Preparation method of corrosion-resistant non-oriented silicon steel for motor in high-corrosion environment

By employing precise alloy formulation and smelting, multi-stage surface pretreatment, and double-layer gradient coating, the problem of balancing corrosion resistance and magnetic properties of non-oriented silicon steel in highly corrosive environments has been solved, enabling stable operation of motors in such environments.

CN123063669APending Publication Date: 2026-11-10INNER MONGOLIA BAOTOU STEEL UNION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611195922.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing non-oriented silicon steel has insufficient corrosion resistance in highly corrosive environments, cannot achieve both magnetic properties and corrosion resistance, has poor coating adhesion, and weak process adaptability, thus failing to meet the long-term stable operation requirements of motors in highly corrosive environments.

Method used

By employing precise alloy formulation and smelting, combined with three-stage precision annealing and multi-level surface pretreatment, a double-layer gradient corrosion-resistant coating is prepared, including a bottom passivation protective layer and a top corrosion-resistant insulating layer. By controlling the amount of Cr and Ni trace alloying elements added, the substrate's resistance to pitting corrosion and oxidation is improved, and gradient high-temperature curing treatment ensures that the coating is tightly bonded.

Benefits of technology

The prepared non-oriented silicon steel exhibits excellent magnetic properties and corrosion resistance in highly corrosive environments such as marine salt spray and chemical acid and alkali vapors. It has strong coating adhesion and low iron loss, making it suitable for use in motors in highly corrosive environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application discloses a preparation method of a corrosion-resistant non-oriented silicon steel for a motor in a high-corrosion environment, and belongs to the technical field of electrical steel material preparation. The method comprises the following steps: precisely alloying and smelting: preparing molten steel raw materials according to mass percentages, wherein the raw material components comprise the following: Si: 2.8%-3.5%, Al: 0.25%-0.35%, Mn: 0.15%-0.25%, Cr: 0.12%-0.20%, Ni: 0.05%-0.10%, C<=0.003%, S<=0.002%, P<=0.01%, and the balance of Fe and inevitable impurities; casting blank homogenization treatment and hot rolling; cold rolling and precise annealing treatment; multi-stage surface pretreatment; double-layer gradient corrosion-resistant coating coating: gradient high-temperature solidification and finishing treatment. The application aims to overcome the defects of poor high-corrosion resistance of non-oriented silicon steel, the fact that the magnetic performance and corrosion resistance cannot be considered, the fact that the coating is easy to fall off and fail, and weak process adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrical steel material preparation technology, and particularly relates to a method for preparing corrosion-resistant non-oriented silicon steel for motors operating in highly corrosive environments. It is suitable for the large-scale preparation of non-oriented silicon steel for the core cores of industrial motors, marine drive motors, chemical explosion-proof motors, and wind power auxiliary motors operating under highly corrosive conditions such as marine salt spray, chemical acid and alkali vapors, and humid and polluted environments. Background Technology

[0002] Non-oriented silicon steel is the core magnetic material for motor cores. Its magnetic properties, mechanical properties, and corrosion resistance directly determine the motor's operational stability, service life, and maintenance costs. Conventional non-oriented silicon steel is only suitable for dry, clean indoor environments. In harsh environments with high salt spray, high humidity, and acid / alkali corrosion, the silicon steel substrate and surface insulating coating are highly susceptible to oxidation, pitting, peeling, and flaking. This leads to insulation failure in the motor core, a surge in magnetic losses, and severe overheating, ultimately causing short circuits and motor shutdowns. This severely restricts the long-term stable operation of electromechanical equipment under highly corrosive conditions. Currently, there is relevant research on the preparation of corrosion-resistant silicon steel in the industry. However, existing technologies generally suffer from insufficient corrosion resistance, an inability to balance magnetic properties and corrosion resistance, poor coating adhesion, and weak process adaptability, making it difficult to meet the stringent requirements of motors operating in highly corrosive environments.

[0003] Reference 1 (application number 202411124981.0) discloses a corrosion-resistant non-oriented silicon steel and its manufacturing method. This patent discloses that by optimizing the composition of the silicon steel matrix and adding trace amounts of chromium and nickel to improve the basic corrosion resistance of the silicon steel, and by combining it with a conventional organic insulating coating, corrosion-resistant non-oriented silicon steel can be prepared. This technology improves the corrosion resistance of the material through matrix alloying and enhances the oxidation resistance of silicon steel to a certain extent, but it has obvious defects: First, it relies only on trace alloy modification of the matrix and does not design a special protective coating for high salt spray and acid and alkali corrosion conditions. The surface protection layer of silicon steel is single, and local pitting corrosion is prone to occur in long-term high corrosion environment. Second, the annealing and coating curing parameters in the preparation process are adapted to conventional working conditions. The coating is not dense enough and has high porosity, which allows corrosive media to easily penetrate into the matrix and has poor resistance to long-term corrosion. Third, the amount of alloying elements added is limited. Excessive addition will lead to a decrease in the magnetic permeability of silicon steel and an increase in iron loss. It is impossible to balance corrosion resistance and magnetic properties, making it difficult to adapt to high-load and high-corrosion motor application scenarios.

[0004] Reference 2 (application number 202011372065.0) discloses a method for producing corrosion-resistant and high-efficiency non-oriented silicon steel. This patent adopts a process scheme of clean steel smelting, precise hot rolling temperature control, low-temperature annealing, and conventional inorganic coating to prepare non-oriented silicon steel with both magnetic properties and basic corrosion resistance. This technology optimizes the silicon steel rolling and annealing process, improves the uniformity of the matrix structure, and reduces the magnetic loss of the iron core. However, the technology has significant shortcomings: on the one hand, its surface inorganic coating system is simple and lacks modified protective structure, resulting in weak barrier ability against strong corrosive media such as chemical acid and alkali vapors and high-salt spray from the ocean. The coating is easily eroded and peeled off by corrosive media. On the other hand, the process does not include targeted surface activation and passivation pretreatment steps, resulting in weak adhesion between the coating and the silicon steel substrate. Under high-frequency vibration conditions of the motor, the coating is prone to cracking and peeling, and the protective performance fails rapidly. At the same time, the process does not optimize the coating thickness gradient for highly corrosive environments. Thin coatings provide insufficient protection, while thick coatings affect the stacked insulation and motor assembly accuracy, resulting in poor overall adaptability.

[0005] Existing non-oriented silicon steel preparation technologies generally suffer from problems such as low corrosion resistance, incompatibility between magnetic properties and corrosion resistance, poor coating protection stability, and insufficient adaptability to operating conditions. These issues cannot meet the requirements for long-term stable operation of motors in marine, chemical, and humid and hot highly corrosive environments. Therefore, there is an urgent need to develop a method for preparing non-oriented silicon steel for motors in highly corrosive environments that combines excellent magnetic properties, ultra-high corrosion resistance, and high coating adhesion. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing technologies, such as poor high corrosion resistance of non-oriented silicon steel, inability to balance magnetic properties and corrosion resistance, easy coating peeling and failure, and weak process adaptability, and to provide a method for preparing corrosion-resistant non-oriented silicon steel for motors in high corrosion environments.

[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0008] This invention discloses a method for preparing corrosion-resistant non-oriented silicon steel for motors used in highly corrosive environments, comprising the following steps:

[0009] Precision alloy batching and smelting: Steel raw materials are prepared according to mass percentages, with the following components: Si: 2.8%–3.5%, Al: 0.25%–0.35%, Mn: 0.15%–0.25%, Cr: 0.12%–0.20%, Ni: 0.05%–0.10%, C≤0.003%, S≤0.002%, P≤0.01%, with the balance being Fe and unavoidable impurities. Cr and Ni are core elements for corrosion resistance modification; their trace addition can enhance silicon content without degrading magnetic properties. The passivation ability and pitting corrosion resistance of the steel matrix, the Si and Al elements ensure the basic magnetic properties of silicon steel, and the extremely low C, S and P impurity content can avoid matrix grain boundary defects, reduce magnetic loss and corrosion induction points; the prepared raw materials are sent to a vacuum induction furnace for refining at a temperature of 1580-1620℃ for 25-35 minutes, with high-purity argon gas being introduced throughout the process to remove oxygen and nitrogen inclusions and harmful impurities from the molten steel, ensuring the purity of the molten steel; after refining, continuous casting is carried out to obtain silicon steel billets with a thickness of 200-240 mm;

[0010] Homogenization and hot rolling of the cast billet: The silicon steel cast billet is fed into a heating furnace for homogenization heating at a temperature of 1180–1220℃ and a holding time of 120–150 min to eliminate internal component segregation and internal stress, ensuring the uniformity of the matrix structure. After holding, hot rolling is carried out using a segmented hot rolling process. The roughing rolling start temperature is 1150–1180℃, the roughing rolling pass reduction rate is 65%–75%, the finishing rolling finish temperature is 880–920℃, and the finishing rolling total reduction rate is 85%–90%. After hot rolling, a hot-rolled silicon steel coil with a thickness of 2.0–2.5 mm is obtained. Subsequently, the hot-rolled steel coil is subjected to laminar flow cooling at a cooling rate of 12–18℃ / s. After cooling to room temperature, it is coiled to refine the matrix grains and optimize the basic structure of magnetic properties.

[0011] Cold rolling and precision annealing: Hot-rolled silicon steel coils are pickled to remove oxide scale at a temperature of 55–65℃ for 8–12 seconds, thoroughly removing the surface oxide layer without corroding the substrate. After pickling, multiple cold rolling passes are performed with a total cold rolling compression rate of 78%–82%, yielding thin silicon steel substrates with a thickness of 0.35 mm. The cold-rolled silicon steel substrates are then fed into a continuous annealing furnace for recrystallization annealing. The annealing process employs a three-stage temperature control: a preheating stage at 450–500℃ for 30–40 seconds, slowly increasing the temperature to eliminate rolling stress; a high-temperature annealing stage at 850–880℃ for 90–120 seconds, achieving complete recrystallization, refining grains, and reducing iron loss; and a slow cooling stage cooling to below 300℃ at a rate of 5–8℃ / s, followed by air cooling after removal from the furnace. This ensures that the silicon steel substrate possesses both excellent magnetic properties and a uniform matrix structure, providing a good substrate foundation for subsequent coating adhesion.

[0012] Multi-stage surface pretreatment: The annealed silicon steel substrate undergoes multi-stage refined pretreatment, including alkaline degreasing, water washing, acid activation, passivation, pure water rinsing, and hot air drying. Alkaline degreasing uses a composite degreasing solution of sodium carbonate, trisodium phosphate, and nonionic surfactant at a temperature of 50–55°C for 15–20 seconds to thoroughly remove surface oil and dust impurities. Acid activation uses a low-concentration nitric acid-hydrofluoric acid mixed activation solution for 5–8 seconds to slightly etch the substrate surface. This process creates a microscopic, rough structure, enhancing coating adhesion. Passivation treatment uses a chromate-molybdate composite passivation solution at a temperature of 40–45°C and a time of 10–15 seconds, forming a dense nano-passivation film on the silicon steel substrate surface. This seals microscopic defects on the substrate surface, initially improving the substrate's corrosion resistance. After pretreatment, the substrate is thoroughly rinsed with ultrapure water to prevent residual chemicals from corroding the substrate. Finally, it is dried in a hot air environment at 80–90°C to ensure the substrate surface is clean, free of moisture, and free of impurities.

[0013] Double-layer gradient corrosion-resistant coating: A double-sided roller coating method is used to prepare a double-layer gradient corrosion-resistant protective coating on the surface of the pretreated silicon steel substrate. The coating consists of a bottom passivation protective layer and a top corrosion-resistant insulating layer. The bottom passivation protective layer coating solution is composed of modified aluminum phosphate, nano titanium dioxide, boric acid, and deionized water, with a solid content of 18%–22% and a coating thickness of 2–3 μm. After coating, it is pre-cured at a temperature of 180–200℃ for 40–50 seconds. The top corrosion-resistant insulating layer coating solution is composed of modified epoxy resin, fluorocarbon resin, nano silica, composite phosphate, and environmentally friendly solvent, with a solid content of 25%–30% and a coating thickness of 4–6 μm. It relies on the acid and alkali resistance and salt spray resistance of fluorocarbon resin and the high adhesion and high insulation properties of epoxy resin to construct a high-strength external protective barrier. The total thickness of the double coating is controlled at 6–9 μm, with a reasonable thickness gradient, which ensures protective performance while avoiding excessive coating thickness from affecting the precision and insulation performance of silicon steel lamination.

[0014] Gradient high-temperature curing and finishing: The coated silicon steel undergoes segmented gradient high-temperature curing. The first stage of curing is at 220–240℃ for 60 seconds to fully cure the bottom layer coating and ensure a tight bond between the bottom layer and the substrate. The second stage of curing is at 280–300℃ for 90 seconds to achieve cross-linking and curing of the top layer coating, forming a dense, non-porous overall protective coating. After curing, the coating is slowly cooled to room temperature at a rate of 4–6℃ / s to prevent cracking and peeling due to excessive temperature difference. Finally, the cured silicon steel is subjected to stretching, straightening, edge trimming, and tension leveling to eliminate plate shape defects during production, ensuring a flat surface and dimensional accuracy of the silicon steel plate, ultimately producing a corrosion-resistant non-oriented silicon steel product for motors in highly corrosive environments.

[0015] Furthermore, the mass fractions of sodium carbonate, trisodium phosphate, and nonionic surfactant in the composite degreasing solution are 2%–5%, 1%–3%, and 0.2%–0.8%, respectively, with the remainder being deionized water.

[0016] Furthermore, the ingredients are proportioned by mass percentage as follows: Si: 3.0%, Al: 0.30%, Mn: 0.20%, Cr: 0.15%, Ni: 0.08%, C: 0.002%, S: 0.001%, P: 0.008%, with the balance being Fe and unavoidable impurities.

[0017] Furthermore, specifically:

[0018] The raw materials are fed into a vacuum induction furnace for refining at a temperature of 1600℃ for 30 minutes under high-purity argon protection, and then continuously cast to obtain a 220mm thick silicon steel billet.

[0019] Homogenization treatment and hot rolling of billet: billet heating temperature 1200℃, holding temperature for 135min; roughing rolling start temperature 1165℃, roughing rolling compression rate 70%; finishing rolling finish temperature 900℃, finishing rolling total compression rate 88%, hot rolling to obtain 2.2mm thick hot rolled steel coil; laminar flow cooling rate 15℃ / s, cooling to room temperature and coiling.

[0020] Cold rolling and precision annealing: Hydrochloric acid-sulfuric acid composite pickling is adopted, pickling temperature is 60℃, pickling time is 10s; total cold rolling compression rate is 80%, and 0.35mm thick silicon steel substrate is obtained; three-stage annealing: preheating stage 480℃, holding temperature for 35s, high temperature annealing stage 865℃, holding temperature for 105s, slow cooling stage 6℃ / s cooling to below 300℃, and air cooling after exiting the furnace;

[0021] Multi-stage surface pretreatment: alkaline degreasing at 52℃ for 18s; acidic activation for 6s; chromate-molybdate composite passivation at 42℃ for 12s; ultrapure water rinsing followed by hot air drying at 85℃, resulting in a clean substrate surface without residue.

[0022] Double-layer gradient corrosion-resistant coating: The bottom passivation protective layer has a solid content of 20% and a coating thickness of 2.5μm, and is pre-cured at 190℃ for 45s; the top corrosion-resistant insulating layer has a solid content of 28% and a coating thickness of 5μm, with a total coating thickness of 7.5μm.

[0023] Gradient high-temperature curing and finishing: the first stage of curing temperature is 230℃ and the holding time is 60s; the second stage of curing temperature is 290℃ and the holding time is 90s; the cooling rate is 5℃ / s to cool to room temperature; then the tensile straightening, edge trimming and tension leveling are performed to obtain the finished non-oriented silicon steel.

[0024] Performance test results: Iron loss P1.5 / 50=3.6W / kg, excellent magnetic properties; no corrosion or peeling after 1000h neutral salt spray test; coating adhesion grade 0; insulation resistance ≥1000Ω·cm.

[0025] Furthermore, the ingredients are proportioned by mass percentage as follows: Si: 2.8%, Al: 0.25%, Mn: 0.15%, Cr: 0.12%, Ni: 0.05%, C: 0.0025%, S: 0.0015%, P: 0.009%, with the balance being Fe and unavoidable impurities.

[0026] Furthermore, the refining temperature was 1580℃, the refining time was 35min, and the refining was carried out under argon protection before casting to obtain a 200mm thick silicon steel billet.

[0027] Homogenization treatment and hot rolling of billet: billet heating temperature 1180℃, holding temperature for 150min; roughing rolling start temperature 1150℃, roughing rolling compression rate 65%; finishing rolling finish temperature 880℃, finishing rolling total compression rate 85%, hot rolling to obtain 2.0mm thick hot rolled steel coil; laminar flow cooling rate 12℃ / s, room temperature coiling;

[0028] Cold rolling and precision annealing: pickling temperature 55℃, pickling time 12s; total cold rolling compression rate 78%, rolling 0.35mm silicon steel substrate; three-stage annealing: preheating stage 450℃, holding for 40s, high temperature annealing stage 850℃, holding for 120s, slow cooling stage 5℃ / s cooling to below 300℃, air cooling after exiting the furnace;

[0029] Multi-stage surface pretreatment: alkaline degreasing at 50℃ for 20s; acid activation for 5s; passivation at 40℃ for 15s; rinsing with ultrapure water followed by hot air drying at 80℃.

[0030] Double-layer gradient corrosion-resistant coating: bottom layer with 18% solid content, 2μm coating thickness, pre-cured at 180℃ for 50s; top layer with 25% solid content, 4μm coating thickness, total thickness of both layers is 6μm.

[0031] Gradient high-temperature curing and finishing: First stage curing at 220℃ for 60s, second stage curing at 280℃ for 90s; cooling rate of 4℃ / s to room temperature; after straightening, trimming, and leveling, the finished product is obtained;

[0032] Performance test results: Iron loss P1.5 / 50=3.5W / kg, magnetic loss is even lower; no corrosion after 850h of neutral salt spray test, excellent resistance to acid and alkali vapor corrosion; coating adhesion grade 0.

[0033] Furthermore, the ingredients are proportioned by mass percentage as follows: Si: 3.5%, Al: 0.35%, Mn: 0.25%, Cr: 0.20%, Ni: 0.10%, C: 0.002%, S: 0.001%, P: 0.007%, with the balance being Fe and unavoidable impurities.

[0034] Furthermore, the refining temperature was 1620℃, the refining time was 25 minutes, and high-purity argon gas was used for protection, resulting in a 240mm thick silicon steel billet.

[0035] Homogenization treatment and hot rolling of billet: billet heating temperature 1220℃, holding temperature for 120min; roughing rolling start temperature 1180℃, roughing rolling compression rate 75%; finishing rolling finish temperature 920℃, finishing rolling total compression rate 90%, hot rolling to obtain 2.5mm thick hot rolled steel coil; laminar flow cooling rate 18℃ / s, room temperature coiling;

[0036] Cold rolling and precision annealing: pickling temperature 65℃, pickling time 8s; total cold rolling compression rate 82%, rolling 0.35mm silicon steel substrate; three-stage annealing: preheating stage 500℃, holding for 30s, high temperature annealing stage 880℃, holding for 90s, slow cooling stage 8℃ / s cooling to below 300℃, air cooling after exiting the furnace;

[0037] Multi-stage surface pretreatment: alkaline degreasing at 55℃ for 15s; acid activation for 8s; passivation at 45℃ for 10s; rinsing with ultrapure water followed by hot air drying at 90℃.

[0038] Double-layer gradient corrosion-resistant coating: the bottom layer has a solid content of 22% and a coating thickness of 3μm, and is pre-cured at 200℃ for 40s; the top layer has a solid content of 30% and a coating thickness of 6μm, with a total thickness of 9μm for both layers.

[0039] Gradient high-temperature curing and finishing: First stage curing at 240℃ for 60s, second stage curing at 300℃ for 90s; cooling rate of 6℃ / s to room temperature; finished silicon steel is obtained after finishing.

[0040] Performance test results: Iron loss P1.5 / 50=3.7W / kg, magnetic properties are stable; no corrosion or blistering was observed after 1200h of neutral salt spray testing, indicating the best high corrosion resistance; the coating has excellent impact and vibration resistance.

[0041] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0042] This invention precisely controls the addition of trace corrosion-resistant alloying elements Cr and Ni, combined with low-impurity smelting and a three-stage precision annealing process. This not only improves the pitting corrosion and oxidation resistance of the silicon steel matrix through alloy modification, but also avoids the problems of decreased magnetic permeability and increased iron loss caused by excessive alloying elements. The resulting non-oriented silicon steel has an iron loss P1.5 / 50≤3.8W / kg and excellent magnetic permeability. It can also withstand strong corrosive environments such as marine salt spray and chemical acid and alkali vapors, completely solving the technical pain point of traditional corrosion-resistant silicon steel that cannot simultaneously achieve both magnetic properties and corrosion resistance. Detailed Implementation

[0043] Example 1

[0044] This embodiment provides a method for preparing corrosion-resistant non-oriented silicon steel for motors used in highly corrosive environments. The specific process steps are as follows:

[0045] Precision alloy batching and smelting: The raw materials are batched by mass percentage as follows: Si: 3.0%, Al: 0.30%, Mn: 0.20%, Cr: 0.15%, Ni: 0.08%, C: 0.002%, S: 0.001%, P: 0.008%, with the balance being Fe and unavoidable impurities. The raw materials are fed into a vacuum induction furnace for refining at a temperature of 1600℃ for 30 minutes under high-purity argon protection. Continuous casting yields a 220mm thick silicon steel billet.

[0046] Homogenization treatment and hot rolling of billet: The billet is heated to 1200℃ and held for 135 min; the roughing rolling start temperature is 1165℃ and the roughing rolling compression rate is 70%; the finishing rolling finish temperature is 900℃ and the finishing rolling total compression rate is 88%, and a 2.2 mm thick hot-rolled steel coil is obtained by hot rolling; the laminar flow cooling rate is 15℃ / s, and the coil is cooled to room temperature.

[0047] Cold rolling and precision annealing: Hydrochloric acid-sulfuric acid composite pickling is adopted, pickling temperature is 60℃, pickling time is 10s; total cold rolling compression rate is 80%, and 0.35mm thick silicon steel substrate is obtained; three-stage annealing: preheating stage 480℃, holding temperature for 35s, high temperature annealing stage 865℃, holding temperature for 105s, slow cooling stage 6℃ / s cooling to below 300℃, and air cooling after exiting the furnace.

[0048] Multi-stage surface pretreatment: alkaline degreasing at 52℃ for 18s; acidic activation for 6s; chromate-molybdate composite passivation at 42℃ for 12s; ultrapure water rinsing followed by hot air drying at 85℃, resulting in a clean substrate surface without residue.

[0049] Double-layer gradient corrosion-resistant coating: The bottom passivation protective layer has a solid content of 20% and a coating thickness of 2.5μm, and is pre-cured at 190℃ for 45s; the top corrosion-resistant insulating layer has a solid content of 28% and a coating thickness of 5μm, with a total coating thickness of 7.5μm.

[0050] Gradient high-temperature curing and finishing: the first stage of curing temperature is 230℃ and the holding time is 60s; the second stage of curing temperature is 290℃ and the holding time is 90s; the cooling rate is 5℃ / s to cool to room temperature; then stretching, straightening, trimming and finishing are performed to obtain the finished non-oriented silicon steel.

[0051] The performance test results of the silicon steel prepared in this embodiment are as follows: iron loss P1.5 / 50=3.6W / kg, excellent magnetic properties; no corrosion or peeling after 1000h neutral salt spray test; coating adhesion grade 0; insulation resistance ≥1000Ω·cm.

[0052] Example 2

[0053] This embodiment provides a method for preparing corrosion-resistant non-oriented silicon steel for motors used in highly corrosive environments. The specific process steps are as follows:

[0054] Precision alloy batching and smelting: The alloy is batched by mass percentage as follows: Si: 2.8%, Al: 0.25%, Mn: 0.15%, Cr: 0.12%, Ni: 0.05%, C: 0.0025%, S: 0.0015%, P: 0.009%, with the balance being Fe and unavoidable impurities; the refining temperature is 1580℃, the refining time is 35min, and the refining is carried out under argon protection before casting to obtain a 200mm thick silicon steel billet.

[0055] Homogenization treatment and hot rolling of billet: billet heating temperature 1180℃, holding temperature 150min; roughing rolling start temperature 1150℃, roughing rolling compression rate 65%; finishing rolling finish temperature 880℃, finishing rolling total compression rate 85%, hot rolling to obtain 2.0mm thick hot rolled steel coil; laminar flow cooling rate 12℃ / s, room temperature coiling.

[0056] Cold rolling and precision annealing: pickling temperature 55℃, pickling time 12s; total cold rolling compression rate 78%, rolling 0.35mm silicon steel substrate; three-stage annealing: preheating stage 450℃, holding for 40s, high-temperature annealing stage 850℃, holding for 120s, slow cooling stage 5℃ / s cooling to below 300℃, air cooling after exiting the furnace.

[0057] Multi-stage surface pretreatment: alkaline degreasing at 50℃ for 20s; acid activation for 5s; passivation at 40℃ for 15s; rinsing with ultrapure water followed by hot air drying at 80℃.

[0058] Double-layer gradient corrosion-resistant coating: the bottom layer has a solid content of 18% and a coating thickness of 2μm, and is pre-cured at 180℃ for 50s; the top layer has a solid content of 25% and a coating thickness of 4μm, with a total double-layer thickness of 6μm.

[0059] Gradient high-temperature curing and finishing: the first stage of curing is at 220℃ and held for 60s, the second stage of curing is at 280℃ and held for 90s; the cooling rate is 4℃ / s to cool to room temperature; the finished product is obtained after straightening, trimming and leveling.

[0060] The performance test results of the silicon steel prepared in this embodiment are as follows: iron loss P1.5 / 50=3.5W / kg, magnetic loss is even lower; no corrosion was observed after 850h of neutral salt spray test, and the corrosion resistance of acid and alkali vapors is excellent; the coating adhesion is grade 0.

[0061] Example 3

[0062] This embodiment provides a method for preparing corrosion-resistant non-oriented silicon steel for motors used in highly corrosive environments. The specific process steps are as follows:

[0063] Precision alloy batching and smelting: The alloy is batched by mass percentage as follows: Si: 3.5%, Al: 0.35%, Mn: 0.25%, Cr: 0.20%, Ni: 0.10%, C: 0.002%, S: 0.001%, P: 0.007%, with the balance being Fe and unavoidable impurities; the refining temperature is 1620℃, the refining time is 25min, and high-purity argon gas is used for protection, resulting in a 240mm thick silicon steel billet.

[0064] Homogenization treatment and hot rolling of billet: billet heating temperature 1220℃, holding temperature for 120min; roughing rolling start temperature 1180℃, roughing rolling compression rate 75%; finishing rolling finish temperature 920℃, finishing rolling total compression rate 90%, hot rolling to obtain 2.5mm thick hot rolled steel coil; laminar flow cooling rate 18℃ / s, room temperature coiling.

[0065] Cold rolling and precision annealing: pickling temperature 65℃, pickling time 8s; total cold rolling compression rate 82%, rolling 0.35mm silicon steel substrate; three-stage annealing: preheating stage 500℃, holding for 30s, high-temperature annealing stage 880℃, holding for 90s, slow cooling stage 8℃ / s cooling to below 300℃, air cooling after exiting the furnace.

[0066] Multi-stage surface pretreatment: alkaline degreasing at 55℃ for 15s; acidic activation for 8s; passivation at 45℃ for 10s; rinsing with ultrapure water followed by hot air drying at 90℃.

[0067] Double-layer gradient corrosion-resistant coating: the bottom layer has a solid content of 22% and a coating thickness of 3μm, and is pre-cured at 200℃ for 40s; the top layer has a solid content of 30% and a coating thickness of 6μm, with a total double-layer thickness of 9μm.

[0068] Gradient high-temperature curing and finishing: the first stage of curing is at 240℃ and held for 60s, the second stage of curing is at 300℃ and held for 90s; the cooling rate is 6℃ / s to cool to room temperature; after finishing, the finished silicon steel is obtained.

[0069] The performance test results of the silicon steel prepared in this embodiment are as follows: iron loss P1.5 / 50=3.7W / kg, stable magnetic properties; no corrosion or blistering after 1200h of neutral salt spray test, indicating the best high corrosion resistance; and excellent impact and vibration resistance of the coating.

[0070] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for preparing corrosion-resistant non-oriented silicon steel for motors operating in highly corrosive environments, characterized in that: Includes the following steps: Precision alloy batching and smelting: Steel raw materials are prepared according to mass percentages, with the following components: Si: 2.8%–3.5%, Al: 0.25%–0.35%, Mn: 0.15%–0.25%, Cr: 0.12%–0.20%, Ni: 0.05%–0.10%, C≤0.003%, S≤0.002%, P≤0.01%, with the balance being Fe and unavoidable impurities. The prepared raw materials are then sent to a vacuum induction furnace for refining at a temperature of 1580–1620℃ for 25–35 minutes, with high-purity argon gas used throughout the process to remove oxygen and nitrogen inclusions and harmful impurities from the steel, ensuring the purity of the steel. After refining, continuous casting is performed to obtain silicon steel billets with a thickness of 200–240 mm. Homogenization and hot rolling of the cast billet: The silicon steel cast billet is fed into a heating furnace for homogenization heating at a temperature of 1180–1220℃ and a holding time of 120–150 min to eliminate internal component segregation and internal stress, ensuring the uniformity of the matrix structure. After holding, hot rolling is carried out using a segmented hot rolling process. The roughing rolling start temperature is 1150–1180℃, the roughing rolling pass reduction rate is 65%–75%, the finishing rolling finish temperature is 880–920℃, and the finishing rolling total reduction rate is 85%–90%. After hot rolling, a hot-rolled silicon steel coil with a thickness of 2.0–2.5 mm is obtained. Subsequently, the hot-rolled steel coil is subjected to laminar flow cooling at a cooling rate of 12–18℃ / s. After cooling to room temperature, it is coiled to refine the matrix grains and optimize the basic structure of magnetic properties. Cold rolling and precision annealing: Hot-rolled silicon steel coils are pickled to remove oxide scale at a temperature of 55–65℃ for 8–12 seconds, thoroughly removing the surface oxide layer without corroding the substrate. After pickling, multiple cold rolling passes are performed with a total cold rolling compression rate of 78%–82%, yielding thin silicon steel substrates with a thickness of 0.35 mm. The cold-rolled silicon steel substrates are then fed into a continuous annealing furnace for recrystallization annealing. The annealing process employs a three-stage temperature control: a preheating stage at 450–500℃ for 30–40 seconds, slowly increasing the temperature to eliminate rolling stress; a high-temperature annealing stage at 850–880℃ for 90–120 seconds, achieving complete recrystallization, refining grains, and reducing iron loss; and a slow cooling stage cooling to below 300℃ at a rate of 5–8℃ / s, followed by air cooling after removal from the furnace. This ensures that the silicon steel substrate possesses both excellent magnetic properties and a uniform matrix structure, providing a good substrate foundation for subsequent coating adhesion. Multi-stage surface pretreatment: The annealed silicon steel substrate undergoes multi-stage refined pretreatment, including alkaline degreasing, water washing, acid activation, passivation, pure water rinsing, and hot air drying. Alkaline degreasing uses a composite degreasing solution of sodium carbonate, trisodium phosphate, and nonionic surfactant at a temperature of 50–55°C for 15–20 seconds to thoroughly remove surface oil and dust impurities. Acid activation uses a low-concentration nitric acid-hydrofluoric acid mixed activation solution for 5–8 seconds to slightly etch the substrate surface. This process creates a microscopic, rough structure, enhancing coating adhesion. Passivation treatment uses a chromate-molybdate composite passivation solution at a temperature of 40–45°C and a time of 10–15 seconds, forming a dense nano-passivation film on the silicon steel substrate surface. This seals microscopic defects on the substrate surface, initially improving the substrate's corrosion resistance. After pretreatment, the substrate is thoroughly rinsed with ultrapure water to prevent residual chemicals from corroding the substrate. Finally, it is dried in a hot air environment at 80–90°C to ensure the substrate surface is clean, free of moisture, and free of impurities. Double-layer gradient corrosion-resistant coating: A double-sided roller coating method is used to prepare a double-layer gradient corrosion-resistant protective coating on the surface of the pretreated silicon steel substrate. The coating consists of a bottom passivation protective layer and a top corrosion-resistant insulating layer. The bottom passivation protective layer coating solution is composed of modified aluminum phosphate, nano titanium dioxide, boric acid, and deionized water, with a solid content of 18%–22% and a coating thickness of 2–3 μm. After coating, it is pre-cured at a temperature of 180–200℃ for 40–50 seconds. The top corrosion-resistant insulating layer coating solution is composed of modified epoxy resin, fluorocarbon resin, nano silica, composite phosphate, and environmentally friendly solvent, with a solid content of 25%–30% and a coating thickness of 4–6 μm. It relies on the acid and alkali resistance and salt spray resistance of fluorocarbon resin and the high adhesion and high insulation properties of epoxy resin to construct a high-strength external protective barrier. The total thickness of the double coating is controlled at 6–9 μm, with a reasonable thickness gradient, which ensures protective performance while avoiding excessive coating thickness from affecting the precision and insulation performance of silicon steel lamination. Gradient high-temperature curing and finishing: The coated silicon steel undergoes segmented gradient high-temperature curing. The first stage of curing is at 220–240℃ for 60 seconds to fully cure the undercoat and ensure a tight bond between the undercoat and the substrate. The second stage of curing is at 280–300℃ for 90 seconds to achieve cross-linking of the topcoat. The coating is cured to form a dense, non-porous overall protective coating. After curing, it is slowly cooled to room temperature at a rate of 4-6℃ / s to avoid cracking and peeling of the coating due to excessive temperature difference. Finally, the cured silicon steel is subjected to stretching, straightening, edge trimming, and tension leveling to eliminate plate shape defects in the production process, ensure that the silicon steel plate surface is flat and the dimensional accuracy meets the standards, and finally obtain corrosion-resistant non-oriented silicon steel finished products for motors in high-corrosion environments.

2. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 1, characterized in that: The composite degreasing solution contains sodium carbonate, trisodium phosphate, and nonionic surfactant at mass fractions of 2%–5%, 1%–3%, and 0.2%–0.8%, respectively, with the remainder being deionized water.

3. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 1, characterized in that: The ingredients are proportioned by weight as follows: Si: 3.0%, Al: 0.30%, Mn: 0.20%, Cr: 0.15%, Ni: 0.08%, C: 0.002%, S: 0.001%, P: 0.008%, with the balance being Fe and unavoidable impurities.

4. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 3, characterized in that: Specifically: The raw materials are fed into a vacuum induction furnace for refining at a temperature of 1600℃ for 30 minutes under high-purity argon protection, and then continuously cast to obtain a 220mm thick silicon steel billet. Homogenization treatment and hot rolling of billet: billet heating temperature 1200℃, holding temperature for 135min; roughing rolling start temperature 1165℃, roughing rolling compression rate 70%; finishing rolling finish temperature 900℃, finishing rolling total compression rate 88%, hot rolling to obtain 2.2mm thick hot rolled steel coil; laminar flow cooling rate 15℃ / s, cooling to room temperature and coiling. Cold rolling and precision annealing: Hydrochloric acid-sulfuric acid composite pickling is adopted, pickling temperature is 60℃, pickling time is 10s; total cold rolling compression rate is 80%, and 0.35mm thick silicon steel substrate is obtained; three-stage annealing: preheating stage 480℃, holding temperature for 35s, high temperature annealing stage 865℃, holding temperature for 105s, slow cooling stage 6℃ / s cooling to below 300℃, and air cooling after exiting the furnace; Multi-stage surface pretreatment: alkaline degreasing at 52℃ for 18s; acidic activation for 6s; chromate-molybdate composite passivation at 42℃ for 12s; ultrapure water rinsing followed by hot air drying at 85℃, resulting in a clean substrate surface without residue. Double-layer gradient corrosion-resistant coating: The bottom passivation protective layer has a solid content of 20% and a coating thickness of 2.5μm, and is pre-cured at 190℃ for 45s; the top corrosion-resistant insulating layer has a solid content of 28% and a coating thickness of 5μm, with a total coating thickness of 7.5μm. Gradient high-temperature curing and finishing: the first stage of curing temperature is 230℃ and the holding time is 60s; the second stage of curing temperature is 290℃ and the holding time is 90s; the cooling rate is 5℃ / s to cool to room temperature; then the tensile straightening, edge trimming and tension leveling are performed to obtain the finished non-oriented silicon steel. Performance test results: Iron loss P1.5 / 50=3.6W / kg, excellent magnetic properties; no corrosion or peeling after 1000h neutral salt spray test; coating adhesion grade 0; insulation resistance ≥1000Ω·cm.

5. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 1, characterized in that: The ingredients are proportioned by weight as follows: Si: 2.8%, Al: 0.25%, Mn: 0.15%, Cr: 0.12%, Ni: 0.05%, C: 0.0025%, S: 0.0015%, P: 0.009%, with the balance being Fe and unavoidable impurities.

6. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 5, characterized in that: Specifically: The refining temperature was 1580℃, the refining time was 35min, and the silicon steel billet was cast after argon protection. Homogenization and hot rolling of billet: billet heating temperature 1180℃, holding temperature for 150min; The roughing rolling temperature is 1150℃, and the roughing compression rate is 65%; the finishing rolling temperature is 880℃, and the total finishing compression rate is 85%, resulting in a 2.0mm thick hot-rolled steel coil; the laminar flow cooling rate is 12℃ / s, and the coil is wound at room temperature. Cold rolling and precision annealing: pickling temperature 55℃, pickling time 12s; The total cold rolling compression rate is 78%, and 0.35mm silicon steel substrate is rolled; three-stage annealing: preheating stage 450℃, holding for 40s, high temperature annealing stage 850℃, holding for 120s, slow cooling stage 5℃ / s cooling to below 300℃, and air cooling after exiting the furnace. Multi-stage surface pretreatment: alkaline degreasing at 50℃ for 20s; acid activation for 5s; passivation at 40℃ for 15s; rinsing with ultrapure water followed by hot air drying at 80℃. Double-layer gradient corrosion-resistant coating: bottom layer with 18% solid content, 2μm coating thickness, pre-cured at 180℃ for 50s; top layer with 25% solid content, 4μm coating thickness, total thickness of both layers is 6μm. Gradient high-temperature curing and finishing: First stage curing at 220℃ for 60s, second stage curing at 280℃ for 90s; cooling rate of 4℃ / s to room temperature; after straightening, trimming, and leveling, the finished product is obtained; Performance test results: Iron loss P1.5 / 50=3.5W / kg, magnetic loss is even lower; no corrosion after 850h of neutral salt spray test, excellent resistance to acid and alkali vapor corrosion; coating adhesion grade 0.

7. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 1, characterized in that: The ingredients are proportioned by weight as follows: Si: 3.5%, Al: 0.35%, Mn: 0.25%, Cr: 0.20%, Ni: 0.10%, C: 0.002%, S: 0.001%, P: 0.007%, with the balance being Fe and unavoidable impurities.

8. The method for preparing corrosion-resistant non-oriented silicon steel for motors in highly corrosive environments according to claim 7, characterized in that: Specifically: The refining temperature was 1620℃, the refining time was 25min, and high-purity argon gas was used for protection to cast a 240mm thick silicon steel billet. Homogenization treatment and hot rolling of billet: billet heating temperature 1220℃, holding temperature for 120min; The roughing rolling temperature is 1180℃, and the roughing compression rate is 75%; the finishing rolling temperature is 920℃, and the total finishing compression rate is 90%, resulting in a 2.5mm thick hot-rolled steel coil; the laminar flow cooling rate is 18℃ / s, and the coil is wound at room temperature. Cold rolling and precision annealing: pickling temperature 65℃, pickling time 8s; total cold rolling compression rate 82%, rolling 0.35mm silicon steel substrate; three-stage annealing: preheating stage 500℃, holding for 30s, high temperature annealing stage 880℃, holding for 90s, slow cooling stage 8℃ / s cooling to below 300℃, air cooling after exiting the furnace; Multi-stage surface pretreatment: alkaline degreasing at 55℃ for 15s; acid activation for 8s; passivation at 45℃ for 10s; rinsing with ultrapure water followed by hot air drying at 90℃. Double-layer gradient corrosion-resistant coating: the bottom layer has a solid content of 22% and a coating thickness of 3μm, and is pre-cured at 200℃ for 40s; the top layer has a solid content of 30% and a coating thickness of 6μm, with a total thickness of 9μm for both layers. Gradient high-temperature curing and finishing: First stage curing at 240℃ for 60s, second stage curing at 300℃ for 90s; cooling rate of 6℃ / s to room temperature; finished silicon steel is obtained after finishing. Performance test results: Iron loss P1.5 / 50=3.7W / kg, magnetic properties are stable; no corrosion or blistering was observed after 1200h of neutral salt spray testing, indicating the best high corrosion resistance; the coating has excellent impact and vibration resistance.

Citation Information

Patent Citations

  • Non-oriented silicon steel plate with excellent corrosion resistance for high-efficiency motor and production method

    CN112609128A

  • A production method for corrosion-resistant and high-efficiency non-oriented silicon steel

    CN118639119B