A low-loss shielded cable
By combining a three-layer co-extruded coating structure with an aluminum foil shielding layer, the problems of dielectric loss and insulation performance of shielded cables are solved, and the long-term operational stability and dielectric performance of the cables are improved.
Patent Information
- Application Number
- CN202611554679.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-10
AI Technical Summary
Existing shielded cables suffer from high dielectric loss, insulation degradation, and space charge accumulation during long-term operation. In particular, the dielectric loss of polyolefin materials increases and the interfacial compatibility is poor, which affects the operational stability and lifespan of the cables.
It adopts a three-layer co-extruded coating structure, with the inner, middle and outer layers composed of polyolefin matrix, modified filler and additives in specific proportions, respectively. Combined with an aluminum foil shielding layer, it forms a multi-layer insulation structure through interface modification and charge control technology to reduce dielectric loss.
This achieves low dielectric loss and dielectric loss factor during long-term operation, improves the reliability and stability of the cable, and reduces the impact of electric field inhomogeneity and space charge accumulation.
Smart Images

Figure CN123072832A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable material technology, and specifically to a low-loss shielded cable. Background Technology
[0002] With the rapid development of new energy power systems, smart grids, and high-voltage transmission technology, cables, as an important carrier of electrical energy transmission, are facing increasingly higher operating voltage levels and long-term service requirements. Shielded cables, due to their good electromagnetic compatibility performance, can effectively reduce the impact of external electromagnetic interference on signal transmission and power transmission processes, and are widely used in high-voltage transmission, industrial control, rail transportation, and new energy equipment.
[0003] In the existing technology, polyolefin materials are widely used in the preparation of cable insulation layers due to their low dielectric constant, good mechanical properties and excellent processing performance. However, polyolefin materials are non-polar polymer materials, and they have microscopic defects such as molecular chain defects, microporous structures and impurity residues. Under the action of long-term alternating electric fields, they are prone to problems such as increased dielectric loss, accumulation of space charge and decay of insulation performance, which in turn affect the operational stability and service life of cables.
[0004] Meanwhile, in order to reduce cable insulation loss, low dielectric fillers, nanofiller modification, or the introduction of cross-linked structures are often used to improve insulation performance. To a certain extent, this reduces the dielectric loss of the material and improves thermal stability. However, the interfacial compatibility between inorganic fillers and polymers is poor, which can easily cause filler agglomeration and local electric field concentration, thus limiting the effect of reducing dielectric loss. Furthermore, simply increasing the degree of cross-linking of the material may lead to a decrease in processing performance and still cannot effectively solve the problems of space charge migration and long-term accumulation. In addition, shielded cables usually only improve the external electromagnetic environment by setting a metal shielding layer, while ignoring the impact of internal charge behavior and dielectric property changes of the insulation material on the long-term operational reliability of the cable.
[0005] To address this technical deficiency, a solution is proposed. Summary of the Invention
[0006] The purpose of this invention is to provide a low-loss shielded cable to solve the technical problem that the dielectric loss, insulation performance and long-term operational stability of shielded cables in the prior art need to be further improved.
[0007] The objective of this invention can be achieved through the following technical solution: a low-loss shielded cable, comprising a plurality of cable cores, wherein the cable cores are provided with a shielding layer on the outside;
[0008] The cable core is formed by co-extruding an inner layer, a middle layer, and an outer layer of mixed material onto the conductor surface, thus creating a low-loss insulation layer on the conductor surface.
[0009] Furthermore, the low-loss shielded cable also includes: filler rope, wrapping layer and outer sheath layer located between several cable cores.
[0010] Furthermore, the outer sheath layer is formed by adding low-density polyethylene and polyolefin elastomer into a twin-screw extruder, melting and extruding them to cover the outside of the wrapping layer, forming an outer sheath layer, and obtaining a low-loss shielded cable.
[0011] Furthermore, the conductor is formed by stranding several copper wires with a diameter of 1.42 mm, and its diameter is 17 mm. The thickness of the low-loss insulation layer is 4-5 mm. The shielding layer is formed by wrapping aluminum foil around the outside of the cable core.
[0012] Furthermore, the inner layer mixture is composed of a polyolefin matrix, methyltriallylsilane, and additives in a weight ratio of 100:2-3:0.3, and the thickness of the inner layer accounts for 20%.
[0013] Furthermore, the intermediate layer mixture is composed of a polyolefin matrix, a vinyl-modified filler, methyltriallylsilane, and additives in a weight ratio of 100:9-11:1.9-2.2:0.3, and the thickness of the intermediate layer accounts for 60%.
[0014] Furthermore, the outer layer mixture is composed of a polyolefin matrix, vinyl-modified filler, activated modified barium titanate, methyltriallylsilane, and additives in a weight ratio of 90:7-8:4-5:1.2-1.6:0.3, and the thickness of the outer layer accounts for 20%.
[0015] Furthermore, the polyolefin matrix is obtained by melt mixing and purification of low-density polyethylene, polyolefin elastomer, maleic anhydride and dicumyl peroxide. The specific preparation method is as follows: low-density polyethylene, polyolefin elastomer, maleic anhydride and dicumyl peroxide are mixed and then added to a torque rheometer at a temperature of 160-170℃, the rotation speed is set to 60-80 rpm, melt mixing is performed for 8-10 minutes, and then purified to obtain the polyolefin matrix.
[0016] Furthermore, the weight ratio of the low-density polyethylene, polyolefin elastomer, maleic anhydride, and dicumyl peroxide is 70:28-32:1.9-2.3:0.1-0.2. The purification operation is as follows: after melt mixing, it is mixed with xylene at a solid-liquid ratio of 1:9 and stirred. The reaction system is heated to 80-90℃ and stirred for 6-8 hours. The reaction system is cooled to room temperature, acetone is added to the reaction system, and the mixture is filtered. The filter cake is washed with acetone three times and then dried. The filter cake is transferred to a drying oven at a temperature of 60-70℃ and dried to constant weight to obtain the polyolefin matrix.
[0017] Furthermore, the vinyl-modified filler is obtained by surface modification of a mixed filler composed of hollow glass microspheres and nano-boron nitride using KH-570. The specific preparation method is as follows:
[0018] Hollow glass microspheres, nano boron nitride, KH-570, and anhydrous ethanol were mixed and stirred. The reaction system was heated to 60-70℃, and ammonia water was added to the reaction system. The reaction was kept at this temperature for 4-5 hours. After post-treatment, vinyl-modified filler was obtained.
[0019] Furthermore, the ratio of hollow glass microspheres, nano boron nitride, KH-570, anhydrous ethanol, and ammonia is 10g:2.2-2.8g:1.6-2.0g:100mL:10mL, and the concentration of ammonia is 0.5-0.7mol / L. The post-treatment includes: after the reaction is complete, cooling the reaction system to room temperature, filtering, washing the filter cake with deionized water until neutral, transferring the filter cake to a drying oven at 60-70℃, and drying to constant weight to obtain vinyl-modified filler.
[0020] Furthermore, the preparation method of activated modified barium titanate is as follows: polydopamine is coated on nano barium titanate to obtain PDA-coated barium titanate, and then the PDA-coated barium titanate undergoes a ring-opening amidation reaction with 2-octenylsuccinic anhydride to obtain activated modified barium titanate.
[0021] The present invention has the following beneficial effects:
[0022] 1. This invention reduces the impact of small molecule impurities on conductivity loss under a power frequency electric field by purifying the polyolefin molecular chains through melt grafting followed by xylene dissolution and acetone precipitation. It also gives the polyolefin molecular chains a polar connection structure, improving the interfacial bonding between the polymer and the modified filler, and reducing polarization losses caused by interfacial defects. Simultaneously, methyltriallylsilane forms a slightly cross-linked network under the action of free radicals, which is beneficial for improving the bonding degree between polymer molecular chains and restricting carrier migration. Furthermore, the multilayer insulation structure formed by three-layer co-extrusion allows different functional components to act on different regions, achieving uniform electric field distribution and space charge regulation. This enables the cable to maintain a low dielectric loss tangent and dielectric loss factor even after long-term operation, improving the long-term reliability of low-loss shielded cables.
[0023] 2. This invention also uses KH-570 to surface-modify hollow glass microspheres and nano-boron nitride, introducing vinyl structures on the filler surface to improve its bonding ability with the polyolefin matrix. Barium titanate is coated with PDA and activated with maleic anhydride, forming a dielectric buffer layer and a chemical bonding layer on the surface of the barium titanate particles. This avoids interfacial polarization directly caused by the high-dielectric filler. Simultaneously, the polar structure in the PDA provides charge trapping. In the multilayer insulation structure formed by three-layer co-extrusion, the inner layer near the conductor utilizes the polyolefin matrix and micro-crosslinked structure to improve interfacial compactness and reduce carrier injection; the middle layer uses vinyl-modified filler to reduce material polarization and hinder space charge migration; the outer layer uses PDA / maleic anhydride-activated modified barium titanate to provide charge trapping sites, restricting and gradually dissipating carriers migrating to the outside of the insulation layer. Through dielectric strength and charge regulation among the three layers, the electric field distribution inside the insulation layer becomes more uniform, reducing space charge accumulation and thus reducing dielectric loss variations during long-term operation.
[0024] 3. The present invention also provides an aluminum foil shielding layer outside the three-layer composite insulation layer to shield external electromagnetic interference and reduce the influence of external alternating electric fields on the insulation system, so that the composite insulation structure can work in a more stable electric field environment. The shielding layer and the three-layer composite insulation structure work together to improve the dielectric stability of the cable from the two aspects of external electromagnetic environment control and internal charge migration regulation, so that the shielded cable maintains a low dielectric loss tangent and dielectric loss factor under long-term operating conditions, thereby improving the long-term service reliability of the cable. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a schematic diagram of the cross-sectional structure of the low-loss shielded cable of the present invention;
[0027] Figure 2 This is a schematic diagram of the cable core structure of the present invention.
[0028] In the diagram: 100, cable core; 1000, conductor; 1001, inner layer; 1002, middle layer; 1003, outer layer; 200, shielding layer; 300, wrapping layer; 400, outer sheath layer. Detailed Implementation
[0029] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0030] In this invention, the particle size of the hollow glass microspheres is 325 mesh;
[0031] In this invention, the boron nitride nanoparticles have a particle size of 10-100 nm and are in the form of flakes;
[0032] In this invention, KH-570 is γ-methacryloyloxypropyltrimethoxysilane, with a content of 99.9%;
[0033] In this invention, the nano-barium titanate has a particle size of 80-100 nm and a purity of 99.9%.
[0034] In this invention, the low-density polyethylene is selected from commercially available products from Yanshan Petrochemical, with an extrusion grade and a grade of 1875.
[0035] In this invention, the polyolefin elastomer is a commercially available ethylene octene copolymer, selected from Dow Chemical Company, model number 8842.
[0036] Example 1
[0037] Please see Figure 1-2 This embodiment provides a manufacturing process for a low-loss shielded cable, including the following steps:
[0038] Step 1: Preparation of vinyl-modified fillers
[0039] Weigh out 100g of hollow glass microspheres, 22g of nano boron nitride, 16g of KH-570, and 1L of anhydrous ethanol and add them to a reaction flask. Stir the mixture and heat the reaction flask to 60℃. Add 100mL of 0.5mol / L ammonia water to the reaction flask and keep the mixture at this temperature for 4h. Cool the reaction flask to room temperature and filter the mixture. Wash the filter cake with deionized water until neutral. Transfer the filter cake to a drying oven at 60℃ and dry it to constant weight to obtain the vinyl-modified filler.
[0040] Step 2: Preparation of activated modified barium titanate
[0041] Weigh out 50g of nano barium titanate, 500mL of 0.1mol / L Tris-HCl buffer solution (pH=8.5) and 8g of dopamine hydrochloride, add them to a reaction flask and stir. Stir and react at room temperature for 12h. Filter the mixture, wash the filter cake with purified water until neutral, and then dry it. Transfer the filter cake to a drying oven at 60℃ and dry it to constant weight to obtain PDA-coated barium titanate.
[0042] Weigh out 50g of PDA-coated barium titanate, 500mL of N,N-dimethylformamide, 12g of maleic anhydride, and 1g of 4-dimethylaminopyridine and add them to a reaction flask under nitrogen protection. Stir the mixture and heat it to 60℃. Keep the temperature for 6 hours. Cool the reaction flask to room temperature and filter it. Wash the filter cake three times with N,N-dimethylformamide and then three times with purified water. Transfer the filter cake to a drying oven at 60℃ and dry it to constant weight to obtain activated modified barium titanate.
[0043] Step 3: Preparation of polyolefin matrix
[0044] Weigh out the following by weight: 70 parts of low-density polyethylene, 28 parts of polyolefin elastomer, 1.9 parts of maleic anhydride and 0.1 parts of dicumyl peroxide. Mix them and add them to a torque rheometer at 160℃. Set the speed to 60 rpm and melt-mix for 8 minutes. Crush and pass through a 20-mesh sieve to obtain a polyolefin matrix preform.
[0045] The polyolefin matrix preform and xylene were added to a reaction vessel at a solid-liquid ratio of 1:9 and stirred. The reaction vessel was heated to 80°C and stirred for 6 hours. The reaction vessel was then cooled to room temperature. Acetone with a volume three times that of xylene was added to the reaction vessel. The mixture was filtered, and the filter cake was washed three times with acetone and then dried. The filter cake was transferred to a drying oven at 60°C and dried to constant weight to obtain the polyolefin matrix.
[0046] Step 4: Prepare the cable core
[0047] Several copper wires with a diameter of 1.42 mm are twisted together to obtain a conductor 1000 with a diameter of 17 mm;
[0048] Dicumyl peroxide, antioxidant 1010, and antioxidant 168 are mixed in a weight ratio of 4:2:1 to obtain the additive, which is then set aside.
[0049] The polyolefin matrix, methyltriallylsilane, and additives are mixed in a weight ratio of 100:2:0.3 and then added to a single-screw extruder at a temperature of 170°C for melt mixing to obtain the inner layer mixture.
[0050] The polyolefin matrix, vinyl-modified filler, methyltriallylsilane, and additives are mixed in a weight ratio of 100:9:1.9:0.3 and then added to a single-screw extruder at a temperature of 175°C for melt mixing to obtain the intermediate layer mixture.
[0051] The polyolefin matrix, vinyl-modified filler, activated modified barium titanate, methyltriallylsilane, and additives were mixed in a weight ratio of 90:7:4:1.2:0.3 and then added to a single-screw extruder at a temperature of 170℃ for melt mixing to obtain the outer layer mixture.
[0052] With an inner layer 1001 thickness of 0.8 mm, a middle layer 1002 thickness of 2.4 mm, and an outer layer 1003 thickness of 0.8 mm, the above-mentioned inner layer mixture, middle layer mixture, and outer layer mixture are extruded layer by layer through a three-layer co-extrusion die and coated onto the conductor surface to form a three-layer composite low-loss insulation layer on the conductor surface, thus obtaining cable core 100.
[0053] Step 5: Prepare low-loss shielded cable
[0054] With an overlap rate of 15%, aluminum foil is wrapped around the outside of the cable core to form a shielding layer of 200.
[0055] Several cable cores with shielding layers are placed in parallel, filler strips are placed between the cable cores, and then polyester wrapping tape is used to wrap and cover them to form a wrapping layer of 300.
[0056] Low-density polyethylene and polyolefin elastomer are added to a twin-screw extruder at a weight ratio of 7:3. The temperatures of the six temperature zones of the twin-screw extruder are set to 165℃, 170℃, 170℃, 170℃, and 170℃ respectively, the die temperature is set to 175℃, and the screw speed is set to 70 r / min. The melt extrusion coats the outside of the sheath layer, forming an outer sheath layer 400 with a thickness of 3.0±0.1mm, resulting in a low-loss shielded cable.
[0057] Example 2
[0058] Please see Figure 1-2 This embodiment provides a manufacturing process for a low-loss shielded cable, including the following steps:
[0059] Step 1: Preparation of vinyl-modified fillers
[0060] Weigh out 100g of hollow glass microspheres, 25g of nano boron nitride, 18g of KH-570, and 1L of anhydrous ethanol and add them to a reaction flask. Stir the mixture and heat the reaction flask to 65℃. Add 100mL of 0.6mol / L ammonia water to the reaction flask and keep it at this temperature for 4.5h. Cool the reaction flask to room temperature and filter it. Wash the filter cake with deionized water until neutral. Transfer the filter cake to a drying oven at 65℃ and dry it to constant weight to obtain vinyl-modified filler.
[0061] Step 2: Preparation of activated modified barium titanate
[0062] Weigh out 50g of barium titanate nanoparticles, 500mL of 0.1mol / L Tris-HCl buffer solution (pH=8.5), and 9g of dopamine hydrochloride. Add them to a reaction flask and stir. Stir and react at room temperature for 14h. Filter the mixture. Wash the filter cake with purified water until neutral and then dry it. Transfer the filter cake to a drying oven at 65℃ and dry it to constant weight to obtain PDA-coated barium titanate.
[0063] Weigh out 50g of PDA-coated barium titanate, 500mL of N,N-dimethylformamide, 13g of maleic anhydride, and 1g of 4-dimethylaminopyridine and add them to a reaction flask under nitrogen protection. Stir the mixture and heat it to 65℃. Keep the temperature for 7 hours. Cool the reaction flask to room temperature and filter it. Wash the filter cake three times with N,N-dimethylformamide and then three times with purified water. Transfer the filter cake to a drying oven at 65℃ and dry it to constant weight to obtain activated modified barium titanate.
[0064] Step 3: Preparation of polyolefin matrix
[0065] Weigh out the following by weight: 70 parts of low-density polyethylene, 30 parts of polyolefin elastomer, 2.0 parts of maleic anhydride and 0.15 parts of dicumyl peroxide. Mix them and add them to a torque rheometer at 165℃. Set the speed to 70 rpm and melt-mix for 9 minutes. Crush and pass through a 20-mesh sieve to obtain a polyolefin matrix preform.
[0066] The polyolefin matrix preform and xylene were added to a reaction vessel at a solid-liquid ratio of 1:9 and stirred. The reaction vessel was heated to 85°C and stirred for 7 hours. The reaction vessel was then cooled to room temperature. Acetone with a volume three times that of xylene was added to the reaction vessel. The mixture was filtered, and the filter cake was washed three times with acetone and then dried. The filter cake was transferred to a drying oven at 65°C and dried to constant weight to obtain the polyolefin matrix.
[0067] Step 4: Prepare the cable core
[0068] Several copper wires with a diameter of 1.42 mm are twisted together to obtain a conductor 1000 with a diameter of 17 mm;
[0069] Dicumyl peroxide, antioxidant 1010, and antioxidant 168 are mixed in a weight ratio of 4:2:1 to obtain the additive, which is then set aside.
[0070] The polyolefin matrix, methyltriallylsilane, and additives are mixed in a weight ratio of 100:2.5:0.3 and then added to a single-screw extruder at a temperature of 170°C for melt mixing to obtain the inner layer mixture.
[0071] The polyolefin matrix, vinyl-modified filler, methyltriallylsilane, and additives are mixed in a weight ratio of 100:10:2.0:0.3 and then added to a single-screw extruder at a temperature of 175°C for melt mixing to obtain the intermediate layer mixture.
[0072] The polyolefin matrix, vinyl-modified filler, activated modified barium titanate, methyltriallylsilane, and additives were mixed in a weight ratio of 90:7.5:4.5:1.4:0.3 and then added to a single-screw extruder at a temperature of 170℃ for melt mixing to obtain the outer layer mixture.
[0073] With an inner layer 1001 thickness of 0.9 mm, a middle layer 1002 thickness of 2.7 mm, and an outer layer 1003 thickness of 0.9 mm, the above-mentioned inner layer mixture, middle layer mixture, and outer layer mixture are extruded layer by layer through a three-layer co-extrusion die and coated onto the conductor surface to form a three-layer composite low-loss insulation layer on the conductor surface, thus obtaining cable core 100.
[0074] Step 5: Prepare low-loss shielded cable
[0075] With an overlap rate of 15%, aluminum foil is wrapped around the outside of the cable core to form a shielding layer of 200.
[0076] Several cable cores with shielding layers are placed in parallel, filler strips are placed between the cable cores, and then polyester wrapping tape is used to wrap and cover them to form a wrapping layer of 300.
[0077] Low-density polyethylene and polyolefin elastomer are added to a twin-screw extruder at a weight ratio of 7:3. The temperatures of the six temperature zones of the twin-screw extruder are set to 165℃, 170℃, 170℃, 170℃, and 170℃ respectively, the die temperature is set to 175℃, and the screw speed is set to 70 r / min. The melt extrusion coats the outside of the sheath layer, forming an outer sheath layer 400 with a thickness of 3.0±0.1mm, resulting in a low-loss shielded cable.
[0078] Example 3
[0079] Please see Figure 1-2 This embodiment provides a manufacturing process for a low-loss shielded cable, including the following steps:
[0080] Step 1: Preparation of vinyl-modified fillers
[0081] Weigh out 100g of hollow glass microspheres, 28g of nano boron nitride, 20g of KH-570, and 1L of anhydrous ethanol and add them to a reaction flask. Stir the mixture and heat the reaction flask to 70℃. Add 100mL of 0.7mol / L ammonia water to the reaction flask and keep it at this temperature for 5h. Cool the reaction flask to room temperature and filter it. Wash the filter cake with deionized water until neutral. Transfer the filter cake to a drying oven at 70℃ and dry it to constant weight to obtain vinyl-modified filler.
[0082] Step 2: Preparation of activated modified barium titanate
[0083] Weigh out 50g of nano barium titanate, 500mL of 0.1mol / L Tris-HCl buffer solution (pH=8.5) and 10g of dopamine hydrochloride, add them to a reaction flask and stir. Stir and react at room temperature for 16h. Filter the mixture, wash the filter cake with purified water until neutral, and then dry it. Transfer the filter cake to a drying oven at 70℃ and dry it to constant weight to obtain PDA-coated barium titanate.
[0084] Weigh out 50g of PDA-coated barium titanate, 500mL of N,N-dimethylformamide, 14g of maleic anhydride, and 1g of 4-dimethylaminopyridine and add them to a reaction flask under nitrogen protection. Stir the mixture and heat it to 70℃. Keep the temperature for 8 hours. Cool the reaction flask to room temperature and filter it. Wash the filter cake three times with N,N-dimethylformamide and then three times with purified water. Transfer the filter cake to a drying oven at 70℃ and dry it to constant weight to obtain activated modified barium titanate.
[0085] Step 3: Preparation of polyolefin matrix
[0086] Weigh out the following by weight: 70 parts of low-density polyethylene, 32 parts of polyolefin elastomer, 2.3 parts of maleic anhydride and 0.2 parts of dicumyl peroxide. Mix them and add them to a torque rheometer at 170℃. Set the speed to 80 rpm and melt-mix for 10 minutes. Then crush and pass through a 20-mesh sieve to obtain a polyolefin matrix preform.
[0087] The polyolefin matrix preform and xylene were added to a reaction vessel at a solid-liquid ratio of 1:9 and stirred. The reaction vessel was heated to 90°C and stirred for 8 hours. The reaction vessel was then cooled to room temperature. Acetone with a volume three times that of xylene was added to the reaction vessel. The mixture was filtered, and the filter cake was washed three times with acetone and then dried. The filter cake was transferred to a drying oven at 70°C and dried to constant weight to obtain the polyolefin matrix.
[0088] Step 4: Prepare the cable core
[0089] Several copper wires with a diameter of 1.42 mm are twisted together to obtain a conductor 1000 with a diameter of 17 mm;
[0090] Dicumyl peroxide, antioxidant 1010, and antioxidant 168 are mixed in a weight ratio of 4:2:1 to obtain the additive, which is then set aside.
[0091] The polyolefin matrix, methyltriallylsilane, and additives are mixed in a weight ratio of 100:3:0.3 and then added to a single-screw extruder at a temperature of 170°C for melt mixing to obtain the inner layer mixture.
[0092] The polyolefin matrix, vinyl-modified filler, methyltriallylsilane, and additives were mixed in a weight ratio of 100:11:2.2:0.3 and then added to a single-screw extruder at a temperature of 175°C for melt mixing to obtain the intermediate layer mixture.
[0093] The polyolefin matrix, vinyl-modified filler, activated modified barium titanate, methyltriallylsilane, and additives are mixed in a weight ratio of 90:8:5:1.6:0.3 and then added to a single-screw extruder at a temperature of 170℃ for melt mixing to obtain the outer layer mixture.
[0094] With an inner layer 1001 thickness of 1.0 mm, a middle layer 1002 thickness of 3.0 mm, and an outer layer 1003 thickness of 1.0 mm, the above-mentioned inner layer mixture, middle layer mixture, and outer layer mixture are extruded layer by layer through a three-layer co-extrusion die and coated onto the conductor surface to form a three-layer composite low-loss insulation layer on the conductor surface, thus obtaining cable core 100.
[0095] Step 5: Prepare low-loss shielded cable
[0096] With an overlap rate of 15%, aluminum foil is wrapped around the outside of the cable core to form a shielding layer of 200.
[0097] Several cable cores with shielding layers are placed in parallel, filler strips are placed between the cable cores, and then polyester wrapping tape is used to wrap and cover them to form a wrapping layer of 300.
[0098] Low-density polyethylene and polyolefin elastomer are added to a twin-screw extruder at a weight ratio of 7:3. The temperatures of the six temperature zones of the twin-screw extruder are set to 165℃, 170℃, 170℃, 170℃, and 170℃ respectively, the die temperature is set to 175℃, and the screw speed is set to 70 r / min. The melt extrusion coats the outside of the sheath layer, forming an outer sheath layer 400 with a thickness of 3.0±0.1mm, resulting in a low-loss shielded cable.
[0099] Comparative Example 1
[0100] The difference between this comparative example and Example 3 is that hollow glass microspheres were not added in step 1.
[0101] Comparative Example 2
[0102] The difference between this comparative example and Example 3 is that step 2 is omitted, and the activated modified barium titanate in step 4 is replaced with nano barium titanate.
[0103] Comparative Example 3
[0104] The difference between this comparative example and Example 3 is that in step 4, the inner layer mixture, the middle layer mixture, and the outer layer mixture are mixed evenly and then extruded to coat the outside of the conductor, with a thickness consistent with the thickness of the low-loss insulation layer in Example 3.
[0105] Comparative Example 4
[0106] The difference between this comparative example and Example 3 is that no shielding layer is provided in step 5.
[0107] Performance testing:
[0108] The dielectric loss tangent tanδ of the low-loss shielded cable samples prepared in Examples 1-3 and Comparative Examples 1-4 was determined according to the standard GB / T 3048.11-2025 "Test Methods for Electrical Performance of Wires and Cables - Part 11: Dielectric Loss Tangent Test" at a power frequency voltage of 1.5U0 (U0=21kV) and 50Hz.
[0109] The relative permittivity and dielectric loss factor of the low-loss insulation layer in the low-loss shielded cable samples prepared in Examples 1-3 and Comparative Examples 1-4 were determined by the bridge method in reference standard GB / T 31838.8-2024 "Dielectric and resistive properties of solid insulating materials - Part 8: Determination of dielectric properties (AC method) - Relative permittivity and dielectric loss factor (frequency 1MHz~300MHz)".
[0110] The low-loss shielded cables prepared in Examples 1-3 and Comparative Examples 1-4 were used continuously for 1000 hours. The dielectric loss tangent, relative permittivity, and dielectric loss factor of the samples were measured. The specific test data are shown in Table 1 below.
[0111] Table 1 - Performance Test Data of Samples
[0112]
[0113] Data Analysis:
[0114] Comparative analysis of the data in Table 1 shows that the dielectric loss tangent of the low-loss shielded cable prepared by this invention reaches 0.96-1.42×10⁻⁶. -4 After 1000 hours of operation, the dielectric loss tangent reached 1.08-1.61×10⁻⁶. -4 The relative permittivity of the low-loss insulating layer of the sample reached 1.95-2.05, and the dielectric loss factor reached 1.86-2.65×10⁻⁶. -4 After 1000 hours of operation, the relative permittivity of the low-loss insulation layer of the sample reached 2.00-2.08, and the dielectric loss factor reached 2.10-3.05×10-4.
[0115] The difference between Comparative Example 1 and Example 3 is that hollow glass microspheres were not added in step 1. The dielectric loss tangent of the sample prepared in Comparative Example 1 before operation was 1.68 × 10⁻⁶. -4 The relative permittivity is 2.16, and the dielectric loss factor is 3.12 × 10⁻⁶. -4 All of them are higher than the 0.96×10 corresponding to Example 3. -4 1.97 and 1.86×10 -4 After 1000 hours of operation, its dielectric loss tangent further increased to 1.94 × 10⁻⁶. -4The dielectric loss factor increased to 3.65 × 10⁻⁶. -4 This indicates that the hollow structure inside the hollow glass microspheres, with its low dielectric constant, can reduce the overall polarization of the material in a composite insulation system and decrease the dipole response under an alternating electric field. Simultaneously, the hollow structure can reduce the dielectric difference between the inorganic filler and the polyolefin matrix, thus reducing interfacial polarization.
[0116] The difference between Comparative Example 2 and Example 3 is that step 2 is omitted, and nano-barium titanate is directly used instead of activated modified barium titanate. The sample prepared in Comparative Example 2 achieved a dielectric loss tangent of 2.26 × 10⁻⁶ before operation. -4 The relative permittivity increased to 2.32, and the dielectric loss factor increased to 4.18 × 10⁻⁶. -4 After 1000 hours of operation, the dielectric loss tangent reached 2.71 × 10⁻⁶. -4 The dielectric loss factor further increased to 5.06 × 10⁻⁶. -4 This indicates that barium titanate, a high-dielectric-constant inorganic material, is directly added to a polyolefin matrix without surface modification. Due to the significant dielectric difference between the inorganic particles and the organic polymer, local electric field concentration easily forms at the filler interface, resulting in strong interfacial polarization. Simultaneously, unmodified nano-barium titanate is prone to agglomeration, creating high-dielectric-constant defect structures in localized areas, further increasing dielectric loss. After PDA coating and maleic anhydride activation, a dielectric buffer layer and a chemical bonding layer are formed on the barium titanate surface, reducing the interfacial polarization between barium titanate and the polymer, improving filler dispersibility, and utilizing the polar functional groups in the PDA to form charge-trapping sites, restricting space charge migration.
[0117] The difference between Comparative Example 3 and Example 3 is that in step 4, the three-layer co-extrusion structure of the inner, middle, and outer layers is omitted. Instead, the mixture of each layer is uniformly mixed and extruded in one step to form a single-layer insulation structure. The dielectric loss tangent of Comparative Example 3 before operation was 1.73 × 10⁻⁶. -4 The relative permittivity is 2.12, and the dielectric loss factor is 3.25 × 10⁻⁶. -4 This is significantly higher than the data corresponding to Example 3; after 1000 hours of operation, its dielectric loss tangent increased to 2.15 × 10⁻⁶. -4 The dielectric loss factor increased to 4.02 × 10⁻⁶. -4Although Comparative Example 3 still contains functional components such as vinyl-modified filler, activated modified barium titanate, and methyltriallylsilane, the elimination of the three-layer insulation structure prevents these functional components from functioning according to the electric field distribution in their respective regions. This results in a lack of effective charge buffering structures near the conductor, the inability of the middle region to fully utilize its low dielectric resistance barrier function, and the inability of the outer region to form effective charge trapping and dissipation. Furthermore, the uniform dispersion of various fillers easily leads to localized differences in dielectric properties, reducing the uniformity of the electric field distribution and promoting space charge accumulation. This demonstrates that the three-layer co-extruded multilayer insulation structure of this invention is not a simple layered combination, but rather achieves continuous regulation of charge injection suppression, space charge migration barrier, and charge trapping and dissipation through the synergistic configuration of functional materials in different regions, thereby improving the dielectric stability of the insulation material during long-term operation.
[0118] The difference between Comparative Example 4 and Example 3 is that no aluminum foil shielding layer was provided in step 5. The dielectric loss tangent of Comparative Example 4 before operation was 1.05 × 10⁻⁶. -4 The relative permittivity is 1.98, and the dielectric loss factor is 1.92 × 10⁻⁶. -4 The changes compared to Example 3 are minor; after 1000 hours of operation, its dielectric loss tangent increases to 1.21 × 10⁻⁶. -4 The dielectric loss factor increased to 2.22 × 10⁻⁶. -4 This indicates that the aluminum foil shielding layer does not directly participate in the dielectric polarization process inside the insulation material, but it can suppress leakage current on the insulation surface and external electromagnetic disturbances during long-term operation. Together with the three-layer composite insulation structure, it forms a synergistic protection system that combines external shielding and internal charge regulation, thereby improving the dielectric stability of low-loss shielded cables during long-term operation.
[0119] The above description is merely an example and illustration of the structure of the present invention. Those skilled in the art can make various modifications, additions, or similar substitutions to the specific embodiments described, as long as they do not deviate from the structure of the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
[0120] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0121] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A low-loss shielded cable, comprising a plurality of cable cores (100), characterized in that, The cable core (100) is provided with a shielding layer (200) on the outside. The cable core (100) is formed by co-extruding an inner layer mixture, a middle layer mixture, and an outer layer mixture onto the conductor surface, and then forming a low-loss insulation layer composed of an inner layer (1001), a middle layer (1002), and an outer layer (1003) on the conductor (1000) surface.
2. The low-loss shielded cable according to claim 1, characterized in that, The conductor (1000) is formed by stranding several copper wires with a diameter of 1.42 mm, and its diameter is 17 mm. The thickness of the low-loss insulation layer is 4-5 mm. The shielding layer is formed by wrapping aluminum foil around the outside of the cable core.
3. The low-loss shielded cable according to claim 1, characterized in that, The inner layer mixture is composed of a polyolefin matrix, methyltriallylsilane, and additives in a weight ratio of 100:2-3:0.3, and the thickness of the inner layer (1001) accounts for 20%.
4. A low-loss shielded cable according to claim 1, characterized in that, The intermediate layer mixture is composed of a polyolefin matrix, a vinyl-modified filler, methyltriallylsilane, and additives in a weight ratio of 100:9-11:1.9-2.2:0.3, and the thickness of the intermediate layer (1002) accounts for 60%.
5. A low-loss shielded cable according to claim 1, characterized in that, The outer layer mixture is composed of a polyolefin matrix, vinyl modified filler, activated modified barium titanate, methyltriallylsilane, and additives in a weight ratio of 90:7-8:4-5:1.2-1.6:0.3, and the thickness of the outer layer (1003) accounts for 20%.
6. A low-loss shielded cable according to claim 1, characterized in that, The polyolefin matrix is obtained by purifying low-density polyethylene, polyolefin elastomer, maleic anhydride and dicumyl peroxide through melt blending.
7. A low-loss shielded cable according to claim 1, characterized in that, The vinyl-modified filler is obtained by surface modification of a mixed filler consisting of hollow glass microspheres and nano boron nitride using KH-570.
8. A low-loss shielded cable according to claim 1, characterized in that, The preparation method of activated modified barium titanate is as follows: barium titanate nanoparticles are coated with polydopamine to obtain PDA-coated barium titanate. Then, the PDA-coated barium titanate undergoes a ring-opening amidation reaction with 2-octenylsuccinic anhydride to obtain activated modified barium titanate.