-film thermoelectric material is the same as that in Example 2.

[0080] The preparation method of thin-film thermoelectric materials includes the following steps: The block thermoelectric material prepared in Example 2 was cut into cubes with a thickness of 25 mm and a side length of 515 mm. These cubes were then placed in a hot roller press at a temperature of 353 K, a pressure of 100 MPa, a rolling speed of 0.5 cm / s, and 5 rolling passes to obtain a thin film with a thickness of 30 μm. This yielded the final thin-film thermoelectric material AgCu. 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 and AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 The rare earth elements were then transferred to a vacuum chamber for storage and testing to reduce their oxidation in the air.

[0081] In addition, as a comparison, this embodiment also prepared a thin-film thermoelectric material AgCu using the method described above. 0.99 Se 0.98 S 0.02 Ce 0.01 .

[0082] The thin-film thermoelectric materials in Examples 3 and 4 were tested: (1) Regarding the thin-film thermoelectric material AgCu in Example 4 0.97 Se 0.98 S 0.02 Ce 0.03 Scanning electron microscopy (SEM) was performed, and the results are as follows: Figure 8 As shown, the film surface has multiple slip bands, proving that the bulk thermoelectric material has undergone plastic deformation.

[0083] (2) The performance of each thin-film thermoelectric material in Examples 3 and 4 was tested at different temperatures, and the results are as follows: Figure 9 and Figure 10 As shown, the film obtained by hot rolling not only successfully retains the electrical performance characteristics of the corresponding bulk thermoelectric material, but also the thin-film thermoelectric material AgCu... 0.98 Se 0.98 S 0.02 Zn 0.02The room temperature power factor reached 19 μWcm -1 K -2 The highest power factor is 22.2 μWcm at 400K. -1 K -2 Thin-film thermoelectric material AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 Its conductivity (at 300K) can still reach 48×10 4 Sm -1 The power factor can reach 27.3 μWcm in the room temperature range. -1 K -2 This value is lower than that of corresponding bulk n-type thermoelectric materials, possibly due to the oxidation of rare earth elements. However, this value is significantly better than that of other inorganic plastic semiconductor materials.

[0084] The above analysis shows that the power factor of the thin-film thermoelectric material obtained by hot rolling is comparable to, and even surpasses, that of most inorganic plastic semiconductor materials, further demonstrating the enormous application potential of thin-film thermoelectric materials. Therefore, the next step will be to use thin-film thermoelectric materials to fabricate flexible thermoelectric devices and evaluate their practical application potential.

[0085] Example 5 Fabrication of out-of-plane flexible thermoelectric devices: like Figure 11 As shown, two PI (polyimide) films are designated PI-1 and PI-2, respectively. Several copper conductive plates (4 mm × 10 mm) are attached to both films. Solder paste is then applied to both ends of each copper conductive plate on the PI-1 film (within the dashed box in the figure) and spread evenly. N-type and P-type thermoelectric elements are then alternately placed on the solder paste-applied positions. The particles are placed as close as possible to the edges of the copper conductive plates to avoid solder paste precipitation during bonding, which could cause a short circuit. Subsequently, another layer of solder paste is applied to the corresponding positions of each copper conductive plate on the PI-2 film. Finally, the PI-2 film is placed on top of the PI-1 film, and then reflow soldering is performed at a temperature controlled within the range of 138–145 °C.

[0086] Among them, the N-type thermoelectric element is the thin-film thermoelectric material AgCu in Example 4. 0.97 Se 0.98 S 0.02 Ce 0.03 Its dimensions are 4 mm × 4 mm × 30 μm. The material of the P-type thermoelectric element is (AgCu). 0.999 Te 0.69 Se 0.3 S0.01 The dimensions of the P-type thermoelectric element are 4 mm × 4 mm × 35 μm.

[0087] The relationship between output voltage and output current, and the relationship between output power and output current, of the out-of-plane flexible thermoelectric device under different temperature differences were tested. The results are as follows: Figure 12 As shown.

[0088] When the input current in the circuit is 0, the test circuit is equivalent to an open circuit, and the device's output voltage is the open-circuit voltage. When the voltage across the external load resistor is 0, it is equivalent to the thermoelectric device being directly connected by a wire. In this case, the resistance connected to the entire circuit is only the internal resistance of the device, and the resulting current is the maximum current in the circuit. Therefore, it can be... Figure 12 The internal resistance of the flexible thermoelectric device was calculated to be approximately 160 mΩ by averaging the absolute values ​​of the slopes of multiple output voltage versus output current curves. This internal resistance is further calculated by considering the temperature difference (…). As the temperature difference (T) increases, the open-circuit voltage and maximum current of the flexible thermoelectric device continuously increase. At an actual temperature difference of 3.93 K, the open-circuit voltage reaches 5.66 V, and the open-circuit current exceeds 30 mA. Under this temperature difference, the maximum power of the flexible device can reach 43.5 μW, and its maximum normalized power density reaches 0.8 μWcm². -2 K -2 This indicates that the thermoelectric materials prepared above have very promising application prospects.

[0089] In summary, this invention provides a thermoelectric material, its preparation method, and a thermoelectric device. Compared to the thermoelectric material AgCuSe, the thermoelectric material provided by this invention exhibits higher electrical conductivity and power factor. Specifically, the embodiments of this invention improve the electrical transport properties and enhance the electrical conductivity and power factor of the thermoelectric material AgCuSe by performing synergistic doping with S and Ce or synergistic doping with S and Zn.

[0090] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.

Claims

1. A thermoelectric material, characterized in that, The chemical formula of the thermoelectric material is AgCu. 1-x Se 1-γ S γ M x M is Zn or Ce; When M is Zn, 0.01≤x≤0.04, 0.01≤γ≤0.04; When M is Ce, 0.02≤x≤0.04, 0.01≤γ≤0.

04.

2. The thermoelectric material according to claim 1, characterized in that, The chemical formula of the thermoelectric material is AgCu. 0.99 Se 0.98 S 0.02 Zn 0.01 AgCu 0.98 Se 0.98 S 0.02 Zn 0.02 AgCu 0.97 Se 0.98 S 0.02 Zn 0.03 AgCu 0.96 Se 0.98 S 0.02 Zn 0.04 AgCu 0.98 Se 0.98 S 0.02 Ce 0.02 AgCu 0.97 Se 0.98 S 0.02 Ce 0.03 or AgCu 0.96 Se 0.98 S 0.02 Ce 0.04 .

3. A method for preparing the thermoelectric material according to claim 1, characterized in that, Includes the following steps: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, then melting and cooling them to obtain a block-shaped thermoelectric material.

4. A method for preparing the thermoelectric material according to claim 1, characterized in that, Includes the following steps: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder and M particles, melting them, and cooling them to obtain a block-shaped thermoelectric material. The block-shaped thermoelectric material is subjected to deformation heat treatment to extend the block-shaped thermoelectric material and obtain a thin film-shaped thermoelectric material.

5. The method for preparing the thermoelectric material according to claim 4, characterized in that, The deformation heat treatment is performed at a temperature of 323~470 K and at a pressure of 10~1000 MPa.

6. The method for preparing the thermoelectric material according to claim 3 or 4, characterized in that, According to AgCu 1-x Se 1-γ S γ M x The specific steps for smelting Ag particles, Cu particles, Se particles, sulfur powder, and M particles, based on the stoichiometric ratio of each element, include: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, placing them in a first container, and then sealing the first container after evacuating it. The sealed first container was placed in a muffle furnace for melting.

7. The method for preparing the thermoelectric material according to claim 3 or 4, characterized in that, According to AgCu 1-x Se 1-γ S γ M x The specific steps for smelting Ag particles, Cu particles, Se particles, sulfur powder, and M particles, based on the stoichiometric ratio of each element, include: According to AgCu 1-x Se 1-γ S γ M x The stoichiometric ratio of each element in the mixture is determined by mixing Ag particles, Cu particles, Se particles, sulfur powder, and M particles, placing them in a first container, and then sealing the first container after evacuating it. Place the sealed first container into the second container, and then evacuate and seal the second container. The sealed second container was placed in a muffle furnace for melting.

8. The method for preparing the thermoelectric material according to claim 7, characterized in that, The inner wall of the first container is coated with a carbon film.

9. The method for preparing the thermoelectric material according to claim 7, characterized in that, The process parameters for smelting are as follows: First, heat the material to 200-400 ℃ at a rate of 1-10 ℃ / min and hold it at 200-400 ℃ for 240 min. Then, heat the material to 1100-1300 ℃ at a rate of 0.1-20 ℃ / min and hold it at 1100-1300 ℃ for 720 min. Next, cool the material to 450-550 ℃ at a rate of 0.1-10 ℃ / min and hold it at 450-550 ℃ for 2 days. Finally, cool the material to room temperature at a rate of 1-20 ℃ / min.

10. A thermoelectric device, said thermoelectric device comprising alternating N-type thermoelectric elements and P-type thermoelectric elements, characterized in that, The N-type thermoelectric element comprises the thermoelectric material as described in any one of claims 1-2.