A method for preparing a paper-based decorative material with double-layer coated, sun-resistant titanium dioxide.
By forming a continuous silica-alumina-hydroxyl composite inorganic barrier layer and an organosiloxane layer containing 3-hydroxyazocyclobutane groups on the surface of titanium dioxide, covalent anchoring of titanium dioxide and fibers is achieved, solving the problem of easy desorption and shedding of titanium dioxide in paper-based finishing materials in the prior art, and improving the sun resistance and interface stability.
Patent Information
- Application Number
- CN202611234820.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-10
Smart Images

Figure CN123064048A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of titanium dioxide surface treatment technology, specifically relating to a double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials and its preparation method. Background Technology
[0002] Paper-based finishing materials include melamine decorative paper, veneer paper, and impregnated paper, which are ultimately applied to the surface of engineered wood products to form the finishing layer of furniture, flooring, and decorative panels. Their core functional requirements include high opacity, excellent whiteness, good sun resistance, and physical stability after impregnation and hot-pressing processes. Rutile titanium dioxide, due to its high refractive index, excellent whiteness, and strong opacity, is the main white pigment component in this type of paper-based finishing material. However, the surface of titanium dioxide lattice contains photoactivated sites, which, under ultraviolet light irradiation, can catalyze the generation of reactive oxygen species and migrate to the cellulose matrix, leading to yellowing, chalking, and a decrease in mechanical strength of the paper. The industry-standard solution is to construct an inorganic oxide passivation layer on the surface of titanium dioxide particles to occupy the photoactive sites, and then add an organic modification layer outside the inorganic layer to adjust the surface polarity, water dispersibility, and interfacial affinity with the fiber matrix.
[0003] The prior art CN109705630B discloses a rutile titanium dioxide for decorative laminated paper and its preparation method. It involves sequentially forming a dense aluminum phosphate layer, a loose silica-alumina composite layer, a loose boehmite hydrated alumina layer, and an amine-based organic treatment layer on the surface of a titanium dioxide core. This multi-layer inorganic coating passivates photocatalytic activity, and amine modification generates a positive surface potential to improve retention in fiber pulp. However, the amine-based organic layer relies on protonated amine groups to generate a positive charge, the intensity of which is sensitively controlled by the pH of the system. Increased ionic strength in the white water system or shear conditions weaken the particle-fiber interface bonding. Furthermore, the amine-modified layer and the inorganic inner layer are physically adsorbed or weakly hydrogen-bonded, lacking chemical anchoring, making the organic layer prone to migration or detachment during subsequent impregnation and hot pressing. CN111253781A discloses a titanium dioxide pigment modified by sequential coating with silica, alumina, and silane. The outer silane layer is fixed to the inorganic inner layer by hydrolysis and condensation with a silane coupling agent to form Si-OM bonds. However, the silane coupling agent is a conventional aminosilane, epoxysilane, or methacryloyloxysilane, whose function is limited to adjusting the surface polarity and water dispersibility of particles. The functional groups at the outer end of the silane molecule do not participate in the chemical fixation reaction with the fiber matrix. In the wet end system of papermaking, the particle-fiber interface is still dominated by electrostatic adsorption, and the tendency of particle loss has not been fundamentally improved.
[0004] In summary, there is an urgent need to develop a double-layer coated titanium dioxide with an inorganic sun-resistant passivation layer, a covalently anchored organic layer, and chemical reactivity with the fiber matrix on the particle surface, so as to maintain stable sun resistance, particle retention rate, and interfacial bonding strength during the processing and service life of paper-based decorative materials. Summary of the Invention
[0005] This invention discloses a double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials and its preparation method, aiming to solve the problems of existing decorative titanium dioxide where the outer organic modification relies on electrostatic adsorption, leading to easy desorption of the particle-fiber interface under wet ionic strength or shear; the lack of chemical anchoring between the outer and inorganic inner layers, resulting in detachment during subsequent processing; and the lack of active functional groups on the particle surface that can directly react with nucleophilic sites of the cellulose matrix.
[0006] The specific technical solution is as follows: A paper-based finishing material uses a double-layer coating of sun-resistant titanium dioxide, comprising a core, a first coating layer, and a second coating layer. The core is rutile titanium dioxide. The first coating layer is a continuous silica-alumina-hydroxyl composite inorganic barrier layer coated on the surface of the core. The second coating layer is an organosiloxane layer containing 3-hydroxyazine-butane groups covering the outer surface of the first coating layer. The second coating layer is fixed to the M-OH sites on the surface of the first coating layer via Si-OM bonds, where M is Si, Al, or Ti. The organosiloxane layer containing 3-hydroxyazine-butane groups is formed by the hydrolysis and condensation of a siloxane precursor, the structure of which is... , where R is H, CH3 or CH2-CH(OH)-CH2-Cl.
[0007] Furthermore, in the continuous silica-alumina composite inorganic barrier layer, based on the mass of the core, the amount of silica deposited in the first coating layer is 2.0~4.0 wt%, the amount of alumina deposited is 1.0~4.0 wt%, and the mass ratio of silica to alumina is 1:(0.25~1.0); based on the mass of the core, the loading amount of the second coating layer is 0.25~0.65 wt%.
[0008] Furthermore, the preparation method of the paper-based decorative material with double-layer coated sun-resistant titanium dioxide includes the following steps: S1: Dissolve N-methyl-3-aminopropyltrimethoxysilane in a water / anhydrous ethanol mixture to prepare a solution with a concentration of 1.2 mol / L; heat under nitrogen protection and add epichlorohydrin dropwise, maintain the temperature and react until the content of the product containing 3-hydroxy-nitro-heterocyclic butyronitrile group is not less than 95% of the nitrogen-containing main product, cool to room temperature and remove volatiles under reduced pressure to obtain the siloxane precursor; S2: Rutile titanium dioxide cores and sodium hexametaphosphate were added to deionized water for high-shear dispersion to obtain an aqueous slurry. After heating, the pH of the system was adjusted to 9.5±0.2 with sodium hydroxide aqueous solution. Under stirring, sodium silicate nonahydrate aqueous solution was added dropwise first, followed by aluminum sulfate octadecahydrate aqueous solution. During the dropwise addition, the pH fluctuation range of the system was controlled to not exceed ±0.5. After the dropwise addition was completed, the pH of the system was adjusted back to 6.5±0.2 with dilute sulfuric acid and aged at the temperature. After filtration and washing, titanium dioxide intermediate filter cake containing the first coating layer was obtained. S3: The titanium dioxide intermediate filter cake containing the first coating layer is redispersed in deionized water, and the pH of the system is adjusted to 4.5±0.2 with dilute hydrochloric acid to obtain a titanium dioxide slurry containing the first coating layer; the siloxane precursor is diluted with a water / isopropanol mixed solution and pre-hydrolyzed to obtain a pre-hydrolyzed solution; the pre-hydrolyzed solution is added to the titanium dioxide slurry containing the first coating layer, and after the reaction is carried out at a constant temperature and stirred, the pH of the system is adjusted to 6.0±0.2 with dilute ammonia and aged at a constant temperature. After filtration, washing, vacuum drying and air jet pulverization, the double-coated sun-resistant titanium dioxide is obtained.
[0009] Furthermore, the molar ratio of epichlorohydrin to N-methyl-3-aminopropyltrimethoxysilane in step S1 is (2.5~4.0):1.
[0010] Furthermore, in step S1, the volume ratio of the water / anhydrous ethanol mixed solvent is 1:3; the temperature for adding epichlorohydrin and maintaining the reaction temperature is 60℃±5℃, and the adding time is 60 minutes; the vacuum degree for removing volatiles by vacuum distillation is not less than 0.09MPa, and the temperature is not higher than 50℃.
[0011] Furthermore, in step S2, the solid content of the water slurry is 300 g / L; the amount of sodium hexametaphosphate added is 0.2% of the core mass; the high-shear dispersion speed is 4000 r / min and the time is 60 minutes; the heating temperature is 75℃±5℃.
[0012] Furthermore, in step S2, the mass concentration of the sodium silicate nonahydrate aqueous solution is 10%~20%, and the mass concentration of the aluminum sulfate octadecahydrate aqueous solution is 8%~15%; the heat preservation aging conditions are: aging at 75°C for 80 minutes; the washing is carried out until the conductivity of the filtrate is not higher than 100 μS / cm.
[0013] Furthermore, in step S3, the solid content of the titanium dioxide slurry containing the first coating layer is 280 g / L; the pH of the water / isopropanol mixed solution is 4.2 and the volume ratio is 1:1; the concentration of the active component after dilution of the siloxane precursor is 0.15 g / mL, and the active component is calculated based on the content of compounds containing 3-hydroxyazine cyclobutane groups; the pre-hydrolysis temperature is 25°C and the time is 30 minutes.
[0014] Furthermore, the pre-hydrolyzed solution mentioned in step S3 is added within 40 minutes under stirring at 400 r / min, and the system temperature does not exceed 30°C during the addition process; the time for the heat preservation and stirring reaction is 60 minutes.
[0015] Furthermore, the heat preservation and aging conditions in step S3 are as follows: aging at 35°C for 40 minutes; washing is carried out until the conductivity of the filtrate is not higher than 50 μS / cm; and the pressure of the airflow pulverization is 0.8 MPa.
[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention designs a functionalized siloxane precursor containing a 3-hydroxyazacyclobutane group as a key structural component of the second coating layer. This precursor achieves nucleophilic addition and intramolecular cyclization of the secondary amine end of N-methyl-3-aminopropyltrimethoxysilane with epichlorohydrin in a single water / cosolvent reaction system, generating a permanently positively charged azacyclobutane four-membered ring group. Simultaneously, the ring-opening reaction of the partial hydrolysis of Si-OH on silicon atoms by excess epichlorohydrin in the same system generates mixed-substituted siloxane units containing chlorohydrin ether end groups. In the coating step, this precursor is anchored to a silica-alumina-hydroxyl oxide inorganic barrier layer on the surface of titanium dioxide particles via Si-OM bonds, forming a chemically immobilized layer that is difficult to desorb during high salt, high shear, or subsequent impregnation and hot-pressing processes.
[0017] (2) The 3-hydroxy-nitro-butane groups exposed on the outer surface of the second coating layer of the present invention electrostatically adsorb onto the carboxylate sites on negatively charged cellulose fibers, carboxylated nanocellulose or carboxymethyl cellulose through positive charge in the wet part of the slurry. Subsequently, during the paper drying and impregnation hot pressing stages, the four-membered ring undergoes a nucleophilic ring-opening reaction driven by ring tension, forming a covalent ester bond with the fiber carboxylate, thus transforming the electrostatic adsorption between titanium dioxide particles and fibers into a covalent fixation interface. The uniformity of particle distribution and retention rate in the paper are improved, and the tendency of particles to be lost in the white water system is alleviated, without the need for large-dose addition of external high-molecular wet-strength resin.
[0018] (3) The present invention achieves passivation of the photocatalytic activity of titanium dioxide and chemical fixation of the particle-fiber interface by combining the silica-alumina-hydroxyl oxide continuous composite inorganic barrier layer with the covalently anchored 3-hydroxyacyclobutane organosiloxane layer. Since the second coating layer is anchored to the first coating layer by covalent bonds, the organic layer is not easy to migrate or fall off during subsequent processing. The sun resistance function of the inorganic barrier layer remains stable throughout the entire processing and service cycle of the paper-based finishing material, and the sun resistance stability and interface stability are improved. Attached Figure Description
[0019] Figure 1This is a schematic diagram illustrating the preparation, hydrolysis, and coating of the siloxane precursor of the present invention; Figure 2 This is the 1H NMR spectrum of the product after hydrolysis of the siloxane precursor of this invention. Detailed Implementation
[0020] The present invention proposes a double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials, comprising a core, a first coating layer, and a second coating layer.
[0021] The core is rutile titanium dioxide with a rutile content of not less than 96 wt%. The core provides high refractive index and hiding power, and is the basic pigment that constitutes the whiteness and hiding effect of the finishing material.
[0022] The first coating layer is a continuous silica-alumina composite inorganic barrier layer, directly coated on the surface of the core. Based on the mass of the titanium dioxide core, the silica deposition in the first coating layer is 2.0~4.0 wt%, and the alumina deposition is 1.0~4.0 wt%, with a silica to alumina mass ratio of 1:(0.25~1.0). The first coating layer occupies photoactive sites on the core surface, blocking the migration of photogenerated carriers and active species to the fiber matrix.
[0023] The second coating layer is an organosiloxane layer containing 3-hydroxyazacyclobutane groups, covering the outer surface of the first coating layer. The loading of the second coating layer is 0.25~0.65 wt% based on the mass of the titanium dioxide core. The second coating layer is fixed to the M-OH sites on the surface of the first coating layer via Si-OM bonds, where M is Si, Al, or Ti. The organosiloxane layer containing 3-hydroxyazacyclobutane groups is formed by the hydrolysis and condensation of a siloxane precursor, the structure of which is as follows: Where R is H, CH3, or CH2-CH(OH)-CH2-Cl chloroethanol ether end group; R can be all the same, partially the same, or different from each other; when R is H, it indicates that the corresponding silicon-oxygen bond end group is hydroxyl; when R is CH3, it indicates that the corresponding silicon-oxygen bond end group is methoxy; when R is CH2-CH(OH)-CH2-Cl, it indicates that the corresponding silicon-oxygen bond end group is chloroethanol ether. (See attached...) Figure 1 The diagram shows the hydrolysis and coating process for preparing siloxane precursors.
[0024] The specific preparation process of the double-layer coated, sun-resistant titanium dioxide particles is as follows: S1. Synthesis of siloxane precursors N-Methyl-3-aminopropyltrimethoxysilane was dissolved in a 1:3 (v / v) water / anhydrous ethanol mixture to prepare a 1.2 mol / L solution. Under nitrogen protection, the reaction system was heated to 60℃±5℃, and epichlorohydrin was slowly added dropwise, controlling the molar ratio of epichlorohydrin to N-methyl-3-aminopropyltrimethoxysilane at (2.5~4.0):1, with a dropping time of 60 minutes. The excess epichlorohydrin undergoes nucleophilic addition with the secondary amine in the N-methyl-3-aminopropyltrimethoxysilane molecule to form a chlorohydrin intermediate, which then undergoes intramolecular nucleophilic substitution to form a 3-hydroxyazacyclobutane four-membered ring cation. Simultaneously, some epichlorohydrin undergoes a ring-opening reaction with the Si-OH atoms exposed by partial hydrolysis on the silicon atoms to generate a Si-O-CH2-CH(OH)-CH2-Cl chlorohydrin ether end group. After the addition is complete, maintain the temperature at 60℃±5℃ and continue stirring. Samples are taken hourly during the reaction, and the reaction system is monitored using high-performance liquid chromatography (HPLC). The reaction is considered complete when the product containing the 3-hydroxyazine-containing heterocyclic butylene group accounts for no less than 95% of the nitrogen-containing main product. The system is then cooled to room temperature, and volatiles are removed under reduced pressure, maintaining a vacuum of no less than 0.09 MPa and a evaporation temperature no higher than 50℃. The siloxane precursor is then obtained and stored at 5–10℃ in a light-protected, airtight container for later use.
[0025] S2. Formation of the first covering layer (1) Add rutile titanium dioxide core to deionized water to prepare a water slurry with a solid content of 300 g / L. Add 0.2% sodium hexametaphosphate as an inorganic dispersant based on the mass of titanium dioxide core. Disperse the water slurry under high shear at 4000 r / min for 60 minutes to obtain a uniformly dispersed water slurry.
[0026] (2) Heat the water slurry to 75℃±5℃ and adjust the pH of the system to 9.5±0.2 using a sodium hydroxide aqueous solution with a concentration of 0.5~1.0mol / L.
[0027] (3) Under stirring conditions of 500~1000r / min, first slowly add a sodium silicate nonahydrate aqueous solution with a mass concentration of 10%~20% to the water slurry. After the addition is completed, continue to slowly add an aluminum sulfate octadecahydrate aqueous solution with a mass concentration of 8%~15%. During the addition process, control the pH fluctuation range of the system to not exceed ±0.5. Adjust the amount of sodium silicate and aluminum sulfate added so that the deposition mass ratio of silicon dioxide and aluminum oxide in the final first coating layer is 1:(0.25~1.0). Based on the mass of titanium dioxide core, the amount of silicon dioxide deposited is 2.0~4.0wt% and the amount of aluminum oxide deposited is 1.0~4.0wt%.
[0028] (4) After the addition is complete, the pH of the system is slowly adjusted to 6.5±0.2 with dilute sulfuric acid of 0.5~1.0mol / L. The system is aged at 75℃ for 80 minutes at this pH to further transform and condense the silicates and aluminum salts deposited on the surface of the titanium dioxide particles, forming a continuous and dense silica-alumina-hydroxyl composite inorganic barrier layer structure.
[0029] (5) Filtration: The filter cake is washed with deionized water until the conductivity of the filtrate is not higher than 100 μS / cm, thus obtaining the titanium dioxide intermediate filter cake with the first coating layer.
[0030] S3. Formation and post-processing of the second coating layer (1) The titanium dioxide intermediate filter cake with the first coating layer obtained in S2 is redispersed in deionized water to prepare a titanium dioxide water slurry with a solid content of 280 g / L containing the first coating layer. The pH of the system is adjusted to 4.5 ± 0.2 using dilute hydrochloric acid with a concentration of 0.5~1.0 mol / L.
[0031] (2) Take the siloxane precursor obtained from S1 and dilute it with a water / isopropanol mixed solution at pH 4.2 and a volume ratio of 1:1 to a concentration of 0.15 g / mL for its active component. The active component is calculated based on the content of compounds containing 3-hydroxy-nitro-butane groups. Pre-hydrolyze it at 25°C for 30 minutes to hydrolyze the residual Si-O-CH3 and / or Si-O-CH2-CH(OH)-CH2-Cl chlorohydrin ether end groups on the silicon atoms to generate Si-OH active sites, providing reaction sites for the subsequent condensation reaction with the M-OH sites on the surface of the first coating layer. See attached. Figure 2 The image shows the 1H NMR spectrum of the product after hydrolysis of the siloxane precursor.
[0032] (3) Under stirring conditions of 400 r / min, the pre-hydrolyzed solution is uniformly added to the titanium dioxide slurry containing the first coating layer within 40 minutes. By adjusting the amount of pre-hydrolyzed solution added, the loading of the second coating layer formed in the end is 0.25~0.65 wt% based on the mass of the titanium dioxide core. During the addition process, the system temperature is controlled not to exceed 30℃. After the addition is completed, the temperature and stirring speed are maintained and the reaction continues for 60 minutes.
[0033] (4) The pH of the system was slowly adjusted to 6.0±0.2 using 3% dilute ammonia water. The system was aged at 35°C for 40 minutes at this pH to promote the condensation reaction between the Si-OH groups in the organosiloxane molecules containing 3-hydroxy-nitro-butane groups after pre-hydrolysis and the M-OH sites on the surface of the first coating layer to form Si-OM bonds, thereby achieving covalent anchoring of the second coating layer.
[0034] (5) Filtration: The filter cake is washed 3-5 times with low conductivity deionized water until the conductivity of the filtrate is not higher than 50 μS / cm to remove unreacted siloxane precursors, free organic matter and soluble inorganic salts. Vacuum drying is used to remove moisture from the filter cake. The vacuum drying conditions are 60-80℃, vacuum degree not lower than 0.09MPa, and drying time is 8-16 hours.
[0035] (6) The dried material is deagglomerated and pulverized using an air jet mill at a pressure of 0.8 MPa to obtain the double-layer coated, sun-resistant titanium dioxide of the present invention.
[0036] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0037] The preferred embodiments of the present invention are described in detail below; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
[0038] Example 1 S1: In a reaction flask equipped with a mechanical stirrer, thermometer, constant-pressure dropping funnel, reflux condenser, and nitrogen protection device, add 120 mL of anhydrous ethanol and 40 mL of deionized water, mix well, add 38.7 g (0.20 mol) of N-methyl-3-aminopropyltrimethoxysilane, and stir to dissolve; under nitrogen protection, heat the reaction system to 60 °C, and slowly add 55.5 g (0.60 mol) of epichlorohydrin through a constant-pressure dropping funnel over 60 minutes; After the addition was complete, the mixture was stirred at 60°C for 7 hours. A sample was taken from the control room, and high-performance liquid chromatography (HPLC) showed that the product containing the 3-hydroxy-nitro-heterocyclic butylene group accounted for 96.3% of the nitrogen-containing main product. The reaction was then stopped. The reaction solution was cooled to room temperature and transferred to a rotary evaporator. The volatiles were removed by vacuum evaporation at a water bath temperature of 45°C and a vacuum degree of 0.095 MPa to obtain the siloxane precursor with an active component content of 97.2 wt%. The obtained siloxane precursor was sealed and transferred to a brown glass bottle and stored in a refrigerator at 5°C in the dark for later use.
[0039] S2: In a reactor equipped with mechanical stirring, a pH electrode, a thermometer, and a constant-temperature water bath, add 1L of deionized water and 300g of rutile titanium dioxide nuclei (rutile content 98.2wt%, D50 0.28μm) to prepare a slurry with a solid content of 300g / L; add 0.59g of sodium hexametaphosphate and disperse at 4000r / min under high shear for 60 minutes; heat the slurry to 75℃ and adjust the pH to 9.5 with a 0.8mol / L sodium hydroxide aqueous solution; then, under stirring at 800r / min, add 15% (w / w) of silica nonahydrate dropwise to the slurry using a horizontal flow pump. A sodium silicate aqueous solution (containing 42.6 g of sodium silicate nonahydrate, corresponding to a silica deposition of 3.0 wt%) was added dropwise. After the addition was complete, a 12% (w / w) aluminum sulfate octadechydrate aqueous solution (containing 48.1 g of aluminum sulfate octadechydrate, corresponding to an alumina deposition of 2.5 wt%) was added dropwise. During the addition, the pH fluctuation range of the system was controlled to not exceed ±0.5. After the addition was complete, the pH of the system was slowly adjusted to 6.5 with 0.8 mol / L dilute sulfuric acid, and the system was aged at 75°C for 80 minutes. The mixture was then filtered, and the filter cake was washed with deionized water at 60°C until the conductivity of the filtrate was 95.6 μS / cm, yielding the titanium dioxide intermediate filter cake with the first coating layer.
[0040] S3: The titanium dioxide intermediate filter cake with the first coating layer obtained in S2 was redispersed in deionized water to prepare a slurry with a solid content of 280 g / L; the pH of the system was adjusted to 4.5 with 0.8 mol / L dilute hydrochloric acid; 1.39 g of the siloxane precursor obtained in S1 (1.35 g of active component), accounting for 0.46 wt% of the core mass, was added to the solution. 4.2. 9.0 mL of a 1:1 volume ratio of deionized water / anhydrous isopropanol mixture was pre-hydrolyzed at 25°C for 30 minutes. Under stirring at 400 rpm, the pre-hydrolyzed solution was uniformly added to the titanium dioxide slurry containing the first coating layer via a constant-pressure dropping funnel over 40 minutes, with the system temperature controlled to not exceed 30°C during the addition. After addition, the temperature and stirring speed were maintained for another 60 minutes. The pH of the system was slowly adjusted to 6.2 with 3% (w / w) dilute ammonia, and aged at 35°C for 40 minutes at this pH. The mixture was filtered, and the filter cake was washed four times with deionized water until the conductivity of the filtrate reached 45.1 μS / cm. The filter cake was transferred to a vacuum drying oven and dried at 70°C and a vacuum of 0.095 MPa for 12 hours. The dried material was then pulverized using an air jet mill at a pressure of 0.8 MPa to obtain double-coated, sun-resistant titanium dioxide.
[0041] Example 2 Same as Example 1, except that in S3, 0.76 g of siloxane precursor concentrate (0.74 g of active component, accounting for 0.25 wt% of the core mass) was taken and added to 5.0 mL of water / isopropanol mixed solution for pre-hydrolysis for 10 minutes.
[0042] Example 3 Same as Example 1, except that in S3, 2.0 g of siloxane precursor concentrate (1.9 g of active component, accounting for 0.64 wt% of the core mass) was taken and added to 13.0 mL of water / isopropanol mixed solution for pre-hydrolysis for 30 minutes.
[0043] Example 4 Same as Example 1, except that in S2, a 20% sodium silicate nonahydrate aqueous solution (containing 27.9g of sodium silicate nonahydrate, corresponding to 2.0wt% silica deposition) and a 15% aluminum sulfate octadechydrate aqueous solution (containing 19.2g of aluminum sulfate octadechydrate, corresponding to 1.0wt% alumina deposition) are used.
[0044] Example 5 Same as Example 1, except that in S2, a 10% sodium silicate nonahydrate aqueous solution (containing 55.7g of sodium silicate nonahydrate, corresponding to 4.0wt% silica deposition) and an 8% aluminum sulfate octadechydrate aqueous solution (containing 77.0g of aluminum sulfate octadechydrate, corresponding to 4.0wt% alumina deposition) are used.
[0045] Example 6 Same as Example 1, except that in S2, a 15% sodium silicate nonahydrate aqueous solution (containing 55.7g of sodium silicate nonahydrate, corresponding to 4.0wt% silica deposition) and a 12% aluminum sulfate octadechydrate aqueous solution (containing 19.2g of aluminum sulfate octadechydrate, corresponding to 1.0wt% alumina deposition) are used.
[0046] Example 7 Same as Example 1, except that in S1, the amount of epichlorohydrin added was adjusted to 46.3 g (0.50 mol), the molar ratio of epichlorohydrin to N-methyl-3-aminopropyltrimethoxysilane was 2.5:1, the dropping time was 45 minutes, and after 7 hours of reaction, the product containing 3-hydroxyazacyclobutane groups accounted for 96.5% of the nitrogen-containing main product in the high-performance liquid chromatography. The content of the active component of the obtained siloxane precursor was 97.0 wt%.
[0047] Example 8 Same as Example 1, except that in S1, the amount of epichlorohydrin added was adjusted to 74.0 g (0.80 mol), the molar ratio of epichlorohydrin to N-methyl-3-aminopropyltrimethoxysilane was 4.0:1, the dropping time was 45 minutes, and after 7 hours of reaction, the content of the product containing the 3-hydroxyazine butylene group in the nitrogen-containing main product reached 98.6% in the high performance liquid chromatography. The content of the active component of the obtained siloxane precursor was 99.0 wt%.
[0048] Comparative Example 1 Same as Example 1, except that: only the first coating layer is prepared, and the second coating layer is not deposited. Step S1 is omitted; the operation of S2 is the same as in Example 1; the titanium dioxide intermediate filter cake with the first coating layer obtained in S2 is directly washed, vacuum dried and air-jet pulverized.
[0049] Comparative Example 2 γ-aminopropyltriethoxysilane was used to replace the siloxane precursor as the second coating layer. Step S1 was omitted; in S3, 1.35 g of γ-aminopropyltriethoxysilane (0.45 wt% of the core mass) was directly taken and added to 9.0 mL of a water / isopropanol mixed solution with pH 4.2 and a volume ratio of 1:1, and pre-hydrolyzed at 25 °C for 20 minutes; subsequent feeding, pH adjustment, aging, filtration, drying, and pulverization were the same as in Example 1.
[0050] Comparative Example 3 Titanium dioxide powder with only a first coating layer was physically adsorbed and modified using a conventional polyamidoamine-epoxychloropropane (PAE) wet strength agent, without forming a second coating layer covalently anchored to the particle surface. The PAE wet strength agent used contains 3-hydroxyazacyclobutane groups. Step S1 is omitted; Step S2 is the same as in Example 1. After obtaining the titanium dioxide intermediate filter cake with the first coating layer, it is washed, vacuum dried, and air-jet pulverized to obtain titanium dioxide powder with only the first coating layer. 300g of this powder is redispersed in 1000mL of deionized water, and 10.8g of PAE aqueous solution (solid content 12.5wt%, PAE feed amount 0.45wt% based on core mass) is added. The mixture is stirred and adsorbed at 40℃ for 60 minutes, filtered, and dried at 60℃ for 12 hours.
[0051] Comparative Example 4 The first coating layer is omitted, and the second coating layer of the present invention is deposited directly on the bare titanium dioxide core. Operation S1 is the same as in Example 1; step S2 is omitted; 300g of rutile titanium dioxide core is directly dispersed in 1070mL of deionized water to prepare a water slurry with a solid content of 280g / L. After adjusting the pH to 4.5 with dilute hydrochloric acid, operation S3 is directly performed, and the rest is the same as in Example 1.
[0052] Performance testing: 1. Surface Zeta potential measurement Refer to GB / T 32668-2016 "General Rules for Electrophoresis Method for Zeta Potential Analysis of Colloidal Particles".
[0053] Sample preparation: The samples obtained from each example and comparative example were prepared into suspensions with a concentration of 0.1 g / L. The dispersion medium was a 1 mmol / L potassium chloride aqueous solution. The pH was adjusted to 5.5 with 0.1 mol / L hydrochloric acid. The samples were sonicated for 5 minutes and then tested immediately.
[0054] Test method: A dynamic light scattering particle size analyzer was used, and the electrophoretic pool was a disposable folded capillary electrophoretic pool; the test temperature was 25℃, and the sample was equilibrated for 2 minutes before the test. Each sample was tested 5 times, and the average value was taken after removing the maximum and minimum values. The zeta potential (mV) was recorded.
[0055] 2. Nitrogen Element Retention Rate Determination Sample preparation: Take 12.0g of each sample from the examples and comparative examples and divide them into two portions of 6.0g each. The first portion is used to determine the initial nitrogen content N0. The sample does not require water washing pretreatment. It is directly dried in a vacuum drying oven at 60℃ for 4 hours to remove surface adsorbed moisture. After cooling to room temperature, 50mg is weighed and placed into a tin foil sample boat. The particle nitrogen content N0 is determined using an organic elemental analyzer according to the following test method. The second sample is used to determine the nitrogen content after anti-desorption elution. 6.0g of the sample is added to 100mL of 1wt% sodium chloride aqueous solution and washed for 30 minutes at 25℃ and 200r / min with stirring. After filtration, it is washed three times with deionized water to remove surface adsorbed sodium chloride residue. It is then vacuum dried at 60℃ for 8 hours. After cooling to room temperature, the nitrogen content N1 is determined using the same method.
[0056] Test method: An Elementar vario EL cube or equivalent organic elemental analyzer was used. The combustion tube temperature was 1150℃, the reduction tube temperature was 850℃, and the carrier gas was high-purity helium. Each sample weighed approximately 50 mg. Nitrogen retention rate (%) = N1 / N0 × 100%; each sample was tested 3 times and the average value was taken.
[0057] 3. Determination of first-pass retention rate in decorative base paper Sample preparation: Bleached sulfate softwood pulp and hardwood pulp were mixed at a mass ratio of 3:7 and beaten to a freeness of 42°SR, and the pulp concentration was adjusted to 0.5wt%. 200g of the above pulp (corresponding to 1.0g of oven-dry fiber) was placed in the reaction vessel of the Britt dynamic water filter, and 0.35g of titanium dioxide to be tested in the examples and comparative examples was added at 35% of the oven-dry mass of the pulp. That is, the amount of titanium dioxide added M was 0.35g. The mixture was stirred at 1000r / min for 15 minutes to ensure that the filler was fully dispersed in the pulp.
[0058] Test Method: Start the Britt dynamic water filter and collect 150 mL of white water by opening the bottom valve while stirring at 1000 rpm for approximately 30 seconds. Place the collected white water in a pre-weighed porcelain crucible, first evaporate and concentrate it to approximately 30 mL on a hot plate, then transfer it to a muffle furnace and ignite at 550°C for 2 hours. After cooling to room temperature, place it in a desiccator for 30 minutes and weigh the residual ash mass m1 using an analytical balance. Simultaneously, without adding titanium dioxide to the same batch of pulp, repeat the above procedure of collecting 150 mL of white water and igniting, and measure the background ash mass m0 of the pulp, which is used as a deduction item for the fiber background. The mass of titanium dioxide lost through the white water in 150 mL of white water is (m1-m0). Since the total volume of pulp in the reactor is approximately 200 mL and the white water sampling volume is 150 mL, the ratio of the sampling volume to the total pulp volume is k = 150 / V. 总 V 总 The total volume of the slurry in the reactor is recorded accurately based on the actual batching; then the total amount of titanium dioxide lost through the white water in the entire reaction system is M. pass =(m1-m0) / k; First-pass retention rate η (%) = (M 加入 -M pass ) / M 加入 ×100%. Each sample group was tested 3 times and the average value was taken.
[0059] 4. Test of colorfastness to sunlight Refer to GB / T 8427-2019 "Textiles - Tests for color fastness to artificial light: Xenon arc".
[0060] Sample preparation: Take samples from the examples and comparative examples and add filler at a rate of 35% of the oven-dry weight of the pulp to prepare samples with a basis weight of 80 g / m³. 2 Decorative base paper was handmade, calendered, and then cut into 60mm×60mm samples.
[0061] Test method: An Atlas Ci4000 xenon lamp aging test chamber was used, with a black panel temperature of 63℃±3℃, relative humidity of 50%±5%, a combination of daylight filters, and an irradiance of 1.10W / m². 2 @420nm, exposed for 72 hours; before and after the test, the Lab value of the sample was measured using an X-Rite Ci7800 spectrophotometer, and the color difference ΔE*ab was calculated.
[0062] 5. Determination of photocatalytic yellowing index Sample preparation: Take 0.10 g of each sample from the examples and comparative examples and add it to 50 mL of 20 mg / L methyl orange aqueous solution. Disperse by sonication for 10 minutes.
[0063] Test method: Under ultraviolet light irradiation (dominant wavelength 365nm, irradiation intensity 1.5mW / cm²), 2The reaction mixture was stirred for 120 minutes, with 5 mL samples taken every 20 minutes by centrifugation. The absorbance (A) of the supernatant was measured at 464 nm using a UV-Vis spectrophotometer, after background subtraction. Photocatalytic decolorization rate (%) = (A0 - A) t ) / A0×100%, where A0 is the initial absorbance before the reaction, A t The absorbance at reaction time t is given; the decolorization rate at 120 minutes is reported as an indicator of photocatalytic activity, with a smaller value indicating a better passivation effect.
[0064] 6. Determination of whiteness of decorative base paper Refer to GB / T 7974-2013 "Determination of blue light diffuse reflectance factor D65 luminance of paper, paperboard and pulp (diffuse / vertical method, outdoor daylight conditions)".
[0065] Sample preparation: The preparation of decorative base paper handmade sheets is the same as the above-mentioned lightfastness test.
[0066] Test method: Elrepho automatic whiteness meter, D65 light source, 2° viewing angle, 10mm test aperture was used; 6 different positions were measured for each sample, and the average value was taken.
[0067] Table 1 Surface structure parameters of each embodiment and comparative example Table 2. Application performance of decorative base paper in each embodiment and comparative example. Results analysis: (1) As shown in Tables 1 and 2, the double-coated lightfast titanium dioxide obtained in Examples 1 to 8 all showed stable technical effects in terms of surface structure parameters and application performance of decorative base paper: the zeta potential of the particle surface was in a high positive range, the nitrogen retention rate was in a high level, the ultraviolet photocatalytic decolorization rate was maintained at a low level, and the first pass retention rate, lightfastness and whiteness of the decorative base paper were in a better range. This shows that the siloxane precursor containing 3-hydroxy-nitro-heterocyclic butyronitrile group described in this invention can stably achieve the three technical effects of permanent positive charge on particle surface, covalent fixation of particle-fiber interface and passivation of titanium dioxide photocatalytic activity when the loading amount of the second coating layer, the composition and ratio of the first coating layer, the molar ratio of epichlorohydrin to secondary amine and other core parameters within the range described in this invention are changed. Among them, Example 1 adopted the median combination of core parameters, and all performances were in a better level, indicating that the technical solution of this invention has good robustness and feasibility.
[0068] (2) Comparative Example 1 omitted the second coating layer, and the particle surface lacked permanently positively charged groups, resulting in a significantly negative Zeta potential. The particle-fiber interface lacked electrostatic adsorption and covalent fixation, leading to a significant decrease in the first-pass retention rate. Although the lightfastness and photocatalytic passivation performance of Comparative Example 1 were similar to those of the Example, the whiteness of the decorative base paper decreased due to the loss of a large number of particles, indicating that the second coating layer is a necessary technical feature that determines the fixation ability of the particle-fiber interface. Comparative Example 2 used a conventional aminosilane coupling agent instead of the siloxane precursor containing the 3-hydroxy-nitro-heterocyclic butyronitrile group of the present invention. Although it was covalently anchored to the first coating layer, the amino groups exposed on the outer surface did not have the ring-opening activity to covalently react with the fiber carboxyl groups, resulting in a significantly lower first-pass retention rate than the Example.
[0069] (3) In Comparative Example 3, nitrogen heterocyclic butylene groups were introduced using an aqueous polymeric PAE wet-strength agent and a retention aid. Although PAE itself contains a four-membered ring structure capable of ring-opening reactions, it was introduced in the form of an aqueous polymer and did not form a covalent anchor with the particle surface. As a result, a large amount of PAE molecules were lost during washing and processing, and the nitrogen retention rate of the particles was significantly lower than that of the Example. Although the first-pass retention rate was improved compared to Comparative Example 1, it was still significantly lower than that of the Example of the Present Invention. This indicates that the design of a second coating layer that covalently anchors the nitrogen heterocyclic butylene groups to the particle surface in the form of small molecules is necessary for a lasting fixation effect. Comparative Example 4 omitted the first coating layer. Although the second coating layer can provide a high Zeta potential and a first-pass retention rate, the photoactive sites on the surface of the titanium dioxide core were not passivated, and a large number of reactive oxygen species were generated under ultraviolet aging conditions, resulting in a significant increase in the color difference value and a significant increase in the photocatalytic decolorization rate. This indicates that the continuous inorganic barrier layer structure of the first coating layer is a necessary technical feature for achieving the sun-resistant function.
[0070] In summary, this invention achieves passivation of the photocatalytic activity of titanium dioxide and chemical fixation of the particle-fiber interface by sequentially forming a continuous silica-alumina composite inorganic barrier layer as the first coating layer and an organosiloxane layer formed by hydrolysis and condensation covalent anchoring of a siloxane precursor containing a 3-hydroxy-nitro-heterocyclic butyronitrile group as the second coating layer on the surface of the rutile titanium dioxide core. This solves the problems of particle loss and organic layer detachment caused by the reliance on physical adsorption and electrostatic adsorption in the modification of the outer layer of existing decorative titanium dioxide.
Claims
1. A double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials, comprising a core, a first coating layer, and a second coating layer, characterized in that, The core is rutile titanium dioxide; the first coating layer is a continuous silica-alumina-hydroxyl composite inorganic barrier layer coating the surface of the core; the second coating layer is an organosiloxane layer containing 3-hydroxyazocyclobutane groups covering the outer surface of the first coating layer; the second coating layer is fixed to the M-OH sites on the surface of the first coating layer by Si-OM bonds, where M is Si, Al, or Ti; the organosiloxane layer containing 3-hydroxyazocyclobutane groups is formed by hydrolysis and condensation of a siloxane precursor, the structure of which is... , where R is H, CH3 or CH2-CH(OH)-CH2-Cl.
2. The double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials as described in claim 1, characterized in that, In the continuous silica-alumina composite inorganic barrier layer, based on the mass of the core, the amount of silica deposited in the first coating layer is 2.0~4.0 wt%, the amount of alumina deposited is 1.0~4.0 wt%, and the mass ratio of silica to alumina is 1:(0.25~1.0); based on the mass of the core, the loading of the second coating layer is 0.25~0.65 wt%.
3. The method for preparing double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials according to any one of claims 1 to 2, characterized in that, Includes the following steps: S1: Dissolve N-methyl-3-aminopropyltrimethoxysilane in a water / anhydrous ethanol mixture to prepare a solution with a concentration of 1.2 mol / L; heat under nitrogen protection and add epichlorohydrin dropwise, maintain the temperature and react until the content of the product containing 3-hydroxy-nitro-heterocyclic butyronitrile group is not less than 95% of the nitrogen-containing main product, cool to room temperature and remove volatiles under reduced pressure to obtain the siloxane precursor; S2: Rutile titanium dioxide cores and sodium hexametaphosphate were added to deionized water for high-shear dispersion to obtain an aqueous slurry. After heating, the pH of the system was adjusted to 9.5±0.2 with sodium hydroxide aqueous solution. Under stirring, sodium silicate nonahydrate aqueous solution was added dropwise first, followed by aluminum sulfate octadecahydrate aqueous solution. During the dropwise addition, the pH fluctuation range of the system was controlled to not exceed ±0.
5. After the dropwise addition was completed, the pH of the system was adjusted back to 6.5±0.2 with dilute sulfuric acid and aged at the temperature. After filtration and washing, titanium dioxide intermediate filter cake containing the first coating layer was obtained. S3: The titanium dioxide intermediate filter cake containing the first coating layer is redispersed in deionized water, and the pH of the system is adjusted to 4.5±0.2 with dilute hydrochloric acid to obtain a titanium dioxide slurry containing the first coating layer; the siloxane precursor is diluted with a water / isopropanol mixed solution and pre-hydrolyzed to obtain a pre-hydrolyzed solution; the pre-hydrolyzed solution is added to the titanium dioxide slurry containing the first coating layer, and after the reaction is carried out at a constant temperature and stirred, the pH of the system is adjusted to 6.0±0.2 with dilute ammonia and aged at a constant temperature. After filtration, washing, vacuum drying and air jet pulverization, the double-coated sun-resistant titanium dioxide is obtained.
4. The preparation method of double-layer coated light-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, The molar ratio of epichlorohydrin to N-methyl-3-aminopropyltrimethoxysilane in step S1 is (2.5~4.0):
1.
5. The preparation method of double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, In step S1, the volume ratio of the water / anhydrous ethanol mixed solvent is 1:3; the temperature for adding epichlorohydrin and maintaining the reaction temperature is 60℃±5℃, and the adding time is 60 minutes; the vacuum degree for removing volatiles by vacuum distillation is not less than 0.09MPa, and the temperature is not higher than 50℃.
6. The preparation method of double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, In step S2, the solid content of the water slurry is 300 g / L; the amount of sodium hexametaphosphate added is 0.2% of the core mass; the high-shear dispersion speed is 4000 r / min and the time is 60 minutes. The temperature for the heating is 75℃±5℃.
7. The preparation method of double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, In step S2, the mass concentration of the sodium silicate nonahydrate aqueous solution is 10%~20%, and the mass concentration of the aluminum sulfate octadecahydrate aqueous solution is 8%~15%; the heat preservation aging conditions are: aging at 75℃ for 80 minutes; the washing is carried out until the conductivity of the filtrate is not higher than 100μS / cm.
8. The preparation method of double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, In step S3, the solid content of the titanium dioxide aqueous slurry containing the first coating layer is 280 g / L; the pH of the water / isopropanol mixed solution is 4.2 and the volume ratio is 1:1; the concentration of the active component after dilution of the siloxane precursor is 0.15 g / mL, and the active component is calculated based on the content of compounds containing 3-hydroxyazine cyclobutane groups; the pre-hydrolysis temperature is 25°C and the time is 30 minutes.
9. The preparation method of double-layer coated light-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, The pre-hydrolyzed solution mentioned in step S3 is added within 40 minutes under stirring at 400 r / min, and the system temperature does not exceed 30°C during the addition process; the time for the heat preservation and stirring reaction is 60 minutes.
10. The method for preparing double-layer coated, sun-resistant titanium dioxide for paper-based decorative materials as described in claim 3, characterized in that, The heat preservation and aging conditions in step S3 are as follows: aging at 35°C for 40 minutes; washing is carried out until the conductivity of the filtrate is not higher than 50 μS / cm; and the pressure of the air jet pulverizer is 0.8 MPa.
Citation Information
Patent Citations
A method for preparing titanium dioxide pigment for high lightfastness laminated paper
CN109705630B
Composite modified titanium dioxide as well as preparation method and application thereof
CN111253781A