Nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distributor plate and its preparation method
By using nickel-chromium-molybdenum-vanadium self-lubricating ductile iron material and a stepped quenching and tempering process, the problem of insufficient strength retention of the distribution plate material under high temperature conditions was solved, achieving a balance between self-lubricating performance and high-temperature toughness, thus improving the stability and lifespan of the hydraulic motor.
Patent Information
- Application Number
- CN202611522024.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-10
AI Technical Summary
Existing distribution plate materials have insufficient strength retention under high temperature, high pressure and alternating load conditions. After heat treatment, it is difficult to balance strength and toughness, which leads to adhesive wear and internal leakage of the friction pair, affecting the stability and life of the hydraulic motor.
Using nickel-chromium-molybdenum-vanadium self-lubricating ductile iron material, through specific composition design and stepped quenching and tempering process, fine dispersed carbides and spherical graphite are formed, which improves the self-lubricating performance and high-temperature toughness of the material, and avoids the use of toxic elements such as lead.
It achieves excellent self-lubricating properties of materials under high temperature conditions, synergistic high-temperature strength and toughness, strict control of impurities, reduces equipment maintenance frequency, and improves the volumetric efficiency and output stability of hydraulic motors.
Smart Images

Figure CN123063679A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydraulic motor component material manufacturing technology, specifically relating to nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distributor plates, and also relating to a method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distributor plates. Background Technology
[0002] Piston-type hydraulic motors are core actuators in the hydraulic power systems of high-temperature industrial equipment such as metallurgical die casting and thermoforming equipment. Their distributor plate and cylinder end face form a critical friction pair, continuously undergoing high-speed relative sliding and grinding during equipment operation, and alternately enduring the coupled effects of high-pressure alternating extrusion loads and cyclical temperature changes. In hydraulic equipment used in metallurgy, die casting, and thermoforming, the working medium temperature can reach 200–500℃. The friction pair simultaneously bears the multiple coupled effects of high temperature, high pressure, high speed, and alternating stress, making the operating conditions extremely harsh. The service reliability of the distributor plate directly determines the volumetric efficiency, output stability, and overall lifespan of the hydraulic motor. Once the friction pair softens, adheres, or experiences abnormal wear, it can lead to increased internal leakage and decreased efficiency, or even serious accidents such as plate burnout, seizure, or complete machine shutdown. Therefore, developing distributor plate materials that combine high temperature, high strength, toughness, built-in self-lubrication, and high resistance to adhesive wear is a crucial technological bottleneck that urgently needs to be overcome in the field of high-temperature hydraulic equipment.
[0003] However, current mainstream distribution plate materials all have inherent defects that are difficult to overcome, and cannot simultaneously meet the above core requirements: lead bronze bimetallic distribution plates rely on lead-containing phases in the matrix to improve friction performance, but the load-bearing capacity of the copper alloy matrix decreases with increasing temperature; at the same time, lead poses environmental and occupational health risks during manufacturing and use. Ordinary QT700 ductile iron does not undergo Mo, V, and other alloying and heat treatment control for high-temperature service, and is prone to matrix softening and uneven carbide distribution at higher temperatures, resulting in insufficient high-temperature strength retention and wear resistance. Quenched carbon steel distribution plates do not contain spheroidal graphite solid lubricating phases, and when the lubricating oil film is insufficient, adhesive wear easily occurs on the friction pair surface, affecting the operational stability of the distribution plate. Although existing isothermal quenched ductile iron has good room temperature strength and toughness, its high-temperature microstructure stability is affected by the matrix composition and tempering process, and may undergo microstructure transformation and performance degradation under long-term heating. Therefore, it is necessary to achieve stable strengthened matrix and dispersed carbides while retaining spheroidal graphite through synergistic control of alloy composition design and heat treatment process.
[0004] In summary, existing ductile iron for distribution plates suffers from insufficient strength retention under high-temperature service conditions and difficulty in achieving both strength and toughness after heat treatment, making it difficult to meet the long-term stable service requirements of distribution plates under high temperature, high pressure, and alternating load conditions. Summary of the Invention
[0005] One objective of this invention is to provide nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates, which solves the problems of insufficient strength retention of existing ductile iron distribution plates under high-temperature conditions and difficulty in achieving both strength and toughness after heat treatment.
[0006] Another object of the present invention is to provide a method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates.
[0007] The first technical solution adopted in this invention is that the hydraulic motor distribution plate is made of nickel-chromium-molybdenum-vanadium self-lubricating ductile iron. The raw materials include the following by mass percentage: C: 3.50%~3.55%, Si: 3.10%~3.20%, Ni: 1.6%~1.70%, Cr: 0.35%~0.40%, Mo: 1.10%~1.15%, V: 0.55%~0.60%, with the balance being Fe and unavoidable impurities. The unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0008] The second technical solution adopted in this invention is a method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates, specifically as follows: Step 1: Weigh the raw materials according to the mass fraction percentage of each component. Step 2: Prepare a blank from the raw materials weighed in Step 1; Step 3: High-temperature austenite homogenization treatment is performed; Step 4: The treated sample is then subjected to a stepped quenching process. Step 5: The quenched distribution plate blank is then subjected to a stepped tempering process to obtain the final product.
[0009] The invention is further characterized in that: Step 1 is as follows: Weigh the raw materials according to the mass percentage of each component, including C: 3.50%~3.55%, Si: 3.10%~3.20%, Ni: 1.6%~1.70%, Cr: 0.35%~0.40%, Mo: 1.10%~1.15%, V: 0.55%~0.60%, with the balance being Fe and unavoidable impurities. Unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0010] In step 2, the raw materials are smelted to obtain molten iron, which is then subjected to simultaneous wire feeding, spheroidization, and inoculation treatment. The treated molten iron is then introduced into a horizontal continuous casting crystallizer equipped with an ultrasonic oscillation device and a water cooling device, and continuously drawn to obtain profiles. After the profiles are cooled, they are machined into distribution plate blanks.
[0011] Step 3: Place the machined distribution plate blank from Step 2 into an argon-protected furnace, evacuate the furnace, and introduce argon gas for protection.
[0012] Increase the temperature to 1000℃~1100℃ at a rate of 6℃ / min and hold for 8h~8.5h.
[0013] Step 4: Cool the temperature to 850℃~900℃ at a uniform step rate of 2℃ / min, maintain the temperature for 1h~4h, and immediately cool it to room temperature with water after the heat preservation is completed.
[0014] Step 5: Heat to 500℃, hold for 1 hour, then air cool to room temperature. Perform two air cooling cycles to complete the tempering process.
[0015] The beneficial effects of the present invention are as follows: 1. Excellent self-lubricating performance: The high carbon-silicon ratio stably generates high-density spherical graphite. When the distribution plate is rubbed at high speed, the graphite is continuously transferred to the friction interface to form self-lubrication. Under the dry friction condition of hydraulic oil film rupture, the cylinder and distribution plate will not stick and seize. Toxic lubricating elements such as lead are eliminated, making it environmentally friendly and safe. 2. High temperature and toughness synergy: Low Cr combined with high Ni composite system avoids casting white iron and network brittle carbide caused by high Cr; Mo and V composite precipitation of fine and dispersed carbides; 3. Strict impurity control: Mn, P and S are in extremely low limits, eliminating grain boundary phosphorus eutectic and brittle sulfide phases. The distribution plate is precision ground without microcracks, and the high-pressure alternating fatigue life is greatly improved. 4. The stepped quenching and tempering heat treatment process thoroughly eliminates casting composition segregation through long-term homogenization, solving the defects of ordinary ductile iron such as carbides cutting the matrix and poor toughness; stepped quenching can control the precipitation of nano carbides, balance the ratio of martensite and retained austenite, and achieve a stable quenching hardness of over 60 HRC; two tempering processes at 500℃ are suitable for high-temperature service temperatures, fully releasing quenching stress, dispersing alloy carbides and continuously precipitating, taking into account the comprehensive mechanical properties at room temperature and high temperature, without the need for additional nitriding and boronizing surface strengthening processes, thus reducing processing costs; 5. The high-temperature hydraulic motor distribution plate made of this material, compared with bronze distribution plates and ordinary ductile iron distribution plates, is suitable for high-temperature plunger hydraulic motors used in metallurgy, die casting, and thermoforming equipment, significantly reducing the frequency of equipment maintenance and replacement. Attached Figure Description
[0016] Figure 1(a) is the OM diagram of the 1000℃ stepped quenched sample in Example 4 of the present invention; Figure 1(b) is the OM diagram of the 950℃ stepped quenched sample in Example 4 of the present invention; Figure 1(c) is the OM diagram of the 900℃ stepped quenched sample in Example 4 of the present invention; Figure 1(d) is the OM diagram of the 850℃ stepped quenched sample in Example 4 of the present invention; Figure 2(a) is a SEM image of the 1000℃ stepped quenched sample in Example 4 of the present invention; Figure 2(b) is a SEM image of the 950℃ stepped quenched sample in Example 4 of the present invention; Figure 2(c) is a SEM image of the 900℃ stepped quenched sample in Example 4 of the present invention; Figure 2(d) is a SEM image of the 850℃ stepped quenched sample in Example 4 of the present invention; Figure 3(a) is the OM diagram of the sample in the stepped quenched state at 1000℃ after tempering at 500℃×1h in Example 5 of the present invention; Figure 3(b) is the OM diagram of the sample in the stepped quenched state at 950℃ after tempering at 500℃ for 1h in Example 5 of the present invention; Figure 3(c) is the OM diagram of the sample in the stepped quenched state at 900℃ after tempering at 500℃ for 1h in Example 5 of the present invention. Figure 3(d) is the OM diagram of the sample in the stepped quenched state at 850℃ after tempering at 500℃ for 1h in Example 5 of the present invention. Figure 4(a) is a SEM image of the stepped cooling sample of the present invention after tempering at 500℃ for 1 hour and then stepped quenching at 1000℃. Figure 4(b) is a SEM image of the stepped cooling sample of the present invention after tempering at 500℃ for 1 hour and then step-quenched at 950℃. Figure 4(c) is a SEM image of the stepped cooling sample of the present invention after tempering at 500℃ for 1 hour and then step-quenching at 900℃. Figure 4(d) is a SEM image of the stepped cooling sample of the present invention after tempering at 500℃ for 1 hour and then step-quenched at 850℃. Figure 5(a) is the OM diagram of the stepped cooling sample of the present invention after being tempered twice at 500℃ for 1 hour and then stepped quenched at 1000℃. Figure 5(b) is the OM diagram of the stepped cooling sample of the present invention after being tempered twice at 500℃ for 1 hour and then stepped quenched at 950℃. Figure 5(c) is the OM diagram of the stepped cooling sample of the present invention after being tempered twice at 500℃ for 1 hour and then stepped quenched at 900℃. Figure 5(d) is the OM diagram of the stepped cooling sample of the present invention after being tempered twice at 500℃ for 1 hour and then stepped quenched at 850℃. Figure 6(a) is a SEM image of the sample of the present invention after being tempered twice at 500 ℃ for 1 h and then stepped quenched at 1000 ℃. Figure 6(b) is a SEM image of the sample of the present invention after being tempered twice at 500 ℃ for 1 h and then stepped quenched at 950 ℃. Figure 6(c) is a SEM image of the sample of the present invention after being tempered twice at 500 ℃ for 1 h and then stepped quenched at 900 ℃. Figure 6(d) is a SEM image of the sample of the present invention after being tempered twice at 500 ℃ for 1 h and then stepped quenched at 850 ℃. Figure 7 The graph shows the changes in tensile strength and elongation of the stepped-cooled specimens after tempering at 500℃ for different times. Figure 8 The graph shows the changes in compressive strength and compression amount of the stepped cooling sample after tempering at 500℃ for different times. Detailed Implementation
[0017] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0018] This invention provides nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates. The raw materials, by mass fraction percentage, include: C: 3.50%~3.55%, Si: 3.10%~3.20%, Ni: 1.6%~1.70%, Cr: 0.35%~0.40%, Mo: 1.10%~1.15%, V: 0.55%~0.60%, with the balance being Fe and unavoidable impurities. The unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0019] The hydraulic motor distributor plate of this invention uses nickel-chromium-molybdenum-vanadium self-lubricating ductile iron. By adding elements such as Cr, Mo, and V, it is easy to combine with iron and carbon atoms to form mixed carbides, which have a higher hardness than cementite. The presence of high-hardness mixed carbides and dispersed blocky or dot-shaped carbides in the matrix enhances the microhardness of ferrite and pearlite, resulting in a higher overall hardness of the sample. On the other hand, the use of Ni element can improve the hardenability of the steel, thereby increasing the hardness and strength of the steel in the quenched state.
[0020] This invention also provides a method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates, specifically: Step 1: Weigh the raw materials according to the mass fraction percentage of each component. Step 1 is as follows: Weigh the raw materials according to the mass percentage of each component, including C: 3.50%~3.55%, Si: 3.10%~3.20%, Ni: 1.6%~1.70%, Cr: 0.35%~0.40%, Mo: 1.10%~1.15%, V: 0.55%~0.60%, with the balance being Fe and unavoidable impurities. Unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0021] Step 2: Prepare a blank from the raw materials weighed in Step 1; The weighed raw materials are smelted to obtain molten iron, which is then subjected to simultaneous wire feeding, spheroidization, and inoculation treatment. The treated molten iron is then introduced into a horizontal continuous casting crystallizer equipped with an ultrasonic oscillation device and a water cooling device, and continuously drawn to obtain nickel-chromium-molybdenum-vanadium ductile iron profiles. After the profiles are cooled, they are machined according to the dimensions of the distribution plate to obtain the distribution plate blank.
[0022] Step 3: High-temperature austenite homogenization treatment is performed; The distribution plate blank obtained in step 2 is placed in an argon-protected furnace. After evacuation, argon gas is introduced and heated to the homogenization temperature at a set heating rate and held at that temperature. The temperature is then increased to 1000℃~1100℃ at a rate of 6℃ / min and held for 8h~8.5h.
[0023] High-temperature austenite homogenization treatment can promote the reduction of casting component segregation and the dissolution of some coarse carbides, making the alloying elements more uniform in austenite, creating conditions for the formation of fine and dispersed carbides during subsequent quenching and tempering processes.
[0024] Step 4: The treated sample is then subjected to a stepped quenching process. The temperature is gradually reduced to 850℃~900℃ at a constant rate of 2℃ / min, and held at that temperature for 1h~4h. After the holding period, the temperature is immediately and rapidly water-cooled to room temperature. This process yields more martensite than direct quenching, and increases the amount of dispersed dotted carbides in the microstructure. Solid-solution carbon combines with alloying elements to form alloy carbides.
[0025] Step 5: The quenched distribution plate blank is then subjected to a stepped tempering process to obtain the final product.
[0026] The temperature is raised to 500℃, held for 1 to 1.5 hours, and then air-cooled to room temperature. The tempering is completed by air-cooling twice, which causes the solid solution in the matrix to produce alloy carbides. These carbides are highly dispersed and do not easily aggregate and grow. The pinned dislocations hinder movement and achieve a dispersion strengthening effect.
[0027] Example 1 The preparation method of the nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for the hydraulic motor distribution plate of the present invention is as follows: Step 1: Weigh the raw materials according to the mass fraction percentage of each component. Step 1 is as follows: Weigh the raw materials according to the mass fraction percentage of each component, including C: 3.50%, Si: 3.10%, Ni: 1.6%, Cr: 0.35%, Mo: 1.10%, V: 0.55%, with the balance being Fe and unavoidable impurities. The unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0028] Step 2: Prepare a blank from the raw materials weighed in Step 1; The weighed raw materials are smelted to obtain molten iron, which is then subjected to simultaneous wire feeding, spheroidization, and inoculation treatment. The treated molten iron is then introduced into a horizontal continuous casting crystallizer equipped with an ultrasonic oscillation device and a water cooling device, and continuously drawn to obtain nickel-chromium-molybdenum-vanadium ductile iron profiles. After the profiles are cooled, they are machined according to the dimensions of the distribution plate to obtain the distribution plate blank.
[0029] Step 3: High-temperature austenite homogenization treatment is performed; The distribution plate blank obtained in step 2 is placed in an argon-protected furnace. After evacuation, argon gas is introduced and heated to the homogenization temperature at a set heating rate and held at that temperature. The temperature is then increased to 1000℃ at a rate of 6℃ / min and held for 8 hours.
[0030] Step 4: The treated sample is then subjected to a stepped quenching process. The temperature was gradually reduced to 850℃ at a constant rate of 2℃ / min, held at that temperature for 1 hour, and then immediately and rapidly water-cooled to room temperature. This process yielded more martensite than direct quenching, and increased the number of dispersed dotted carbides in the microstructure. Solid-solution carbon combined with alloying elements to form alloy carbides.
[0031] Step 5: The quenched distribution plate blank is then subjected to a stepped tempering process to obtain the final product.
[0032] Heat to 500℃, hold for 1 hour, then air cool to room temperature. Perform two air cooling cycles to complete the tempering process.
[0033] Example 2 The preparation method of the nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for the hydraulic motor distribution plate of the present invention is as follows: Step 1: Weigh the raw materials according to the mass fraction percentage of each component. Step 1 is as follows: Weigh the raw materials according to the mass fraction percentage of each component, including C: 3.55%, Si: 3.20%, Ni: 1.70%, Cr: 0.40%, Mo: 1.15%, V: 0.60%, with the balance being Fe and unavoidable impurities. The unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0034] Step 2: Prepare a blank from the raw materials weighed in Step 1; The weighed raw materials are smelted to obtain molten iron, which is then subjected to simultaneous wire feeding, spheroidization, and inoculation treatment. The treated molten iron is then introduced into a horizontal continuous casting crystallizer equipped with an ultrasonic oscillation device and a water cooling device, and continuously drawn to obtain nickel-chromium-molybdenum-vanadium ductile iron profiles. After the profiles are cooled, they are machined according to the dimensions of the distribution plate to obtain the distribution plate blank.
[0035] Step 3: High-temperature austenite homogenization treatment is performed; The distribution plate blank obtained in step 2 is placed in an argon-protected furnace, and after evacuation, argon gas is introduced to raise the temperature to the homogenization temperature at a set heating rate and hold it at that temperature; preferably, the temperature is raised to 1100℃ at 6℃ / min and held for 8.5h.
[0036] High-temperature austenite homogenization treatment can promote the reduction of casting component segregation and the dissolution of some coarse carbides, making the alloying elements more uniform in austenite, creating conditions for the formation of fine and dispersed carbides during subsequent quenching and tempering processes.
[0037] Step 4: The treated sample is then subjected to a stepped quenching process. The temperature was gradually reduced to 900℃ at a constant rate of 2℃ / min, held at that temperature for 4 hours, and then rapidly water-cooled to room temperature immediately after the holding period. This process yielded more martensite than direct quenching, and increased the number of dispersed dotted carbides in the microstructure. Solid-solution carbon combined with alloying elements to form alloy carbides.
[0038] Step 5: The quenched distribution plate blank is then subjected to a stepped tempering process to obtain the final product.
[0039] Heat to 500℃, hold for 1.5 hours, then air cool to room temperature. Perform two air cooling cycles to complete the tempering process.
[0040] This invention discloses a method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates. Through compositional design and stepped quenching and tempering heat treatment process control, large carbides are transformed into fine, dispersed particles, reducing stress concentration and significantly improving the material's toughness and thermal fatigue resistance. This method achieves uniform dispersion of graphite in a fine, spherical / granular morphology, without the formation of large amounts of harmful carbides. After quenching and tempering, it meets the comprehensive requirements of high-temperature hydraulic motor distribution plates for strength, toughness, and wear resistance. The method is low-cost, highly operable, and suitable for large-scale production.
[0041] Example 3 The preparation method of the nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for the hydraulic motor distribution plate of the present invention is as follows: Step 1: Weigh the raw materials according to the mass fraction percentage of each component. Step 1 is as follows: Weigh the raw materials according to the mass fraction percentage of each component, including C: 3.52%, Si: 3.19%, Ni: 1.64%, Cr: 0.39%, Mo: 1.13%, V: 0.60%, with the balance being Fe and unavoidable impurities. The unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
[0042] Step 2: Prepare a blank from the raw materials weighed in Step 1; Profiles were prepared by synchronous wire feeding spheroidization and ultrasonic oscillation water cooling modified horizontal continuous casting. Subsequent machining yielded a distribution plate blank, with the resulting microstructure consisting of "bull's-eye" ferrite + pearlite + spheroidal graphite + a small amount of carbides.
[0043] Step 3: High-temperature austenite homogenization treatment is performed; The machined distribution plate blank was placed in an argon-protected furnace, vacuumed, and argon gas was introduced for protection. The temperature was raised to 1050℃ at a heating rate of 6℃ / min and held at a constant temperature for 8 hours. Step 4: The treated sample is then subjected to a stepped quenching process. The sample after high-temperature austenite homogenization treatment was cooled to 900℃ at a uniform step rate of 2℃ / min, held at the same temperature for 2 hours, and immediately removed and water-cooled to room temperature after the holding time was completed. The resulting microstructure was: martensite + retained austenite + carbides + spheroidal graphite.
[0044] Step 5: The quenched distribution plate blank is then subjected to a stepped tempering process to obtain the final product.
[0045] The quenched distribution plate blank is heated to 500℃, held for 1 hour, and then air-cooled to room temperature. It is then heated to 500℃ again and held for 1 hour, followed by a second air cooling to complete the tempering. The resulting microstructure is tempered martensite + carbides + a small amount of retained austenite.
[0046] The finished product prepared in this embodiment has the following properties: Rockwell hardness 50.5 HRC, high temperature strength at 500℃ 908.7 MPa, and compressive strength 1920.6 MPa.
[0047] Example 4 The preparation method of nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plate of the present invention, based on Example 3, compares the step cooling temperature in this example, specifically as follows: Under the same austenitizing conditions of 1050℃ for 8 hours and tempering at 500℃, stepped cooling platforms of 1000℃, 950℃, 900℃, and 850℃ were set up for comparison. As shown in Figures 1(a)-1(d), after tempering at 500℃, the quenched microstructure recovered, and fine carbides in the matrix further precipitated. As shown in Figures 2(a)-2(d), after multiple temperings, the carbide distribution tended to be uniform, and the quenching stress in the microstructure was released. As the stepped cooling temperature decreased, the number of dispersed point-like carbides in the quenched matrix gradually increased. The XRD results were consistent with the metallographic and SEM results, showing that martensite, retained austenite, and carbides were mainly present.
[0048] After tempering, the amount of retained austenite decreases and the carbide peaks are enhanced, indicating that more carbides are precipitated. At the same time, the full width at half maximum (FWHM) of the diffraction peaks in the tempered state decreases, indicating that the lattice distortion of the microstructure is alleviated and the internal stress is reduced.
[0049] Example 5 This invention relates to a method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates. Based on Example 3, this example compares tempering times, as shown in Figures 3(a)-3(d). With a tempering temperature of 500℃, samples with different stepped cooling times were tempered for 1h, 2h, and 4h. The results show that the samples corresponding to the 900℃ stepped cooling time, after tempering for 1h, 2h, and 4h, exhibit tensile strengths of 1036.3MPa, 947.4MPa, and 1206.4MPa, and compressive strengths of 1996.1MPa, 2124.5MPa, and 1929.4MPa, respectively; and corresponding Rockwell hardnesses of 51.7HRC, 53.5HRC, and 52.8HRC, respectively. This demonstrates that different tempering times have different effects on tensile and compressive properties: 4h tempering is beneficial for obtaining higher room temperature tensile strength, while 2h tempering corresponds to higher room temperature compressive strength. Therefore, the present invention can select a specific regime within the preferred tempering time range based on the actual load characteristics of the distribution plate.
[0050] Example 6 The preparation method of nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plate of the present invention, based on Example 3, compares the number of tempering times in this example; Different tempering cycles were set under a 500℃ holding time of 1 hour condition. The results showed that with increasing tempering cycles, the overall tensile strength increased, and the compressive strength also showed an increasing trend, indicating that multiple tempering cycles promoted further precipitation of fine, dispersed carbides. After three tempering cycles at 500℃ for 1 hour, the sample exhibited the highest room temperature tensile strength of 1176.7 MPa and the highest compressive strength of 2036.6 MPa. Considering both high-temperature performance and process efficiency, this invention preferably uses two tempering cycles.
[0051] High-temperature performance tests show that the high-temperature tensile strength of the samples tempered twice is about 200 MPa higher than that of the samples tempered once, and the high-temperature compressive strength is in the range of 1800-1900 MPa. Among them, the material that is austenitized at 1050℃ for 8 hours, cooled stepwise at 900℃ for 2 hours, water-cooled, and then held at 500℃ for 1 hour has a tensile strength of 908.7 MPa and a compressive strength of 1920.6 MPa at 500℃.
[0052] As shown in Figures 4(a)-4(d), the samples were homogenized at 1050℃ and then stepped down to 1000℃, 950℃, 900℃ and 850℃ respectively, followed by water cooling. The matrix consisted of martensite, retained austenite, carbides and spheroidal graphite. As the stepped cooling temperature decreased, the overall amount of dispersed point-like carbides in the matrix increased, indicating that the stepped cooling temperature can regulate the precipitation morphology of carbides and the matrix structure.
[0053] As shown in Figures 5(a)-5(d), after tempering at 500℃ for 1 hour, the quenched microstructure recovered, and fine carbides precipitated in the matrix. The number and distribution of carbides varied among samples obtained at different stepped cooling temperatures, with the microstructure of the sample cooled at 900℃ showing a more uniform distribution.
[0054] As shown in Figures 6(a)-6(d), after two tempering processes, fine carbides further precipitate in the matrix, and the microstructure distribution tends to be more uniform. Combined with the mechanical property results, it can be seen that multiple tempering processes are beneficial for releasing quenching stress and improving the strength and microstructure stability of the material.
[0055] like Figure 7 As shown, different stepped cooling temperatures and tempering times have different effects on tensile strength and elongation. After being tempered at 500℃ for 1h, 2h and 4h respectively, the tensile strengths of the samples cooled at 900℃ were 1036.3MPa, 947.4MPa and 1206.4MPa, respectively, with the sample tempered for 4h having the highest tensile strength.
[0056] like Figure 8 As shown, the compressive strength and compression of the samples obtained under different heat treatment regimes differ. The compressive strengths of the samples subjected to a step cooling of 900℃ and tempered at 500℃ for 1h, 2h and 4h were 1996.1MPa, 2124.5MPa and 1929.4MPa, respectively, with the sample tempered for 2h exhibiting the highest compressive strength.
[0057] This invention is based on a nickel-chromium-molybdenum-vanadium composite alloyed ductile iron system. Through high-temperature austenite homogenization and controlled phase transformation in the austenite region via stepped cooling, combined with rapid quenching and multiple tempering near 500℃, the material achieves a composite microstructure consisting of tempered martensite, a small amount of retained austenite, spheroidal graphite, and dispersed alloy carbides. This balances high-temperature strength, wear resistance, self-lubrication, and microstructural stability. By designing a precise alloy composition and matching it with a dedicated stepped quenching and tempering process, a novel material suitable for high-temperature hydraulic motor distribution plates was prepared. Under conditions of holding at 1050℃ for 8 hours, cooling to 900℃ for 2 hours followed by water cooling, and tempering twice at 500℃ for 1 hour, the material achieved a tensile strength of 908.7 MPa and a compressive strength of 1920.6 MPa at 500℃. This indicates that the material retains high load-bearing capacity under high-temperature conditions, thus improving the problems of insufficient high-temperature strength retention and poor microstructural stability in existing ductile iron distribution plates.
Claims
1. A self-lubricating ductile iron (nickel-chromium-molybdenum-vanadium) for a hydraulic motor distributor plate, characterized in that, The raw materials, by mass fraction percentage, include: C: 3.50%~3.55%, Si: 3.10%~3.20%, Ni: 1.6%~1.70%, Cr: 0.35%~0.40%, Mo: 1.10%~1.15%, V: 0.55%~0.60%, with the balance being Fe and unavoidable impurities. Unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
2. A method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates, characterized in that, Specifically: Step 1: Weigh the raw materials according to the mass fraction percentage of each component. Step 2: Prepare a blank from the raw materials weighed in Step 1; Step 3: High-temperature austenite homogenization treatment is performed; Step 4: The treated sample is then subjected to a stepped quenching process. Step 5: The quenched distribution plate blank is then subjected to a stepped tempering process to obtain the final product.
3. The method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates according to claim 2, characterized in that, Step 1 is as follows: Weigh the raw materials according to the mass percentage of each component, including C: 3.50%~3.55%, Si: 3.10%~3.20%, Ni: 1.6%~1.70%, Cr: 0.35%~0.40%, Mo: 1.10%~1.15%, V: 0.55%~0.60%, with the balance being Fe and unavoidable impurities. Unavoidable impurities are controlled to be Mn≤0.1%, P≤0.04%, and S≤0.01%, and the total mass percentage of each component is 100%.
4. The method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates according to claim 3, characterized in that, In step 2, the raw materials are smelted to obtain molten iron, which is then subjected to simultaneous wire feeding, spheroidization, and inoculation treatment. The treated molten iron is then introduced into a horizontal continuous casting crystallizer equipped with an ultrasonic oscillation device and a water cooling device, and continuously drawn to obtain profiles. After the profiles are cooled, they are machined into distribution plate blanks.
5. The method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates according to claim 4, characterized in that, Step 3: Place the machined distribution plate blank from Step 2 into an argon-protected furnace, evacuate the furnace, and introduce argon gas for protection.
6. The method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates according to claim 5, characterized in that, Step 3: Increase the temperature to 1000℃~1100℃ at a rate of 6℃ / min and hold for 8h~8.5h.
7. The method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates according to claim 6, characterized in that, Step 4: Cool the temperature to 850℃~900℃ at a uniform step rate of 2℃ / min, maintain the temperature for 1h~4h, and immediately cool it to room temperature with water after the heat preservation is completed.
8. The method for preparing nickel-chromium-molybdenum-vanadium self-lubricating ductile iron for hydraulic motor distribution plates according to claim 7, characterized in that, Step 5: Heat to 500℃, hold for 1 hour, then air cool to room temperature. Perform two air cooling cycles to complete the tempering process.