5-Hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating and its preparation method
By introducing HMF modification into lignin molecules, a dual-mode self-healing mechanism of furan ring and hydroxymethyl group is constructed, which solves the problem that existing lignin-based coatings require temperature-triggered repair. It achieves preliminary repair at room temperature and complete repair under heating, thereby improving the protective performance and applicability of the coating.
Patent Information
- Application Number
- CN202611280648.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-23
- Publication Date
- 2026-11-10
AI Technical Summary
Existing lignin-based Diels-Alder self-healing coatings require temperatures of 60-130°C to trigger repair, limiting their application in environments where heating is not possible. Furthermore, the coatings have poor interfacial compatibility, which affects their protective performance.
By introducing 5-hydroxymethylfurfural (HMF) into lignin molecules for modification, furan rings and hydroxymethyl functional groups are formed simultaneously. A Diels-Alder reversible covalent bond network of furan rings and maleimide and a hydrogen bond network of hydroxymethyl groups are constructed, realizing a dual-mode self-repair mechanism of room temperature hydrogen bond pre-repair and heated DA complete repair.
The coating achieves initial repair of microcracks at room temperature and complete repair after heating, expanding its application boundaries, improving the coating's density and corrosion resistance, and making it suitable for a variety of metal substrates.
Smart Images

Figure CN123063084A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal surface corrosion protection technology, specifically relating to a dual-mode self-healing corrosion-resistant coating composition with 5-hydroxymethylfurfural modified lignin as the functional skeleton, which combines room temperature hydrogen bond repair and heated Diels-Alder repair, its preparation method and application. Background Technology
[0002] Metal corrosion is one of the main forms of failure in industrial equipment and marine facilities, resulting in annual economic losses of approximately 2% to 4% of GDP in various countries. Organic protective coatings are the most widely used anti-corrosion method, but during service, these coatings are susceptible to microcracks and scratches due to the combined effects of mechanical impact, temperature changes, ultraviolet radiation, and corrosive media. Once these defects form, corrosive media (water, oxygen, chloride ions, etc.) penetrate along the cracks into the coating / metal interface, causing interfacial delamination and under-film corrosion, ultimately leading to the loss of protective function. Currently, maintenance mainly relies on regular manual inspections and recoating, which is a complex and costly process that cannot achieve immediate repair.
[0003] Self-healing coating technology offers a new approach to addressing the aforementioned problems and can be categorized into two types: exogenous and intrinsic. Exogenous coatings achieve healing by releasing repair agents through carriers such as microcapsules, but the repair agents are consumed only once, the carriers are prone to premature leakage, and the coating's density and mechanical properties are affected. Intrinsic coatings, based on reversible covalent chemistry or supramolecular chemistry, achieve multiple repairs through the breaking and recombination of dynamic bonds at the molecular level. Among these, the Diels-Alder (DA) reaction has attracted significant attention due to its temperature-response reversibility: heating triggers a reverse reaction that dissociates the cross-linked network, and cooling allows for rebonding and network reconstruction, combining the dimensional stability of thermosetting materials with the reprocessability of thermoplastic materials.
[0004] Lignin, as the most abundant aromatic biomass polymer in nature, boasts advantages such as wide availability, renewability, and biodegradability. Its phenolic hydroxyl groups, alcoholic hydroxyl groups, and rigid benzene rings endow it with natural antioxidant, UV-resistant, and thermally stable properties, making it an ideal functional component for anti-corrosion coatings. In recent years, furanization modification has been used to add furan rings to the side chains of lignin, leading to a DA reaction with a maleimide-containing crosslinking agent. This has successfully prepared lignin-based self-healing anti-corrosion coatings that can reduce corrosion rates by more than three orders of magnitude.
[0005] However, existing lignin-based DA self-healing coatings generally require temperatures of 60-130°C to initiate the repair process, which severely limits their practical application in scenarios where heating is impossible, such as large steel structures, outdoor pipelines, ship decks, and wind turbine towers. How to introduce room-temperature repair capabilities while retaining the advantages of reversible crosslinking of DA has become a core technological bottleneck in this field.
[0006] 5-Hydroxymethylfurfural (HMF) is a representative platform compound in the field of biomass resource utilization. It can be prepared from a hexose via one-step acid-catalyzed dehydration. Its molecule contains both a furan ring (DA reaction site) and a hydroxymethyl group (hydrogen bond site). Previous studies have utilized the hydrogen bonds between HMF and lignin to improve adhesive properties or to prepare HMF-based thermo-repairing polyurethane coatings. However, research on using HMF directly as a chemical modifier for lignin, simultaneously introducing furan rings and hydroxymethyl groups, and then constructing a dual-mode self-healing anti-corrosion coating with "room temperature hydrogen bond repair + heated DA repair" has not yet been reported.
[0007] Based on this, the present invention modifies industrial lignin with HMF to prepare bifunctional modified lignin with both furan ring and hydroxymethyl group, thereby constructing a dual-mode self-healing anti-corrosion coating, providing a new solution for the high-value utilization of lignin and the breakthrough of heating dependence bottleneck of DA coating. Summary of the Invention
[0008] The purpose of this invention is to overcome the technical defect that existing lignin-based DA self-healing anticorrosive coatings must rely on heating to trigger repair, and to provide a 5-hydroxymethylfurfural modified lignin dual-mode self-healing anticorrosive coating and its preparation method. This coating and its preparation method construct a dual-mode self-healing mechanism of room temperature hydrogen bond pre-repair + heating DA complete repair.
[0009] The core technical concept of this invention is as follows: using industrial lignin as the matrix material and 5-hydroxymethylfurfural (HMF) as the functional modifier, HMF is covalently grafted onto the lignin molecule through a condensation reaction, simultaneously introducing furan rings and hydroxymethyl functional groups. The grafted furan ring, acting as a diene, forms a thermally reversible DA covalent bond with the maleimide group in the bismaleimide crosslinking agent, constituting the high-temperature repair mechanism of the coating; the hydroxymethyl group retained in the HMF molecule forms a hydrogen bond network with the phenolic hydroxyl groups of the lignin itself and the polar groups in the epoxy resin matrix, constituting the room-temperature repair mechanism of the coating. The two mechanisms work synergistically under different temperature conditions—at room temperature, the hydrogen bond network responds first to crack damage, achieving initial crack closure through rapid dynamic exchange; after heating, the DA bonds undergo thermally reversible breakage and recombination, achieving complete crack repair. The thus constructed dual-mode self-repair mechanism of "room-temperature hydrogen bond pre-repair + heating DA complete repair" fundamentally breaks through the limitations of the single thermal repair mode of existing lignin-based DA coatings. Furthermore, the introduction of hydroxymethyl groups into the HMF molecule effectively improves the interfacial compatibility between the modified lignin and the epoxy resin matrix. The polarity of the hydroxymethyl group enhances the intermolecular interaction between the modified lignin and the epoxy resin, promotes the uniform dispersion of lignin in the coating, reduces interfacial defects, and thus improves the density and corrosion barrier properties of the coating.
[0010] To achieve the above-mentioned technical objectives, the technical solution adopted by the present invention is as follows:
[0011] A 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating comprises the following raw materials in parts by weight:
[0012] 25-45 parts by weight of 5-hydroxymethylfurfural modified lignin, 15-30 parts by weight of bismaleimide, 30-50 parts by weight of epoxy resin, 10-20 parts by weight of curing agent, and 40-60 parts by weight of organic solvent.
[0013] The 5-hydroxymethylfurfural modified lignin is prepared by reacting industrial alkali lignin with 5-hydroxymethylfurfural under acid catalysis, and its molecular structure contains both furan ring and hydroxymethyl functional group.
[0014] The coating is endowed with thermally stimulated self-healing ability through the reversible Diels-Alder covalent bond between the furan ring and the maleimide group, and room temperature assisted repair ability is endowed by the hydrogen bond network between the hydroxymethyl group, the lignin phenolic hydroxyl group and the epoxy resin polar group, forming a dual-mode self-healing mechanism of room temperature hydrogen bond pre-repair and heated Diels-Alder complete repair.
[0015] As a further improvement to the present invention, the raw materials include the following parts by weight:
[0016] 30-40 parts by weight of 5-hydroxymethylfurfural modified lignin, 18-25 parts by weight of bismaleimide, 35-45 parts by weight of epoxy resin, 12-18 parts by weight of curing agent, and 45-55 parts by weight of organic solvent.
[0017] To achieve the above-mentioned technical objectives, another technical solution adopted by the present invention is as follows:
[0018] A method for preparing a 5-hydroxymethylfurfural modified lignin bimodal self-healing anti-corrosion coating includes the following steps:
[0019] (1) Preparation of 5-hydroxymethylfurfural modified lignin: 10-20g of industrial alkali lignin was dissolved in an organic solvent and heated to 80-120℃ under nitrogen protection. 8-15g of 5-hydroxymethylfurfural was added, and the mixture was reacted for 6-12 hours with p-toluenesulfonic acid as a catalyst under stirring. After the reaction was completed, the product was poured into deionized water to precipitate, filtered, washed alternately with deionized water and ethanol, and dried under vacuum at 60℃ to constant weight to obtain 5-hydroxymethylfurfural modified lignin. The product molecule simultaneously introduces furan rings and hydroxymethyl functional groups.
[0020] (2) Preparation of the coating main agent: Take 25-45 parts by weight of the 5-hydroxymethylfurfural modified lignin obtained in step (1), 30-50 parts by weight of epoxy resin, add 40-60 parts by weight of organic solvent, and disperse in a high-speed disperser at 1200-2000 rpm for 30-60 minutes. Then, ultrasonically treat for 20-30 minutes to obtain a uniform dispersion. Add 15-30 parts by weight of bismaleimide to the dispersion and continue stirring for 10-20 minutes.
[0021] (3) Addition of curing agent before coating: Before coating, add 10 to 20 parts of curing agent to the above mixture, stir evenly, and vacuum degas for 15 to 30 minutes to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating.
[0022] (4) Coating and Curing: The prepared coating is applied to the surface of the pretreated metal substrate by spraying, brushing, or dipping, with the wet film thickness controlled at 80~200μm. After coating, the substrate is placed in an oven and cured according to a stepped temperature program: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours. After curing, the substrate is allowed to cool naturally to room temperature to obtain the dual-mode self-healing anti-corrosion coating with a dry film thickness of 40~100μm.
[0023] As a further improvement of the present invention, in step (1), the weight ratio of industrial alkali lignin to 5-hydroxymethylfurfural is 1:0.7 to 1:0.9, the reaction temperature is 90 to 110°C, and the reaction time is 8 to 10 hours. Preferably, the weight ratio of industrial alkali lignin to 5-hydroxymethylfurfural is 1:0.75 to 1:0.83.
[0024] As a further improvement of the present invention, the organic solvent in step (1) is 100~200mL of anhydrous N,N-dimethylformamide.
[0025] As a further improved technical solution of the present invention, the bismaleimide in step (2) is N,N′-(4,4′-methylenediphenyl)bismaleimide or N,N′-(1,3-phenylene)bismaleimide.
[0026] As a further improvement of the present invention, the epoxy resin is a bisphenol A type epoxy resin or a bisphenol F type epoxy resin; the organic solvent is one or more of acetone, butanone or ethyl acetate.
[0027] As a further improvement of the present invention, the molar ratio of furan group to maleimide group in step (2) is 1:0.8 to 1:1.2.
[0028] As a further improvement of the present invention, in step (3), the curing agent is an amine curing agent or an acid anhydride curing agent.
[0029] To achieve the above-mentioned technical objectives, another technical solution adopted by the present invention is as follows:
[0030] A method for using a 5-hydroxymethylfurfural modified lignin bimodal self-healing anti-corrosion coating involves applying the coating to the surface of a metal substrate and curing it according to a stepped heating procedure. If microcracks develop in the coating during service due to mechanical forces or environmental stress, placing it at room temperature for 2-12 hours will cause dynamic breakage and recombination of the hydrogen bond network within the coating, achieving initial repair of the microcracks. Subsequently, heating the coating to 80-120°C and maintaining this temperature for 20-60 minutes causes thermally reversible breakage and recombination of the DA bonds, achieving complete repair of the microcracks. The coating can withstand multiple damage-repair cycles.
[0031] The beneficial effects of this invention are as follows:
[0032] This invention represents a technological leap from "single thermal repair" to "room temperature + heating dual-mode repair" for lignin-based self-healing coatings. Existing lignin-based DA self-healing coatings require temperatures of 60-130°C to initiate repair after damage, severely limiting their application in large components, outdoor facilities, and other environments where heating is impossible. This invention, by simultaneously introducing DA reaction sites (furan rings) and hydrogen bonding sites (hydroxymethyl groups) into the lignin framework, enables the coating to achieve initial repair of microcracks at room temperature through the dynamic exchange of hydrogen bonds. When conditions permit, heating is then used to achieve complete repair of the DA bonds. This dual-mode design endows the coating with broad adaptability to different service environments, effectively expanding the application boundaries of lignin-based self-healing coatings.
[0033] This invention pioneered the introduction of biomass platform molecule HMF into a lignin-based DA self-healing coating system, constructing a complete "biomass-biomass" raw material route. Existing lignin-based DA self-healing coatings utilize furan sources (such as furfuryl alcohol and furfural methylamine) that often require multiple chemical conversions. This invention directly uses HMF as a modifying agent. HMF can be obtained from hexoses such as fructose and glucose through a one-step acid-catalyzed dehydration process, making it widely available and using mature technology. The synergistic conversion of HMF and lignin achieves high-value utilization of biomass resources from raw materials to functional coating materials, aligning with the core concepts of green chemistry and sustainable development.
[0034] This invention improves the interfacial compatibility between lignin and the epoxy resin matrix by introducing hydroxymethyl groups (HMF). When lignin is simply blended into epoxy resin as a filler, the significant difference in polarity between the two leads to lignin agglomeration and phase separation, resulting in increased coating defects and decreased protective performance. After HMF modification, the hydroxymethyl groups enhance the polarity of lignin molecules, forming stronger intermolecular hydrogen bonds with the epoxy resin matrix, promoting uniform dispersion and interfacial bonding of lignin in the coating. This improvement in molecular-level compatibility significantly enhances the density and mechanical integrity of the coating without the addition of additional dispersants or coupling agents.
[0035] This invention fully utilizes the multiple inherent functions of lignin. The rigid benzene ring structure of the lignin molecule endows the coating with excellent resistance to UV aging and thermal stability; the corrosion-inhibiting function of lignin itself can synergistically enhance the metal protection effect of the coating. The grafting modification of HMF not only does not weaken these natural advantages of lignin, but also further enhances the interfacial bonding between the coating and the metal substrate through the introduction of hydroxymethyl groups.
[0036] This invention utilizes inexpensive raw materials and employs a simple and easy-to-implement process, exhibiting high compatibility with existing industrial coating systems. Industrial alkali lignin is a major byproduct of the pulp and paper industry, with low prices and stable supply; HMF production technology is becoming increasingly mature, and costs are continuously decreasing. The coating preparation and application process of this invention is fully compatible with existing epoxy resin coating lines, requiring no special equipment investment, and possesses excellent industrialization feasibility and market competitiveness. Attached Figure Description
[0037] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0038] The specific embodiments of the present invention will be further described below with reference to the accompanying drawings:
[0039] In each embodiment of the present invention, the furan group content in 5-hydroxymethylfurfural modified lignin is calculated by the HMF grafting rate (approximately 15%~20%, i.e., approximately 0.08~0.11 mol of furan groups per 100g of modified lignin) and the maleimide group content in bismaleimide. In each embodiment, the molar ratio of furan groups to maleimide groups is controlled within the range of 1:0.8~1:1.2 to ensure the full construction of the DA reaction crosslinking network.
[0040] Example 1:
[0041] This embodiment provides a method for preparing a 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating, such as... Figure 1 As shown, it includes the following steps:
[0042] (1) Dissolve 15.0 g of industrial alkali lignin in 150 mL of anhydrous N,N-dimethylformamide and heat to 100 °C under nitrogen protection. Add 12.0 g of 5-hydroxymethylfurfural and react for 8 hours with p-toluenesulfonic acid as a catalyst under stirring. After the reaction is complete, pour the product into deionized water to precipitate, filter, wash alternately with deionized water and ethanol, and dry under vacuum at 60 °C to constant weight to obtain 5-hydroxymethylfurfural modified lignin.
[0043] (2) Take 35.0 g of 5-hydroxymethylfurfural modified lignin and 40.0 g of bisphenol A epoxy resin obtained in step (1), add 50.0 g of acetone, and disperse in a high-speed disperser at 1500 rpm for 45 minutes. Then, sonicate for 25 minutes to obtain a uniform dispersion. Add 22.0 g of N,N′-(4,4′-methylenediphenyl)bismaleimide to the dispersion and continue stirring for 15 minutes.
[0044] (3) Before coating, add 15.0g of amine curing agent to the above mixture, stir evenly, and vacuum degas for 20 minutes to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating.
[0045] (4) The prepared coating was applied to the surface of a pretreated Q235 carbon steel substrate by spraying, with the wet film thickness controlled at 120 μm. After coating, the substrate was placed in an oven and cured according to a stepped temperature program: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours. After curing, the substrate was allowed to cool naturally to room temperature, and the dry film thickness was measured to be approximately 60 μm, thus obtaining the dual-mode self-healing anti-corrosion coating.
[0046] Example 2:
[0047] (1) Dissolve 10.0 g of industrial alkali lignin in 100 mL of anhydrous N,N-dimethylformamide and heat to 80 °C under nitrogen protection. Add 8.0 g of 5-hydroxymethylfurfural and react for 10 hours with p-toluenesulfonic acid as a catalyst under stirring. After the reaction is complete, pour the product into deionized water to precipitate, filter, wash alternately with deionized water and ethanol, and dry under vacuum at 60 °C to constant weight to obtain 5-hydroxymethylfurfural modified lignin.
[0048] (2) Take 25.0 g of 5-hydroxymethylfurfural modified lignin and 35.0 g of bisphenol F epoxy resin obtained in step (1), add 45.0 g of butanone, and disperse in a high-speed disperser at 1200 rpm for 50 minutes. Then, sonicate for 20 minutes to obtain a uniform dispersion. Add 18.0 g of N,N′-(1,3-phenylene)bismaleimide to the dispersion and continue stirring for 15 minutes.
[0049] (3) Before coating, add 12.0g of anhydride curing agent to the above mixture, stir evenly, and vacuum degas for 15 minutes to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating.
[0050] (4) The prepared coating is applied to the surface of the pretreated aluminum alloy substrate by brushing, and the wet film thickness is controlled at 100 μm. After coating, it is placed in an oven and cured according to the stepped temperature program: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours. After curing, it is naturally cooled to room temperature, and the dry film thickness is measured to be about 50 μm, which is the dual-mode self-healing anti-corrosion coating.
[0051] Example 3:
[0052] (1) Dissolve 20.0 g of industrial alkali lignin in 200 mL of anhydrous N,N-dimethylformamide and heat to 120 °C under nitrogen protection. Add 15.0 g of 5-hydroxymethylfurfural and react for 9 hours with p-toluenesulfonic acid as a catalyst under stirring. After the reaction is complete, pour the product into deionized water to precipitate, filter, wash alternately with deionized water and ethanol, and dry under vacuum at 60 °C to constant weight to obtain 5-hydroxymethylfurfural modified lignin.
[0053] (2) Take 45.0 g of 5-hydroxymethylfurfural modified lignin and 50.0 g of bisphenol A epoxy resin obtained in step (1), add 60.0 g of ethyl acetate, and disperse in a high-speed disperser at 2000 rpm for 35 minutes. Then, sonicate for 30 minutes to obtain a uniform dispersion. Add 30.0 g of N,N′-(4,4′-methylenediphenyl)bismaleimide to the dispersion and continue stirring for 20 minutes.
[0054] (3) Before coating, add 20.0g of amine curing agent to the above mixture, stir evenly, and vacuum degas for 30 minutes to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating.
[0055] (4) The prepared coating was applied to the surface of the pretreated stainless steel substrate by dip coating, and the wet film thickness was controlled at 150 μm. After coating, the substrate was placed in an oven and cured according to a stepped temperature program: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours. After curing, the substrate was allowed to cool naturally to room temperature, and the dry film thickness was measured to be approximately 75 μm, thus obtaining the dual-mode self-healing anti-corrosion coating.
[0056] Example 4:
[0057] (1) Dissolve 12.0 g of industrial alkali lignin in 120 mL of anhydrous N,N-dimethylformamide and heat to 95 °C under nitrogen protection. Add 10.0 g of 5-hydroxymethylfurfural and react for 6 hours with p-toluenesulfonic acid as a catalyst under stirring. After the reaction is complete, pour the product into deionized water to precipitate, filter, wash alternately with deionized water and ethanol, and dry under vacuum at 60 °C to constant weight to obtain 5-hydroxymethylfurfural modified lignin.
[0058] (2) Take 30.0g of 5-hydroxymethylfurfural modified lignin and 30.0g of bisphenol F epoxy resin obtained in step (1), add 40.0g of acetone, and disperse in a high-speed disperser at 1400rpm for 30 minutes. Then, sonicate for 25 minutes to obtain a uniform dispersion. Add 15.0g of N,N′-(4,4′-methylenediphenyl)bismaleimide to the dispersion and continue stirring for 12 minutes.
[0059] (3) Before coating, add 10.0g of anhydride curing agent to the above mixture, stir evenly, and vacuum degas for 18 minutes to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating.
[0060] (4) The prepared coating is applied to the surface of the pre-treated galvanized steel substrate by spraying, with the wet film thickness controlled at 80 μm. After coating, it is placed in an oven and cured according to a stepped temperature program: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours. After curing, it is naturally cooled to room temperature, and the dry film thickness is measured to be approximately 40 μm, thus obtaining the dual-mode self-healing anti-corrosion coating.
[0061] Example 5:
[0062] (1) Dissolve 18.0 g of industrial alkali lignin in 180 mL of anhydrous N,N-dimethylformamide and heat to 105 °C under nitrogen protection. Add 14.0 g of 5-hydroxymethylfurfural and react with p-toluenesulfonic acid as a catalyst for 12 hours under stirring. After the reaction is complete, pour the product into deionized water to precipitate, filter, wash alternately with deionized water and ethanol, and dry under vacuum at 60 °C to constant weight to obtain 5-hydroxymethylfurfural modified lignin.
[0063] (2) Take 40.0 g of 5-hydroxymethylfurfural modified lignin and 45.0 g of bisphenol A epoxy resin obtained in step (1), add 55.0 g of butanone, and disperse in a high-speed disperser at 1600 rpm for 60 minutes, followed by ultrasonic treatment for 30 minutes to obtain a uniform dispersion. Add 25.0 g of N,N′-(1,3-phenylene)bismaleimide to the dispersion and continue stirring for 18 minutes.
[0064] (3) Before coating, add 18.0g of amine curing agent to the above mixture, stir evenly, and vacuum degas for 22 minutes to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating.
[0065] (4) The prepared coating was applied to the surface of the pretreated copper alloy substrate by brushing, with the wet film thickness controlled at 200 μm. After coating, the substrate was placed in an oven and cured according to a stepped temperature program: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours. After curing, the substrate was allowed to cool naturally to room temperature, and the dry film thickness was measured to be approximately 100 μm, thus obtaining the dual-mode self-healing anti-corrosion coating.
[0066] The 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coatings prepared in Examples 1-5 were coated on the surface of metal substrates and cured according to the step-by-step heating program in step (4) of each example (60℃×2 hours→80℃×1 hour→120℃×2 hours). After natural cooling to room temperature, the dual-mode self-healing anti-corrosion coatings of each example were obtained.
[0067] The 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coatings of each embodiment and the comparative example ordinary epoxy coating (comparative example: a coating made with equal amounts of epoxy resin and curing agent without the addition of 5-hydroxymethylfurfural modified lignin and bismaleimide under the same experimental conditions) were coated into films. Pencil hardness was tested according to GB / T 6739-2022; flexibility was tested according to GB / T 1731-2020; adhesion (pull-off method) was tested according to GB / T 5210-2006; self-healing rate was tested by scratch test; heat resistance temperature was tested according to GB / T 27761-2011; impedance modulus of the coating in 3.5wt% NaCl solution was tested according to electrochemical impedance spectroscopy (EIS); salt spray resistance was tested according to GB / T 1771-2007; surface resistivity was tested according to GB / T 1410-2006; and other tests were conducted according to GB / T 1771-2007. The antibacterial activity of 21866-2008 (Escherichia coli) was tested and compared with that of a control group. The test results are shown in Table 1 below.
[0068] The self-healing rate test method was as follows: An 8×19mm single-edged blade was used to scratch the surface of the experimental sample. The initial scratch width H0 was immediately observed and recorded under a microscope. The samples were then divided into two groups: one group was placed in a room temperature (25℃) environment for 12 hours, and the scratch width was observed and the room temperature repair rate was calculated; the other group was subjected to heat stimulation at 100℃ for 30 minutes, and the scratch width H1 was observed again after cooling. Another portion of damaged samples were placed at room temperature for 2 hours for observation. The results showed that the crack width had significantly decreased, and the room temperature repair rate was approximately 20%~30%, indicating that the coating can initiate dynamic repair of the hydrogen bond network at room temperature. The self-healing rate calculation formula is: Self-healing rate = [(H0-H1) / H0]×100%.
[0069] Table 1 shows the test results:
[0070] Performance indicators Example 1 Example 2 Example 3 Example 4 Example 5 Ordinary epoxy coating (comparative example) Test Standards Hardness (pencil hardness) 2H H 3H H 2H HB GB / T6739-2022 Flexibility (mm) 2 1 3 1 2 5 GB / T1731-2020 Adhesion (pull-off test, MPa) 4.8 4.2 5.2 3.8 4.5 2.5 GB / T5210-2006 Room temperature self-healing rate (%, 25℃×12h) 45 50 40 55 48 0 Scratch method Heating self-healing rate (%, 100℃×30min) 92 88 95 85 90 0 Scratch method Heat resistance temperature (°C) 185 175 195 170 180 150 GB / T 27761-2011 <![CDATA[Impedance modulus (Ω·cm 2 , 0.01 Hz)]]> <![CDATA[5.2×10 8 ]]> <![CDATA[3.8×10 8 ]]> <![CDATA[6.5×10 8 ]]> <![CDATA[2.6×10 8 ]]> <![CDATA[4.5×10 8 ]]> <![CDATA[5.0×10 6 ]]> EIS test Salt spray resistance (h) 520 460 580 400 500 200 Refer to GB / T 1771-2007 <![CDATA[Surface resistivity (10 9 Ω)]]> 1.5 1.8 1.2 2.0 1.6 350 GB / T 1410-2006 Antibacterial activity (%) 90 85 94 82 88 70 GB / T 21866-2008 (Escherichia coli)
[0071] As shown in Table 1, the 5-hydroxymethylfurfural (HMF) modified lignin bimodal self-healing anti-corrosion coating prepared in this invention outperforms ordinary epoxy coatings in terms of mechanical properties such as hardness, flexibility, and adhesion. The improved adhesion is achieved by introducing hydroxymethyl polar groups through HMF modification of lignin, which enhances the interfacial bonding between the coating and the metal substrate. Regarding self-healing performance, the coating achieves 40%–55% crack repair after 12 hours at room temperature. This is attributed to the dynamic exchange of hydrogen bonds formed between the HMF hydroxymethyl groups, lignin phenolic hydroxyl groups, and epoxy resin polar groups at room temperature. After heat treatment at 100℃ for 30 minutes, the repair rate reaches 85%–95%, attributed to the thermally reversible breaking and recombination of the DA bonds between the furan ring and maleimide groups. The coating achieves a low-frequency impedance modulus of 10 in 3.5 wt% NaCl solution. 8 The Ω·cm² level is more than two orders of magnitude higher than that of ordinary epoxy coatings, indicating its excellent corrosion barrier performance. Salt spray resistance time reaches 400–580 hours, far superior to the 200 hours of ordinary epoxy coatings. Furthermore, repair tests were conducted by heating the damaged coating at 80℃ for 60 minutes and at 120℃ for 20 minutes, respectively. The results showed that the repair rate reached over 80% under both conditions, indicating that the coating has good thermally induced complete repair capability within the 80–120℃ range. These results demonstrate that this invention successfully constructs a dual-mode self-healing mechanism of "room temperature hydrogen bond pre-repair + heated DA complete repair," introducing room temperature repair capability to the coating without relying on external energy while retaining the advantages of reversible DA crosslinking.
[0072] This invention utilizes the reversible Diels-Alder covalent bond between the furan ring and the maleimide group to endow the coating with thermally stimulated self-healing ability. Simultaneously, it leverages the hydrogen bond network between the hydroxymethyl group in the 5-hydroxymethylfurfural molecule and the phenolic hydroxyl groups of lignin and the polar groups of the epoxy resin to endow the coating with room-temperature assisted repair ability, constructing a dual-mode self-healing mechanism of "room-temperature hydrogen bond pre-repair + heated DA complete repair." The coating can achieve preliminary repair of microcracks at room temperature, and complete repair can be achieved after heat treatment at 80~120℃. After repair, the coating's impedance modulus recovers to more than 90% of its initial value. This invention synergistically transforms industrial waste lignin and the biomass platform molecule 5-hydroxymethylfurfural into high-value functional components. The coating possesses dual-mode self-healing performance, excellent corrosion resistance, and mechanical strength, making it suitable for long-term corrosion protection and intelligent protection of ships, chemical storage tanks, marine engineering equipment, and large metal components.
[0073] The scope of protection of this invention includes, but is not limited to, the above embodiments. The scope of protection of this invention is defined by the claims. Any substitutions, modifications, or improvements to this technology that are easily conceived by those skilled in the art fall within the scope of protection of this invention.
Claims
1. A 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating, characterized in that, The ingredients include the following parts by weight: 25-45 parts by weight of 5-hydroxymethylfurfural modified lignin, 15-30 parts by weight of bismaleimide, 30-50 parts by weight of epoxy resin, 10-20 parts by weight of curing agent, and 40-60 parts by weight of organic solvent. The 5-hydroxymethylfurfural modified lignin is prepared by reacting industrial alkali lignin with 5-hydroxymethylfurfural under acid catalysis, and its molecular structure contains both furan ring and hydroxymethyl functional group. The coating is endowed with thermally stimulated self-healing ability through the reversible Diels-Alder covalent bond between the furan ring and the maleimide group, and room temperature assisted repair ability is endowed by the hydrogen bond network between the hydroxymethyl group, the lignin phenolic hydroxyl group and the epoxy resin polar group, forming a dual-mode self-healing mechanism of room temperature hydrogen bond pre-repair and heated Diels-Alder complete repair.
2. The 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating according to claim 1, characterized in that, The ingredients include the following parts by weight: 30-40 parts by weight of 5-hydroxymethylfurfural modified lignin, 18-25 parts by weight of bismaleimide, 35-45 parts by weight of epoxy resin, 12-18 parts by weight of curing agent, and 45-55 parts by weight of organic solvent.
3. A method for preparing a 5-hydroxymethylfurfural modified lignin bimodal self-healing anti-corrosion coating as described in claim 1 or 2, characterized in that, Includes the following steps: (1) Industrial alkali lignin and 5-hydroxymethylfurfural are dissolved in an organic solvent and reacted under acid catalysis. After precipitation, washing and drying, 5-hydroxymethylfurfural modified lignin is obtained. (2) Add the 5-hydroxymethylfurfural modified lignin and epoxy resin obtained in step (1) to an organic solvent, disperse them evenly, then add bismaleimide and continue stirring until evenly mixed; (3) Before coating, add curing agent to the product obtained in step (2), stir evenly and degas to obtain 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating. (4) Apply the coating to the surface of the substrate, cure it by step heating, and then cool it naturally to room temperature after curing to obtain the dual-mode self-healing anti-corrosion coating.
4. The preparation method according to claim 3, characterized in that, The weight ratio of industrial alkali lignin to 5-hydroxymethylfurfural in step (1) is 1:0.7 to 1:0.9, the reaction temperature is 80 to 120°C, and the reaction time is 6 to 12 hours.
5. The preparation method according to claim 4, characterized in that, The weight ratio of industrial alkali lignin to 5-hydroxymethylfurfural in step (1) is 1:0.75~1:0.
83.
6. The preparation method according to claim 3, characterized in that, The organic solvent in step (1) is anhydrous N,N-dimethylformamide, and the acid catalyst is p-toluenesulfonic acid; the reaction in step (1) is carried out under nitrogen protection, the washing method is alternating washing with deionized water and ethanol, and the drying condition is vacuum drying at 60°C to constant weight.
7. The preparation method according to claim 3, characterized in that, The bismaleimide mentioned in step (2) is N,N′-(4,4′-methylenediphenyl)bismaleimide or N,N′-(1,3-phenylene)bismaleimide; the epoxy resin is bisphenol A type epoxy resin or bisphenol F type epoxy resin; the organic solvent is one or more of acetone, butanone or ethyl acetate.
8. The preparation method according to claim 3, characterized in that, In step (2), the stirring rate for high-speed dispersion is 1200-2000 rpm, and the stirring time is 30-60 minutes; the ultrasonic treatment time is 20-30 minutes; after adding bismaleimide, stirring is continued for 10-20 minutes. In step (2), the molar ratio of furan group to maleimide group is 1:0.8 to 1:1.
2.
9. The preparation method according to claim 3, characterized in that, In step (3), the curing agent is an amine curing agent or an anhydride curing agent; the vacuum degassing time is 15 to 30 minutes; In step 4, the substrate is a metal substrate, and the coating method is spraying, brushing or dipping. The wet film thickness is 80-200 μm and the dry film thickness is 40-100 μm. The stepped temperature curing program is: 60℃×2 hours, 80℃×1 hour, 120℃×2 hours.
10. A method of using the 5-hydroxymethylfurfural modified lignin dual-mode self-healing anti-corrosion coating prepared by the method described in claim 3, characterized in that, The coating is applied to the surface of the substrate and cured by step heating to form a coating. After the coating is damaged and microcracks are generated, it is placed at room temperature for 2 to 12 hours to achieve preliminary repair of microcracks through dynamic repair of hydrogen bond network. Subsequently, it is heated to 80 to 120°C and held for 20 to 60 minutes to achieve complete repair of microcracks through Diels-Alder bond thermal reversible reaction.