An adhesive and method for bonding a metal matrix to an impregnated metal carbon slide
By using inorganic-organic composite adhesives and precise curing processes, the problem of low bonding strength of metal-carbon dip plate was solved, achieving a combination of high-temperature stability and long service life, reducing friction and wear, and ensuring the stability and safety of subway train current collection.
Patent Information
- Application Number
- CN202611511633.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-10
AI Technical Summary
The existing bonding process for metal-carbon dipped sliding plates used in subway trains has problems such as low bonding strength, easy cracking and voids at the interface, and high-temperature bonding failure. As a result, the sliding plates are prone to falling off, abnormal wear, or excessive contact resistance under high-speed operation and complex working conditions, which affects the current collection quality and train operation safety.
An inorganic-organic composite adhesive is used, comprising borate glass powder, phenolic resin, inorganic reinforcing filler and curing accelerator. Combined with roughening treatment of the metal matrix and precise high-temperature curing process, it forms a dual effect of physical locking and chemical bonding to ensure interface stability.
It significantly improves the bonding strength of the metal-carbon interface, ensuring no delamination or cracking under high temperature and high pressure conditions, extending the service life to more than 100,000 kilometers, reducing the friction and wear rate, and improving the long-term reliable current collection of the pantograph system.
Smart Images

Figure CN123063115A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon sliding plate technology for electric locomotives, and more particularly to an adhesive and bonding method for bonding a metal substrate to a metal-impregnated carbon sliding plate. Background Technology
[0002] With the rapid development of urban rail transit, the demand for the localization of key components of subway trains, as an important public transportation tool, is becoming increasingly urgent. The pantograph contactor, as a core component of the subway train's power transmission system, directly affects the train's operational stability and safety. Currently, metal-impregnated carbon contactors are widely used in subway trains due to their excellent overall performance; however, the high-temperature bonding technology in their manufacturing process remains one of the challenges in localization.
[0003] The bonding process of metal-carbon dipped sliding plates for subway trains in the existing technology generally has defects such as low bonding strength, easy cracking and voids at the interface, and high temperature bonding failure. As a result, the sliding plates are prone to falling off, abnormal wear or excessive contact resistance under high speed and complex working conditions, which seriously affects the current collection quality and train operation safety. Summary of the Invention
[0004] In view of this, the purpose of this invention is to provide an adhesive and bonding method for bonding a metal substrate to a metal-impregnated carbon plate. The adhesive and bonding method of this invention can significantly improve the bonding strength between the metal-impregnated carbon plate and the metal substrate, exhibiting excellent high-temperature stability and long service life, meeting the stringent operating requirements of subway trains. Furthermore, it has a low frictional wear rate, ensuring long-term reliable current collection for the pantograph system, thus achieving a balance between performance improvement and reliability.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides an adhesive for bonding a metal substrate to a metal-impregnated carbon slide plate, comprising the following components by weight percentage: 30-40% borate glass powder, 20-30% phenolic resin, 5-10% inorganic reinforcing filler, 2-5% curing accelerator, and the balance being an organic solvent. The inorganic reinforcing filler includes at least one of boron nitride, graphene, and copper powder; The adhesive has a viscosity of 5000~8000 mPa·s at 25°C and a solid content of ≥75%.
[0006] Preferably, the curing accelerator includes a titanate coupling agent.
[0007] Preferably, the organic solvent includes xylene.
[0008] This invention provides a method for bonding a metal substrate to a metal-impregnated carbon sliding plate, comprising the following steps: Roughen the metal base to obtain a roughened metal base; Coat the surface of the roughened metal base with the adhesive of any one of claims 1-4, and then align and press the preheated metalized carbon slide plate with the adhesive-coated base to obtain an assembly; the coating thickness is 0.1-0.3 mm; Cure the assembly under vacuum or inert atmosphere protection; the curing procedure is: heating from room temperature to 180-200℃ at a rate of 2-3℃ / min, holding for 28-32 min, and then heating to 550-600℃ at a rate of 4-5℃ / min, holding for 58-62 min.
[0009] Preferably, the roughening method comprises sandblasting.
[0010] Preferably, the sandblasting conditions comprise: sandblasting pressure of 0.3-0.5 MPa, sand particle size of 60-80 mesh, and sandblasting time of 5-10 min.
[0011] Preferably, the pressing pressure is 5-10 MPa, and the pressure holding time is 5-6 min.
[0012] Preferably, when curing under vacuum, the vacuum degree is ≤10 Pa.
[0013] Preferably, the metal base comprises an aluminum alloy base.
[0014] Preferably, the coating method comprises doctor blading or screen printing.
[0015] Compared with the prior art, the present application has the following beneficial effects: (1) Significantly improves the metal-carbon interface bonding strength, and effectively prevents adhesive failure under high-temperature environment The present application roughens the metal base to increase the surface roughness, and cooperates with a special high-temperature adhesive (inorganic-organic composite system, containing borate glass powder, phenolic resin and inorganic reinforcing filler) to promote the interface chemical reaction and mechanical interlocking during high-temperature curing. The adhesive and the base form a dual action of "physical locking + chemical bonding", and the shear strength is ≥35 MPa (in line with GB / T 7124 standard), ensuring no delamination or cracking under high-temperature (≥600℃) and high-pressure working conditions, and significantly enhancing the interface stability.
[0016] (2) Excellent high-temperature stability and long service life, meeting the stringent operation requirements of subway trains The present application adds high-temperature-resistant fillers (boron nitride, graphene, copper powder) in the adhesive formula, adopts vacuum or inert atmosphere protection in the curing process, and combines precise curing condition control (stepwise heating and holding), so as to inhibit thermal stress concentration, make the metal-impregnated carbon slide plate run long-term without thermal degradation under high temperature and strong current conditions (400 A current), prolong the service life to ≥100,000 kilometers (the traditional process is usually ≤80,000 kilometers), and effectively reduce the maintenance frequency and replacement cost.
[0017] (3) Low friction and wear rate, guaranteeing long-term reliable current collection of the pantograph system The present application can reduce the friction coefficient and wear by optimizing the thickness of the adhesive layer (0.1-0.3 mm) and combining the interface densification after high-temperature curing. The friction and wear test shows that under the simulated subway running conditions (speed of 80 km / h), the wear rate is ≤0.5 mm / 10,000 pantograph times, which is reduced by 20% compared with the existing slide plate, reduces the arc risk of the pantograph-catenary system, and improves the stability of train current collection and the service life of the contact wire. BRIEF DESCRIPTION OF DRAWINGS
[0018] Figure 1 It is an adhesive picture of the pantograph carbon slide plate, which includes different adhesive examples, collected test samples and sample blocks. DETAILED DESCRIPTION
[0019] The present application provides an adhesive for bonding a metal matrix and a metal-impregnated carbon slide plate, which comprises the following components in mass percentage: borate glass powder 30-40%, phenolic resin 20-30%, inorganic reinforcing filler 5-10%, curing accelerator 2-5%, and the balance is organic solvent.
[0020] The adhesive provided by the present application comprises borate glass powder 30-40% in mass percentage, which can be 30%, 33%, 35%, 38% or 40% in specific embodiments. In the present application, the particle size D50 of the borate glass powder is preferably 3-5 μm. The present application controls the particle size of the borate glass powder in the above range, taking into account the sintering density and slurry processability. In the embodiments of the present application, the borate glass powder is specifically zinc barium borate glass powder.
[0021] The adhesive provided by the present application comprises phenolic resin 20-30% in mass percentage, which can be 20%, 23%, 25%, 28% or 30% in specific embodiments. In the embodiments of the present application, the phenolic resin is specifically RS-518 thermosetting phenolic resin.
[0022] The adhesive provided by the present application comprises 5-10% of inorganic reinforcing fillers in terms of mass percentage, and in specific embodiments, the inorganic reinforcing fillers can be 5%, 8% or 10%. In the present application, the inorganic reinforcing fillers preferably comprise at least one of boron nitride, graphene and copper powder, and more preferably boron nitride and graphene. The present application adds the above-mentioned fillers in the adhesive formula, which can improve the high-temperature resistance of the adhesive, and further improve the high-temperature stability of the metal-impregnated carbon slide after bonding.
[0023] The adhesive provided by the present application comprises 2-5% of curing accelerators in terms of mass percentage, and in specific embodiments, the curing accelerators can be 2%, 3%, 4% or 5%. In the present application, the curing accelerators preferably comprise titanate coupling agents, and the titanate coupling agents can be specifically tetrabutyl titanate and isopropyl titanate.
[0024] The adhesive provided by the present application further comprises a residual amount of solvent. In the present application, the organic solvent preferably comprises xylene.
[0025] In the present application, the viscosity of the adhesive at 25°C is 5000-8000 mPa·s, and the solid content is ≥75%. In the embodiments of the present application, the viscosity of the adhesive at 25°C is 5000, 6500 or 8000 mPa·s, and the solid content is 75%, 78% or 80%.
[0026] The present application improves the high-temperature stability (≥600°C) and shear strength (≥30 MPa) of the adhesive through an inorganic-organic composite system.
[0027] The present application provides a preparation method of the adhesive described in the above scheme, which comprises the following steps: ball-milling and dispersing each component, and then vacuum degassing to obtain the adhesive.
[0028] In the present application, the rotation speed of the ball-milling and dispersing is preferably 200-300 rpm, and the ball-milling and dispersing time is preferably 1-3 hours, and more preferably 2 hours. In the present application, the vacuum degree of the vacuum degassing is preferably ≤-0.095 MPa, and the time is preferably 30 minutes. The present application eliminates the bubbles inside the adhesive through vacuum degassing.
[0029] The present application provides a bonding method of a metal substrate and a metal-impregnated carbon slide, which comprises the following steps: coarsening the metal substrate to obtain a coarsened metal substrate; coating the above-mentioned adhesive on the surface of the coarsened metal substrate, and then aligning and pressing the preheated metal-impregnated carbon slide and the substrate coated with the adhesive to obtain an assembly; the coating thickness is 0.1-0.3 mm; The assembly is cured under vacuum or inert atmosphere protection; the curing procedure is as follows: the temperature is increased from room temperature to 180-200℃ at a rate of 2-3℃ / min and held for 28-32min, and then increased to 550-600℃ at a rate of 4-5℃ / min and held for 58-62min.
[0030] The present invention roughens the metal matrix to obtain a roughened metal matrix.
[0031] The present invention does not impose any special requirements on the type of metal substrate, and any metal substrate well known in the art is acceptable. In the embodiments of the present invention, the metal substrate is specifically an aluminum alloy support.
[0032] In this invention, the roughening treatment includes sandblasting. The sandblasting conditions include: a sandblasting pressure preferably of 0.3~0.5 MPa, which can be 0.3, 0.4, or 0.5 MPa in specific embodiments; a sand particle size preferably of 60~80 mesh, which can be 60, 70, or 80 mesh in specific embodiments; and a sandblasting time preferably of 5~10 min, which can be 5, 8, or 10 min in specific embodiments. This invention removes oxide layers, oil stains, and impurities from the surface of a metal substrate through roughening treatment, increasing surface roughness. More importantly, roughening treatment increases the surface energy of the metal substrate, enhancing the mechanical intercalation and chemical bonding between the adhesive and the substrate. The surface of the metal substrate naturally contains an oxide layer and hydroxyl groups (-OH), which can form hydrogen bonds or covalent bonds with the polar groups in the adhesive (hydroxyl groups in phenolic resins).
[0033] After the roughening treatment is completed, the present invention preferably further includes ultrasonic cleaning of the roughened metal substrate; the ultrasonic cleaning preferably uses anhydrous ethanol or acetone solution; the ultrasonic cleaning frequency is preferably 20~40 kHz, and the ultrasonic cleaning time is preferably 10~15 minutes; the ultrasonic cleaning is preferably performed at room temperature. The present invention removes residual particles and organic matter through ultrasonic cleaning.
[0034] After obtaining the roughened metal substrate, the present invention coats the surface of the roughened metal substrate with the above-mentioned adhesive, and then aligns and presses the preheated metal-impregnated carbon slide plate with the substrate coated with adhesive to obtain the assembly.
[0035] In this invention, the coating method preferably includes scraping or screen printing; the coating thickness is 0.1~0.3 mm, and in specific embodiments it can be 0.1, 0.15, 0.2, 0.25 or 0.3 mm. By controlling the coating thickness within the above range, and in conjunction with the adhesive formulation and subsequent high-temperature curing process, the interface becomes denser after high-temperature curing, which can reduce the coefficient of friction and reduce wear.
[0036] The present application does not have special requirements for the metal-impregnated carbon slide plate, and the metal-impregnated carbon slide plate known in the art can be used. In the present application, the preheating temperature of the metal-impregnated carbon slide plate is preferably 30-40℃.
[0037] In the present application, the pressure of the pressing is preferably 5-10 MPa, and the pressure holding time is 5-6 min. In specific embodiments, the pressure of the pressing can be 5, 8 or 10 MPa. The present application controls the coating thickness and the conditions of pressing in the above range, ensuring that the adhesive layer is uniform and defect-free, and the initial bonding is tight.
[0038] After obtaining the assembly, the present application cures the assembly under vacuum or inert atmosphere protection; the curing procedure is: heating from room temperature to 180-200℃ at a rate of 2-3℃ / min, holding for 28-32 min, and then heating to 550-600℃ at a rate of 4-5℃ / min, holding for 58-62 min.
[0039] In the curing process of the present application, high temperature promotes the crosslinking reaction of the adhesive and the interfacial diffusion, forming a dense bonding layer and eliminating internal stress.
[0040] The parameters of each step (sandblasting pressure, curing temperature curve, adhesive ratio) of the present application are quantitatively designed, the equipment compatibility is strong, and the proportion of low-cost inorganic components in the adhesive formula is high (≥30%), replacing part of the expensive organic materials. The process of the present application can be standardized, the production cycle is shortened by 15%, the cost is reduced by 15-20% compared with the traditional process, which promotes the large-scale application of domestic slide plates and improves the economy.
[0041] The results show that the use of the adhesive and the bonding method of the present application improves the bonding strength between the metal-impregnated carbon slide plate and the metal matrix, the shear strength is ≥35 MPa according to the GB / T 7124 standard for shear strength test; and has excellent high-temperature stability and long service life, thermal cycle test: -40℃-80℃ (100 cycles) after detection of interface cracking; and low friction and wear rate, simulating the running conditions of the subway (current: 400 A, speed: 80 km / h), testing the wear rate, the wear rate is ≤0.5 mm / ten thousand bow times. The present application can ensure that the metal-impregnated carbon slide plate meets the long-term reliability requirements of the subway train under severe working conditions.
[0042] The adhesive and the bonding method for bonding the metal matrix and the metal-impregnated carbon slide plate provided by the present application will be described in detail below in conjunction with examples, but they should not be understood as limiting the scope of protection of the present application.
[0043] The phenolic resin used in the following examples and comparative examples is a commercially available RS-518 thermosetting phenolic resin; the borate glass powder is a commercially available zinc barium borate glass powder; the titanate coupling agent is specifically isopropyl tri-titanate FT-311W.
[0044] Example 1 Step 1: Surface pretreatment of the substrate The surface of the aluminum alloy support substrate is subjected to sandblasting treatment by mechanical roughening method, the sandblasting pressure is 0.4 MPa, the sand particle size is 70 mesh, the treatment time is 8 min, the oxide layer, oil stains and impurities are removed, and the surface roughness is increased. Subsequently, ultrasonic cleaning is performed, the ultrasonic frequency is 30 kHz, anhydrous ethanol is used for cleaning for 12 min at room temperature, and residual particles and organic matter are removed.
[0045] Step 2: Preparation of special high-temperature adhesive The components are weighed according to the percentage by weight: borate glass powder 35%, phenolic resin 25%, boron nitride 5%, graphene 5%, titanate coupling agent 3%, and the balance is dimethylbenzene. After mixing the components according to the ratio, ball milling dispersion is carried out for 2 hours (rotation speed 250 rpm) to obtain a uniform slurry. Vacuum degassing treatment (vacuum degree -0.098 MPa, time 30 min) is performed to eliminate internal bubbles. The slurry viscosity is 6500 mPa·s (25℃), and the solid content is 78%.
[0046] Step 3: Adhesive coating and assembly The adhesive is uniformly coated on the surface of the pretreated aluminum alloy support substrate by using the blade coating method, the coating thickness is 0.2 mm, and the coating speed is 1.5 m / min. The metal-impregnated carbon slide strip preheated at 30-40℃ is aligned and pressed with the adhesive-coated substrate, the pressing pressure is 8 MPa, and the pressure holding time is 5 min.
[0047] Step 4: High-temperature curing and post-treatment The assembled piece is placed in a vacuum furnace and cured according to the set temperature curve: room temperature→200℃ (heating rate 2℃ / min, holding time 30 min); 200℃→600℃ (heating rate 5℃ / min, holding time 60 min). The vacuum degree is 8 Pa. After curing, it is naturally cooled to room temperature, and surface finishing (chamfering, grinding, polishing) is performed.
[0048] Quality detection and performance verification Shear strength test (GB / T 7124 standard): 42 MPa.
[0049] Thermal cycle test (-40℃~80℃, 100 cycles): no delamination or cracks at the interface.
[0050] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.35 mm / ten thousand bows.
[0051] Example 2 Step 1: Substrate surface pretreatment The surface of the aluminum alloy support substrate was sandblasted using a mechanical roughening method. The sandblasting pressure was 0.3 MPa, the abrasive particle size was 60 mesh, and the treatment time was 5 min. The ultrasonic frequency was 20 kHz, and the substrate was cleaned with acetone solution for 10 min at room temperature.
[0052] Step 2: Preparation of Special High-Temperature Adhesive The mixture consists of 30% borate glass powder, 20% phenolic resin, 5% boron nitride, 5% graphene, 2% titanate coupling agent, and the balance xylene. It was ball-milled for 2 hours (200 rpm) and then degassed under vacuum (vacuum degree -0.095 MPa, time 30 min). The slurry viscosity was 5000 mPa·s (25℃), and the solid content was 75%.
[0053] Step 3: Adhesive application and assembly The adhesive was uniformly applied to the pretreated aluminum alloy support substrate surface using a scraping method, with a coating thickness of 0.1 mm and a coating speed of 1 m / min. The pressing pressure was 5 MPa, and the holding time was 5 min.
[0054] Step 4: High-temperature curing and post-treatment The assembled parts were placed in a vacuum furnace and cured according to the set temperature curve: room temperature → 200℃ (heating rate 2℃ / min, holding for 30min); 200℃ → 600℃ (heating rate 5℃ / min, holding for 60min). Vacuum degree 10 Pa. After natural cooling to room temperature, surface finishing was performed.
[0055] Quality Inspection and Performance Verification Shear strength test (GB / T 7124 standard): 36 MPa.
[0056] Thermal cycling test (-40℃~80℃, 100 cycles): No delamination or cracks at the interface.
[0057] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.48 mm / 10,000 cycles.
[0058] Example 3 Step 1: Surface pretreatment of the substrate The surface of the aluminum alloy support substrate was sandblasted using a mechanical roughening method. The sandblasting pressure was 0.5 MPa, the abrasive particle size was 80 mesh, and the treatment time was 10 min. The ultrasonic frequency was 40 kHz, and the surface was cleaned with anhydrous ethanol for 15 min at room temperature.
[0059] Step 2: Preparation of Special High-Temperature Adhesive The slurry consists of 40% borate glass powder, 30% phenolic resin, 10% boron nitride, 5% graphene, 5% titanate coupling agent, and the balance xylene. It was ball-milled for 2 hours (300 rpm) and then degassed under vacuum (vacuum degree -0.099 MPa, time 30 min). The slurry viscosity was 8000 mPa·s (25℃), and the solid content was 80%.
[0060] Step 3: Adhesive application and assembly The adhesive was uniformly applied to the pretreated aluminum alloy support substrate surface using a scraping method, with a coating thickness of 0.3 mm and a coating speed of 2 m / min. The pressing pressure was 10 MPa, and the holding time was 5 min.
[0061] Step 4: High-temperature curing and post-treatment The assembled parts were placed in a vacuum furnace and cured according to the set temperature curve: room temperature → 200℃ (heating rate 2℃ / min, holding for 30min); 200℃ → 600℃ (heating rate 5℃ / min, holding for 60min). Vacuum degree 5 Pa. After natural cooling to room temperature, surface finishing was performed.
[0062] Quality Inspection and Performance Verification Shear strength test (GB / T 7124 standard): 38 MPa.
[0063] Thermal cycling test (-40℃~80℃, 100 cycles): No delamination or cracks at the interface.
[0064] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.42 mm / 10,000 cycles.
[0065] Comparative Example 1 (Surface pretreatment omitted) Step 1: Surface pretreatment of the substrate No sandblasting or ultrasonic cleaning was performed; the surface of the aluminum alloy support base was simply wiped with a dry cloth to remove visible dirt, without any roughening treatment.
[0066] Steps 2-4: Same as in Example 1.
[0067] Quality Inspection and Performance Verification Shear strength test (GB / T 7124 standard): 24 MPa, a decrease of 42.9% compared to Example 1.
[0068] Thermal cycling test (-40℃~80℃, 50 cycles): Microcracks appeared at the interface, and obvious delamination occurred after 60 cycles.
[0069] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.78 mm / 10,000 cycles, an increase of 122.9% compared to Example 1.
[0070] Comparative Example 2 (using conventional adhesives) Step 1: Surface pretreatment of the substrate: Same as in Example 1.
[0071] Step 2: Preparation of high-temperature adhesive This adhesive is prepared using a standard epoxy resin binder (excluding borate glass powder, boron nitride, graphene, etc.) according to conventional methods. It has a solid content of 65% and a viscosity of 3500 mPa·s (25℃). The specific preparation method is as follows: Step 2-1: Component preparation and heating of matrix resin Preparation of the main agent (component A): Weigh a certain amount of bisphenol A type liquid epoxy resin. If the ambient temperature is low, resulting in a high resin viscosity, preheat it to 40~50℃ in a water bath to reduce the viscosity and facilitate subsequent stirring and degassing.
[0072] Preparation of curing agent (component B): Weigh out the appropriate proportion of amine curing agent.
[0073] Step 2-2: Metering and Mixing According to the mass ratio of the formula (A:B = 100:30), weigh out sufficient amounts of component A and component B using a high-precision electronic balance; pour component A and component B into the clean planetary mixer hopper.
[0074] Steps 2-3: Dispersion and mixing Mechanical mixing: Mixing is performed using a planetary vacuum mixer.
[0075] Speed control: Stir at 800-1500 rpm for 3-5 minutes. Ensure the stirring paddle reaches the bottom and side walls of the container to guarantee full cross-linking and contact between the two components, mixing until uniform in color and without obvious color streaks or layering.
[0076] Steps 2-4: Vacuum degassing Place the mixed adhesive solution into the vacuum chamber of the planetary mixer, control the vacuum level within the range of -0.08 MPa to -0.10 MPa, and continue to evacuate for 3 to 5 minutes.
[0077] Steps 3-4: Same as in Example 1.
[0078] Quality Inspection and Performance Verification Shear strength test (GB / T 7124 standard): 28 MPa, a decrease of 33.3% compared to Example 1.
[0079] Thermal cycling test (-40℃~80℃, 30 cycles): Delamination occurs at the interface, and complete peeling occurs after 45 cycles.
[0080] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.92 mm / 10,000 cycles, an increase of 162.9% compared to Example 1.
[0081] High temperature stability test: After being kept at 600℃ for 2 hours, the adhesive underwent thermal decomposition, lost its adhesive function, and the shear strength dropped to below 5 MPa.
[0082] Comparative Example 3 (inorganic components omitted) Step 1: Surface pretreatment of the substrate Same as Example 1.
[0083] Step 2: Preparation of Special High-Temperature Adhesive The following components were weighed by weight percentage: 0% borate glass powder, 40% phenolic resin, 5% boron nitride, 5% graphene, 3% titanate coupling agent, and the balance being xylene. The components were mixed according to the formula and then ball-milled for 2 hours (250 rpm) to obtain a homogeneous slurry. Vacuum degassing treatment (vacuum degree -0.098 MPa, time 30 minutes) was performed to eliminate internal air bubbles. The slurry viscosity was 6800 mPa·s (25℃), and the solid content was 76%.
[0084] Steps 3-4: Same as in Example 1.
[0085] Step 5: Quality Inspection and Performance Verification Shear strength test (GB / T 7124 standard): 31 MPa, a decrease of 26.2% compared to Example 1.
[0086] Thermal cycling test (-40℃~80℃, 75 cycles): Delamination occurs at the interface.
[0087] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.62 mm / 10,000 cycles, an increase of 77.1% compared to Example 1.
[0088] High temperature stability test: After being kept at 600℃ for 2 hours, the organic matrix of the adhesive underwent thermal degradation, and the shear strength dropped to 15 MPa.
[0089] Comparative Example 4 (Curing process does not meet requirements) Step 1: Surface pretreatment of the substrate Same as Example 1.
[0090] Step 2: Preparation of Special High-Temperature Adhesive Same as Example 1.
[0091] Step 3: Adhesive application and assembly Same as Example 1.
[0092] Step 4: High-temperature curing and post-treatment The assembled parts were placed in a vacuum oven, and the curing program was changed to: room temperature → 200℃ (heating rate 10℃ / min, holding for 15 minutes); 200℃ → 600℃ (heating rate 15℃ / min, holding for 30 minutes). The vacuum level was maintained at ≤10 Pa. After curing, the parts were allowed to cool naturally to room temperature, and then surface finishing was performed (beveling, grinding, polishing).
[0093] (Note: If the heating rate is too fast and the holding time is insufficient, and the curing is not carried out according to the temperature curve specified in this invention, the adhesive will not cross-link sufficiently.) Step 5: Quality Inspection and Performance Verification Shear strength test (GB / T 7124 standard): 34 MPa, a decrease of 19.0% compared to Example 1.
[0094] Thermal cycling test (-40℃~80℃, 80 cycles): Microcracks appeared at the interface, and delamination occurred after 90 cycles.
[0095] Friction and wear test (current 400 A, speed 80 km / h): wear rate 0.52 mm / 10,000 cycles, an increase of 48.6% compared to Example 1.
[0096] High temperature stability test: After being kept at 600℃ for 2 hours, there were incomplete cross-linked areas inside the adhesive, and the shear strength dropped to 22 MPa, which was significantly lower than that of Example 1.
[0097] Figure 1 Images show actual bonding of the pantograph carbon sliding plate, including test sample blocks collected for different bonding examples. The bonding conditions and performance of Examples 1-3 and Comparative Examples 1-2 are summarized in Table 1.
[0098] Table 1. Bonding conditions and performance of the examples and comparative examples
[0099] Note: (Explanation of the 600℃ High Temperature Performance Evaluation Standard) In this article, "Good" means that after 2 hours of heat preservation at 600℃, the adhesive shows no thermal decomposition and the shear strength retention rate is ≥80%; "Average" means that after 2 hours of heat preservation at 600℃, the adhesive shows slight performance degradation but is not completely ineffective, and the shear strength retention rate is between 50% and 80%; "Poor" means that after 2 hours of heat preservation at 600℃, the adhesive shows significant degradation and the shear strength retention rate is between 20% and 50%; "Very Poor" means that after 2 hours of heat preservation at 600℃, the adhesive undergoes thermal decomposition, completely loses its adhesive function, and the shear strength retention rate is less than 20%.
[0100] The following conclusions can be drawn from the comparison data of the above embodiments and comparative examples: (1) Examples 1 to 3 are all within the parameter range defined by the claims of this invention. The shear strength is ≥35 MPa, no delamination or cracks are found after 100 thermal cycles, and the wear rate is ≤0.5 mm / 10,000 cycles. All performance indicators meet the usage requirements of subway trains under harsh working conditions, which verifies the feasibility and effectiveness of the process scheme of this invention.
[0101] (2) Comparative Example 1 omitted the substrate surface pretreatment steps (sandblasting roughening + ultrasonic cleaning), and only wiped the surface with a dry cloth. The results showed that the shear strength dropped sharply from 42 MPa to 24 MPa (a decrease of 42.9%), delamination occurred after 50-60 thermal cycles, and the wear rate increased by 122.9%. This indicates that surface pretreatment is crucial for establishing mechanical interlocking and chemical bonding between the metal substrate and the adhesive.
[0102] (3) Comparative Example 2 used a common epoxy resin adhesive instead of the inorganic-organic composite adhesive of the present invention. The results showed that the shear strength dropped to 28 MPa, delamination occurred after only 30-45 thermal cycles, the wear rate was as high as 0.92 mm / 10,000 cycles, and the adhesive completely failed due to thermal decomposition at 600℃. This indicates that the borate glass powder, boron nitride, graphene and other components in the special high-temperature adhesive of the present invention play a decisive role in achieving high-temperature stability and high adhesive strength.
[0103] (4) Comparative Example 3 omitted the inorganic component (borate glass powder) in the adhesive, retaining only the organic modifier (phenolic resin) and reinforcing filler. The results showed that the shear strength decreased to 31 MPa (a decrease of 26.2%), delamination occurred after only 75 thermal cycles, the wear rate increased by 77.1% to 0.62 mm / 10,000 cycles, and the organic matrix underwent thermal degradation at 600℃, resulting in a significant decrease in shear strength. This indicates that the inorganic-organic composite system formed by the inorganic component (borate glass powder) and the organic modifier (phenolic resin) plays a crucial role in achieving high-temperature stability and high adhesive strength, and a single organic system cannot simultaneously achieve both high-temperature performance and interfacial stability.
[0104] (5) The curing procedure of Comparative Example 4 did not meet the requirements of this invention. The heating rate was too fast (10℃ / min and 15℃ / min, much higher than the 2℃ / min and 5℃ / min of this invention) and the holding time was insufficient (15 minutes and 30 minutes, much lower than the 30 minutes and 60 minutes of this invention). The results showed that the shear strength dropped to 34 MPa (a decrease of 19.0%), delamination occurred after only 80-90 thermal cycles, the wear rate increased by 48.6% to 0.52 mm / 10,000 cycles, and there were incompletely cross-linked areas inside the adhesive at 600℃, with the shear strength dropping to 22 MPa. This indicates that the segmented heating rate and holding time specified in this invention play a key role in ensuring that the adhesive is fully cross-linked and forms a dense bonding layer. The curing procedure deviating from the optimal parameters will lead to a significant decrease in adhesive performance.
[0105] (6) The performance differences between Examples 1 to 3 show that, within the parameter range defined in the claims, each parameter affects the final performance. Example 1 (with intermediate parameters) has the best overall performance, with a shear strength of 42 MPa and the lowest wear rate (0.35 mm / 10,000 bow strokes), indicating that the parameter range of the present invention was carefully designed to achieve the best balance among various performance characteristics.
[0106] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. An adhesive for bonding a metal substrate to a metal-impregnated carbon slide plate, characterized in that, By mass percentage, it includes the following components: 30-40% borate glass powder, 20-30% phenolic resin, 5-10% inorganic reinforcing filler, 2-5% curing accelerator, and the balance is organic solvent. The inorganic reinforcing filler includes at least one of boron nitride, graphene, and copper powder; The adhesive has a viscosity of 5000~8000 mPa·s at 25°C and a solid content of ≥75%.
2. The adhesive according to claim 1, characterized in that, The curing accelerator includes a titanate coupling agent.
3. The adhesive according to claim 1, characterized in that, The organic solvent includes xylene.
4. A method for bonding a metal substrate to a carbon-impregnated sliding plate, characterized in that, Includes the following steps: The metal matrix is roughened to obtain a roughened metal matrix; The adhesive according to any one of claims 1 to 4 is coated on the roughened metal substrate surface, and then a preheated metal-coated carbon slide plate is aligned and pressed with the substrate coated with adhesive to obtain an assembly; the coating thickness is 0.1 to 0.3 mm. The assembly is cured under vacuum or inert atmosphere protection; the curing procedure is as follows: the temperature is increased from room temperature to 180℃~200℃ at a rate of 2~3℃ / min and held for 28~32min, and then the temperature is increased to 550℃~600℃ at a rate of 4~5℃ / min and held for 58~62min.
5. The bonding method according to claim 4, characterized in that, The roughening process includes sandblasting.
6. The bonding method according to claim 5, characterized in that, The conditions for sandblasting include: sandblasting pressure of 0.3~0.5 MPa, sand particle size of 60~80 mesh, and sandblasting time of 5~10 min.
7. The bonding method according to claim 4, characterized in that, The pressing pressure is 5~10 MPa, and the holding time is 5~6 min.
8. The bonding method according to claim 4, characterized in that, When curing is performed under vacuum conditions, the vacuum level is ≤10Pa.
9. The bonding method according to claim 4, characterized in that, The metal matrix includes an aluminum alloy matrix.