A method for short-time continuous cooling aging heat treatment of high-temperature alloys for gas turbine disks
By employing a short-time continuous cooling aging heat treatment method, the problems of long heat treatment cycles and high energy consumption of GH4169 alloy were solved, enabling efficient manufacturing of gas turbine disks, improving the strength and plasticity of the alloy, and reducing energy consumption.
Patent Information
- Application Number
- CN202611277335.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-10
AI Technical Summary
The existing GH4169 alloy has a long heat treatment cycle, high energy consumption, and insufficient cooling path control, making it difficult to meet the needs of efficient manufacturing and performance improvement of gas turbine components.
A short-time continuous cooling aging heat treatment method is adopted, including solution treatment, temperature stabilization treatment and two-stage variable speed continuous cooling. By controlling the cooling rate between 800-820 ℃ and 600-620 ℃ for continuous cooling, the traditional two-stage isothermal aging is replaced, which shortens the process time and optimizes the distribution of precipitated phases.
It significantly shortens the heat treatment cycle, improves the yield strength and tensile strength of the alloy, while maintaining or improving plasticity, reducing energy consumption and production costs, and is suitable for the efficient manufacturing of gas turbine disks.
Smart Images

Figure CN123063702A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature alloy heat treatment technology, specifically relating to a short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine disks. Background Technology
[0002] Gas turbines are core equipment in energy power, aviation propulsion, and ship propulsion. Their hot-end components, such as turbine disks, turbine blades, and combustion chambers, must operate under high temperature, high pressure, and complex stress conditions for extended periods, placing extremely stringent requirements on the high-temperature strength, fatigue resistance, and service life of materials. GH4169 alloy is an age-hardening high-temperature alloy that exhibits excellent high-temperature strength, fatigue resistance, and oxidation resistance within a temperature range of -253 ℃ to 700 ℃, making it one of the most widely used high-temperature alloys in the manufacture of hot-end components for gas turbines.
[0003] The mechanical properties of GH4169 alloy are highly dependent on the heat treatment process. The main strengthening phases in this type of alloy typically include γ″ and γ′ phases, with γ″ being the most dominant. In addition, some alloys precipitate δ phases at grain boundaries, which play a crucial role in controlling grain size and improving notch sensitivity. Controlling the quantity, size, morphology, and distribution of each precipitated phase through a reasonable heat treatment regime is key to obtaining the target mechanical properties.
[0004] Currently, the industrial standard heat treatment regime for GH4169 alloy commonly employs a two-stage isothermal aging process combined with solution treatment. A typical process is as follows: solution treatment (holding at 950–980℃ for 1 hour, followed by air or water cooling), then aging treatment (holding at 720℃ for 8 hours, furnace cooling to 620℃ at a rate of 50℃ / hour, holding for another 8 hours, followed by air cooling). In this process, the total aging stage takes approximately 18 hours, with the isothermal holding time reaching 16 hours. Including the furnace cooling transition time, the entire heat treatment cycle is quite long. In production practice, the following problems exist: First, the aging cycle of up to 18 hours severely restricts production efficiency and increases energy consumption and manufacturing costs; Second, the two-stage isothermal aging only involves long-term holding at two fixed temperatures of 720 ℃ and 620 ℃, artificially dividing the precipitation process of each major precipitated phase into two independent stages, making it difficult to fully utilize its kinetic characteristics of continuous precipitation over a wide temperature range, and leaving room for further optimization of the size distribution and volume fraction of the precipitated phases; Third, the cooling rate from 720 ℃ to 620 ℃ in standard aging is approximately 50 ℃ / h. Although some precipitated phases also precipitate during this cooling stage, the contribution is relatively limited due to the fast cooling rate and limited temperature window.
[0005] Therefore, there is an urgent need to provide a new heat treatment method that can significantly shorten the heat treatment cycle of high-temperature alloys, reduce energy consumption, and at the same time maintain or improve the comprehensive mechanical properties of alloys, so as to meet the dual requirements of efficient manufacturing and performance improvement of gas turbine components. Summary of the Invention
[0006] In order to overcome the problems existing in the prior art, the present invention provides a short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine disks, so as to solve the problems of long heat treatment cycle, high energy consumption, long isothermal holding time and insufficient cooling path control in the traditional two-stage isothermal aging process. While significantly shortening the process time, it can maintain or improve mechanical properties, and achieve the beneficial effects of short time, low energy consumption and increased strength.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] This invention provides a short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine disks, comprising the following steps: S1: The high-temperature alloy is subjected to solution treatment, and after the solution treatment is completed, it is cooled to room temperature; S2: The high-temperature alloy after solution treatment is heated to the continuous cooling aging starting temperature T1 in a heat treatment furnace. T1 is 800-820 ℃, and is held at this temperature for 10-30 min to complete the temperature stabilization treatment. S3: After the temperature stabilization treatment is completed, the heat treatment furnace is continuously cooled from T1 to the intermediate temperature Tm at a first cooling rate V1, where Tm is 720-740 ℃; no isothermal holding is performed at Tm, and the furnace is immediately continuously cooled from Tm to the final temperature T2 at a second cooling rate V2, where T2 is 600-620 ℃, completing two continuous cooling cycles; where V1 is 28-34 ℃ / h and V2 is 17-22 ℃ / h. S4: The high-temperature alloy after two consecutive coolings is taken out of the heat treatment furnace and air-cooled to room temperature to obtain the heat-treated high-temperature alloy.
[0009] Furthermore, in step S1, the solution treatment temperature is 960~1000 ℃, the holding time is 0.5~2 h, and after the holding time is completed, the solution is cooled to room temperature at a cooling rate no less than that of air cooling.
[0010] Furthermore, the solution treatment temperature is 970~990 ℃, the holding time is 0.75~1.25 h, and the cooling method is water cooling.
[0011] Further, step S2 specifically involves: first, heating the heat treatment furnace to T1, then placing the solution-treated high-temperature alloy into the heat treatment furnace, and maintaining the furnace temperature at T1±5℃ for 10 to 30 minutes.
[0012] Furthermore, in step S2, T1 is 805-815 ℃, and after the heat treatment furnace temperature is restored to T1±5 ℃, the holding time at this temperature is 15-25 min.
[0013] Furthermore, in step S3, Tm is 725–735 °C and T2 is 605–615 °C.
[0014] Furthermore, in step S3, V1 / V2 is 1.4 to 2.0, and the total time for the two continuous cooling stages is 8 to 11 hours.
[0015] Furthermore, in step S3, V1 is 29–32 ℃ / h, V2 is 18–21 ℃ / h, and V1 / V2 is 1.45–1.75.
[0016] Furthermore, in step S3, V1 and V2 are the average furnace temperature drop rates for the first cooling stage and the second cooling stage, respectively.
[0017] Furthermore, the high-temperature alloy is a GH4169 alloy turbine disk forging.
[0018] The beneficial effects of this invention are: (1) The present invention adopts a two-stage variable speed continuous cooling aging process that continuously decreases from the starting temperature T1 through the intermediate temperature Tm to the final temperature T2, and does not set isothermal heat preservation at Tm. The continuous cooling aging replaces the traditional two-stage long-term isothermal aging, which eliminates the long heat preservation process at 720 ℃ and 620 ℃ in the traditional process, thereby shortening the aging treatment cycle and improving the heat treatment production efficiency. (2) In this invention, the cooling rate of the first cooling stage is greater than that of the second cooling stage. The first cooling stage is located in a higher temperature region, where the solute atoms have a stronger diffusion ability. However, the precipitated phase is prone to grow and coarsen, and the δ phase is also more likely to precipitate. Therefore, by adopting a higher cooling rate V1, high-temperature diffusion can be used to promote the short-range segregation of elements such as Nb and the nucleation of the enhanced phase. At the same time, the high-temperature residence time is shortened, which limits the coarsening of the enhanced phase and the excessive precipitation of the δ phase, and retains enough enhanced elements for subsequent precipitation. (3) In this invention, the second cooling stage adopts a lower cooling rate. When the temperature drops below the intermediate temperature Tm, the thermodynamic driving force for the precipitation of γ″ and γ′ phases increases, while the long-range diffusion of solute atoms gradually slows down. The lower cooling rate in the second cooling stage can prolong the effective aging time of the workpiece in the sensitive range of precipitation at medium and low temperatures, so that the crystal nuclei formed in the first stage continue to grow in a controlled manner and promote the continuous nucleation of new fine strengthening phases, thereby forming a precipitation process with continuous nucleation, batch growth and no excessive coarsening. This is beneficial to obtaining fine, dispersed and uniformly distributed γ″ and γ′ phases, enhancing the resistance to dislocation movement, improving yield strength and tensile strength while shortening the aging time, and maintaining good plasticity. (4) The two-stage variable speed continuous cooling process of the present invention can be realized by the program temperature control system of a conventional heat treatment furnace without the need for additional special equipment; at the same time, the solution treatment process can follow the existing production system and is highly compatible with the existing production line. Since the long-term isothermal heat preservation in the traditional two-stage aging process is eliminated, the equipment occupancy time can be shortened, and it is also beneficial to reduce the heat treatment energy consumption and production cost per batch. Attached Figure Description
[0019] Figure 1 Overall process flow diagram of the short-time continuous cooling aging heat treatment method provided by the present invention; Figure 2 Design drawings for GH4169 alloy turbine disk; Figure 3 Figure (a) shows the metallographic structure of the GH4169 alloy turbine disk in Example 1 and Comparative Example 1 of the present invention, and Figure (b) shows the metallographic structure of Example 1. Figure 4 Figure (a) shows the tensile fracture morphology of the GH4169 alloy turbine disk in Example 1 and Comparative Example 1 of the present invention, and Figure (b) shows the tensile fracture morphology of Example 1. Figure 5 These are stress-strain curves of Embodiments 1-3 and Comparative Examples 1-2 of the present invention; Figure 6 These are polarization curves of Examples 1-3 and Comparative Examples 1-2 of the present invention; Figure 7 This is a schematic diagram of the process principle of Embodiment 1 of the present invention. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] like Figure 1 As shown, this invention provides a short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine disks, including solution treatment, short-time temperature stabilization treatment, two-stage variable-speed continuous cooling aging, and air cooling after furnace exit. Details are as follows: Step 1: Solution treatment The high-temperature alloy (GH4169 alloy turbine disk forging) is heated to 960~1000 ℃ and held at this temperature for 0.5~2 h. After holding, it is air-cooled or cooled to room temperature at a faster rate. Preferably, the solution treatment temperature can be set to 970~990 ℃, the holding time is 0.75~1.25 h, and the cooling method is water cooling. Solution treatment allows a large amount of age-hardening elements such as Nb, Al, and Ti in the GH4169 alloy to dissolve in the γ matrix, and a small amount of residual δ phase exists at the grain boundaries, which can provide solute conditions for the subsequent precipitation of γ″ and γ′ phases.
[0022] Step 2: Temperature stabilization treatment: First, the heat treatment furnace is heated to the continuous cooling aging starting temperature T1, which is 800–820 °C. Then, the solution-treated high-temperature alloy is placed in the furnace. After the furnace temperature recovers to T1 ± 5 °C, it is held at this temperature for 10–30 minutes. Preferably, T1 can be set to 805–815 °C, and the holding time at this temperature is 15–25 minutes. This temperature stabilization step can make the internal and external temperatures of the high-temperature alloy workpiece more uniform, providing a consistent temperature starting point for subsequent continuous cooling. Simultaneously, the short holding time can reduce the coarsening of precipitated phases and excessive consumption of strengthening elements caused by prolonged exposure of the high-temperature alloy workpiece to high temperatures.
[0023] Step 3: Two-stage variable speed continuous cooling aging treatment: After the temperature stabilization treatment is completed, the first cooling stage and the second cooling stage are carried out in sequence, and there is no isothermal heat preservation between the two cooling stages.
[0024] The first cooling stage involves controlling the heat treatment furnace to continuously reduce the temperature from T1 to an intermediate temperature Tm at a first cooling rate V1, where Tm is 720–740 ℃ and V1 is 28–34 ℃ / h. In this stage, the temperature is relatively high, and the solute atoms such as Nb, Al, and Ti in the high-temperature alloy have strong diffusion capabilities, which is conducive to short-range diffusion and local segregation, providing compositional conditions for the nucleation of the γ″ and γ′ phases. Because a high cooling rate V1 is used in this stage, the high-temperature alloy workpiece can quickly pass through the high-temperature range where precipitates easily grow and coarsen. This utilizes the high-temperature diffusion effect while reducing the possibility of excessive coarsening of the strengthening phase and excessive precipitation of the δ phase, and retaining more strengthening elements for subsequent stages.
[0025] The second cooling stage: After the furnace temperature of the heat treatment furnace is reduced to Tm, isothermal holding is not performed. Instead, the temperature is directly reduced to the termination temperature T2 at a second cooling rate V2 lower than V1. V2 is 17–22 °C / h, and T2 is 600–620 °C. During this process, as the temperature decreases from Tm to T2, within the effective precipitation temperature range of the strengthening phase, the supersaturation degree of the γ matrix increases, the precipitation driving force of the γ″ and γ′ phases is enhanced, and the diffusion rate of solute atoms gradually decreases. Using a lower cooling rate V2 can appropriately prolong the residence time of the high-temperature alloy workpiece within the effective precipitation temperature range of the strengthening phase, allowing the γ″ and γ′ phase nuclei formed in the first cooling stage to grow in a controlled manner, and promoting the continuous nucleation and precipitation of new fine strengthening phases. Through the combination of two cooling stages, the γ″ and γ′ phases precipitate in stages along the continuous cooling path, forming a fine, dispersed and relatively uniformly distributed strengthening phase structure, which effectively hinders dislocation movement and is conducive to improving the yield strength and tensile strength of the alloy. At the same time, it can suppress the formation of coarse strengthening phase and continuous δ phase structure at grain boundaries, which is conducive to maintaining the plasticity and deformation coordination of the alloy.
[0026] Step 4: Cooling after removing from the oven: After the furnace temperature of the heat treatment furnace drops to T2, the high-temperature alloy workpiece that has undergone two consecutive cooling processes is taken out of the heat treatment furnace and air-cooled to room temperature to obtain the heat-treated high-temperature alloy.
[0027] Example 1 This invention provides a short-time continuous cooling aging heat treatment method for GH4169 alloy turbine disk forgings for gas turbines, comprising the following steps: Step S1, Solution treatment: The forging is placed in a heat treatment furnace, heated to 980±5 ℃, held for 1 h, and then removed from the furnace and water-cooled to room temperature.
[0028] Step S2, Temperature Stabilization Treatment: Heat the heat treatment furnace to 810 ℃, load the solution-treated forgings into the heat treatment furnace, and hold for 20 min after the furnace temperature recovers to 810±5 ℃.
[0029] Step S3, Two consecutive cooling processes: Start the program temperature control to continuously reduce the heat treatment furnace temperature from 810 ℃ to 730 ℃ at a rate of 30 ℃ / h. After reaching 730 ℃, do not perform isothermal holding, but directly reduce the temperature to 610 ℃ at a rate of 20 ℃ / h. The total continuous cooling time is 8.67 h, and V1 / V2 is 1.50.
[0030] Step S4, air cooling after removal from the furnace: When the furnace temperature of the heat treatment furnace drops to 610 ℃, the forging is removed from the furnace and air cooled to room temperature to obtain the heat-treated turbine disk forging.
[0031] Example 2 This invention provides a short-time continuous cooling aging heat treatment method for GH4169 alloy turbine disk forgings for gas turbines, comprising the following steps: Step S1, Solution treatment: The forging is placed in a heat treatment furnace, heated to 980±5 ℃, held for 1 h, and then removed from the furnace and water-cooled to room temperature.
[0032] Step S2, Temperature Stabilization Treatment: Heat the heat treatment furnace to 800 ℃, and load the solution-treated forgings into the furnace; after the furnace temperature recovers to 800±5 ℃, maintain it for 20 min.
[0033] Step S3, Two consecutive cooling processes: Start the program temperature control to continuously reduce the heat treatment furnace temperature from 800 ℃ to 720 ℃ at a rate of 28 ℃ / h. After reaching 720 ℃, do not perform isothermal holding, but directly reduce the temperature to 600 ℃ at a rate of 18 ℃ / h. The total continuous cooling time is 9.52 h, and V1 / V2 is 1.56.
[0034] Step S4, Furnace Removal and Air Cooling: When the furnace temperature drops to 600 ℃, the forging is removed from the furnace and air-cooled to room temperature to obtain the heat-treated turbine disk forging.
[0035] Example 3 This invention provides a short-time continuous cooling aging heat treatment method for GH4169 alloy turbine disk forgings for gas turbines, comprising the following steps: Step S1, Solution treatment: The forging is placed in a heat treatment furnace, heated to 980±5 ℃, held for 1 h, and then removed from the furnace and water-cooled to room temperature.
[0036] Step S2, Temperature Stabilization Treatment: Heat the heat treatment furnace to 820 ℃, and load the solution-treated forgings into the furnace; after the furnace temperature recovers to 820±5 ℃, maintain it for 20 min.
[0037] Step S3, Two consecutive cooling processes: Start the program temperature control to continuously reduce the heat treatment furnace temperature from 820 ℃ to 730 ℃ at a rate of 34 ℃ / h. After reaching 730 ℃, do not perform isothermal holding, but directly reduce the temperature to 610 ℃ at a rate of 17 ℃ / h. The total continuous cooling time is 9.71 h, and V1 / V2 is 2.0.
[0038] Step S4, air cooling after furnace removal: When the furnace temperature drops to 610 ℃, the forging is removed from the furnace and air cooled to room temperature to obtain the heat-treated turbine disk forging.
[0039] Comparative Example 1: Two-stage isothermal aging process The specific steps for Comparative Example 1 are as follows: Step S1, Solution treatment: The GH4169 alloy turbine disk forging is placed in a heat treatment furnace, heated to 980±5 ℃, held for 1 h, and then removed from the furnace and water-cooled to room temperature. Step S2, Two-stage isothermal aging treatment: The heat treatment furnace is heated to 720 ℃, and the solution-treated forgings are placed into the furnace. After the furnace temperature recovers to 720±5 ℃, it is held at that temperature for 8 hours. Then, the heat treatment furnace temperature is continuously reduced from 720 ℃ to 620 ℃ at a rate of 50 ℃ / h, and held at that temperature for another 8 hours, followed by air cooling. The total aging time is approximately 18 hours.
[0040] Comparative Example 2 The specific steps for Comparative Example 2 are as follows: Step S1, Solution treatment: The GH4169 alloy turbine disk forging is placed in a heat treatment furnace, heated to 980±5 ℃, held for 1 h, and then removed from the furnace and water-cooled to room temperature.
[0041] Step S2: Heat the heat treatment furnace to 810 ℃, and load the solution-treated forgings into the furnace; after the furnace temperature recovers to 810±5 ℃, maintain it for 20 min.
[0042] Step S3: Start the program temperature control to continuously reduce the furnace temperature from 810 ℃ to 730 ℃ at a rate of 18 ℃ / h. After reaching 730 ℃, do not perform isothermal heat preservation, but directly reduce the temperature to 610 ℃ at a rate of 25 ℃ / h. The total continuous cooling time is 9.24 h, and V1 / V2 is 0.72.
[0043] Step S4: When the furnace temperature drops to 610 ℃, the forging is taken out of the furnace and air-cooled to room temperature to obtain the heat-treated turbine disk forging.
[0044] The forgings treated in Examples 1-3 and Comparative Examples 1-2 were subjected to mechanical property tests and electrochemical corrosion tests, respectively. The results are shown in Tables 1 and 2.
[0045] Table 1: Room temperature tensile properties of GH4169 alloy under different heat treatment regimes and their aging time reduction
[0046] Table 2: Electrochemical corrosion properties of GH4169 alloy under different heat treatment regimes
[0047] As shown in Table 1, the yield strength and tensile strength of each embodiment are significantly higher than those of the two comparative examples, indicating that the aging treatment system adopted in this invention has a significant advantage in improving alloy strength compared to the traditional long-term isothermal aging system of Comparative Example 1. Regarding elongation after fracture, the values of the embodiments are all higher than those of Comparative Example 1, indicating that the system of this invention does not sacrifice plasticity while improving strength; on the contrary, it improves plasticity. Although Comparative Example 2 achieved the highest elongation, its strength level is significantly lower than that of the embodiments, indicating an imbalance between strength and plasticity. This suggests that the configuration sequence of the two-stage cooling rates affects the strength-plasticity matching of the GH4169 alloy. In terms of aging treatment efficiency, the total aging time reduction of each embodiment is controlled between 44% and 50%, indicating that the system of this invention significantly shortens the aging treatment cycle, significantly improves heat treatment efficiency, and still achieves better comprehensive mechanical properties than the comparative examples.
[0048] As shown in Table 2, the self-corrosion potential of each embodiment is higher than that of the two comparative examples, with Example 1 having the highest potential, followed by Example 2, and then Example 3. The self-corrosion potentials of the two comparative examples are significantly lower. A higher self-corrosion potential indicates better thermodynamic stability and stronger corrosion resistance of the material in the corrosive medium. Regarding the self-corrosion current density, the current density of each embodiment is lower than that of the two comparative examples, with Example 1 having the lowest, followed by Examples 2 and 3. The current density of the two comparative examples increases, especially that of Comparative Example 2. A lower self-corrosion current density indicates a slower corrosion rate and better corrosion resistance. Therefore, the corrosion resistance of each embodiment is superior to that of the two comparative examples, with Example 1 showing the best performance. This indicates that the aging treatment regime adopted in this invention can significantly improve the corrosion resistance of GH4169 alloy compared to the traditional regime.
[0049] This invention replaces the traditional two-stage isothermal aging process with a two-stage variable-speed continuous cooling method. The high-temperature stage employs a faster cooling rate to promote the nucleation of the γ″ / γ′ phase and limit the coarsening of the strengthening phase and excessive precipitation of the δ phase. The medium- and low-temperature stages use a slower cooling rate to prolong the effective precipitation time of the strengthening phase, resulting in fine, dispersed, and uniformly distributed strengthening phases. This shortens the traditional two-stage isothermal aging cycle while maintaining or improving the strength and plasticity of the turbine disk. This method reduces the long isothermal operation time of the heat treatment furnace, offering advantages in increased production efficiency and reduced energy consumption, and is suitable for manufacturing gas turbine disk forgings.
[0050] The above are merely preferred embodiments of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should be considered within the scope of protection of the present invention.
Claims
1. A short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks, characterized in that, Includes the following steps: S1: The high-temperature alloy is subjected to solution treatment, and after the solution treatment is completed, it is cooled to room temperature; S2: The high-temperature alloy after solution treatment is heated to the continuous cooling aging starting temperature T1 in a heat treatment furnace. T1 is 800-820 ℃, and is held at this temperature for 10-30 min to complete the temperature stabilization treatment. S3: After the temperature stabilization treatment is completed, the heat treatment furnace is controlled to continuously decrease from T1 to the intermediate temperature Tm at the first cooling rate V1, where Tm is 720-740 ℃; then, it is continuously decreased from Tm to the final temperature T2 at the second cooling rate V2, where T2 is 600-620 ℃, completing two continuous cooling cycles; where V1 is 28-34 ℃ / h and V2 is 17-22 ℃ / h. S4: The high-temperature alloy after two consecutive coolings is taken out of the heat treatment furnace and air-cooled to room temperature to obtain the heat-treated high-temperature alloy.
2. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: In step S1, the solution treatment temperature is 960~1000 ℃, the holding time is 0.5~2 h, and after the holding time is completed, the solution is cooled to room temperature at a cooling rate no less than that of air cooling.
3. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 2, characterized in that: The solution treatment temperature is 970~990 ℃, the holding time is 0.75~1.25 h, and the cooling method is water cooling.
4. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: Step S2 specifically involves: First, the heat treatment furnace is heated to T1. Then, the high-temperature alloy after solution treatment is placed in the heat treatment furnace. After the furnace temperature recovers to T1±5 ℃, it is maintained at this temperature for 10 to 30 minutes.
5. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 4, characterized in that: In step S2, T1 is 805-815 ℃. After the heat treatment furnace temperature is restored to T1±5 ℃, the holding time at this temperature is 15-25 min.
6. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: In step S3, Tm is 725–735 °C and T2 is 605–615 °C.
7. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: In step S3, V1 / V2 is 1.4 to 2.0, and the total time for the two continuous cooling stages is 8 to 11 hours.
8. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: In step S3, V1 is 29–32 ℃ / h, V2 is 18–21 ℃ / h, and V1 / V2 is 1.45–1.
75.
9. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: In step S3, V1 and V2 are the average furnace temperature drop rates for the first and second cooling stages, respectively.
10. The short-time continuous cooling aging heat treatment method for high-temperature alloys used in gas turbine turbine disks according to claim 1, characterized in that: The high-temperature alloy is a GH4169 alloy turbine disk forging.