High-temperature-resistant high-adhesion graphite-fluororesin composite wear-resistant coating and preparation method thereof
By forming a protective structure of an inner layer of silica and an outer layer of alumina on the graphite surface, and using PAI, PPS and PFA materials in the composite underlayer, the problems of oxidation and insufficient adhesion of graphite-fluororesin coatings under high temperature conditions are solved, and the high temperature stability and wear resistance of the coating are achieved.
Patent Information
- Application Number
- CN202611425996.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-10
AI Technical Summary
Existing graphite-fluororesin composite coatings are prone to oxidation and reduced lubrication performance under high temperature conditions, and their adhesion to metal substrates is weak, which leads to microcracks and reduced adhesion during thermal cycling.
A gradient shell modified graphite method is adopted, which forms a protective structure of an inner silica layer and an outer alumina layer on the graphite surface, and uses PAI, PPS and PFA materials in the composite underlayer to form a continuous transition layer, thereby improving the high-temperature structural stability and adhesion of the coating.
It effectively extends the oxidation path of graphite flakes, reduces local filler enrichment, improves the wear resistance and adhesion of the coating, alleviates microcracks caused by thermal cycling, and ensures that the coating maintains its integrity under high temperature and thermal cycling conditions.
Smart Images

Figure CN123063013A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating technology, specifically to a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating and its preparation method. Background Technology
[0002] Graphite-fluororesin composite coatings combine low friction, chemical resistance, and wear resistance, making them suitable for surface protection of high-temperature equipment components, molds, valves, pump bodies, and friction-moving parts. Fluororesin forms a continuous, dense protective film, while graphite, through its layered structure, slips during friction, thereby reducing frictional resistance and surface wear.
[0003] Under high-temperature operating conditions, graphite edges and crystal defects are prone to oxidation upon contact with oxygen, causing the graphite sheets to gradually lose their integrity and thus reducing the coating's lubrication and wear resistance. Simultaneously, graphite has poor surface wettability and tends to distribute unevenly in water-based fluoropolymer systems. If localized graphite agglomeration occurs, filler-rich zones may form within the coating, affecting the continuous film formation of the fluoropolymer. Therefore, improving the high-temperature stability of graphite requires effective protection of its easily oxidized areas without excessively covering the graphite slip surfaces or disrupting its solid lubrication properties.
[0004] Fluoropolymers have low surface energy and weak interfacial interactions with metal substrates such as steel. The rough surface structure created solely by ordinary sandblasting is insufficient to guarantee stable adhesion of the coating under high temperatures, shear loads, and repeated temperature fluctuations. While adding highly polar, high-stiffness, heat-resistant adhesives can improve initial adhesion, excessive amounts can weaken the continuous phase of the fluoropolymer and potentially create significant differences in stiffness and thermal deformation between the underlayer and toplayer.
[0005] When a heat-resistant inorganic protective layer forms on the graphite surface, the local stiffness of the graphite particles increases and their thermal expansion decreases. Simultaneously, the highly adhesive underlayer strengthens the constraint between the top layer and the metal substrate. When the coating cools from its high film-forming temperature or undergoes repeated temperature fluctuations during use, the thermal shrinkage generated by the fluoropolymer matrix is difficult to fully release through interfacial slippage, easily leading to localized stress concentrations around the modified graphite particles and in the transition area between the underlayer and the top layer. Repeated accumulation of this stress may generate microcracks at the thermal cycling interface, reducing the coating's adhesion retention.
[0006] Therefore, the technical problem to be solved by this invention is how to improve the high-temperature structural stability and adhesion to metal substrates of the graphite-fluororesin composite wear-resistant coating while maintaining the continuous film formation of fluororesin and the lubricating effect of graphite during processing, and at the same time alleviate the micro-cracks at the thermal cycling interface caused by the mutual constraint between the heat-resistant graphite structure and the high adhesion interface, thereby obtaining a composite coating that can maintain integrity, adhesion, and wear resistance under high temperature and repeated thermal cycling conditions. Summary of the Invention The purpose of this invention is to provide a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating and its preparation method, so as to solve the technical problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating includes the following steps: (1) Surface activation of flake graphite in an ozone atmosphere; pre-hydrolysis of tetraethyl orthosilicate under acidic conditions, and condensation of the pre-hydrolysis product on the surface of activated flake graphite under weakly alkaline conditions to form a silica inner layer; using aluminum nitrate as aluminum source and urea as uniform precipitant, hydrated alumina is deposited on the surface of the silica inner layer, and after washing, drying and heat treatment in an inert atmosphere, modified graphite with a silica inner layer and an alumina outer layer from the inside out is obtained. (2) A water-based aromatic polyamide-imide precursor, polyphenylene sulfide micro powder and perfluoroalkoxy resin aqueous dispersion are mixed to prepare a primer coating. The primer coating is applied to the surface of a pretreated metal substrate and subjected to segmented heat treatment to form a composite underlayer. (3) The modified graphite, cordierite powder, acicular wollastonite and perfluoroalkoxy resin aqueous dispersion are mixed to form a topcoat, and the topcoat is applied to the composite substrate. After drying and melting sintering, the graphite-fluororesin composite wear-resistant coating is obtained.
[0008] Preferably, in step (1), the purity of the flake graphite is not less than 99%, and the D50 is 3-8 μm; The surface activation is carried out at 25-35°C, the ozone volume concentration in the ozone-containing atmosphere is 1500-2500 ppm, the oxygen content is not higher than 10%, the balance is nitrogen, and the treatment time is 30-45 min. The flow rate of the ozone-containing atmosphere is calculated as 1.5 to 2.5 L / min per 100g of flake graphite.
[0009] Preferably, in step (1), the amount of tetraethyl orthosilicate used is 6.9 to 13.9 parts by mass, based on 100 parts by mass of flake graphite; The tetraethyl orthosilicate is dissolved in ethanol and hydrolysate containing hydrochloric acid is added. The mixture is pre-hydrolyzed at 35-45°C for 45-60 min. The molar ratio of water to tetraethyl orthosilicate is 6-8:1 and the molar ratio of hydrochloric acid to tetraethyl orthosilicate is 0.005-0.015:1. The obtained pre-hydrolyzed product was added to the activated flake graphite dispersion, and the apparent pH of the system was adjusted to 8.0–8.8 with ammonia water. The reaction was carried out at 28–35 °C for 4–6 h.
[0010] Preferably, in step (1), based on 100 parts by mass of flake graphite, the flake graphite with the silica inner layer formed is dispersed in water, and 22.1 to 36.8 parts by mass of aluminum nitrate nonahydrate and urea are added to the system to make Al... 3+ The concentration is 0.05–0.10 mol / L, urea and Al 3+ The molar ratio is 6–9:1; the reaction is carried out at 90–95℃ for 3–5 h, and the final pH of the system is made to reach 6.0–7.0; the mixture is filtered and washed with water until the conductivity of the final washing solution is not higher than 200 μS / cm, dried at 105–120℃ for 6–8 h, and then heated to 530–560℃ at 2℃ / min and held for 2–3 h in a nitrogen atmosphere with an oxygen content of less than 100 ppm.
[0011] Preferably, in step (2), based on the total dry solids of the perfluoroalkoxy resin, polyamide-imide and polyphenylene sulfide as 100 parts by weight, the perfluoroalkoxy resin is 45-55 parts by weight, the polyamide-imide is 20-30 parts by weight, the polyphenylene sulfide is 20-30 parts by weight, and the sum of the three is 100 parts by weight. The solid content of the perfluoroalkoxy resin aqueous dispersion is 50-60% by mass and the pH is 9-10. The aqueous aromatic polyamide-imide precursor is an aqueous precursor that has been neutralized by amine and contains ammonium acid units that can be further imidized. The D50 of the polyphenylene sulfide micro powder is 3-8 μm.
[0012] Preferably, in step (2), the metal substrate is a carbon steel substrate or a stainless steel substrate; after the metal substrate is degreased, washed and dried, it is sandblasted with 60-100 mesh alumina abrasive to make its surface roughness Ra 3-5 μm; The dry film thickness of the composite substrate is 8-12 μm, and the segmented heat treatment sequentially includes holding at 60°C for 10 min, holding at 90°C for 20 min, holding at 160°C for 20 min, and holding at 250°C for 15 min.
[0013] Preferably, in step (3), based on 100 parts by weight of perfluoroalkoxy resin dry resin, the amount of modified graphite is 15-20 parts by weight, the amount of cordierite powder is 4-7 parts by weight, and the amount of acicular wollastonite is 2-5 parts by weight. The cordierite powder is a sintered cordierite powder with a D50 of 3-5 μm and a D90 of no more than 12 μm. The needle-shaped wollastonite has a D50 of 2.5–5 μm, a D98 of no more than 20 μm, and an aspect ratio of 5–10.
[0014] Preferably, in step (3), the modified graphite and cordierite powder are first pre-dispersed in water, then the perfluoroalkoxy resin aqueous dispersion is added and mixed at a speed not exceeding 300 r / min, then needle-shaped wollastonite is added and mixed at 100-200 r / min for 5-10 min, so that the solid content of the obtained surface coating is 40-48% by mass.
[0015] Preferably, in step (3), the topcoat is applied to the composite substrate in 4 to 5 coats, each coat forming a dry film with a thickness of 10 to 15 μm, and dried at 100°C for 10 to 15 min, so that the total thickness of the topcoat is 55 to 70 μm; then, it is kept at 100°C for 20 min, at 200°C for 10 min, heated to 315°C at 3 to 5°C / min and kept for 5 min, and then heated to the measured temperature of the workpiece metal reaching 375 to 385°C and kept for 5 to 8 min, and then cooled to below 150°C at 3 to 5°C / min.
[0016] A high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating is prepared by the above method.
[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. The silica inner layer on the graphite surface exhibits good continuity, covering the edges and defects of the graphite sheets and extending the path for oxygen to enter the graphite surface. The alumina outer layer reinforces the inner layer, reducing the possibility of through-holes forming in the protective layer during drying, sintering, and thermal cycling. The gradient protective structure formed by the inner and outer layers slows down the oxidation of graphite in high-temperature oxygen-containing environments, allowing the graphite sheets to maintain their solid lubrication and load-bearing functions even after prolonged use. Simultaneously, the modified graphite is more easily and uniformly distributed in the water-based PFA system, reducing localized filler enrichment and ensuring continuous PFA film formation. This structure does not increase the decomposition temperature of the PFA molecular chains themselves, but rather improves the structural integrity and wear resistance retention of the coating within the permissible operating temperature range of PFA.
[0018] 2. The composite underlayer composed of PAI, PPS, and PFA forms a continuous transition between the metal substrate and the graphite-containing top layer. The side closest to the metal substrate, with its high polarity PAI as the main load-bearing component, can fully wet the micro-uneven structure formed after sandblasting. PPS maintains good strength and dimensional stability at high temperatures, capable of bearing the shear load transferred from the top layer to the underlayer. The PFA contained on the outer side of the underlayer can melt together with the PFA in the top layer during final sintering, creating a continuous weld zone between the underlayer and the top layer. Therefore, when the coating is subjected to friction or thermal cycling, the external load can be gradually transferred to the metal substrate, avoiding the concentration of all load on a single interface, thereby improving the initial adhesion and adhesion retention of the coating after high-temperature use.
[0019] 3. The heat-resistant shell layer increases the edge stiffness of graphite particles and reduces their local thermal expansion, while the composite underlayer firmly binds the top layer to the metal substrate. When the coating cools from a high-temperature sintering state, or undergoes repeated heating and cooling during use, the thermal expansion and contraction of the PFA matrix cannot be fully released through interfacial slippage. This leads to thermal deformation differences concentrating around the modified graphite particles and in the transition area between the underlayer and the top layer. These thermal stresses accumulate repeatedly at the edges of the graphite particles and in the interlayer transition area, causing local stresses to exceed the bearing capacity of the PFA matrix or interface, thus initiating fine cracks. As the number of thermal cycles increases, the cracks gradually expand and connect along the particle-resin interface and the underlayer-top layer transition area during periodic opening and closing, weakening the effective load-bearing area and load transfer capacity of the interface, ultimately forming microcracks at the thermal cycling interface and causing a decrease in the adhesion retention rate of the coating after thermal cycling; in severe cases, local lifting or peeling may occur. Low-expansion cordierite and acicular wollastonite address this problem from two aspects: "reducing stress generation" and "limiting crack propagation," respectively. Uniformly distributed cordierite powder has a low coefficient of thermal expansion, which can limit excessive shrinkage of the surrounding PFA matrix, reduce the effective thermal expansion of the surface layer, and disperse the thermal deformation difference originally concentrated at the edges of a few particles to a larger coating area. However, cordierite is a rigid particle, and when used alone, it mainly reduces stress sources and lacks the ability to bridge existing microcracks. Acicular wollastonite has a large aspect ratio, and its long axis can span the local transition region between the PFA matrix, modified graphite, and cordierite, forming multi-directional load transfer channels within the coating. When local microcracks begin to form, acicular wollastonite can bear part of the tensile and shear loads on both sides of the crack, reduce the stress intensity at the crack tip, and cause the crack to deflect, bifurcate, or terminate. However, when used alone, it cannot fundamentally reduce the thermal deformation difference between the PFA matrix and rigid particles. When used together, cordierite first reduces the driving force for microcracks generated during thermal cycling, while acicular wollastonite further disperses residual stress and prevents the continued propagation of microcracks. This forms a continuous process of "reducing thermal deformation difference—transferring interfacial load—bridging crack regions," thereby alleviating the microcracks at the thermal cycling interface and the resulting decrease in adhesion retention. Because the amounts of the two structural phases are controlled, PFA can still maintain continuous film formation and will not form a brittle surface layer due to excessive inorganic material content. Attached Figure Description
[0020] Figure 1 This is a low-magnification SEM image of the cross-section of the high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating prepared in Example 1 of the present invention.
[0021] Figure 2 This is a high-magnification SEM image of the cross-section of the high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating prepared in Example 1 of the present invention. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Example 1 A method for preparing a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating includes the following steps: 1. Preparation of Gradient Shell Modified Graphite 100.0g of natural flake graphite with a purity of 99.0% and a D50 of 3μm was placed in a grounded, sealed drum reactor. A mixed gas with an ozone volume concentration of 1500ppm, an oxygen content of 10% (by volume), and the remainder being nitrogen was introduced at 25℃ at a rate of 1.5L / min, and the reactor was agitated for 30 minutes. After treatment, nitrogen was introduced for purging for 20 minutes, and the exhaust gas was treated by an ozone decomposition device.
[0024] Dissolve 6.900 g of tetraethyl orthosilicate in 30.000 g of anhydrous ethanol. Mix 2.982 g of deionized water with 0.604 g of 1% hydrochloric acid solution, and add the mixture dropwise to the tetraethyl orthosilicate solution over 15 min. Stir at 35 °C for 45 min. The molar ratio of water to tetraethyl orthosilicate is 6:1, and the molar ratio of hydrochloric acid to tetraethyl orthosilicate is 0.005:1.
[0025] All activated graphite was added to 80,000 g of anhydrous ethanol and dispersed at 1200 r / min for 20 min. The pre-hydrolyzed solution was added over 45 min, followed by the addition of 0.160 g of 2% ammonia solution in batches to adjust the apparent pH of the system to 8.0. The mixture was stirred at 28 °C for 4 h. After filtration, the graphite was washed twice with a 1:1 mixture of 200 g of ethanol and water each time, followed by two washes with 200 g of deionized water each time. The graphite was then vacuum dried at 80 °C for 4 h.
[0026] Dissolve 22.100g of aluminum nitrate nonahydrate and 21.230g of urea in deionized water and bring the volume to 1.178L, so that Al 3+ A concentration of 0.050 mol / L, urea and Al 3+ The molar ratio was 6:1. All the silica-coated graphite was added, and the mixture was refluxed and stirred at 90°C until the pH reached 6.0, with a total holding time of 3 hours. After filtration, the mixture was washed four times with 500g of deionized water each time, ensuring the conductivity of the final wash solution did not exceed 200μS / cm.
[0027] The resulting filter cake was dried at 105℃ for 6 hours and slightly depolymerized. Nitrogen gas with a purity of not less than 99.9% was introduced at 1.0 L / min for 30 minutes to purge the oxygen content in the furnace to below 100 ppm. The temperature was then increased to 530℃ at 2℃ / min and held for 2 hours. Finally, the temperature was cooled to below 100℃ under nitrogen protection to obtain modified graphite.
[0028] 2. Preparation of the composite substrate The Q235 carbon steel substrate was subjected to alkaline degreasing, water washing and drying in sequence, and sandblasted with 60-mesh alumina abrasive to achieve a surface roughness Ra of 3μm. Construction was carried out within 2 hours after dust removal.
[0029] Mix 58.57 g of deionized water with 71.43 g of amine-neutralized aqueous aromatic polyamide-imide precursor with a solid content of 35% and stir at 500 r / min for 5 min; add 30.00 g of polyphenylene sulfide micro powder with a D50 of 3 μm within 10 min and continue to disperse for 20 min; reduce the speed to 300 r / min and add 90.00 g of perfluoroalkoxy resin aqueous dispersion with a solid content of 50% and a pH of 9.0 within 10 min and continue to stir for 10 min.
[0030] The resulting primer contains 45.00g of perfluoroalkoxy resin dry solids, 25.00g of polyamide-imide dry solids and 30.00g of polyphenylene sulfide, with a total dry solids content of 100.00g and a primer solids content of 40%.
[0031] After filtering, the primer was sprayed onto the substrate surface, and the dry film thickness of the bottom layer was controlled to be 8 μm. The substrate was then kept at 60°C for 10 min, 90°C for 20 min, 160°C for 20 min, and 250°C for 15 min, and then cooled to room temperature.
[0032] 3. Preparation of surface layer and coating layer 81.50g of deionized water, 15.00g of the modified graphite described above, and 4.00g of sintered cordierite powder with a D50 of 3μm and a D90 of 12μm were mixed and dispersed at 1200r / min for 15min. The rotation speed was reduced to 300r / min, and 200.00g of perfluoroalkoxy resin aqueous dispersion with a solid content of 50% was slowly added and stirred for 10min. Then, 2.00g of acicular wollastonite with a D50 of 2.5μm, a D98 of 12μm, and an aspect ratio of 5 was added and stirred at 100r / min for 5min to obtain a topcoat with a solid content of 40%.
[0033] The topcoat was sprayed onto the composite substrate in 5 coats, with dry film thicknesses of 10μm, 10μm, 10μm, 10μm and 15μm for each coat, respectively. Each coat was dried at 100℃ for 10 minutes after spraying, and the total dry film thickness of the topcoat was 55μm.
[0034] After spraying, maintain the temperature at 100℃ for 20 minutes, at 200℃ for 10 minutes, increase the temperature to 315℃ at 3℃ / min and maintain it for 5 minutes, continue to increase the temperature to the actual measured temperature of the workpiece metal at 375℃ and maintain it for 5 minutes, then cool it to below 150℃ at 3℃ / min, and then allow it to cool naturally.
[0035] Example 2 A method for preparing a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating includes the following steps: 1. Preparation of Gradient Shell Modified Graphite 100.0 g of natural flake graphite with a purity of 99.5% and a D50 of 5.5 μm was placed in a grounded, sealed drum reactor. A mixed gas with an ozone volume concentration of 2000 ppm, an oxygen content of 9% (by volume), and the remainder being nitrogen was introduced at 2.0 L / min at 30 °C, and the reactor was agitated for 35 min. After treatment, nitrogen was introduced for purging for 20 min.
[0036] Dissolve 10.400 g of tetraethyl orthosilicate in 40.000 g of anhydrous ethanol. Mix 4.493 g of deionized water with 1.820 g of 1% hydrochloric acid solution, and add the mixture dropwise to the tetraethyl orthosilicate solution over 18 min. Stir at 40 °C for 52 min. The molar ratio of water to tetraethyl orthosilicate is 7:1, and the molar ratio of hydrochloric acid to tetraethyl orthosilicate is 0.010:1.
[0037] All activated graphite was added to 100,000 g of anhydrous ethanol and dispersed at 1200 r / min for 20 min. The pre-hydrolyzed solution was added over 50 min, followed by the addition of 0.450 g of 2% ammonia solution in batches to adjust the apparent pH of the system to 8.4. The mixture was stirred at 32 °C for 5 h. After filtration, the graphite was washed twice with a 1:1 mixture of 200 g of ethanol and water, followed by two washes with 200 g of deionized water each time. The graphite was then vacuum dried at 80 °C for 4 h.
[0038] Dissolve 33.100g of aluminum nitrate nonahydrate and 39.750g of urea in deionized water and bring the volume to 1.176L, so that Al 3+ A concentration of 0.075 mol / L, urea and Al 3+ The molar ratio was 7.5:1. All the silica-coated graphite was added, and the mixture was refluxed and stirred at 93°C until the pH reached 6.5, with a total holding time of 4 hours. After filtration, the mixture was washed four times with 500g of deionized water each time, ensuring the conductivity of the final wash solution did not exceed 200μS / cm.
[0039] The obtained filter cake was dried at 112℃ for 7 hours. Nitrogen gas with a purity of not less than 99.9% was introduced at 1.0 L / min for 30 minutes to replace the oxygen content in the furnace and reduce it to less than 100 ppm. The temperature was then increased to 545℃ at 2℃ / min and held for 2.5 hours. Finally, the temperature was cooled to below 100℃ under nitrogen protection to obtain modified graphite.
[0040] 2. Preparation of the composite substrate The 304 stainless steel substrate was subjected to alkaline degreasing, water washing and drying in sequence, and sandblasted with 80-mesh alumina abrasive to achieve a surface roughness Ra of 4μm. Construction was carried out within 2 hours after dust removal.
[0041] 41.47 g of deionized water was mixed with 85.71 g of amine-neutralized aqueous aromatic polyamide-imide precursor with a solid content of 35%, and stirred at 850 r / min for 5 min. 20.00 g of polyphenylene sulfide micro powder with a D50 of 5 μm was added within 10 min, and dispersion was continued for 20 min. The stirring speed was reduced to 250 r / min, and 90.91 g of perfluoroalkoxy resin aqueous dispersion with a solid content of 55% and a pH of 9.5 was added within 10 min, and stirring was continued for 10 min.
[0042] The resulting primer contains 50.00g of perfluoroalkoxy resin dry solids, 30.00g of polyamide-imide dry solids and 20.00g of polyphenylene sulfide, with a total dry solids content of 100.00g and a primer solids content of 42%.
[0043] After filtering, the primer was sprayed onto the substrate surface, and the dry film thickness of the bottom layer was controlled to be 10 μm. The substrate was then kept at 60°C for 10 min, 90°C for 20 min, 160°C for 20 min, and 250°C for 15 min, and then cooled to room temperature.
[0044] 3. Preparation of surface layer and coating layer 79.82 g of deionized water, 18.00 g of the modified graphite described above, and 5.50 g of sintered cordierite powder with a D50 of 4 μm and a D90 of 10 μm were mixed and dispersed at 1200 r / min for 15 min. The rotation speed was reduced to 250 r / min, and 181.82 g of perfluoroalkoxy resin aqueous dispersion with a solid content of 55% was slowly added and stirred for 10 min. Then, 3.50 g of acicular wollastonite with a D50 of 4 μm, a D98 of 15 μm, and an aspect ratio of 8 was added and stirred at 150 r / min for 8 min to obtain a topcoat with a solid content of 44%.
[0045] The topcoat was sprayed onto the composite substrate in 5 coats, each coat having a dry film thickness of 12.5 μm. After each coat, it was dried at 100℃ for 12 min, resulting in a total dry film thickness of 62.5 μm.
[0046] After spraying, maintain the temperature at 100℃ for 20 minutes, at 200℃ for 10 minutes, increase the temperature to 315℃ at 4℃ / min and maintain it for 5 minutes, continue to increase the temperature to the actual measured temperature of the workpiece metal of 380℃ and maintain it for 6.5 minutes, then cool it to below 150℃ at 4℃ / min, and then allow it to cool naturally.
[0047] Example 3 A method for preparing a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating includes the following steps: 1. Preparation of Gradient Shell Modified Graphite 100.0g of natural flake graphite with a purity of 99.5% and a D50 of 8μm was placed in a grounded, sealed drum reactor. A mixed gas with an ozone volume concentration of 2500ppm, an oxygen content of 8% (by volume), and the remainder being nitrogen was introduced at 35℃ at a rate of 2.5L / min, and the reactor was agitated for 45min. After the treatment, nitrogen was introduced to purge for 20min.
[0048] Dissolve 13.900 g of tetraethyl orthosilicate in 50.000 g of anhydrous ethanol. Mix 6.003 g of deionized water with 3.649 g of 1% hydrochloric acid solution, and add the mixture dropwise to the tetraethyl orthosilicate solution over 20 min. Stir at 45 °C for 60 min. The molar ratio of water to tetraethyl orthosilicate is 8:1, and the molar ratio of hydrochloric acid to tetraethyl orthosilicate is 0.015:1.
[0049] All activated graphite was added to 120,000 g of anhydrous ethanol and dispersed at 1200 r / min for 20 min. The pre-hydrolyzed solution was added over 60 min, followed by the addition of 0.900 g of 2% ammonia solution in batches to adjust the apparent pH of the system to 8.8. The mixture was stirred at 35 °C for 6 h. After filtration, the graphite was washed twice with a 1:1 mixture of 250 g of ethanol and water, followed by two washes with 250 g of deionized water each time. The graphite was then vacuum dried at 80 °C for 4 h.
[0050] Dissolve 36.800g of aluminum nitrate nonahydrate and 53.030g of urea in deionized water and bring the volume to 0.981L, so that Al 3+ A concentration of 0.100 mol / L, urea and Al 3+ The molar ratio was 9:1. All the silica-coated graphite was added, and the mixture was refluxed and stirred at 95°C until the pH reached 7.0, with a cumulative holding time of 5 hours. After filtration, the mixture was washed five times with 500g of deionized water each time, ensuring the conductivity of the final wash solution did not exceed 200μS / cm.
[0051] The obtained filter cake was dried at 120℃ for 8 hours. Nitrogen gas with a purity of not less than 99.9% was introduced at 1.0 L / min for 30 minutes to replace the oxygen content in the furnace and reduce it to less than 100 ppm. The temperature was then increased to 560℃ at 2℃ / min and held for 3 hours. Finally, the temperature was cooled to below 100℃ under nitrogen protection to obtain modified graphite.
[0052] 2. Preparation of the composite substrate The Q235 carbon steel substrate was subjected to alkaline degreasing, water washing and drying in sequence, and sandblasted with 100-mesh alumina abrasive to achieve a surface roughness Ra of 5μm. Construction was carried out within 2 hours after dust removal.
[0053] 76.19 g of deionized water was mixed with 57.14 g of amine-neutralized aqueous aromatic polyamide-imide precursor with a solid content of 35%, and stirred at 1200 r / min for 5 min. 25.00 g of polyphenylene sulfide micro powder with a D50 of 8 μm was added within 10 min, and dispersion was continued for 20 min. The stirring speed was reduced to 300 r / min, and 91.67 g of perfluoroalkoxy resin aqueous dispersion with a solid content of 60% and a pH of 10.0 was added within 10 min, and stirring was continued for 10 min.
[0054] The resulting primer contains 55.00g of perfluoroalkoxy resin dry solids, 20.00g of polyamide-imide dry solids and 25.00g of polyphenylene sulfide, with a total dry solids content of 100.00g and a primer solids content of 40%.
[0055] After filtering, the primer was sprayed onto the substrate surface, and the dry film thickness of the bottom layer was controlled to be 12 μm. The substrate was then kept at 60°C for 10 min, 90°C for 20 min, 160°C for 20 min, and 250°C for 15 min, and then cooled to room temperature.
[0056] 3. Preparation of surface layer and coating layer 76.33 g of deionized water, 20.00 g of the modified graphite described above, and 7.00 g of sintered cordierite micro powder with a D50 of 5 μm and a D90 of 12 μm were mixed and dispersed at 1200 r / min for 15 min. The rotation speed was reduced to 300 r / min, and 166.67 g of perfluoroalkoxy resin aqueous dispersion with a solid content of 60% was slowly added and stirred for 10 min. 5.00 g of needle-shaped wollastonite with a D50 of 5 μm, a D98 of 20 μm, and an aspect ratio of 10 was added and stirred at 200 r / min for 10 min to obtain a topcoat with a solid content of 48%.
[0057] The topcoat was sprayed onto the composite substrate in 5 coats, with dry film thicknesses of 15μm, 15μm, 15μm, 15μm and 10μm for each coat, respectively. Each coat was dried at 100℃ for 15 minutes after spraying, and the total dry film thickness of the topcoat was 70μm.
[0058] After spraying, maintain the temperature at 100℃ for 20 minutes, at 200℃ for 10 minutes, increase the temperature to 315℃ at 5℃ / min and maintain it for 5 minutes, continue to increase the temperature to the actual measured temperature of the workpiece metal at 385℃ and maintain it for 8 minutes, then cool it to below 150℃ at 5℃ / min, and then allow it to cool naturally.
[0059] Comparative Example 1: Compared with Example 1, 15.0g of flake graphite of the same specification that has not been ozone activated and treated with silica-alumina composite coating was used to replace 15.0g of modified graphite. The amount of other raw materials, preparation steps and process parameters were the same as in Example 1.
[0060] Comparative Example 2: Compared with Example 1, after ozone activation and silica inner layer coating, the flake graphite was directly subjected to nitrogen heat treatment according to the conditions of Example 1, without the step of uniform precipitation of aluminum nitrate-urea to form an alumina outer layer. The remaining raw material amounts, preparation steps and process parameters were the same as in Example 1.
[0061] Comparative Example 3: Compared with Example 1, the composite primer was replaced with a pure PFA primer composed of 200.0g of PFA aqueous dispersion with a solid content of 50% and 50.0g of deionized water, while maintaining the bottom dry film thickness at 8μm. The remaining raw material amounts, preparation steps and process parameters were the same as in Example 1.
[0062] Comparative Example 4: Compared with Example 1, 4.0g of low-expansion cordierite and 2.0g of needle-shaped wollastonite were not added to the topcoat, the amount of 100.0g of PFA dry resin and 15.0g of modified graphite remained unchanged, and the amount of deionized water was adjusted so that the solid content of the topcoat was still 40%. The remaining preparation steps and process parameters were the same as in Example 1.
[0063] Comparative Example 5: Compared with Example 1, 6.0g of low-expansion cordierite of the same specification as in Example 1 was added to the topcoat without adding acicular wollastonite, so that the total amount of structural functional phase was kept at 6.0g. The amount of other raw materials, preparation steps and process parameters were the same as in Example 1.
[0064] Comparative Example 6: Compared with Example 1, 6.0g of needle-shaped wollastonite of the same specification as in Example 1 was added to the topcoat, but low-expansion cordierite was not added, so that the total amount of structural functional phase was kept at 6.0g. The amount of other raw materials, preparation steps and process parameters were the same as in Example 1.
[0065] Performance testing 1. Initial pull-off adhesion: The single-sided pull-off method was used according to GB / T 5210—2006. Without abrading the surface layer, the bonding area was lightly and evenly roughened with P600 sandpaper and dust was removed. A 20mm diameter steel test column was bonded with a room-temperature cured two-component epoxy adhesive with a rated adhesive strength of not less than 12MPa. The column was cured at (23±2)℃ for 24 hours. The coating was then cut through to the substrate along the perimeter of the test column using the same cutting tool, ensuring the tensile stress was perpendicular to the test plate and continuously increased at a rate not exceeding 1MPa / s, with failure occurring within 90s. The adhesion strength was calculated by dividing the breaking force by the bonding area of the test column and expressed in MPa. The location of failure—substrate / base layer, base layer / top layer, or inside the coating—was recorded. If prior failure occurred between the adhesive and the test column or between the adhesive and the coating surface, this test point was not considered the coating adhesion result, and a new sample was prepared for testing.
[0066] 2. 260℃ Heat Aging Resistance: Following the general procedure of GB / T 1735—2009, three independent test plates were vertically placed in a forced-air constant-temperature oven with exhaust ventilation, with a spacing of not less than 20mm between the plates. The oven was continuously maintained at (260±2)℃ for 168 hours, with the temperature overshoot controlled to not exceed 3℃. After the test, the test plates were removed and allowed to recover in a standard environment for 24 hours. Bubbling, cracking, and peeling were checked. The pull-off adhesion after heat aging was then determined according to the aforementioned method of GB / T 5210—2006. The adhesion strength point values after recovery are recorded in the table. The adhesion retention rate after heat aging is calculated as "adhesion strength after heat aging ÷ initial adhesion strength × 100%". 260℃ is a condition specified in this test and should not be used to infer long-term continuous use capability at higher temperatures.
[0067] 3. Adhesion and interfacial microcracks after thermal cycling: Referring to the change rate of Nb specified in GB / T 2423.22—2012, and adopting the thermal cycling severity agreed in this case: the test plate was held at (25±2)℃ for 30 min, then increased to (260±2)℃ at (5±1) K / min, and held at 258℃ for 30 min after the test plate reached 258℃. Then it was reduced to (25±2)℃ at (5±1) K / min and held for 30 min. One cycle was completed, and a total of 100 cycles were carried out. Water quenching was not used throughout the process. After the last cycle, the samples were placed in a standard environment for 24 hours, and the pull-off adhesion was determined according to GB / T 5210—2006. In addition, cross-sections were cut at equal intervals from each test plate, cut at low speed, cold-mounted, and ground and polished step by step. The interface between the bottom layer and the top layer and the 20μm area on both sides of the interface were observed under a 200x optical microscope. The total length of the observed interface on each test plate was not less than 20mm. The number of cracks with a width of not less than 2μm that intersect with the interface was counted. The interface microcrack density was calculated as "number of cracks ÷ total length of observed interface" and expressed as cracks / mm.
[0068] 4. Abrasion resistance of rotating rubber grinding wheels: Tested according to GB / T 1768—2006, using a 100mm×100mm test plate with a center mounting hole, CS-10 rubber grinding wheels, and a load of 1000g per wheel. The rotation speed of the turntable was controlled at (60±2) r / min. Before the test, the grinding wheels were refurbished with the specified refurbishing medium and refurbished again after 500 revolutions. The dust suction nozzle was 1-2mm away from the test plate, and the negative pressure was controlled at 1.5-1.6kPa. After the test plate was adjusted and weighed, it was worn for 1000 revolutions. The floating debris was removed, the plate was readjusted, and the plate was weighed again to confirm that the wear marks had not penetrated to the metal substrate. The wear amount was expressed as the difference in mass before and after wear, in mg / 1000 revolutions. The arithmetic mean of the three test plates in each group was taken and rounded to 1mg. The smaller the value, the better the wear resistance.
[0069] 5. Steady-state dry friction coefficient: Referring to the sliding block method in GB / T 10006—2021, the coated test plate was fixed horizontally with a bottom area of 40 cm². 2 A slider with a total mass of (200±2)g was used as the loading body. The bottom of the slider was covered with a flat 304 stainless steel sheet of the same batch, which had been cleaned with ethanol and dried, so that the steel sheet and the coating formed a dry friction pair. Under the conditions of (23±2)℃ and (50±5)% relative humidity, the slider was pulled by (100±10)mm / min for 60mm, and the traction force was continuously recorded. The starting peak value was discarded and the average friction force Fd of the stable section was taken. The dynamic friction coefficient was calculated according to μd=Fd / 1.96. Three non-overlapping tracks were selected for each test plate and the clean steel sheet was replaced. The average value of the tracks was taken as the result of the plate.
[0070] 6. Pencil Hardness: Tested according to GB / T 6739—2022, using 9B to 9H drawing pencils from the same manufacturer and batch. After removing the wood, a 5-6 mm complete cylindrical lead was retained, and the end face of the lead was smoothed with P400 sandpaper. The pencil axis was kept at (45±1)° with the coating surface, and a load of (7.35±0.15) N was applied and advanced at a uniform speed for no less than 7 mm. After 30 seconds of testing, the results were observed. For each hardness grade, three parallel tests were conducted in the untested area. The highest pencil hardness, in which at least two tests did not show visible plastic deformation or cohesive failure, was taken as the result of the test plate.
[0071] Table 1: Based on Example 1, its adhesion retention rate after 260℃×168h was 89.9%, and after 100 thermal cycles it was 83.5%, with an abrasion loss of 13 mg / 1000 rpm. Comparative Example 1, without graphite surface activation and composite coating, had corresponding retention rates of 81.4% and 70.0%, respectively, with an abrasion loss of 21 mg / 1000 rpm, and the interfacial microcrack density increased to 0.74 cracks / mm after thermal cycling. Comparative Example 2, which only formed a silica inner layer and lacked an alumina outer layer, fell between the two, with a heat resistance retention rate of 85.3%, a thermal cycling retention rate of 76.0%, and an abrasion loss of 16 mg / 1000 rpm. This progressive relationship is consistent with the structural role of the silica inner layer covering graphite edge defects, and the alumina outer layer further bearing local loads and extending the oxygen diffusion path.
[0072] Comparative Example 3, using a pure PFA underlayer of the same dry film thickness instead of the PAI / PPS / PFA composite underlayer, showed an initial pull-off adhesion of 3.2 MPa, 2.4 MPa after aging at 260°C, and only 1.6 MPa after 100 thermal cycles, significantly lower than the 7.9, 7.1, and 6.6 MPa of Example 1. This difference indicates that the polar wetting zone, load-bearing transition zone, and fusion zone with the PFA surface layer formed by the composite underlayer can gradually transition the mechanical anchoring of the metal surface to a low surface energy layer, thereby reducing abrupt changes in interfacial load.
[0073] Comparative Example 4, without the two mineral phases, exhibited an initial adhesion strength of 8.0 MPa, slightly higher than the 7.9 MPa of Example 1, indicating that the two minerals did not function by simply increasing the initial bond strength. However, after 100 thermal cycles, the adhesion strength of Comparative Example 4 decreased to 5.0 MPa, with a retention rate of only 62.5%, and the interfacial microcrack density reached 0.96 cracks / mm. Comparative Example 5, with only an equal amount of low-expansion cordierite added, showed an increased adhesion strength of 5.9 MPa and a decrease in microcrack density to 0.52 cracks / mm after thermal cycling, indicating that the low-expansion particles can reduce the effective thermal deformation of the surface layer and disperse the stress peaks at the particle edges; however, the particle morphology is difficult to cross the already formed crack zone, thus its ability to inhibit further crack propagation is limited. Comparative Example 6, which only added an equal amount of acicular wollastonite, showed an adhesion strength of 5.5 MPa and a microcrack density of 0.61 cracks / mm after thermal cycling. Acicular particles can cross adjacent particles and local interface regions, bearing part of the tensile and shear loads after crack initiation, causing crack deflection, passivation, or termination. However, they cannot completely eliminate the thermal deformation difference between the PFA surface layer and the rigid particles. In Example 1, after adding 4.0 g of cordierite and 2.0 g of acicular wollastonite, the adhesion strength reached 6.6 MPa and the retention rate reached 83.5% after thermal cycling, while the microcrack density decreased to 0.18 cracks / mm. This demonstrates that both additives act on two consecutive aspects: "reducing crack driving force" and "bridging and limiting crack propagation," respectively, forming a combined advantage of reducing thermal deformation difference, dispersing interface loads, and bridging crack zones. They address the same technical problem: the microcracks at the interface generated by the coupling of strong adhesion constraints and rigid coated particles during thermal cycling.
[0074] Comparative Example 4, lacking cordierite and acicular wollastonite, exhibited the lowest simulated friction coefficient of 0.132. However, its wear rate was 18 mg / 1000 rpm, and its thermal cycling microcrack density was high, indicating that a lower friction coefficient alone does not represent better wear resistance. With increasing amounts of acicular wollastonite and total inorganic structural phases, the pencil hardness of Comparative Example 6 and Example 3 reached 3H, and the wear rate decreased to 14 and 10 mg / 1000 rpm, respectively. However, the steady-state friction coefficient slightly increased to 0.151 and 0.153. This trend aligns with the principle that hard minerals enhance load-bearing and anti-ploughing capabilities while slightly increasing the shear resistance of the mating contact.
[0075] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating, characterized in that, Includes the following steps: (1) Surface activation of flake graphite in an ozone atmosphere; pre-hydrolysis of tetraethyl orthosilicate under acidic conditions, and condensation of the pre-hydrolysis product on the surface of activated flake graphite under weakly alkaline conditions to form a silica inner layer; using aluminum nitrate as aluminum source and urea as uniform precipitant, hydrated alumina is deposited on the surface of the silica inner layer, and after washing, drying and heat treatment in an inert atmosphere, modified graphite with a silica inner layer and an alumina outer layer from the inside out is obtained. (2) A water-based aromatic polyamide-imide precursor, polyphenylene sulfide micro powder and perfluoroalkoxy resin aqueous dispersion are mixed to prepare a primer coating. The primer coating is applied to the surface of a pretreated metal substrate and subjected to segmented heat treatment to form a composite underlayer. (3) The modified graphite, cordierite powder, acicular wollastonite and perfluoroalkoxy resin aqueous dispersion are mixed to form a topcoat, and the topcoat is applied to the composite substrate. After drying and melting sintering, the graphite-fluororesin composite wear-resistant coating is obtained.
2. The preparation method according to claim 1, characterized in that, In step (1), the purity of the flake graphite is not less than 99%, and the D50 is 3-8 μm; The surface activation is carried out at 25-35°C, the ozone volume concentration in the ozone-containing atmosphere is 1500-2500 ppm, the oxygen content is not higher than 10%, the balance is nitrogen, and the treatment time is 30-45 min. The flow rate of the ozone-containing atmosphere is calculated as 1.5 to 2.5 L / min per 100g of flake graphite.
3. The preparation method according to claim 1, characterized in that, In step (1), the amount of tetraethyl orthosilicate used is 6.9 to 13.9 parts by mass based on 100 parts by mass of flake graphite; The tetraethyl orthosilicate is dissolved in ethanol and hydrolysate containing hydrochloric acid is added. The mixture is pre-hydrolyzed at 35-45°C for 45-60 min. The molar ratio of water to tetraethyl orthosilicate is 6-8:1 and the molar ratio of hydrochloric acid to tetraethyl orthosilicate is 0.005-0.015:
1. The obtained pre-hydrolyzed product was added to the activated flake graphite dispersion, and the apparent pH of the system was adjusted to 8.0–8.8 with ammonia water. The reaction was carried out at 28–35 °C for 4–6 h.
4. The preparation method according to claim 1, characterized in that, In step (1), based on 100 parts by mass of flake graphite, the flake graphite with the aforementioned silica inner layer is dispersed in water, and 22.1–36.8 parts by mass of aluminum nitrate nonahydrate and urea are added to the system to make Al... 3+ The concentration is 0.05–0.10 mol / L, urea and Al 3+ The molar ratio is 6–9:1; the reaction is carried out at 90–95℃ for 3–5 h, and the final pH of the system is made to reach 6.0–7.0; the mixture is filtered and washed with water until the conductivity of the final washing solution is not higher than 200 μS / cm, dried at 105–120℃ for 6–8 h, and then heated to 530–560℃ at 2℃ / min and held for 2–3 h in a nitrogen atmosphere with an oxygen content of less than 100 ppm.
5. The preparation method according to claim 1, characterized in that, In step (2), based on the total dry solids of the three components—perfluoroalkoxy resin, polyamide-imide, and polyphenylene sulfide—to be 100 parts by weight, the perfluoroalkoxy resin is 45-55 parts by weight, the polyamide-imide is 20-30 parts by weight, and the polyphenylene sulfide is 20-30 parts by weight, and the sum of the three is 100 parts by weight. The solid content of the perfluoroalkoxy resin aqueous dispersion is 50-60% by mass and the pH is 9-10. The aqueous aromatic polyamide-imide precursor is an aqueous precursor that has been neutralized by amine and contains ammonium acid units that can be further imidized. The D50 of the polyphenylene sulfide micro powder is 3-8 μm.
6. The preparation method according to claim 5, characterized in that, In step (2), the metal substrate is a carbon steel substrate or a stainless steel substrate; after the metal substrate is degreased, washed and dried, it is sandblasted with 60-100 mesh alumina abrasive to make its surface roughness Ra 3-5 μm; The dry film thickness of the composite substrate is 8-12 μm, and the segmented heat treatment sequentially includes holding at 60°C for 10 min, holding at 90°C for 20 min, holding at 160°C for 20 min, and holding at 250°C for 15 min.
7. The preparation method according to claim 1, characterized in that, In step (3), based on 100 parts by weight of perfluoroalkoxy resin dry resin, the amount of modified graphite is 15-20 parts by weight, the amount of cordierite powder is 4-7 parts by weight, and the amount of acicular wollastonite is 2-5 parts by weight. The cordierite powder is a sintered cordierite powder with a D50 of 3-5 μm and a D90 of no more than 12 μm. The needle-shaped wollastonite has a D50 of 2.5–5 μm, a D98 of no more than 20 μm, and an aspect ratio of 5–10.
8. The preparation method according to claim 7, characterized in that, In step (3), the modified graphite and cordierite powder are first pre-dispersed in water, then the perfluoroalkoxy resin aqueous dispersion is added and mixed at a speed not exceeding 300 r / min, then needle-shaped wollastonite is added and mixed at 100-200 r / min for 5-10 min, so that the solid content of the obtained surface coating is 40-48% by mass.
9. The preparation method according to claim 1, characterized in that, In step (3), the topcoat is applied to the composite substrate in 4 to 5 coats, each coat forming a dry film with a thickness of 10 to 15 μm, and dried at 100°C for 10 to 15 min, so that the total thickness of the topcoat is 55 to 70 μm; then, it is kept at 100°C for 20 min, then at 200°C for 10 min, then heated to 315°C at 3 to 5°C / min and kept for 5 min, then heated to the measured temperature of the workpiece metal reaching 375 to 385°C and kept for 5 to 8 min, and then cooled to below 150°C at 3 to 5°C / min.
10. A high-temperature resistant, high-adhesion graphite-fluororesin composite wear-resistant coating, characterized in that, It is prepared by the method described in any one of claims 1 to 9 above.