Optical laminate and image display device using the optical laminate
By setting a reinforcing layer with high-pressure elastic modulus and a compatible region in the optical laminate, and combining it with another phase difference layer, the problem of phase difference layer cracking under high temperature and high humidity conditions was solved, and the durability of the optical laminate was improved.
Patent Information
- Application Number
- CN202610622783.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-05-08
- Publication Date
- 2026-11-10
AI Technical Summary
Existing optical laminates are prone to developing cracks in the phase retardation layer under harsh high temperature and humidity environments, affecting their performance and reliability.
By setting a reinforcing layer on the side opposite to the polarizer of the phase retardation layer, the compressive elastic modulus of the reinforcing layer is higher than that of the phase retardation layer, and a compatible region is formed between the two, reducing adhesive penetration. This, combined with another phase retardation layer, suppresses crack formation.
It effectively suppresses cracks in the phase retardation layer under harsh high temperature and high humidity environments, thereby improving the durability and reliability of optical laminates.
Smart Images

Figure CN123066909A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate and an image display device using the same. Background Art
[0002] In recent years, image display devices typified by liquid crystal display devices and electroluminescent (EL) display devices (for example, organic EL display devices and inorganic EL display devices) have been rapidly popularized. Polarizing plates and retardation plates are typically used in image display devices. In practice, an optical laminate in which a polarizing plate and a retardation plate are integrated is widely used (for example, Patent Document 1). In recent years, as the applications of image display devices have expanded, various performances have been expected to be improved for optical laminates. For example, optical laminates are sometimes required to have durability under severe high-temperature and high-humidity environments that have not been conventionally required.
[0003] Description of Related Art Patent Documents Patent Document 1: Japanese Patent No. 3325560 Summary of the Invention
[0004] Problems to be Solved by the Invention The present invention has been made to solve the above-mentioned conventional problems, and a main object thereof is to provide an optical laminate in which the occurrence of cracks in the retardation layer is suppressed even under a severe high-temperature and high-humidity environment.
[0005] Means for Solving the Problems [1] An optical laminate according to an embodiment of the present invention sequentially has a polarizing plate including a polarizer, a retardation layer, and a reinforcing layer; the retardation layer is composed of a stretched film of a resin film and satisfies a relationship of Re(450) < Re(550); the reinforcing layer is a cured layer of an active energy ray-curable resin composition; and an indentation elastic modulus of a cross section of the reinforcing layer is equal to or higher than an indentation elastic modulus of a cross section of the retardation layer. Here, Re(450) and Re(550) are in-plane retardations measured with light having wavelengths of 450 nm and 550 nm, respectively, at 23°C.
[0006] [2] In the above [1], Re(550) of the retardation layer is from 100 nm to 200 nm, and an angle formed by a slow axis of the retardation layer and an absorption axis of the polarizer is from 40° to 50° or from 130° to 140°.
[0007] [3] In the above [1] or [2], the optical laminate further has another retardation layer exhibiting refractive index characteristics of nz > nx = ny on a side of the reinforcing layer opposite to the retardation layer.
[0008] [4] In any of the above [1] to [3], the optical laminate further has a blocking layer between the polarizer and the phase difference layer.
[0009] [5] In any of the above [1] to [4], the phase difference layer contains a resin, the resin comprising at least one bonding group selected from the group consisting of carbonate bonds and ester bonds and at least one structural unit selected from the group consisting of structural units represented by the following general formula (1) and structural units represented by the following general formula (2), and having positive refractive index anisotropy.
[0010] [Chemical Formula 1] [Chemical Formula 2] In general formulas (1) and (2), R 1 ~R 3 Each is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, R 4 ~R 9 Each of the following is independently a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 4 to 10 carbon atoms, a substituted or unsubstituted acyl group having 1 to 10 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, a substituted or unsubstituted aryloxy group having 1 to 10 carbon atoms, a substituted or unsubstituted amino group, a substituted or unsubstituted vinyl group having 1 to 10 carbon atoms, a substituted or unsubstituted ethynyl group having 1 to 10 carbon atoms, a sulfur atom having a substituent, a silicon atom having a substituent, a halogen atom, a nitro group, or a cyano group; wherein, R 4 ~R 9 They can be the same or different, R 4 ~R 9 At least two adjacent groups can also bond to each other to form a ring.
[0011] [6] In any of the above [1] to [5], the polarizer includes a protective layer on the side of the polarizer opposite to the phase difference layer, the Re (550) of the protective layer is less than 20 nm, and the Re (450) / Re (550) is 0.98 to 1.03.
[0012] [7] In the above [6], the protective layer comprises a polycarbonate resin comprising a structural unit derived from at least one dihydroxy compound selected from the group consisting of isosorbide, isomannitol and isotretinoin.
[0013] [8] In any of the above [3] to [7], in the above optical laminate, an adhesive layer is provided between the above reinforcing layer and the other phase difference layer.
[0014] [9] In any of the above [3] to [7], the above-mentioned reinforcing layer also functions as an adhesive layer.
[0015]
[10] In the above [9], the active energy ray curable resin composition constituting the above-mentioned reinforcing layer comprises a difunctional monomer, a trifunctional monomer, an oligomer and boric acid.
[0016]
[11] In any of the above [1] to
[10] , a compatible region, namely an intermediate layer, containing the components of the phase difference layer and the reinforcement layer is formed between the phase difference layer and the reinforcement layer, and the thickness of the intermediate layer is 0.8 μm or less.
[0017]
[12] According to another aspect of the present invention, an image display device is provided. The image display device includes the optical laminates described above [1] to
[11] .
[0018] Invention Effects According to embodiments of the present invention, it is possible to realize an optical laminate that suppresses the generation of cracks in the retardation layer even under harsh high temperature and high humidity environments. Attached Figure Description
[0019] Figure 1 This is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention.
[0020] Figure 2 This is a schematic cross-sectional view of an optical laminate according to another embodiment of the present invention.
[0021] Explanation of symbols 10 Polarizing filters 11. Polarizer 12 First protective layer 13 Second protective layer 21 First phase difference layer 22 Second phase difference layer 30 Reinforcement Layers 40 barrier layers 100 optical laminates 101 Optical Laminate Detailed Implementation
[0022] The following describes representative embodiments of the present invention, but the present invention is not limited to these embodiments.
[0023] (Definitions of terms and symbols) The definitions of terms and symbols used in this specification are as follows.
[0024] (1) Refractive index (nx, ny, nz) “nx” is the refractive index in the direction where the refractive index is maximum (i.e., the slow axis direction), “ny” is the refractive index in the direction orthogonal to the slow axis (i.e., the fast axis direction), and “nz” is the refractive index in the thickness direction.
[0025] (2) In-plane phase difference (Re) “Re(λ)” is the in-plane phase difference of the film measured at 23°C using light with a wavelength of λ nm. For example, “Re(450)” is the in-plane phase difference of the film measured at 23°C using light with a wavelength of 450 nm. When the thickness of the film is set to d (nm), Re(λ) is obtained by the formula: Re = (nx - ny) × d.
[0026] (3) Phase difference in the thickness direction (Rth) “Rth(λ)” is the phase difference in the thickness direction of the film measured at 23°C using light with a wavelength of λ nm. For example, “Rth(450)” is the phase difference in the thickness direction of the film measured at 23°C using light with a wavelength of 450 nm. When the thickness of the film is set to d (nm), Rth(λ) is obtained by the formula: Rth = (nx - nz) × d.
[0027] (4) Nz coefficient The Nz coefficient is obtained by Nz=Rth / Re.
[0028] (5) Angle When angles are mentioned in this instruction manual, unless otherwise specified, the angle includes both clockwise and counterclockwise angles. Therefore, "45°" refers to ±45°.
[0029] A. Overall composition of optical laminates Figure 1 This is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. The optical laminate 100 of the example figure sequentially includes a polarizer 10, a retardation layer 21, and a reinforcing layer 30. The polarizer 10 and the retardation layer 21 are typically laminated together via an adhesive layer. The reinforcing layer 30 is typically laminated directly (i.e., without an adhesive layer) onto the retardation layer 21. The polarizer 10 includes a polarizer 11, a first protective layer 12 disposed on one side of the polarizer 11, and a second protective layer 13 disposed on the other side of the polarizer 11. Depending on the purpose, at least one of the first protective layer 12 and the second protective layer 13 may be omitted. That is, the polarizer 10 can be a so-called two-protection polarizer, a so-called single-protection polarizer, or it can be constituted solely by the polarizer. For example, in the optical laminate 100 of the example figure, the retardation layer 21 functions as a protective layer, therefore the second protective layer 13 may be omitted.
[0030] The retardation layer 21 is composed of a stretched resin film. Further, the retardation layer 21 satisfies the relationship of Re(450) < Re(550). That is, the retardation layer 21 exhibits reverse dispersion wavelength dependence. Typically, Re(550) of the retardation layer 21 is 100 nm to 200 nm. The angle formed by the slow axis of the retardation layer 21 and the absorption axis of the polarizer 11 is preferably 40° to 50°, more preferably 42° to 48°, still more preferably 44° to 46°, and particularly preferably about 45°; or preferably 130° to 140°, more preferably 132° to 138°, still more preferably 134° to 136°, and particularly preferably about 135°.
[0031] The reinforcing layer 30 is a cured layer of an active energy ray-curable resin composition, and the indentation elastic modulus of the cross section of the reinforcing layer 30 is equal to or higher than the indentation elastic modulus of the cross section of the retardation layer 21. According to the embodiment of the present invention, by providing such a reinforcing layer on the side of the retardation layer opposite to the polarizing plate, it is possible to realize an optical laminate in which the occurrence of cracks in the retardation layer is suppressed even under a severe high-temperature and high-humidity environment. The details are described below. Since the retardation layer used in the embodiment of the present invention exhibits extremely excellent circularly polarized light characteristics, it is possible to realize an optical laminate (circular polarizing plate) having a very excellent antireflection function. Further, by using such a retardation layer in combination with another retardation layer that exhibits a refractive index characteristic relationship of nz>nx=ny as described later, a wide viewing angle of the antireflection function can be achieved. On the other hand, since the stretched resin film constituting such a retardation layer has large thermal shrinkage and high water absorption, the reliability under a high-temperature and high-humidity environment may be insufficient, and further, cracks may occur under a severe high-temperature and high-humidity environment which has become a new characteristic-related standard in recent years. The present inventors have conducted intensive studies on the occurrence of cracks in the retardation layer under a severe high-temperature and high-humidity environment, and as a result, have found that a compatible region (containing the components of the retardation layer and the components of the adhesive) formed by penetration of the monomer component of the adhesive for laminating the retardation layer and a constituent element adjacent to the side of the retardation layer opposite to the polarizing plate (for example, another retardation layer) into the retardation layer is very fragile, and this fragile region can become a crack initiation point. Further, the present inventors have conducted repeated tests on means for suppressing the formation of such a fragile region, and as a result, have found that the formation of the above-mentioned fragile region can be suppressed by providing a layer adjacent to the retardation layer that has an indentation elastic modulus of the cross section equal to or higher than a predetermined value (that is, a hard layer). As a result, it has been found that cracks in the retardation layer can be suppressed even under a severe high-temperature and high-humidity environment, and the present invention has been completed. It should be noted that the above mechanism is a presumption, and this mechanism does not limit or restrict the embodiments of the present invention.
[0032] In this specification, the "indentation modulus of the cross section" can be obtained by cross-sectional analysis using atomic force microscopy (AFM). It is said that cross-sectional analysis using AFM can determine data integrated with nanoindentation at the level of a small area of the cross section. Specifically, the indentation modulus of the cross section can be determined by exposing the cross section by cutting the optical laminate with a cryo-microtome and performing AFM focal mapping on the exposed section. The indentation modulus of the cross section of each layer (e.g., retardation layer, reinforcing layer, adhesive layer) is substantially constant in most of the thickness direction of each layer, but the value can change near the interface with adjacent layers (and can change abruptly depending on the relationship with adjacent layers). In this specification, the indentation modulus of the cross section of each layer (e.g., retardation layer, reinforcing layer, adhesive layer) refers to the value just before it begins to change near the interface with adjacent layers. Hereinafter, the "indentation modulus of the cross section" will sometimes be simply referred to as "indentation modulus".
[0033] The indentation elastic modulus of the reinforcing layer 30 is, as described above, greater than, the indentation elastic modulus of the retardation layer 21, and preferably greater than that of the retardation layer. The indentation elastic modulus of the reinforcing layer 30 may, for example, be 1.5 GPa to 2.5 GPa, or, for example, 1.8 GPa to 2.2 GPa. The indentation elastic modulus of the retardation layer 21 may, for example, be 1.0 GPa to 2.0 GPa, or, for example, 1.2 GPa to 1.8 GPa. The difference between the indentation elastic modulus of the reinforcing layer 30 and the indentation elastic modulus of the retardation layer 21 may, for example, be 0.0 GPa to 1.2 GPa, or, for example, 0.1 GPa to 0.8 GPa, or, for example, 0.3 GPa to 0.8 GPa. If the indentation elastic moduli of the reinforcing layer and the retardation layer are in this relationship, the formation of the aforementioned fragile region can be effectively suppressed. As a result, cracks in the retardation layer can be suppressed even under harsh high-temperature and high-humidity environments.
[0034] As described above, according to embodiments of the present invention, the formation of a fragile region (a compatible region containing components of the phase retardation layer and the adhesive) caused by the adhesive used for lamination with adjacent layers can be suppressed on the side of the phase retardation layer opposite to the polarizer. In other words, an intermediate layer containing components of the phase retardation layer and the reinforcing layer 30 can be formed between the phase retardation layer 21 and the reinforcing layer 30, resulting in a reduction in the thickness of the intermediate layer. As a result, cracking of the phase retardation layer can be suppressed even under harsh high temperature and high humidity environments. The thickness of the intermediate layer is preferably 0.8 μm or less, more preferably 0.7 μm or less, further preferably 0.6 μm or less, and particularly preferably 0.5 μm or less. On the other hand, the thickness of the intermediate layer can be, for example, 0.1 μm or more, and also, for example, 0.2 μm or more. It should be noted that since the phase retardation layer is typically laminated between the adhesive layer and the polarizer, the problem of a fragile region caused by the adhesive, as described above, is not substantially generated at the interface between the phase retardation layer and the polarizer.
[0035] Figure 2 This is a schematic cross-sectional view of an optical laminate according to another embodiment of the present invention. The optical laminate 101 shown in the figure further has another phase retardation layer 22 on the side of the phase retardation layer 21 opposite to the polarizer 10, exhibiting a refractive index characteristic showing a relationship of nz > nx = ny. By providing such another phase retardation layer, reflections in the tilt direction can be effectively prevented, making it possible to widen the anti-reflection function. Hereinafter, for convenience, the phase retardation layer 21 will sometimes be referred to as the "first phase retardation layer," and the other phase retardation layer 22 will sometimes be referred to as the "second phase retardation layer."
[0036] As needed, it can also be as follows Figure 2 As shown, a barrier layer 40 is further provided between the polarizer 10 and the first retardation layer 21. By providing the barrier layer, the movement of moisture within the optical laminate under high temperature and high humidity conditions can be suppressed, resulting in suppression of end-coloration of the polarizer. Furthermore, the barrier layer can suppress the movement of iodine that may be contained in the polarizer, reducing the impact of the polarizer on other components. For example, when the optical laminate is mounted in an image display device (e.g., an organic EL display device), corrosion of the metal components of the image display device can be suppressed. Moreover, by providing such a barrier layer adjacent to the polarizer, the second protective layer can be omitted. The barrier layer is significantly thinner than the second protective layer, thus maintaining good protection of the polarizer and contributing to the thinning of the optical laminate.
[0037] The reinforcing layer 30 can be, for example, a hard coating. In this case, an adhesive layer (not shown) can be provided between the reinforcing layer 30 and the second retardation layer 22. The adhesive layer can typically be composed of an adhesive. By providing a hard coating having the indentation modulus of elasticity as described above as the reinforcing layer, the penetration of monomer components of the active energy ray curable resin composition (resin composition for hard coating formation) into the first retardation layer can be suppressed. As a result, the thickness of the intermediate layer (fragmented layer) can be reduced, and cracking of the first retardation layer can be suppressed. Furthermore, regardless of the type of adhesive used as the adhesive layer (adhesive) for laminating the second retardation layer, the penetration of monomer components of the adhesive into the first retardation layer can be suppressed (essentially blocked) by the hard coating, thus greatly expanding the options for the adhesive layer.
[0038] The reinforcing layer 30 can also function as an adhesive layer, for example. In other words, the reinforcing layer 30 can be an adhesive layer. In this case, the adhesive layer used for laminating the second retardation layer can be omitted. By providing an adhesive layer with the compressive modulus described above as a reinforcing layer, the penetration of monomer components into the first retardation layer can be suppressed even when using an adhesive. As a result, the thickness of the intermediate layer (weak layer) can be reduced, and cracking of the first retardation layer can be suppressed.
[0039] The optical laminate can be in the form of a single sheet or in the form of a strip. In this specification, "strip" refers to an elongated shape whose length is sufficiently long relative to its width, such as an elongated shape whose length is 10 times or more, preferably 20 times or more, than its width. The strip-shaped optical laminate can be rolled into a roll.
[0040] In practical applications, the optical laminate has an adhesive layer (not shown) as the outermost layer on the side opposite to the polarizer, serving as the phasing layer. The adhesive layer allows the optical laminate to be attached to an image display unit. Furthermore, a release liner is preferably temporarily adhered to the surface of the adhesive layer until the optical laminate is put into use. Temporarily adhering the release liner protects the adhesive layer and allows for the formation of a roll of the optical laminate.
[0041] The following describes the constituent elements of optical laminates.
[0042] B. Polarizer As the polarizer 11, any suitable polarizer can be used. For example, the resin film forming the polarizer can be a single-layer resin film or a laminate of two or more layers.
[0043] Specific examples of polarizers composed of single-layer resin films include polarizers obtained by dyeing and stretching hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films using dichroic substances such as iodine or dichroic dyes; and polyene-based oriented films such as dehydrated PVA products or dehydrochlorinated polyvinyl chloride products. From the perspective of superior optical properties, polarizers obtained by dyeing PVA films with iodine and then uniaxially stretching them are preferred.
[0044] The aforementioned dyeing using iodine is performed, for example, by immersing the PVA membrane in an aqueous iodine solution. The stretching ratio for the uniaxial stretching is preferably 3 to 7 times. Stretching can be performed after dyeing or simultaneously with dyeing. Alternatively, dyeing can be performed after stretching. Depending on the needs, the PVA membrane may undergo swelling treatment, cross-linking treatment, washing treatment, drying treatment, etc. For example, by immersing the PVA membrane in water for washing before dyeing, not only can stains and anti-blocking agents on the surface of the PVA membrane be washed away, but the PVA membrane can also swell to prevent uneven dyeing.
[0045] As specific examples of a polarizer obtained using two or more layers, examples include a polarizer obtained using a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a resin substrate and a PVA-based resin layer coated on the resin substrate can be manufactured, for example, by coating a PVA-based resin solution onto a resin substrate and drying it to form a PVA-based resin layer on the resin substrate, thus obtaining a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to form a polarizer from the PVA-based resin layer. In this embodiment, it is preferable to form a polyvinyl alcohol-based resin layer comprising a halide and a polyvinyl alcohol-based resin on one side of the resin substrate. Stretching typically includes immersing the laminate in an aqueous boric acid solution for stretching. Furthermore, stretching may, if necessary, further include air stretching of the laminate at a high temperature (e.g., above 95°C) before stretching in the aqueous boric acid solution. Furthermore, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which it shrinks by more than 2% in the width direction while being heated and conveyed along the length direction. Typically, the manufacturing method of this embodiment includes sequentially performing an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate. By introducing assisted stretching, even when PVA is coated on a thermoplastic resin, the crystallinity of PVA can be improved, resulting in high optical properties. Furthermore, by simultaneously improving the orientation of PVA beforehand, problems such as decreased orientation and dissolution of PVA can be prevented when immersed in water during subsequent dyeing and stretching processes, thus achieving high optical properties. Moreover, when the PVA-based resin layer is immersed in a liquid, compared to the case where the PVA-based resin layer does not contain halides, the disorder of polyvinyl alcohol molecule orientation and the reduction of orientation can be suppressed. Therefore, the optical properties of the polarizer obtained by immersing the laminate in a liquid through dyeing and underwater stretching treatments can be improved. Furthermore, by using the drying shrinkage treatment to shrink the laminate along the width direction, optical properties can be improved. The resulting resin substrate / polarizer laminate can be used directly (i.e., the resin substrate can also be used as a protective layer for the polarizer), or it can be used by laminating any suitable protective layer corresponding to the purpose onto the peel surface obtained by peeling the resin substrate from the resin substrate / polarizer laminate, or onto the surface opposite to the peel surface. Detailed descriptions of such a polarizer manufacturing method are described, for example, in Japanese Patent Application Publication No. 2012-73580 and Japanese Patent No. 6470455. The entire descriptions of these publications are incorporated herein by reference.
[0046] The thickness of the polarizer is preferably 15 μm or less, more preferably 12 μm or less, even more preferably 10 μm or less, particularly preferably 8 μm or less, and especially preferably 5 μm or less. The lower limit of the polarizer thickness can be, for example, 1 μm. If the polarizer thickness is within such a range, curling during heating can be effectively suppressed, and good appearance durability during heating can be obtained.
[0047] The polarizer preferably exhibits absorption dichroism at any wavelength from 380 nm to 780 nm. The transmittance of the polarizer is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, more preferably 44.5% to 46.0%. The polarization degree of the polarizer is preferably 97.0% or higher, more preferably 99.0% or higher, and even more preferably 99.9% or higher.
[0048] C. Protective layer The first protective layer 12 and the second protective layer 13 are each formed of any suitable membrane that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the membrane include cellulose resins such as triacetyl cellulose (TAC), cyclic olefin resins such as polynorbornene, (meth)acrylic resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene, and polycarbonate resins.
[0049] The Re(550) of the first protective layer 12 is preferably 20 nm or less, more preferably 15 nm or less, even more preferably 10 nm or less, particularly preferably 8 nm or less, and especially preferably 5 nm or less. The lower limit of the Re(550) of the first protective layer 12 can be, for example, 0 nm. Furthermore, the first protective layer 12 preferably exhibits a flat wavelength dispersion dependence. In this case, the Re(450) / Re(550) of the first protective layer 12 is preferably 0.95 to 1.05, more preferably 0.98 to 1.03.
[0050] The first protective layer 12 typically comprises a polycarbonate resin. Preferably, the polycarbonate resin comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic diethanol, diethylene glycol, triethylene glycol, or polyethylene glycol, and alkylene glycols or spirodiols. More preferably, the polycarbonate resin comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from alicyclic diethanol and / or structural units derived from diethylene glycol, triethylene glycol, or polyethylene glycol; more preferably, it comprises structural units derived from isosorbide-based dihydroxy compounds and structural units derived from alicyclic diethanol. The polycarbonate resin may also, as needed, comprise structural units derived from other dihydroxy compounds.
[0051] In one embodiment, the polycarbonate resin may also contain unit structures derived from fluorene dihydroxy compounds represented by the following general formula (A).
[0052] [Chemical Formula 3] (In the above general formula (A), R1 to R4 independently represent hydrogen atoms, substituted or unsubstituted alkyl groups having 1 to 20 carbon atoms, substituted or unsubstituted cycloalkyl groups having 6 to 20 carbon atoms, or substituted or unsubstituted aryl groups having 6 to 20 carbon atoms, respectively; X represents substituted or unsubstituted alkylene groups having 2 to 10 carbon atoms, substituted or unsubstituted cycloalkylene groups having 6 to 20 carbon atoms, or substituted or unsubstituted arylene groups having 6 to 20 carbon atoms, respectively; and m and n are independently integers from 0 to 5.) Specific examples of dihydroxy compounds represented by general formula (A) include 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis(4-hydroxy-3-ethylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-propylphenyl)fluorene, 9,9-bis(4-hydroxy-3-isopropylphenyl)fluorene, 9,9-bis(4-hydroxy-3-n-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-sec-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-tert-butylphenyl)fluorene, 9,9-bis(4-hydroxy-3-cyclohexylphenyl)fluorene, 9,9-bis(4-hydroxy-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy) ... Fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methylphenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropoxy)phenyl)fluorene, etc.
[0053] In addition to the structural units described above, the polycarbonate resins may also contain structural units derived from dihydroxy compounds such as isomannitol, isotretinoin, spirodiol, dioxanediol, diethylene glycol (DEG), triethylene glycol (TEG), polyethylene glycol (PEG), and bisphenols. Preferably, the polycarbonate resins may contain structural units derived from at least one dihydroxy compound selected from the group consisting of isomannitol and isotretinoin.
[0054] Details of polycarbonate resins containing structural units derived from dihydroxy compounds are described, for example, in Japanese Patent No. 5204200, Japanese Unexamined Patent Publication No. 2012-67300, Japanese Patent No. 3325560, and WO2014 / 061677. The descriptions in these patent documents are incorporated herein by reference.
[0055] In one embodiment, the polycarbonate resin may also contain oligofluorene structural units. Examples of polycarbonate resins containing oligofluorene structural units include those containing structural units represented by the above general formula (1) and / or the above general formula (2).
[0056] Such polycarbonate resins, as described below, can also be suitably used for the first retardation layer. The first retardation layer typically exhibits an anti-dispersion wavelength dependence, while the first protective layer, as described above, exhibits a flat wavelength dispersion dependence. The wavelength dispersion dependence can be controlled by adjusting the type, number, combination, copolymerization ratio, etc., of the structural units.
[0057] The optical laminate is typically disposed on the visual recognition side of the image display device, as described below, and the first protective layer 12 is typically disposed on its visual recognition side. Therefore, the first protective layer 12 may be subjected to surface treatments such as hard coating, anti-reflective treatment, anti-adhesion treatment, and anti-glare treatment, as needed. Furthermore / or, the first protective layer 12 may be subjected to treatments that improve visual recognition when viewed through polarized sunglasses (typically, imparting (ellipsoidal) polarization or ultra-high phase difference). By implementing such treatments, excellent visual recognition can be achieved even when the displayed image is viewed through polarized lenses such as polarized sunglasses. Therefore, the optical laminate can also be suitably applied to image display devices that can be used outdoors.
[0058] The thickness of the first protective layer is preferably 15 μm to 60 μm, more preferably 25 μm to 45 μm.
[0059] In one embodiment, the second protective layer 13 is preferably optically isotropic. As used herein, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the thickness-direction retardation Rth(550) is -10 nm to +10 nm. It should be noted that, as described above, the second protective layer 13 may be omitted.
[0060] D. First Retardation Layer D-1. Properties of the First Retardation Layer As described above, the in-plane retardation Re(550) of the first retardation layer 21 is 100 nm to 200 nm, preferably 110 nm to 180 nm, more preferably 120 nm to 160 nm, and still more preferably 130 nm to 150 nm. That is, the first retardation layer can function as a so-called λ / 4 plate.
[0061] As described above, the first retardation layer satisfies the relationship of Re(450) < Re(550), and preferably further satisfies the relationship of Re(550) < Re(650). That is, the first retardation layer exhibits reverse dispersion wavelength dependence in which the retardation value increases in accordance with the wavelength of the measurement light. The Re(450) / Re(550) of the first retardation layer is, for example, more than 0.5 and less than 1.0, preferably 0.7 to 0.95, more preferably 0.75 to 0.92, and still more preferably 0.8 to 0.9. Re(650) / Re(550) is preferably 1.0 or more and less than 1.15, and more preferably 1.03 to 1.1.
[0062] Since the first retardation layer has the in-plane retardation as described above, it has a relationship of nx > ny. As long as the first retardation layer satisfies the relationship of nx > ny, it exhibits any appropriate refractive index characteristics. The refractive index characteristics of the first retardation layer typically exhibit a relationship of nx > ny ≥ nz. It should be noted that "ny = nz" herein includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny < nz may be satisfied in some cases. The Nz coefficient of the first retardation layer is preferably 0.9 to 2.0, more preferably 0.9 to 1.5, and still more preferably 0.9 to 1.2. By satisfying such a relationship, extremely excellent reflected hue can be achieved when the optical laminate is used in an image display apparatus.
[0063] The thickness of the first retardation layer can be set in such a manner that it functions most suitably as a λ / 4 plate. In other words, the thickness can be set in such a manner that a desired in-plane retardation can be obtained. Specifically, the thickness is preferably 15 μm to 70 μm, more preferably 20 μm to 60 μm, and most preferably 20 μm to 50 μm.
[0064] The shrinkage rate of the first retardation layer in the slow axis direction during heating at 80°C to 125°C for 180 minutes is, for example, 4% or less, preferably 3.5% or less, and more preferably 3% or less. A lower shrinkage rate is more preferred, and the lower limit can be, for example, 0.5%. If the shrinkage rate of the first retardation layer is within such a range, cracking under harsh high-temperature and high-humidity environments can be suppressed more effectively.
[0065] The elongation at break of the stretched film constituting the first retardation layer is preferably 200% or more, more preferably 210% or more, even more preferably 220% or more, and particularly preferably 245% or more. The upper limit of the elongation at break can be, for example, 500%. If the elongation at break of the stretched film constituting the first retardation layer is within such a range, then, through the synergistic effect with the effect brought about by the aforementioned shrinkage rate, cracking under harsh high-temperature and high-humidity environments can be suppressed more effectively. It should be noted that, in this specification, "elongation at break" refers to the elongation at which the film breaks during uniaxial stretching at a fixed end at a specified stretching temperature (e.g., Tg-2°C).
[0066] The absolute value of the photoelastic coefficient of the first phase difference layer is preferably 20 × 10⁻⁶. -12 (m) 2 ( / N) or less, more preferably 1.0×10 -12 (m) 2 / N)~15×10 -12 (m) 2 / N), further preferably 2.0×10 -12 (m) 2 / N)~12×10 -12 (m) 2 / N). If the absolute value of the photoelastic coefficient is within such a range, then display unevenness can be suppressed when optical laminates are applied to image display devices.
[0067] D-2. Constituent materials of the first phase difference layer The first retardation layer typically contains a resin comprising at least one bonding group selected from the group consisting of carbonate bonds and ester bonds. In other words, the first retardation layer contains a polycarbonate resin, a polyester resin, or a polyester-carbonate resin (hereinafter, sometimes collectively referred to as polycarbonate resin).
[0068] In one embodiment, the polycarbonate resin comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic diethanols, diethylene glycol, triethylene glycol, or polyethylene glycol, and alkylene glycols or spirodiols. Preferably, the polycarbonate resin comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from alicyclic diethanols and / or structural units derived from diethylene glycol, triethylene glycol, or polyethylene glycol; more preferably, it comprises structural units derived from fluorene-based dihydroxy compounds, structural units derived from isosorbide-based dihydroxy compounds, and structural units derived from diethylene glycol, triethylene glycol, or polyethylene glycol. The polycarbonate resin may also, as needed, comprise structural units derived from other dihydroxy compounds. It should be noted that details of the polycarbonate resins suitable for use in this invention are described, for example, in Japanese Patent Application Publication Nos. 2014-10291, 2014-26266, 2015-212816, 2015-212817, and 2015-212818, which are incorporated herein by reference.
[0069] In one embodiment, the polycarbonate resin comprises at least one structural unit selected from the group consisting of structural units represented by general formula (1) and / or structural units represented by general formula (2). These structural units are structural units derived from divalent oligofluorene, hereinafter sometimes referred to as oligofluorene structural units. Such a polycarbonate resin has positive refractive index anisotropy.
[0070] Such polycarbonate resins can also be suitably used in the first protective layer described above. As mentioned above, the first retardation layer typically exhibits an anti-dispersion wavelength dependence, while the first protective layer typically exhibits a flat wavelength dispersion dependence. The wavelength dispersion dependence can be controlled by adjusting the type, number, combination, copolymerization ratio, etc., of the structural units.
[0071] In one embodiment, the first retardation layer may further contain an acrylic resin. The content of the acrylic resin is typically 0.5% to 1.5% by mass. It should be noted that in this specification, the percentage or parts in the unit "mass" has the same meaning as the percentage or parts in the unit "weight".
[0072] D-2-1. Polycarbonate resin <Oligofurene structural unit> The oligomeric fluorene structural unit is represented by the above general formula (1) or (2). In general formulas (1) and (2), R 1 ~R3 Each is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, R 4 ~R 9 Each of the following is independently a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 4 to 10 carbon atoms, a substituted or unsubstituted acyl group having 1 to 10 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, a substituted or unsubstituted aryloxy group having 1 to 10 carbon atoms, a substituted or unsubstituted amino group, a substituted or unsubstituted vinyl group having 1 to 10 carbon atoms, a substituted or unsubstituted ethynyl group having 1 to 10 carbon atoms, a sulfur atom having a substituent, a silicon atom having a substituent, a halogen atom, a nitro group, or a cyano group. Wherein, R 4 ~R 9 They can be the same or different. R 4 ~R 9 At least two adjacent groups can also bond to each other to form a ring.
[0073] The content of oligofluorene structural units in polycarbonate resins relative to the total resin content is preferably 1% to 40% by mass, more preferably 10% to 35% by mass, even more preferably 15% to 30% by mass, and particularly preferably 18% to 25% by mass. Excessive content of oligofluorene structural units may lead to the following problems: the photoelasticity coefficient becomes too large, reliability becomes insufficient, and phase difference performance becomes insufficient. Furthermore, since the proportion of oligofluorene structural units in the resin becomes high, the range of molecular design narrows, sometimes making it difficult to improve the resin when modification is required. On the other hand, even if the desired inverse dispersion wavelength dependence is obtained with a very small amount of oligofluorene structural units, in this case, the optical properties change sensitively depending on the slight inhomogeneity of the oligofluorene structural unit content, making it sometimes difficult to manufacture in a way that includes these properties within a certain range.
[0074] Details of the oligomeric fluorene structural unit are described, for example, in International Publication No. 2015 / 159928. This publication is incorporated herein by reference.
[0075] <Other structural units> Polycarbonate resins, in particular, may contain other structural units besides oligofluorene structural units. In one embodiment, the other structural units are preferably derived from dihydroxy compounds or diester compounds. To exhibit the desired reverse dispersion wavelength characteristics, it is necessary to incorporate structural units with positive intrinsic birefringence together with oligofluorene structural units with negative intrinsic birefringence into the polymer structure. Therefore, as other monomers for copolymerization, dihydroxy compounds or diester compounds that are the raw materials for structural units with positive birefringence are further preferred.
[0076] As comonomers, examples include compounds that can incorporate structural units containing aromatic rings and compounds that do not incorporate structural units containing aromatic rings, i.e., compounds composed of aliphatic structures.
[0077] The following are specific examples of compounds composed of the above-mentioned aliphatic structures. Dihydroxy compounds of straight-chain aliphatic hydrocarbons such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; dihydroxy compounds of branched-chain aliphatic hydrocarbons such as neopentyl glycol and hexanediol; dihydroxy compounds of secondary and tertiary alcohols of alicyclic hydrocarbons, exemplified in 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol; and dihydroxy compounds of 1,2-cyclohexanediethanol, 1,3-cyclohexanediethanol, 1,4-cyclohexanediethanol, tricyclodecanediethanol, and pentacyclopentadecanedimethanol. Dihydroxy compounds that are primary alcohols of alicyclic hydrocarbons, such as 2,6-naphthyldiethanol, 1,5-naphthyldiethanol, 2,3-naphthyldiethanol, 2,3-norbornanediethanol, 2,5-norbornanediethanol, 1,3-adamantanediethanol, and limonene; oxoalkylene glycols such as diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, and polypropylene glycol; dihydroxy compounds with cyclic ether structures such as isosorbide; dihydroxy compounds with cyclic acetal structures such as spirodiol and dioxanediol; alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; and aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, octanoic acid, azelaic acid, and sebacic acid.
[0078] The following are specific examples of compounds that can incorporate structural units containing the aforementioned aromatic rings: 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethyl... Alkane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)decane, bis(4-hydroxy-3-nitrophenyl)methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2- Aromatic bisphenol compounds such as propylbenzene, 2,2-bis(4-hydroxyphenyl)hexafluoropropane, 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl)sulfide, bis(4-hydroxyphenyl)disulfide, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether; 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 2,2-bis(4-(2-) Dihydroxy compounds containing an ether group bonded to an aromatic group, such as hydroxypropoxyphenylpropane, 1,3-bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)biphenyl, and bis(4-(2-hydroxyethoxy)phenyl)sulfone; aromatic dicarboxylic acids such as terephthalic acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenylether dicarboxylic acid, 4,4'-benzophenone dicarboxylic acid, 4,4'-diphenoxyethane dicarboxylic acid, 4,4'-diphenylsulfone dicarboxylic acid, and 2,6-naphthalene dicarboxylic acid.
[0079] It should be noted that the aliphatic and aromatic dicarboxylic acids listed above can use the dicarboxylic acid itself as a raw material for the above-mentioned polyester carbonate, but depending on the manufacturing method, dicarboxylic acid derivatives such as methyl esters, phenyl esters, and dicarboxylic acid halides can also be used as raw materials.
[0080] As comonomers, dihydroxy compounds with fluorene rings, such as 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, as well as dicarboxylic acid compounds with fluorene rings, which are known in the past as compounds containing structural units with negative birefringence, can also be used in combination with oligomeric fluorene compounds.
[0081] In the structural unit that can be introduced by a compound having the above-described alicyclic structure, the resin used in the embodiments of the present invention preferably contains the structural unit represented by the following formula (3) as a copolymer component.
[0082] [Chemical Formula 4] Spirodiol can be used as a dihydroxy compound that can incorporate the structural unit of the above formula (3).
[0083] In the resin used in embodiments of the present invention, the structural unit represented by the above formula (3) preferably contains 5% by mass or more and 90% by mass or less. The upper limit is further preferably 70% by mass or less, and particularly preferably 50% by mass or less. The lower limit is further preferably 10% by mass or more, more preferably 20% by mass or more, and particularly preferably 25% by mass or more. If the content of the structural unit represented by the above formula (3) is above the above lower limit, sufficient mechanical properties, heat resistance, and a low photoelastic coefficient can be obtained. Furthermore, the compatibility with acrylic resins is improved, and the transparency of the obtained resin composition can be further improved. In addition, since the polymerization rate of spirodiol is relatively slow, the polymerization reaction becomes easier to control by suppressing its content to below the above upper limit.
[0084] The resin used in this invention preferably further contains the structural unit represented by the following formula (4) as a copolymer component.
[0085] [Chemical Formula 5] As dihydroxy compounds capable of incorporating the structural unit represented by formula (4) above, examples include isosorbide (ISB), isomannitol, and isoidolitol, which are stereoisomers. They can be used individually or in combination of two or more.
[0086] In the resin used in embodiments of the present invention, the structural unit represented by formula (4) above preferably contains 5% by mass or more and 90% by mass or less. The upper limit is further preferably 70% by mass or less, and particularly preferably 50% by mass or less. The lower limit is further preferably 10% by mass or more, and particularly preferably 15% by mass or more. If the content of the structural unit represented by formula (4) above is above the lower limit, sufficient mechanical properties, heat resistance, and a low photoelasticity coefficient can be obtained. Furthermore, since the structural unit represented by formula (4) above has the characteristic of high water absorption, if the content of the structural unit represented by formula (4) above is below the upper limit, the dimensional changes of the molded article caused by water absorption can be suppressed to an acceptable range.
[0087] The resin used in embodiments of the present invention may further comprise other structural units. It should be noted that these structural units are sometimes referred to as "other structural units." As monomers having other structural units, 1,4-cyclohexanediethanol, tricyclodecanediethanol, and 1,4-cyclohexanedicarboxylic acid (and their derivatives) are more preferably used, with 1,4-cyclohexanediethanol and tricyclodecanediethanol being particularly preferred. Resins comprising structural units derived from these monomers exhibit an excellent balance of optical properties, heat resistance, mechanical properties, etc. Furthermore, since diester compounds have relatively low polymerization reactivity, from the viewpoint of improving reaction efficiency, it is preferable not to use diester compounds other than those containing oligomeric fluorene structural units.
[0088] In embodiments of the present invention, the glass transition temperature (Tg) of the resin used is preferably 110°C or higher and 160°C or lower. The upper limit is further preferably 155°C or lower, more preferably 150°C or lower, and particularly preferably 145°C or lower. The lower limit is further preferably 120°C or higher, and particularly preferably 130°C or higher. If the glass transition temperature is outside the above range, there is a tendency for the heat resistance to deteriorate, which may cause dimensional changes after film formation or deterioration in the reliability of the quality under the conditions of use of the first phase difference layer. On the other hand, if the glass transition temperature is too high, uneven film thickness may sometimes occur during film formation, or the film may become brittle and its tensile strength may deteriorate. Furthermore, the transparency of the film may sometimes be impaired.
[0089] D-2-2. Acrylic resin As an acrylic resin, an acrylic resin that is a thermoplastic resin is used. Examples of monomers that form the structural units of an acrylic resin include: methyl methacrylate, methacrylic acid, methyl acrylate, acrylic acid, benzyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, tridecyl methacrylate, stearyl methacrylate, glycidyl methacrylate, hydroxypropyl methacrylate, 2-methoxyethyl methacrylate, 2-ethoxyethyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, norbornyl methacrylate, dicyclopentenyl methacrylate, dicyclopentyl methacrylate, etc. Dicyclopentenoxyethyl acrylate, tetrahydrofurfuryl acrylate, methacrylate, 2-hydroxyethyl methacrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl maleate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, pentamethylpiperidinyl methacrylate, tetramethylpiperidinyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, cyclopentyl methacrylate, cyclopentyl acrylate, cyclohexyl methacrylate, cyclohexyl acrylate, cycloheptyl methacrylate, cycloheptyl acrylate, cyclooctyl methacrylate, cyclooctyl acrylate, cyclododecyl methacrylate, cyclododecyl acrylate. These can be used alone or in combination of two or more monomers. Examples of combinations of two or more monomers include copolymers of two or more monomers, blends of two or more homopolymers of one monomer, and combinations thereof. Furthermore, other monomers (such as olefin monomers and vinyl monomers) that can copolymerize with these acrylic monomers can also be used.
[0090] The acrylic resin contains structural units derived from methyl methacrylate. The content of the methyl methacrylate-derived structural units in the acrylic resin is preferably 70% by mass or more and 100% by mass or less. A lower limit is more preferably 80% by mass or more, further preferably 90% by mass or more, and particularly preferably 95% by mass or more. Within this range, excellent compatibility with the polycarbonate resin of the present invention can be obtained. As structural units other than methyl methacrylate, methyl acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, and styrene are preferably used. Copolymerizing methyl acrylate can improve thermal stability. By using phenyl (meth)acrylate, benzyl (meth)acrylate, and styrene, the refractive index of the acrylic resin can be adjusted; therefore, by incorporating the refractive index of the combined resin, the transparency of the resulting resin composition can be improved. By using such an acrylic resin, a reverse dispersion phase difference film with excellent tensile strength and phase difference performance and low haze can be obtained.
[0091] The weight-average molecular weight (Mw) of the acrylic resin is 10,000 or more and 200,000 or less. The lower limit is preferably 30,000 or more, particularly preferably 50,000 or more. The upper limit is preferably 180,000 or less, particularly preferably 150,000 or less. If the molecular weight is within this range, compatibility with polycarbonate resins can be obtained, thereby improving the transparency of the final retardation film (retardation layer) and significantly improving the stretchability during stretching. It should be noted that the above-mentioned weight-average molecular weight is the molecular weight converted from polystyrene as determined by GPC. Furthermore, from a compatibility point of view, it is preferable that the acrylic resin does not substantially contain branched structures. The absence of branched structures can be confirmed by the unimodality of the GPC curve of the acrylic resin, etc.
[0092] D-2-3. Blend of polycarbonate resins and acrylic resins In the case of using polycarbonate-based resin and acrylic-based resin together, the polycarbonate-based resin and acrylic-based resin are blended and supplied as a resin composition to a phase retardation film (first phase retardation layer) in a manufacturing method (the manufacturing method is described later in item D-3). The polycarbonate-based resin and acrylic-based resin are preferably blended in a molten state. A representative example of a method for blending in a molten state is melt mixing using an extruder. The mixing temperature (molten resin temperature) is preferably 200°C to 280°C, more preferably 220°C to 270°C, and even more preferably 230°C to 260°C. If the mixing temperature is within this range, thermal decomposition can be suppressed, and granules of a resin composition in which the two resins are uniformly blended can be obtained. If the molten resin temperature in the extruder exceeds 280°C, resin discoloration and / or thermal decomposition may sometimes occur. On the other hand, if the molten resin temperature in the extruder is below 200°C, the resin viscosity may sometimes become too high, causing excessive load on the extruder, or the resin melting may become insufficient. It should be noted that any suitable configuration can be used for the extruder, screw, etc. To obtain the transparency of the resin suitable for optical film applications, a twin-screw extruder is preferred. Furthermore, since residual low-molecular-weight components in the resin and low-molecular-weight thermally decomposed components from extrusion compounding may contaminate the cooling rollers or conveyor rollers during the film-forming and stretching processes, an extruder equipped with vacuum vents is preferred for removal.
[0093] The content of acrylic resin in the resin composition (resulting in the first retardation layer) is, as described above, 0.5% by mass or more and 2.0% by mass or less. The lower limit is more preferably 0.6% by mass or more. The upper limit is preferably 1.5% by mass or less, more preferably 1.0% by weight or less, further preferably 0.9% by weight or less, and particularly preferably 0.8% by mass or less. In this way, by incorporating acrylic resin into the polycarbonate resin at a very specific ratio, the stretchability and retardation performance can be significantly increased. Furthermore, haze can be suppressed. Such an effect was not theoretically clear; it is an unexpectedly excellent effect obtained through repeated experiments. It should be noted that if the content of acrylic resin is too low, the above-mentioned effect may not be obtained. On the other hand, if the content of acrylic resin is too high, haze may increase. In addition, there are many cases where the stretchability and retardation performance become insufficient or even decrease compared to the conditions within the above ranges.
[0094] For the purpose of modifying properties such as mechanical properties and / or solvent resistance, the resin composition may also be further blended with synthetic resins such as aromatic polycarbonate, aliphatic polycarbonate, aromatic polyester, aliphatic polyester, polyamide, polystyrene, polyolefin, acrylic acid, amorphous polyolefin, ABS, AS, polylactic acid, polybutylene succinate, rubber, and combinations thereof.
[0095] The resin composition may further include additives. Specific examples of additives include heat stabilizers, antioxidants, catalyst deactivators, ultraviolet absorbers, light stabilizers, release agents, pigments, impact modifiers, antistatic agents, lubricants, plasticizers, compatibilizers, nucleating agents, flame retardants, inorganic fillers, and foaming agents. The type, number, combination, and content of additives in the resin composition can be appropriately determined according to the purpose.
[0096] D-3. Method for forming the first phase difference layer The first phase difference layer is obtained by forming a film from the polycarbonate-based resin (or a resin composition in the case of an acrylic resin) described in item D-2-1 above, and then stretching the film. Any suitable forming process can be used as the method for forming the film. The stretching conditions (e.g., stretch ratio, stretching temperature, stretching method, stretching direction) can be appropriately set according to the purpose and the desired in-plane phase difference.
[0097] E. Second phase difference layer The second phase retardation layer, as described above, can be a so-called positive C-plate exhibiting a refractive index characteristic of nz > nx = ny. By using a positive C-plate as the second phase retardation layer, reflections in the tilt direction can be effectively prevented, making wide-viewing-angle anti-reflection functionality possible. In this case, the phase difference Rth (550) in the thickness direction of the second phase retardation layer is preferably -50 nm to -300 nm, more preferably -70 nm to -250 nm, even more preferably -90 nm to -200 nm, and particularly preferably -100 nm to -180 nm. Here, "nx = ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. That is, the in-plane phase difference Re (550) of the second phase retardation layer can be less than 10 nm.
[0098] The second retardation layer, having a refractive index characteristic of nz>nx=ny, can be formed from any suitable material. The second retardation layer preferably comprises a film containing a liquid crystal material fixed along a vertical orientation. The vertically oriented liquid crystal material (liquid crystal compound) can be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method for forming the retardation layer are the liquid crystal compound and the method for forming the retardation layer described in Japanese Patent Application Publication Nos. 2002-333642,
[0020] to
[0028] . In this case, the thickness of the second retardation layer is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.
[0099] F. Reinforcement Layer As described above, the reinforcing layer 30 is a cured layer of the active energy ray-curable resin composition. The reinforcing layer 30 can have any suitable configuration as long as it has an indentation modulus of elasticity equal to or greater than that of the first phase difference layer. Specifically, the reinforcing layer 30 can be a hard coating layer or an adhesive layer.
[0100] F-1. Hard coating According to an embodiment of the present invention, a hard coating layer, typically provided as the outermost layer for surface protection, is provided on the side of the first retardation layer opposite to the polarizer (image display panel side, i.e., inner side). The hard coating layer is hard, which inhibits the penetration of the curing component (monomer component) of the resin composition used to form the hard coating layer into the first retardation layer. As a result, compared to the case where the adhesive layer (adhesive) used for laminating the second retardation layer is adjacent to the first retardation layer, the thickness of the intermediate layer (fragmented layer) that can be formed can be reduced, and cracking of the first retardation layer can be suppressed. Furthermore, regardless of the adhesive used as the adhesive layer (adhesive) for laminating the second retardation layer, the hard coating layer inhibits (essentially blocks) the penetration of the monomer component of the adhesive into the first retardation layer, thus significantly expanding the options for adhesive layers.
[0101] The hard coating can have any suitable composition as long as it has an indentation modulus of elasticity greater than or equal to that of the first phase difference layer. The hard coating (essentially a resin composition for forming a hard coating) typically includes a curing component and a photopolymerization initiator. Examples of curing components include active energy ray-curable resins. Examples of active energy rays include ultraviolet light, visible light, and electron beams. Ultraviolet-curable resins are preferred because they allow for efficient hard coating formation with simple processing operations. Specific examples of ultraviolet-curable resins include polyester-based, (meth)acrylate-based, urethane-based, amide-based, silicone-based, epoxy-based, and unsaturated polyester-based ultraviolet-curable resins. (Meth)acrylate-based ultraviolet-curable resins include urethane (meth)acrylates, polyester (meth)acrylates, and epoxy (meth)acrylates. Ultraviolet-curable urethane (meth)acrylates are preferred. Ultraviolet-curable urethane (meth)acrylates include ultraviolet-curable monomers, oligomers, polymers, etc. It should be noted that in this specification, "(meth)acrylic acid" refers to acrylic acid and / or methacrylic acid. Furthermore, (meth)acrylic acid is sometimes simply referred to as acrylic acid.
[0102] The hard coating preferably has a pencil hardness of H or higher, more preferably 2H or higher, and even more preferably 3H or higher. On the other hand, the pencil hardness of the hard coating is preferably 6H or lower, more preferably 5H or lower. If the pencil hardness of the hard coating is within such a range, the desired indentation modulus of elasticity described above can be easily achieved. The pencil hardness can be determined based on the "Pencil Hardness Test" of JIS K 5400.
[0103] The thickness of the hard coating is preferably 5 μm or less, more preferably 0.5 μm to 4 μm, and even more preferably 1 μm to 3.5 μm. If the thickness of the hard coating is within such a range, the penetration of the monomer components of the adhesive used to laminate the second retardation layer into the first retardation layer can be blocked.
[0104] The hard coating can typically be formed directly on the first retardation layer. Specifically, the hard coating can be formed by applying a hard coating forming resin composition to the surface of the first retardation layer and allowing it to dry, then curing the dried coating film by irradiating it with ultraviolet light.
[0105] F-2. Adhesive layer According to an embodiment of the present invention, by constructing the adhesive layer with an active energy radiation-curable adhesive that is significantly harder than conventionally used active energy radiation-curable adhesives and has the desired indentation modulus, the penetration of the monomeric components of the adhesive into the first retardation layer can be suppressed. As a result, the thickness of the intermediate layer (fragile layer) that can be formed can be significantly reduced compared to the case of using conventional active energy radiation-curable adhesives, and cracking of the first retardation layer can be suppressed.
[0106] Examples of active energy ray-cured adhesives that constitute the adhesive layer include, for example, ultraviolet-cured adhesives and electron beam-cured adhesives. Furthermore, from the viewpoint of curing mechanism, examples of active energy ray-cured adhesives include, for example, free radical-curing, cationic-curing, anionic-curing, and mixtures of free radical-curing and cationic-curing types.
[0107] The adhesive and hard coating forming resin composition typically includes a film-forming component (adhesive), a curing component, and a photopolymerization initiator. As a film-forming component, a monofunctional monomer can be representatively listed. Specific examples of film-forming components include butyl acrylate and 4-hydroxybutyl acrylate. As a curing component, representative examples include monomers and / or oligomers with two or more functional groups, such as (meth)acrylate groups and (meth)acrylamide groups. Specific examples of curing components include tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, tricyclodecanediethanol diacrylate, phenoxydiethylene glycol acrylate, neopentyl glycol diacrylate, neopentyl glycol triacrylate, cyclic trimethylolpropane methyl acetal acrylate, dioxanediol diacrylate, EO-modified isocyanuric acid diacrylate, EO-modified isocyanuric acid triacrylate, trimethylolpropane triacrylate, glyceryl triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and EO-modified diglycerol. The curing components include: tetraacrylate, γ-butyrolactone acrylate, polyethylene glycol diacrylate, neopentyl glycol acrylate adduct of hydroxypentanoic acid, acryloylmorpholine, ε-caprolactone modified with unsaturated fatty acid hydroxyalkyl ester, N-methylpyrrolidone, diethylacrylamide, hydroxyethylacrylamide, N-hydroxymethylacrylamide, N-methoxymethylacrylamide, N-ethoxymethylacrylamide, 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexene carboxylic acid ester, neopentyl glycol glycidyl ether, dicyclopentadiene-type epoxy resin, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. The curing components can be used alone or in combination of two or more.
[0108] The adhesive may further contain oligomer components. By using oligomer components, the viscosity of the adhesive before curing can be reduced, improving workability. Representative examples of oligomer components include (meth)acrylic acid oligomers and polyurethane-based (meth)acrylic acid oligomers. The weight-average molecular weight of the oligomer component is preferably 5,000 or more, more preferably 10,000 to 15,000.
[0109] Adhesives may contain coupling agents, boric acid, or a combination of coupling agents and boric acid.
[0110] The preferred combination of adhesives comprises monofunctional (meth)acrylates (monofunctional monomers), polyfunctional (e.g., difunctional or trifunctional) (meth)acrylates (polyfunctional monomers), oligomers, boric acid, and coupling agents. Monofunctional (meth)acrylates can be, for example, 4-hydroxybutyl acrylate. Polyfunctional (meth)acrylates can be, for example, neopentyl glycol diacrylate and triacrylate, isocyanuric acid EO-modified diacrylate and triacrylate, and pentaerythritol triacrylate. Polyfunctional (meth)acrylates can be used alone or in combination.
[0111] The thickness of the adhesive layer can be, for example, 0.5 μm to 5 μm, or, for example, 1 μm to 3.5 μm.
[0112] G. Barrier Layer The barrier layer 40 is typically a solidified or cured coating of an organic solvent solution of resin. With this configuration, the barrier layer exhibits excellent adhesion to the polarizer when disposed adjacent to it. Specifically, the barrier layer can be formed directly on the polarizer without the aid of an adhesive layer. Furthermore, this configuration allows for a very thin barrier layer. The thickness of the barrier layer is, for example, 10 μm or less, preferably 5 μm or less, more preferably 1 μm or less, and even more preferably 0.7 μm or less. The thickness of the barrier layer is preferably 0.05 μm or more, more preferably 0.08 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more.
[0113] The barrier layer 40, as its name suggests, has a barrier function. Relatedly, the barrier layer is typically hard. Specifically, the indentation modulus of the barrier layer is preferably 8 GPa or higher, more preferably 10 GPa to 20 GPa, and even more preferably 11 GPa to 15 GPa. Although the barrier layer is so hard that it is prone to cracking, by providing the barrier layer, cracks in the polarizer and the first phase difference layer can be suppressed.
[0114] Typically, the resin constituting the barrier layer has a glass transition temperature (Tg) of 85°C or higher and a weight-average molecular weight (Mw) of 25,000 or higher. The Tg of the resin constituting the barrier layer is preferably 90°C or higher, more preferably 100°C or higher, even more preferably 110°C or higher, and particularly preferably 120°C or higher. For example, the Tg can be 200°C or lower. Furthermore, the Mw of the resin constituting the barrier layer is preferably 30,000 or higher, more preferably 35,000 or higher, and even more preferably 40,000 or higher. By having the Tg and Mw of the resin constituting the barrier layer within such ranges, excellent barrier function can be achieved even with a very thin thickness.
[0115] As the resin constituting the barrier layer, any suitable resin that is a solidified or cured material (e.g., a thermosetting material) capable of forming an organic solvent solution coating film can be used. Preferably, a thermoplastic resin or thermosetting resin having the Tg and Mw as described above is used as the resin constituting the barrier layer; more preferably, a thermoplastic resin is used. Only one type of resin can be used, or two or more types can be used in combination.
[0116] Examples of the aforementioned thermoplastic resins include acrylic resins and epoxy resins. Acrylic resins and epoxy resins can also be used in combination.
[0117] Acrylic resins typically contain repeating units derived from linear or branched (meth)acrylate monomers as their main components. Acrylic resins may contain repeating units derived from any suitable comonomer appropriate to the purpose. Examples of comonomers include carboxyl-containing monomers, hydroxyl-containing monomers, amide-containing monomers, (meth)acrylates containing aromatic rings, and vinyl monomers containing heterocyclic rings. By appropriately setting the type, number, combination, and copolymerization ratio of monomer units, acrylic resins with the aforementioned specified Mw can be obtained. Specific examples of acrylic resins include boron-containing acrylic resins and acrylic resins containing lactone rings, as described in Japanese Patent Application Publication Nos. 2021-117484
[0034] to
[0056] .
[0118] As the epoxy resin, an epoxy resin having aromatic rings is preferred. Using an epoxy resin having aromatic rings improves the adhesion between the barrier layer and the polarizer. Furthermore, when an adhesive layer is disposed adjacent to the barrier layer, the anchoring force of the adhesive layer can be improved. Examples of epoxy resins having aromatic rings include bisphenol-type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; phenolic varnish-type epoxy resins such as phenolic varnish epoxy resin, cresol phenolic varnish epoxy resin, and hydroxybenzaldehyde phenolic varnish epoxy resin; multifunctional epoxy resins such as glycidyl ether of tetrahydroxyphenylmethane, glycidyl ether of tetrahydroxybenzophenone, and epoxidized polyvinylphenol; naphthol-type epoxy resins; naphthyl-type epoxy resins; and biphenyl-type epoxy resins. Bisphenol A type epoxy resin, biphenyl-type epoxy resin, and bisphenol F type epoxy resin are preferred. Epoxy resin can be used in combination with only one type or two or more types.
[0119] The barrier layer can be typically formed by coating an organic solvent solution of the aforementioned resin to form a coating film, and then solidifying or thermally curing the resulting coating film. As the organic solvent, any suitable organic solvent capable of dissolving or uniformly dispersing the aforementioned resin can be used. Specific examples of organic solvents include ethyl acetate, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclopentanone, and cyclohexanone. The resin concentration of the solution relative to 100 parts by weight of the solvent is preferably 3 to 20 parts by weight. With such a resin concentration, a uniform coating film can be formed.
[0120] H. Image display device The optical laminates described in items A through G above can be applied to image display devices. Therefore, embodiments of the present invention also include image display devices using such optical laminates. Representative examples of image display devices include liquid crystal display devices and organic EL display devices. The image display devices of embodiments of the present invention typically possess the optical laminates described in items A through G above on their visual recognition side.
[0121] Example The present invention will now be specifically described through embodiments, but the present invention is not limited to these embodiments. The evaluation methods in the embodiments are as follows. It should be noted that, unless otherwise specified, "parts" and "%" in the embodiments are based on weight.
[0122] (1) Indentation modulus of the cross section The optical laminates obtained in the examples and comparative examples were cut using a cryo-microtome to expose the cross-section. AFM focus mapping was performed on the exposed cross-section to measure the indentation modulus of the cross-section in the thickness direction for the first retardation layer, the reinforcing layer, and the adhesive layer. The indentation modulus of the cross-section was taken as the value just before it began to change near the interface between the first retardation layer and the reinforcing layer, the reinforcing layer and the adhesive layer, or the interface between the first retardation layer and the adhesive layer. It should be noted that the measurement conditions are as follows. Furthermore, the thickness of the intermediate layer was also derived through this measurement.
[0123] Device: Oxford Instruments, Asylum Research Jupiter XR Measurement mode: AFM focal mapping Cantilever: AC240TS (Si-made, spring constant 3N / m equivalent) Measurement range: 3.5μm tetragonal scanning (512×256 points) Scan speed: 200Hz Atmosphere being measured: Measurement temperature: room temperature (2) Cracks The optical laminates obtained in the examples and comparative examples were subjected to an accelerated HAST test to assess their durability under high temperature and high humidity conditions. The HAST test was conducted according to JIS C60068. Specifically, the optical laminates were heated and humidified by placing them in an oven controlled at 110°C and 85%RH for 36 hours. The state of the heated and humidified optical laminates was observed visually, and the number of cracks generated in the first retardation layer was investigated.
[0124] [Manufacturing Example 1: Preparation of a Hard Coating Resin Composition for Reinforcing Layer Formation] A hard coating resin composition for forming a reinforcing layer was prepared by diluting 80 parts of polyether urethane diacrylate (manufactured by Mitsubishi Chemical Co., Ltd., product name "UT-7314"), 20 parts of urethane acrylate (manufactured by DIC Co., Ltd., product name "ELS-888"), 0.1 parts of leveling agent (manufactured by Kyoeisha Chemical Co., Ltd., product name "LE-303"), and 3 parts of photopolymerization initiator (manufactured by IGM Resins Co., Ltd., product name "Omnirad 907") with methyl isobutyl ketone.
[0125] [Manufacturing Example 2: Preparation of UV-curable adhesive for forming a reinforcing layer] The following mixture was prepared: 35 parts of 4-hydroxybutyl acrylate, 24 parts of neopentyl glycol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "LIGHT ACRYLATE NP-A"), 10 parts of isocyanuric acid EO-modified triacrylate (manufactured by Toa Synthetic Co., Ltd., product name "ARONIX M-315"), 5 parts of pentaerythritol triacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "A-TMM-3LM-N"), 14 parts of polyurethane-based (meth)acrylic acid oligomer (manufactured by Mitsubishi Chemical Co., Ltd., product name "UV3000B"), 1 part of boric acid, 5 parts of epoxy-containing silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBM-303"), and a photopolymerization initiator (manufactured by IGM Resins Co., Ltd., product name "Omnirad"). A UV-curable adhesive for forming a reinforcing layer was prepared by combining 3 parts of 184”, 1 part of photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S"), and 2 parts of photoacid generator (manufactured by San-Apro Co., Ltd., product name "CPI-100P").
[0126] [Manufacturing Example 3: Preparation of UV-curable adhesive] A UV-curable adhesive was prepared by combining 20 parts of acryloylmorpholine (trade name "ACMO", manufactured by KJ CHEMICALS), 50 parts of PLACEL FA1DDM (manufactured by Daicel), 10 parts of polyethylene glycol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "LIGHT ACRYLATE9EG-A"), 15 parts of acrylic oligomer (manufactured by Toa Synthetic Co., Ltd., product name "ARFON UP-1190"), 3 parts of photopolymerization initiator (manufactured by IGM Resins, product name "Omnirad 907"), and 2 parts of photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S").
[0127] [Manufacturing Example 4: Preparation of UV-curable adhesive] A UV-curable adhesive was prepared by combining 10 parts of hydroxyethyl acrylamide, 55 parts of phenoxy diethylene glycol acrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "LIGHT ACRYLATE P2H-A"), 20 parts of 1,9-nonanediol diacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name "LIGHT ACRYLATE 1.9ND-A"), 10 parts of acrylic oligomer (manufactured by Toa Synthetic Co., Ltd., product name "ARFON UP-1190"), 3 parts of photopolymerization initiator (manufactured by IGM Resins Co., Ltd., product name "Omnirad 907"), and 2 parts of photopolymerization initiator (manufactured by Nippon Kayaku Co., Ltd., product name "KAYACURE-DETX-S").
[0128] [Manufacturing Example 5: Fabrication of the retardation film constituting the first retardation layer] (Polymerization of polyester carbonate resins) Polyester carbonate resin was polymerized using a continuous polymerization apparatus comprising three vertical stirred reactors (vertical stirred reactors 1 to 3), one horizontal stirred reactor (horizontal stirred reactor 4), and a twin-screw extruder. First, isosorbide (ISB) was melted in a melting tank (or melting tank) to prepare solutions of spirodiol (SPG) and phenol (PHL), and bis[9-(2-phenoxycarbonylethyl)fluorene-9-yl]methane (BPFM) and diphenyl carbonate (DPC) were melted. PHL was used as a solvent to dissolve the SPG. The mixtures were then prepared with an SPG to PHL weight ratio of 55.0 / 45.0 and a BPFM to DPC weight ratio of 30.3 / 69.7. The ISB melt, SPG / PHL solution, and BPFM / DPC melt were continuously fed into the first vertical stirred reactor at a flow rate of 49.9 parts by weight / hr, 68.5 parts by weight / hr, and 75.3 parts by weight / hr (molar ratios of ISB / SPG / BPFM / DPC = 0.734 / 0.266 / 0.126 / 0.874). Simultaneously, an aqueous solution of calcium acetate monohydrate, serving as a polymerization catalyst, was added to the first vertical stirred reactor at an addition rate of 12 μmol of calcium acetate monohydrate relative to 1 mol of all dihydroxy compounds. The mixture supplied to the first vertical stirred reactor was then continuously fed into the second, third, and fourth vertical stirred reactors. The internal temperature, internal pressure, and residence time of the mixture in each reactor were set as follows: Vertical stirred reactor 1: 195℃, 27kPa, 90 minutes; Vertical stirred reactor 2: 205℃, 20kPa, 70 minutes; Vertical stirred reactor 3: 220℃, 10kPa, 60 minutes; Horizontal stirred reactor 4: 235℃, 0.1–1.0kPa, 150 minutes. The reactor was operated while fine-tuning the vacuum pressure of the horizontal stirred reactor, aiming to achieve a final resin reduction viscosity of 0.45–0.47 dL / g. The resin extracted from the horizontal stirred reactor was fed into a vented twin-screw extruder [manufactured by Nippon Steel Works]. The extruder has two vacuum vents, where residual low molecular weight components in the resin are devolatilized, and 3.7 ppm of phosphonic acid as a catalyst deactivator is added to the polyester carbonate resin before the first vent. After the second vent, 1000 ppm and 100 ppm of Irganox 1010 and PEP36, respectively, were added as heat stabilizers to the polyester carbonate resin. The polycarbonate resin after extrusion was then passed through a 10 μm mesh Ultipleat candle filter [manufactured by PALL Corporation] while still in a molten state to filter out foreign matter.Next, the molten resin is extruded from the die in a filament form, cooled with water, solidified, and then cut into granules using a rotary cutter. The ratio of structural units derived from each monomer is BPFM / ISB / SPG / DPC = 21.5 / 39.4 / 30.0 / 9.1 (mass%).
[0129] (Fabrication of the phase difference film) The obtained polyester carbonate resin (granules) was vacuum dried at 80°C for 5 hours. A 135μm thick elongated resin film was then produced using a film-forming apparatus equipped with a single-screw extruder (Toshiba Machine Co., Ltd., barrel set temperature: 250°C), a T-die (width 200mm, set temperature: 250°C), a chilled roll (set temperature: 120-130°C), and a winding machine. The obtained elongated resin film was stretched along its width at a stretching temperature of 133°C and a stretching ratio of 2.8 times to obtain a 37μm thick retardation film. The obtained retardation film had a Re(550) of 141nm, a Re(450) / Re(550) ratio of 0.82, and an Nz coefficient of 1.12.
[0130] [Manufacturing Example 6: Fabrication of the Liquid Crystal Alignment Fixing Layer Constituting the Second Phase Retardation Layer] A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (I) (where the numbers 65 and 35 represent the molar percentage of monomer units; for convenience, it is represented as a block polymer with a weight-average molecular weight of 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (BASF: Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (Ciba Specialty Chemicals: Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a PET substrate that had undergone vertical alignment treatment using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was cured by irradiating it with ultraviolet light, thereby forming a second retardation layer (3 μm thick) on the substrate exhibiting a refractive index characteristic of nz > nx = ny.
[0131] [Chemical Formula 6] [Example 7: Fabrication of a Polarizing Film] (Making of a polarizer) As a thermoplastic resin substrate, a strip-shaped amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) with a Tg of about 75 °C is used to perform corona treatment on one side of the resin substrate.
[0132] 13 parts by weight of potassium iodide were added to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2 mol%) and acetyl-modified PVA (manufactured by Japan Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER") in a ratio of 9:1. The resulting substance was dissolved in water to prepare a PVA aqueous solution (coating solution).
[0133] A 13 μm thick PVA-based resin layer was formed by coating the above-mentioned PVA aqueous solution onto the corona-treated surface of the resin substrate and drying it at 60°C, thus creating a laminate.
[0134] The resulting laminate was stretched uniaxially to 2.4 times its original length in an oven at 130°C (air-assisted stretching treatment).
[0135] Next, the laminate was immersed in an insoluble bath (an aqueous solution of boric acid prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C for 30 seconds (insoluble treatment).
[0136] Next, the polarizer is immersed in a staining bath at 30°C (an aqueous solution of iodine and potassium iodide prepared by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) for 60 seconds (staining treatment), adjusting the concentration so that the final polarizer's monomer transmittance (Ts) becomes the desired value.
[0137] Next, immerse the sample in a crosslinking bath at 40°C (an aqueous solution of boric acid prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) for 30 seconds (crosslinking treatment).
[0138] Subsequently, the laminate was immersed in a boric acid aqueous solution (boric acid concentration 4 wt%, potassium iodide concentration 5 wt%) at a liquid temperature of 70°C, while being uniaxially stretched (underwater stretching treatment) along the longitudinal direction (length direction) between rollers with different circumferential speeds, with a total stretching ratio of 5.5 times.
[0139] The laminate was then immersed in a washing bath at 20°C (an aqueous solution of 4 parts by weight of potassium iodide relative to 100 parts by weight of water) for washing treatment.
[0140] Then, while drying in an oven maintained at approximately 90°C, it comes into contact with SUS heated rollers with a surface temperature maintained at approximately 75°C (drying shrinkage treatment).
[0141] By operating in this way, a polarizer with a thickness of about 5 μm is formed on the resin substrate, resulting in a polarizer with a resin substrate / polarizer configuration.
[0142] (The creation of the first protective layer) Relative to 81.98 parts by mass of isosorbide (ISB), 47.19 parts by mass of tricyclodecanediethanol (TCDDM), 175.1 parts by mass of diphenyl carbonate (DPC), and 0.979 parts by mass of a 0.2% by mass aqueous solution of cesium carbonate as a catalyst were added to a reaction vessel. As the first step of the reaction, under a nitrogen atmosphere, the vessel was heated to 150°C, and the reactants were dissolved by stirring as needed (approximately 15 minutes). Next, the pressure was set to atmospheric pressure to 13.3 kPa, and the temperature of the heating tank was raised to 190°C over 1 hour while the generated phenol was extracted from the reaction vessel. After maintaining the entire reaction vessel at 190°C for 15 minutes, as the second step, the pressure inside the reaction vessel was set to 6.67 kPa, and the temperature of the heating tank was raised to 230°C over 15 minutes, during which the generated phenol was extracted from the reaction vessel. As the stirring torque of the mixer gradually increased, the temperature was raised to 250°C over 8 minutes. To further remove the generated phenol, the pressure inside the reaction vessel was brought down to below 0.200 kPa. After reaching the specified stirring torque, the reaction was stopped, and the generated reactants were extruded into water to obtain polycarbonate (PC) resin granules. The birefringence Δnxy of the obtained PC resin was 0.015. After vacuum drying the obtained PC resin at 100°C for 12 hours, a PC resin film with a thickness of 25 μm was produced using a film forming apparatus equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., barrel setting temperature: 250°C), a T-die (width 1700 mm, setting temperature: 250°C), a casting roller (setting temperature: 60°C), and a winding machine. The in-plane phase difference Re(550) of the obtained PC resin film was 1 nm, and Re(450) / Re(550) was 1.00. Finally, a hard coating (2 μm thick) is formed on one surface of the PC resin film.
[0143] (Making of polarizers) On the surface of the polarizer obtained above (the side opposite to the resin substrate), an HC-polycarbonate resin film (HC-PC film) obtained above is bonded as a visual recognition side protective layer using a UV-curable adhesive. At this time, the PC film is bonded so that it becomes the polarizer side. Next, the resin substrate is peeled off, resulting in a polarizer P1 having the structure of an HC-PC film (visual recognition side protective layer) / polarizer.
[0144] [Example 8: Fabrication of a Polarizing Film] Except for using an HC-TAC film instead of an HC-PC film as the visual recognition side protective layer, the polarizer P2 was obtained by operating in the same manner as in Manufacturing Example 7. It should be noted that the HC-TAC film is a film on which an HC layer (7 μm thick) is formed on a triacetyl cellulose (TAC) film (25 μm thick), and the TAC film is laminated in such a way that it becomes the polarizer side.
[0145] [Manufacturing Example 9: Preparation of Coating Liquid for Barrier Layer Formation] 97.0 parts of methyl methacrylate (MMA, manufactured by FUJIFILM Wako Chemicals, trade name "Methyl methacrylate monomer"), 3.0 parts of the comonomer represented by formula (E) below, and 0.2 parts of the polymerization initiator (manufactured by FUJIFILM Wako Chemicals, trade name "2,2´-azobis(isobutyronitrile)") were dissolved in 200 parts of toluene. The polymerization reaction was then carried out for 5.5 hours under a nitrogen atmosphere at 70°C to obtain a boron-containing acrylic resin solution (solids concentration: 33%). The obtained boron-containing acrylic polymer (resin) had a Tg of 110°C and a Mw of 80,000. 20 parts of the obtained boron-containing acrylic resin were dissolved in 80 parts of methyl ethyl ketone to obtain a coating solution (20% resin solution) for resin layer formation.
[0146] [Chemical Formula 7] [Example 1] On the polarizer surface of the polarizer P1 obtained in Manufacturing Example 7, the coating liquid for forming the barrier layer of Manufacturing Example 9 was applied using a wire-wound bar. The coating film was then dried at 60°C for 5 minutes to form a barrier layer (400 nm thick) consisting of a solidified coating film of an organic solvent solution of resin. Next, a retardation film (first retardation layer) obtained in Manufacturing Example 5 was bonded to the surface of the barrier layer using an acrylic adhesive. Then, on the surface of the first retardation layer, the hard coating resin composition for forming the reinforcing layer of Manufacturing Example 1 was applied using a wire-wound bar to a cured thickness of 1 μm. After heating at 60°C for 1 minute, the mixture was subjected to a nitrogen atmosphere with a cumulative light intensity of 250 mJ / cm². 2 Ultraviolet light was irradiated to form a hard coating (reinforcement layer). Then, the liquid crystal alignment fixing layer (second retardation layer) of Manufacturing Example 6 was transferred to the surface of the reinforcement layer using the UV-curable adhesive of Manufacturing Example 4 (cured thickness 1.5 μm). This process yielded an optical laminate consisting of an HC-PC film (visual recognition side protective layer: first protective layer), a polarizer, a blocking layer, a first retardation layer, a reinforcement layer (hard coating), an adhesive layer, and a second retardation layer. The obtained optical laminate was evaluated according to (1) and (2) above. The results are shown in Table 1.
[0147] [Example 2] On the polarizer surface of the polarizer P2 obtained in Manufacturing Example 8, the coating liquid for forming the barrier layer of Manufacturing Example 9 was applied using a wire-wound bar. The coating film was then dried at 60°C for 5 minutes to form a barrier layer (400 nm thick) consisting of a solidified coating film of an organic solvent solution of resin. Next, the retardation film (first retardation layer) obtained in Manufacturing Example 5 was bonded to the surface of the barrier layer using an acrylic adhesive. Then, the adhesive for forming the reinforcing layer of Manufacturing Example 2 was applied to the surface of the first retardation layer using a wire-wound bar, with a cured thickness of 1.5 μm. The liquid crystal alignment fixing layer (second retardation layer) of Manufacturing Example 6 was transferred to the surface of the reinforcing layer via this adhesive layer (reinforcing layer). The adhesive layer (reinforcing layer) was heated under a nitrogen atmosphere to a cumulative light intensity of 2000 mJ / cm². 2 The material was cured by irradiating it with ultraviolet light. This process was repeated to obtain an optical laminate consisting of an HC-TAC film (visual recognition side protective layer: first protective layer) / polarizer / blocking layer / first retardation layer / reinforcing layer (adhesive layer) / second retardation layer. The resulting optical laminate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0148] [Comparative Example 1] Instead of the adhesive used to form the reinforcing layer in Manufacturing Example 2, the second retardation layer was transferred using the UV-curable adhesive of Manufacturing Example 3. Otherwise, the process was the same as in Example 2, resulting in an optical laminate comprising an HC-TAC film (visual recognition side protective layer: first protective layer) / polarizer / blocking layer / first retardation layer / adhesive layer / second retardation layer. The obtained optical laminate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0149] [Comparative Example 2] On the polarizer surface of the polarizer P2 obtained in Manufacturing Example 8, the coating liquid for forming the barrier layer of Manufacturing Example 9 was coated using a wire-wound bar. The coated film was then dried at 60°C for 5 minutes to form a barrier layer (400 nm thick) consisting of a solidified coating film of an organic solvent solution of resin, thus producing laminate 1. Next, on the surface of the retardation film (first retardation layer) obtained in Manufacturing Example 5, the hard coating resin composition for forming the reinforcing layer of Manufacturing Example 1 was coated using a wire-wound bar to achieve a cured thickness of 1 μm. After heating at 60°C for 1 minute, the mixture was then subjected to a nitrogen atmosphere with a cumulative light intensity of 250 mJ / cm². 2Ultraviolet light was irradiated to form a hard coating (reinforcing layer), thus forming a laminate 2. Next, laminate 2 was bonded to the barrier layer of laminate 1 using an acrylic adhesive, with the hard coating in contact with the barrier layer. Then, the adhesive of Manufacturing Example 3 was applied to the surface of the first retardation layer using a wire-wound bar, with a cured thickness of 1.5 μm. The liquid crystal alignment fixing layer (second retardation layer) of Manufacturing Example 6 was transferred to the surface using this adhesive. This process was repeated to obtain an optical laminate having the following structure: HC-TAC film (visual recognition side protective layer: first protective layer) / polarizer / barrier layer / reinforcing layer (hard coating layer) / first retardation layer / adhesive layer / second retardation layer. The obtained optical laminate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0150] [evaluate] As shown in Table 1, the optical laminate of the embodiments of the present invention suppresses cracks in the first retardation layer even under harsh high temperature and high humidity conditions.
[0151] Industrial availability The optical laminate of the present invention can be suitably used in image display devices (typically liquid crystal display devices and organic EL display devices).
Claims
1. An optical laminate, which sequentially has a polarizing plate including a polarizer, a retardation layer and a reinforcement layer, the retardation layer is composed of a stretched resin film and satisfies the relationship of Re(450) < Re(550), the reinforcement layer is a cured layer of an active energy ray-curable resin composition, the indentation elastic modulus of the cross section of the reinforcement layer is equal to or higher than the indentation elastic modulus of the cross section of the retardation layer, in, Re(450) and Re(550) are in-plane retardations measured with light at wavelengths of 450 nm and 550 nm at 23°C, respectively.
2. The optical laminate according to claim 1, wherein, Re(550) of the retardation layer is 100 nm to 200 nm, and the angle formed by the slow axis of the retardation layer and the absorption axis of the polarizer is 40° to 50° or 130° to 140°.
3. The optical laminate according to claim 1, wherein, Further comprising another retardation layer on the side of the reinforcement layer opposite to the retardation layer, the another retardation layer exhibiting a refractive index characteristic satisfying the relationship of nz>nx=ny.
4. The optical laminate according to claim 1, wherein, Further comprising a barrier layer between the polarizing plate and the retardation layer.
5. The optical laminate according to claim 1, wherein, The retardation layer contains a resin, the resin comprising at least one bonding group selected from the group consisting of a carbonate bond and an ester bond, and at least one structural unit selected from the group consisting of a structural unit represented by the following general formula (1) and a structural unit represented by the following general formula (2), and having positive refractive index anisotropy, In general formulas (1) and (2), R 1 ~R 3 Each is independently a directly bonded, substituted, or unsubstituted alkylene group having 1 to 4 carbon atoms, R 4 ~R 9 Each of the following is independently a hydrogen atom, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 4 to 10 carbon atoms, a substituted or unsubstituted acyl group having 1 to 10 carbon atoms, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, a substituted or unsubstituted aryloxy group having 1 to 10 carbon atoms, a substituted or unsubstituted amino group, a substituted or unsubstituted vinyl group having 1 to 10 carbon atoms, a substituted or unsubstituted ethynyl group having 1 to 10 carbon atoms, a sulfur atom having a substituent, a silicon atom having a substituent, a halogen atom, a nitro group, or a cyano group; wherein, R 4 ~R 9 They can be the same or different. R 4 ~R 9 At least two adjacent groups can also bond to each other to form a ring.
6. The optical laminate according to claim 1, wherein, The polarizing plate comprises a protective layer on the side of the polarizer opposite to the retardation layer, Re(550) of the protective layer is 20 nm or less, and Re(450) / Re(550) is 0.98 to 1.
03.
7. The optical laminate according to claim 6, wherein, The protective layer comprises a polycarbonate-based resin, The polycarbonate-based resin comprises a structural unit derived from at least one dihydroxy compound selected from the group consisting of isosorbide, isomannide and isoidide.
8. The optical laminate according to claim 3, wherein, An adhesive layer is provided between the reinforcement layer and the another retardation layer.
9. The optical laminate according to claim 3, wherein the reinforcement layer also functions as an adhesive layer.
10. The optical laminate according to claim 9, wherein, The active energy ray-curable resin composition constituting the reinforcement layer comprises a combination of a bifunctional monomer, a trifunctional monomer, an oligomer and boric acid.
11. The optical laminate according to claim 1, wherein, An intermediate layer, which is a compatible region containing the components of the retardation layer and the components of the reinforcement layer, is formed between the retardation layer and the reinforcement layer, and the thickness of the intermediate layer is 0.8 μm or less.
12. An image display device comprising the optical laminate according to any one of claims 1 to 11.
Citation Information
Patent Citations
Fluorescence eye catcher sighhboard by stimulation of ultraaviolet ray s
JP1977004200A
Optically active liquid crystal compound having cyano group
JP1989070455A
Homeotropic alignment liquid-crystalline composition, method for producing homeotropic alignment liquid crystal film and homeotropic alignment liquid crystal film
JP2002333642A
Polycarbonate resin and transparent film comprising the same
JP2012067300A
Manufacturing method of thin polarizing film
JP2012073580A