A pressureless sintering method and application of resin-free nano-gold paste
By employing a multi-stage sintering process for resin-free nano-gold paste and utilizing the volatilization and decomposition kinetics of composite solvents, the problem of high sintering temperature in traditional gold pastes was solved, achieving low-temperature pressureless sintering. This improved interfacial bonding and product performance stability, meeting the connection requirements of high-end electronic devices.
Patent Information
- Application Number
- CN202611255933.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-10
AI Technical Summary
The high sintering temperature of existing gold paste leads to thermal damage to the chip and substrate. Furthermore, traditional processes struggle to achieve low-temperature, pressureless sintering, resulting in unstable interfacial bonding and fluctuating product performance, making it difficult to meet the high consistency and reliability requirements of high-end devices.
Using resin-free nano-gold paste, through precise matching of composite solvents and a multi-stage sintering process, including first-stage sintering, second-stage sintering and third-stage sintering, combined with an inert atmosphere and different heating rates, the densification of gold nanoparticles and interface cleaning are promoted by utilizing the volatilization and decomposition of high-boiling-point solvents and in-situ reactive sintering co-solvents.
This technology enables the creation of sintered bodies with low porosity, high shear strength, and high thermal conductivity, meeting the connectivity requirements of high-end electronic devices and improving device reliability and consistency.
Smart Images

Figure CN123076286A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electronic packaging technology, specifically relating to a pressureless sintering method and application of resin-free nano-gold paste. Background Technology
[0002] In the packaging of high-temperature, high-power, and high-frequency electronic devices (such as SiC MOSFETs, laser diodes, and RF modules), the interconnect material between the chip and the substrate is crucial to the device's performance, reliability, and lifespan.
[0003] Sintered metal interconnect materials, especially sintered silver, possess excellent electrical and thermal conductivity and exhibit low sintering temperatures (200–300°C), making them outstanding in high-performance interconnects. However, the electrochemical and ion migration issues of silver pose reliability risks under high voltage, high humidity, or high-frequency bias. Gold is an ideal material for addressing these problems, but traditional gold paste typically requires sintering temperatures exceeding 400°C, which can cause thermal damage and performance degradation to both the chip and the substrate.
[0004] Current gold paste formulations primarily involve the compounding of gold powder and organic carriers. The technical approach for low-temperature sintering gold paste mainly relies on the size effect of nano / submicron gold powder, using surface diffusion of the gold powder itself to provide the sintering driving force; the organic carrier is limited to dispersing the gold powder and providing rheological properties to the paste, passively volatilizing or decomposing during sintering. This sintering process can achieve sintering at 350℃, but it is highly dependent on pressure.
[0005] To overcome this bottleneck, functional solvent systems are being explored and developed: solvents with different boiling points, evaporation rates, or stability are compounded and volatilized or decomposed at different sintering stages. This not only satisfies the rheological properties of the paste but also generates capillary forces during solvent evaporation, tightly binding adjacent gold nanoparticles together, shortening atomic diffusion distances, and enabling low-temperature, pressureless sintering; an example is the compounding of terpineol and alcohol. However, such composite solvents still face new challenges in actual sintering: (1) Narrow process window and sensitive parameters: If the temperature rises too fast, the high-boiling-point solvent may evaporate rapidly, causing the film to crack; if the temperature rises too slowly, the low-boiling-point solvent may evaporate prematurely at a lower temperature, resulting in insufficient sintering driving force; conventional uniform or simple two-stage heating is difficult to match the evaporation kinetics of composite solvents. (2) High interface sensitivity: The metallurgical bonding strength between the sintered body and the substrate is highly dependent on the cleanliness and activity of the interface. In particular, for substrates that are easily oxidized (such as nickel-plated and copper-plated substrates), traditional processes lack targeted treatment methods, resulting in unstable interface bonding. (3) Lack of dedicated process specifications: The existing technology does not have a standardized sintering process that is deeply coupled with the characteristics of composite solvents and includes precise temperature control curves and programmed atmosphere control, resulting in poor process repeatability, large fluctuations in product performance, and difficulty in meeting the requirements of high consistency and high reliability of high-end devices.
[0006] Resin-free systems lack the adhesive buffering and shape-preserving effects of polymer resins. The sintering process relies entirely on the precise synergy of gold nanoparticle diffusion and solvent evaporation. Existing sintering processes mostly use resin systems or simple step-by-step heating, failing to fully consider the drastically different volatilization kinetics of composite solvents, resulting in high porosity, insufficient shear strength, and insufficient thermal conductivity of the sintered body. Summary of the Invention
[0007] The purpose of this invention is to provide a pressureless sintering method and application for resin-free nano-gold paste. The pressureless sintering method provided by this invention yields sintered bodies with low porosity, high shear strength, and high thermal conductivity.
[0008] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a pressureless sintering method for resin-free nano-gold paste, comprising a first-stage sintering, a second-stage sintering, and a third-stage sintering performed sequentially. The first stage of sintering includes: heating the resin-free nano gold paste to 140-190°C in an inert atmosphere at a heating rate of 5-20°C / min, and holding it at that temperature for 5-30 minutes; The second stage of sintering includes: in an inert atmosphere, continuing to heat to 190~240℃ at a heating rate of 1~5℃ / min, and holding at that temperature for 10~40min; The third stage of sintering includes: in an inert atmosphere, continuing to heat to 240~280℃ at a heating rate of 0.5~3℃ / min, and holding at that temperature for 30~120min; The resin-free nano-gold paste comprises nano-gold powder and a composite solvent; the composite solvent comprises a high-boiling-point solvent and an in-situ reactive sintering aid solvent; the boiling point of the high-boiling-point solvent is 180~350℃; the in-situ reactive sintering aid solvent is a solvent that can decompose upon heating to produce reducing gas, and the decomposition temperature is 150~250℃.
[0009] Preferably, the mass ratio of the high-boiling-point solvent to the in-situ reactive sintering co-solvent is (3~7):(3~7).
[0010] Preferably, the high-boiling-point solvent has an evaporation rate of 2 to 5 relative to butyl acetate.
[0011] Preferably, the high-boiling-point solvent includes one or more of alcohol solvents, glycol ether solvents, and ester solvents.
[0012] Preferably, the in-situ reactive sintering co-solvent has an evaporation rate of 0.02 to 0.5 relative to butyl acetate.
[0013] Preferably, the in-situ reactive sintering co-solvent includes one or more of nitrogen-containing organic solvents and sulfoxide solvents.
[0014] Preferably, the gold nanoparticles are gold nanoparticles with surface-modified organic ligands; the organic ligands include terminal thiol groups and / or terminal amino groups.
[0015] Preferably, the inert atmosphere is a nitrogen atmosphere.
[0016] The present invention also provides the application of the above-mentioned pressureless sintering method in the connection between chip and substrate, including: applying resin-free nano gold paste to the surface of the substrate and then attaching the chip, and then performing pressureless sintering.
[0017] Preferably, the substrate is pretreated before use, and the pretreatment includes one or more of oxygen plasma cleaning, argon-hydrogen plasma cleaning, formic acid vapor fumigation, and coating with solder flux.
[0018] This invention provides a pressureless sintering method for resin-free nano-gold paste. By defining the solvent composition of the gold paste and combining it with a specific sintering process, this invention precisely matches the kinetic requirements of solvent evaporation, flux decomposition, and final densification, widening and optimizing the originally narrow process window. This ensures a stable and thorough sintering process, reducing porosity and increasing thermal conductivity. Switching different heating rates at different sintering stages fully utilizes the solvent evaporation kinetics to improve densification. Using an in-situ reactive sintering flux creates an excellent surface cleaning and reaction environment, significantly improving sintering activity and interface quality, thereby increasing shear strength. Results from the embodiments show that the sintered body obtained by the pressureless sintering method provided by this invention has a porosity of less than 7%, a shear strength higher than 30 MPa, and a thermal conductivity higher than 200 W / (m·K). Attached Figure Description
[0019] Figure 1 This is a cross-sectional SEM image of the sintered body obtained in Example 1 of the present invention; Figure 2 This is a cross-sectional SEM image of the sintered body obtained in Example 2 of the present invention; Figure 3 This is a cross-sectional SEM image of the sintered body obtained in Example 3 of the present invention; Figure 4 This is a cross-sectional SEM image of the sintered body obtained in Comparative Example 1 of the present invention; Figure 5 This is a cross-sectional SEM image of the sintered body obtained in Comparative Example 2 of the present invention. Detailed Implementation
[0020] All raw materials used in this invention are not particularly limited in their source; they can be purchased from the market or prepared using conventional methods known to those skilled in the art.
[0021] There are no particular restrictions on the purity of any of the raw materials used in this invention, but industrially pure raw materials are preferred.
[0022] This invention provides a pressureless sintering method for resin-free nano-gold paste, comprising a first-stage sintering, a second-stage sintering, and a third-stage sintering performed sequentially. The first stage of sintering includes: heating the resin-free nano gold paste to 140-190°C in an inert atmosphere at a heating rate of 5-20°C / min, and holding it at that temperature for 5-30 minutes; The second stage of sintering includes: in an inert atmosphere, continuing to heat to 190~240℃ at a heating rate of 1~5℃ / min, and holding at that temperature for 10~40min; The third stage of sintering includes: in an inert atmosphere, continuing to heat to 240~280℃ at a heating rate of 0.5~3℃ / min, and holding at that temperature for 30~120min; The resin-free nano-gold paste comprises nano-gold powder and a composite solvent; the composite solvent comprises a high-boiling-point solvent and an in-situ reactive sintering aid solvent; the boiling point of the high-boiling-point solvent is 180~350℃; the in-situ reactive sintering aid solvent is a solvent that can decompose upon heating to produce reducing gas, and the decomposition temperature is 150~250℃.
[0023] In this invention, the resin-free nano-gold paste comprises nano-gold powder and a composite solvent. The resin-free nano-gold paste contains no resin, and the solvent can completely evaporate or decompose after sintering, resulting in a pure gold sintered body that meets the requirements of high-end devices.
[0024] In this invention, the gold nanoparticles are preferably gold nanoparticles with surface-modified organic ligands; the organic ligands preferably include terminal thiol groups and / or terminal amino groups. Surface modification of gold nanoparticles with organic ligands can reduce aggregation, improve dispersibility, and further enhance densification; the terminal thiol groups can form Au-S bonds with gold atoms, and the lone pair electrons of the nitrogen atoms of the amino groups can coordinate with gold, allowing the organic ligands to be firmly adsorbed onto the surface of the gold nanoparticles.
[0025] In an embodiment of the present invention, the organic ligand is octylthiol; the preparation method of gold nanoparticles with surface modified octylthiol is as follows: 1 mmol of chloroauric acid is dissolved in 200 mL of ethanol / water with a volume ratio of 1:1, 1.5 mmol of octylthiol is added, 30 mL of 0.1 mol / L ascorbic acid aqueous solution is added dropwise, the reaction is carried out at room temperature for 2 h, and the surface modified octylthiol is obtained by centrifugation, washing and drying.
[0026] In one embodiment of the present invention, the average particle size of the gold nanoparticles can be 300 nm.
[0027] In one embodiment of the present invention, the mass fraction of nano-gold powder in the resin-free nano-gold paste can be 80%.
[0028] In this invention, the composite solvent includes a high-boiling-point solvent and an in-situ reactive sintering co-solvent. The high-boiling-point solvent can reduce the evaporation rate in the early stages of sintering, maintaining the stability of the gold paste; the in-situ reactive sintering co-solvent can decompose during sintering to generate reducing gases, which react with oxides on the bonding interface surface, improving the interface cleanliness.
[0029] In this invention, the boiling point of the high-boiling solvent is 180~350℃, preferably 200~300℃. A boiling point within this range can increase the evaporation temperature, providing a driving force for the interaction of gold nanoparticles.
[0030] In this invention, the evaporation rate of the high-boiling-point solvent relative to butyl acetate is preferably 2 to 5. Within this range, the solvent can evaporate rapidly at the critical temperature for sintering neck formation, which helps to match the solvent evaporation kinetics with the sintering driving force, further improving the densification degree.
[0031] In this invention, the high-boiling-point solvent includes one or more of alcohol solvents, glycol ether solvents, and ester solvents. These solvents exhibit good stability and can evaporate directly during sintering; moreover, they can effectively disperse gold powder and improve the uniformity of the gold paste. In an embodiment of this invention, the high-boiling-point solvent is diethylene glycol butyl ether.
[0032] In this invention, the in-situ reactive sintering flux is a solvent that decomposes upon heating to generate a reducing gas. The decomposition temperature is 150-250°C, preferably 180-220°C. The decomposition temperature of the in-situ reactive sintering flux is within this range, allowing it to decompose at the critical temperature for sintering neck formation. The resulting reducing gas reduces the oxides on the substrate surface, and the instantaneous heat generated during decomposition directly acts on the gold nanoparticles, promoting the formation of the sintering neck.
[0033] In this invention, the evaporation rate of the in-situ reactive sintering flux relative to butyl acetate is preferably 0.02~0.5, more preferably 0.05~0.2. When the relative evaporation rate of the in-situ reactive sintering flux is within the above range, the high-boiling-point solvent can preferentially evaporate during sintering. The heat generated during the decomposition of the in-situ reactive sintering flux can directly act on the gold nanoparticles, and the reducing gas generated during decomposition can also act on the bonding interface between the gold particles and the gold-plated substrate / chip back gold layer, in-situ reducing and removing the oxide film and organic residues at the bonding interface, promoting surface diffusion and grain boundary diffusion of gold atoms.
[0034] In this invention, the in-situ reactive sintering co-solvent preferably comprises one or more of nitrogen-containing organic solvents and sulfoxide solvents. These solvents have relatively high decomposition temperatures, allowing for gradual decomposition after the high-boiling-point solvent has completely evaporated, which is beneficial for the reduction and densification of gold nanoparticles. In an embodiment of this invention, the in-situ reactive sintering co-solvent is N-methylformamide.
[0035] In this invention, the preferred mass ratio of the high-boiling-point solvent to the in-situ reactive sintering flux is (3~7):(3~7). As one embodiment of this invention, the mass ratio can be 3:7, 4:6, 5:5, 6:4, or 7:3. A mass ratio within the above range is beneficial for solvent evaporation stability in the early stages of sintering, and for providing sufficient instantaneous local heat and reducing gas concentration during the decomposition reaction in the middle stages of sintering, further improving the densification degree.
[0036] In one embodiment of the present invention, the mass content of the composite solvent in the resin-free nano gold paste can be 20%.
[0037] In this invention, the sintering includes a first-stage sintering. During the first-stage sintering, the high-boiling-point solvent evaporates, and the gold framework is initially formed.
[0038] In this invention, the sintering atmosphere in the first stage is an inert atmosphere. An inert atmosphere prevents oxidation of the gold nanoparticles and the substrate. Preferably, the inert atmosphere is a nitrogen atmosphere. In one embodiment, the inert atmosphere can be flowing nitrogen. A flowing atmosphere maintains a low partial pressure of solvent vapor around the paste, thereby providing sufficient evaporation driving force, promoting the orderly diffusion and discharge of solvent from the paste according to a predetermined temperature program, and reducing closed pore defects caused by solvent retention or premature surface crusting.
[0039] In this invention, the heating rate of the first stage sintering is 5~20℃ / min, preferably 10~15℃ / min; as one embodiment of this invention, the heating rate of the first stage sintering can be 6℃ / min, 8℃ / min, 10℃ / min, 12℃ / min, 15℃ / min, or 18℃ / min. A heating rate within the above range allows the high-boiling-point solvent to evaporate slowly and completely, forming a preliminary porous gold powder framework and avoiding violent boiling.
[0040] In this invention, the sintering temperature of the first stage is 140~190℃, preferably 150~170℃; as one embodiment of this invention, the sintering temperature of the first stage can be 140℃, 150℃, 160℃, 170℃ or 180℃. A sintering temperature within the above range allows for sufficient evaporation of the high-boiling-point solvent.
[0041] In this invention, the holding time for the first stage sintering is 5-30 min, preferably 10-20 min; as one embodiment of this invention, the holding time for the first stage sintering can be 5 min, 10 min, 15 min, 20 min, or 25 min. The holding time for the first stage sintering is within the above range, allowing the high-boiling-point solvent to fully evaporate.
[0042] In this invention, the sintering includes a second-stage sintering. The second-stage sintering involves in-situ reactive sintering and solvent decomposition, forming sintering necks between the gold nanoparticles.
[0043] In this invention, the atmosphere for the second stage sintering is an inert atmosphere. Preferably, the inert atmosphere is a nitrogen atmosphere. In one embodiment of this invention, the inert atmosphere can be flowing nitrogen.
[0044] In this invention, the volume fraction of the reducing gas in the mixed gas is preferably 1-10%, more preferably 3-6%; as one embodiment of this invention, the volume fraction of the reducing gas in the mixed gas can be 2%, 3%, 5%, 7%, or 9%. A volume fraction of the reducing gas in the mixed gas within the above range is beneficial for reducing the oxides on the substrate surface, further improving the shear strength of the sintered body.
[0045] In this invention, the heating rate of the second-stage sintering is 1~5℃ / min, preferably 3~4℃ / min; as one embodiment of this invention, the heating rate of the second-stage sintering can be 1℃ / min, 1.5℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, or 5℃ / min. A heating rate within the above range allows for the complete decomposition of the in-situ reactive sintering flux, surface cleaning of the gold nanoparticles, and promotion of sintering neck formation.
[0046] In this invention, the sintering temperature of the second stage is 190~240℃, preferably 200~220℃; as one embodiment of this invention, the sintering temperature of the second stage can be 190℃, 200℃, 210℃, or 220℃. A sintering temperature within the above range allows for the complete decomposition of the in-situ reactive sintering flux.
[0047] In this invention, the holding time for the second stage sintering is 10-40 min, preferably 20-30 min; as one embodiment of this invention, the holding time for the second stage sintering can be 10 min, 15 min, 20 min, 25 min, or 30 min. The holding time for the second stage sintering within the above range allows for the complete decomposition of the in-situ reactive sintering flux.
[0048] In this invention, the sintering includes a third-stage sintering process. The third-stage sintering is a process of gold atom diffusion, bubble removal, and densification.
[0049] In this invention, the atmosphere for the third-stage sintering is an inert atmosphere. Preferably, the inert atmosphere is a nitrogen atmosphere. In one embodiment, the inert atmosphere can be flowing nitrogen. Using an inert atmosphere avoids re-oxidation of the gold surface without introducing additional reduction or chemical reaction interference, maintaining the sintered layer surface and grain boundaries in a highly active state, which is beneficial for atomic migration and pore closure. Continuous inert gas purging helps reduce the partial pressure of trace desorbed gases in the furnace cavity, promoting the outward diffusion and discharge of residual gases within the closed pores.
[0050] In this invention, the heating rate of the third-stage sintering is 0.5~3℃ / min, preferably 1~2℃ / min. A heating rate within this range can drive gold atoms to undergo bulk diffusion and grain boundary migration, thereby extruding micropores through grain growth and achieving densification.
[0051] In this invention, the sintering temperature of the third stage is 240~280℃, preferably 250~270℃; as one embodiment of this invention, the sintering temperature of the third stage can be 240℃, 250℃, 260℃, 270℃, or 280℃. A sintering temperature within the above range can densify the sintered body.
[0052] In this invention, the holding time for the third stage sintering is 30-120 min, preferably 60-90 min; as one embodiment of this invention, the holding time for the third stage sintering can be 40 min, 50 min, 60 min, 80 min, 90 min, or 100 min. Holding times within the above ranges for the third stage sintering can densify the sintered body.
[0053] In one embodiment of the present invention, the sintering apparatus can be an atmosphere sintering furnace, and the sintering pressure is atmospheric pressure.
[0054] This invention, by defining the solvent composition of the gold paste and combining it with a specific sintering process, precisely matches the kinetic requirements of solvent evaporation, flux decomposition, and final densification, thus widening and optimizing the originally narrow process window. This ensures a stable and thorough sintering process, reduces porosity, and improves thermal conductivity. By switching different sintering atmospheres at different sintering stages and coordinating with the heating rate, the invention fully utilizes the solvent evaporation kinetics to improve the degree of densification. Furthermore, by using an in-situ reactive sintering flux, an excellent surface cleaning and reaction environment is created, significantly improving sintering activity and interface quality, thereby enhancing shear strength.
[0055] The present invention also provides the application of the above-mentioned pressureless sintering method in the connection between chip and substrate, including: applying resin-free nano gold paste to the surface of the substrate and then attaching the chip, and then performing pressureless sintering.
[0056] In one embodiment of the present invention, the substrate can be a gold-plated substrate, and the resin-free nano-gold paste is applied to the gold-plated surface. The gold-plated substrate can achieve gold-gold interconnects, which is beneficial to improving the connection strength and thermal conductivity of the sintered body.
[0057] In this invention, the substrate is preferably pretreated before use. The pretreatment preferably includes one or more of the following: oxygen plasma cleaning, argon-hydrogen plasma cleaning, formic acid vapor fumigation, and coating with a soldering flux. Pretreatment removes contaminants and oxides from the substrate surface, which is beneficial for the bonding between the substrate and the solder paste, and further improves shear strength.
[0058] In one embodiment of the present invention, the oxygen plasma cleaning and argon-hydrogen plasma cleaning can be performed for 3 minutes; the formic acid vapor fumigation temperature can be 120°C and the time can be 5 minutes.
[0059] As one embodiment of the present invention, the chip may be a gold-backed chip.
[0060] The present invention does not impose any particular limitations on the operation of attaching the chip, as long as the chip can be attached stably and a qualified component is obtained.
[0061] The application provided by this invention enables high-quality connection between chips and substrates, meeting the needs of high-end devices.
[0062] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0063] Example 1 A pressureless sintering method for resin-free nano-gold paste, comprising the following steps: A composite solvent was prepared by mixing diethylene glycol butyl ether and N-methylformamide at a volume ratio of 1:1, and a resin-free nano-gold paste was prepared by mixing the composite solvent and nano-gold powder at a mass ratio of 2:8. The nano-gold powder consisted of gold nanoparticles with a surface modified with octylthiol and an average particle size of 300 nm. The gold-plated DBC substrate was cleaned with argon-hydrogen plasma for 3 minutes. Then, resin-free nano gold paste was applied to the surface of the gold-plated DBC substrate in a cross pattern. A 3×3mm back gold chip was then attached to obtain the component. The components were placed in an atmosphere sintering furnace for pressureless sintering, during which the furnace pressure was atmospheric pressure. First stage sintering: In a nitrogen atmosphere, the temperature is increased to 170℃ at a rate of 10℃ / min and held for 15min; Second stage sintering: In a nitrogen atmosphere, the temperature is increased to 220℃ at a rate of 2℃ / min and held for 25min; The third stage of sintering: the temperature is increased to 260℃ at a rate of 1℃ / min in a nitrogen atmosphere and held for 60min.
[0064] Example 2 A pressureless sintering method for resin-free nano-gold paste, comprising the following steps: A composite solvent was prepared by mixing diethylene glycol butyl ether and N-methylformamide at a volume ratio of 1:1, and a resin-free nano-gold paste was prepared by mixing the composite solvent and nano-gold powder at a mass ratio of 2:8. The nano-gold powder consisted of gold nanoparticles with a surface modified with octylthiol and an average particle size of 300 nm. The gold-plated frame was fumigated with formic acid vapor at 120°C for 5 minutes. Then, resin-free nano gold paste was applied to the surface of the gold-plated frame in a star pattern. A 3×3mm back gold chip was then attached to obtain the component. The components were placed in an atmosphere sintering furnace for pressureless sintering, during which the furnace pressure was atmospheric pressure. First stage sintering: In a nitrogen atmosphere, the temperature is increased to 160℃ at a rate of 8℃ / min and held for 20min; Second stage sintering: In a nitrogen atmosphere, the temperature is increased to 210℃ at a rate of 1.5℃ / min and held for 30min; The third stage of sintering: In a nitrogen atmosphere, the temperature is increased to 250℃ at a rate of 0.5℃ / min and held for 90min.
[0065] Example 3 A pressureless sintering method for resin-free nano-gold paste, comprising the following steps: A composite solvent was prepared by mixing diethylene glycol butyl ether and N-methylformamide at a volume ratio of 1:1, and a resin-free nano-gold paste was prepared by mixing the composite solvent and nano-gold powder at a mass ratio of 2:8. The nano-gold powder consisted of gold nanoparticles with a surface modified with octylthiol and an average particle size of 300 nm. 20mg of no-clean solder paste was applied to the surface of the gold-plated substrate, and then resin-free nano gold paste was applied to the surface of the gold-plated substrate in a star pattern. A 3×3mm back gold chip was then attached to obtain the component. The components were placed in an atmosphere sintering furnace for pressureless sintering, during which the furnace pressure was atmospheric pressure. First stage sintering: In a nitrogen atmosphere, the temperature is increased to 150℃ at a rate of 15℃ / min and held for 10min; Second stage sintering: In a nitrogen atmosphere, the temperature is increased to 200℃ at a rate of 3℃ / min and held for 40min; The third stage of sintering: In a nitrogen atmosphere, the temperature is increased to 240℃ at a rate of 2℃ / min and held for 80min.
[0066] Comparative Example 1 A pressureless sintering method for resin-free nano-gold paste, using the same raw materials as in Example 1, differs in that the first stage involves heating to 150°C at a rate of 25°C / min and holding at that temperature for 10min.
[0067] Comparative Example 2 A pressureless sintering method for resin-free nano-gold paste, using the same raw materials as in Example 1, differs in that the sintering process is as follows: in a nitrogen atmosphere, the temperature is uniformly raised to 260°C at a rate of 5°C / min and held for 60 min.
[0068] Test Example 1 The shear strength and thermal conductivity of the sintered bodies obtained in Examples 1-3 and Comparative Examples 1-2 were tested, and the test results are recorded in Table 1.
[0069] Shear strength test: Fix the sintered component on the stage, so that the blade is close to the side root of the chip and the height is parallel to the substrate; set the shearing height, test speed and safe load; the blade moves forward at a constant speed in the horizontal direction, parallel to the substrate and "scoops" towards the chip; record the pushing force when the chip is pushed away.
[0070] The thermal conductivity test method is as follows: Sintered silver paste is printed onto a flat polytetrafluoroethylene (PTFE) vinyl material, sintered according to the actual process, and the sintered silver sheet is polished into a circular disc with a diameter of 12.7 mm and a thickness of 1-3 mm, with a parallelism of <0.01 mm on both sides. A thin graphite layer is sprayed onto the back side to obtain the test sample. The test sample is placed in a sample holder, ensuring that the laser, the test sample, and the infrared detector are coaxial. Under an inert gas environment, a laser pulse irradiates the back side of the test sample, and the infrared detector records the temperature rise curve of the front side. The software calculates the thermal diffusivity based on the temperature rise half-life, and combines it with specific heat capacity and density to obtain the thermal conductivity. Thermal conductivity = thermal diffusivity. Specific heat capacity density.
[0071] Table 1. Performance test records of sintered bodies obtained by different methods.
[0072] As can be seen from Table 1, the shear strength and thermal conductivity of the sintered bodies obtained in the examples are higher than those in the comparative examples.
[0073] Test Example 2 The cross-sections of the sintered bodies obtained from Examples 1-3 and Comparative Examples 1-2 were observed using a scanning electron microscope, and the SEM images are shown below. Figures 1-5 As shown, the porosity was calculated and statistically analyzed by dividing the pore area by the total area, and the results were 3.5%, 4.8%, 5.5%, 9.1%, and 8.1%, respectively.
[0074] contrast Figure 1 and Figure 5 It can be seen that cracks appeared after sintering in Comparative Example 2, indicating that the heating rate was too fast during the neck formation and densification stages, which was not conducive to the densification of the sintered body.
[0075] As can be seen from the above embodiments and comparative examples, the pressureless sintering method provided by the present invention can reduce porosity and improve shear strength.
[0076] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A pressureless sintering method for resin-free nano-gold paste, characterized in that, This includes the first stage of sintering, the second stage of sintering, and the third stage of sintering, performed sequentially. The first stage of sintering includes: heating the resin-free nano gold paste to 140-190°C in an inert atmosphere at a heating rate of 5-20°C / min, and holding it at that temperature for 5-30 minutes; The second stage of sintering includes: in an inert atmosphere, continuing to heat to 190~240℃ at a heating rate of 1~5℃ / min, and holding at that temperature for 10~40min; The third stage of sintering includes: in an inert atmosphere, continuing to heat to 240~280℃ at a heating rate of 0.5~3℃ / min, and holding at that temperature for 30~120min; The resin-free nano-gold paste comprises nano-gold powder and a composite solvent; the composite solvent comprises a high-boiling-point solvent and an in-situ reactive sintering aid solvent; the boiling point of the high-boiling-point solvent is 180~350℃; the in-situ reactive sintering aid solvent is a solvent that can decompose upon heating to produce reducing gas, and the decomposition temperature is 150~250℃.
2. The pressureless sintering method according to claim 1, characterized in that, The mass ratio of the high-boiling-point solvent to the in-situ reactive sintering flux is (3~7):(3~7).
3. The pressureless sintering method according to claim 1, characterized in that, The high-boiling-point solvent has an evaporation rate of 2 to 5 relative to butyl acetate.
4. The pressureless sintering method according to claim 3, characterized in that, The high-boiling-point solvent includes one or more of alcohol solvents, glycol ether solvents, and ester solvents.
5. The pressureless sintering method according to claim 1, characterized in that, The in-situ reactive sintering co-solvent has an evaporation rate of 0.02 to 0.5 relative to butyl acetate.
6. The pressureless sintering method according to claim 5, characterized in that, The in-situ reactive sintering flux includes one or more of nitrogen-containing organic solvents and sulfoxide solvents.
7. The pressureless sintering method according to claim 1, characterized in that, The gold nanoparticles are gold nanoparticles with surface-modified organic ligands; the organic ligands include terminal thiol groups and / or terminal amino groups.
8. The pressureless sintering method according to claim 1, characterized in that, The inert atmosphere is a nitrogen atmosphere.
9. The application of the pressureless sintering method according to any one of claims 1 to 8 in the connection between a chip and a substrate, characterized in that, include: After applying resin-free nano-gold paste to the substrate surface, the chip is attached and then pressureless sintering is performed.
10. The application according to claim 9, characterized in that, The substrate is pretreated before use. The pretreatment includes one or more of the following: oxygen plasma cleaning, argon-hydrogen plasma cleaning, formic acid vapor fumigation, and coating with solder flux.