Rechargeable battery, method for manufacturing rechargeable battery, and method for manufacturing electrodes of rechargeable battery.
By transferring electrode slurry onto a perforated metal foil and applying pressure, the problem of electrode material leakage was solved, enabling efficient electrode manufacturing and improving battery capacity and energy density.
Patent Information
- Application Number
- CN202480090825.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies make it difficult to effectively form electrodes for rechargeable batteries using perforated metal foil because the electrode material leaks through the through-holes during coating, leading to component breakage or wrinkling during manufacturing and affecting productivity.
The process involves applying electrode paste to a substrate and drying it to form an electrode coating. The substrate is then stacked onto a perforated metal foil and pressure is applied to transfer the electrode coating onto the perforated metal foil. Amorphous carbon or carbon fiber is used as a thickener and binder to optimize the manufacturing process.
This technology enables the easy fabrication of rechargeable battery electrodes using perforated metal foil, reducing component breakage and wrinkling during manufacturing, maintaining the physical strength of the electrodes, and increasing battery capacity and energy density.
Smart Images

Figure CN123076930A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to rechargeable batteries, methods for manufacturing rechargeable batteries, and methods for manufacturing electrodes for rechargeable batteries. Background Technology
[0002] Rechargeable batteries are known for their high energy density, rapid charging and discharging capabilities, and long expected lifespan. For example, it is well known that lithium-ion batteries can be made from a variety of materials, such as ternary lithium-ion batteries using nickel, manganese, and cobalt as cathode materials, and lithium iron phosphate batteries using lithium iron phosphate (LFP: LiFePO4) as cathode material (see, for example, Patent Document 1).
[0003] Existing technology
[0004] Patent documents
[0005] [Patent Document 1] Japanese Unexamined Patent Application Publication No. 2017-212045 Summary of the Invention
[0006] Technical issues
[0007] As a method to further increase the energy density of such rechargeable batteries, increasing their capacity and reducing their weight can be considered. Increasing the capacity of rechargeable batteries is effectively achieved by forming a thick coating of electrode material; however, the physical strength of the electrodes may decrease. Reducing the weight of rechargeable batteries is effectively achieved by making the components thinner; however, during manufacturing, component breakage or wrinkling can occur, leading to reduced productivity. Therefore, the use of perforated metal foil with through-holes is conceivable. However, it is difficult to form electrodes using perforated metal foil because the electrode material leaks through the through-holes when coated onto the perforated metal foil.
[0008] This invention was made with these points in mind, and the object of this invention is to make it possible to easily manufacture electrodes for rechargeable batteries using perforated metal foil.
[0009] Technical solution
[0010] A first aspect of the present invention provides a method for manufacturing an electrode for a rechargeable battery, the method comprising the steps of: forming an electrode slurry comprising (i) an electrode active material, (ii) amorphous carbon or carbon fiber, (iii) a thickener and (iv) a binder; forming an electrode coating on a surface of a substrate by applying the electrode slurry to a substrate and drying the electrode slurry; and transferring the electrode coating onto the perforated metal foil by stacking the substrate on which the electrode coating is formed on its surface onto a surface of a perforated metal foil having a plurality of through holes and applying pressure thereto.
[0011] The thickener may be 1 wt% or less of carboxymethyl cellulose (CMC). The adhesive may be 1 wt% or less of styrene-butadiene rubber (SBR).
[0012] Forming an electrode coating on the surface of a substrate may include: providing two substrates; and forming an electrode coating on the surfaces of the two substrates by applying an electrode paste to the respective substrates and drying the electrode paste, and transferring the electrode coating onto a perforated metal foil may include: transferring two electrode coatings onto the two surfaces of the perforated metal foil by stacking the two substrates onto both surfaces of a perforated metal foil in which a plurality of through holes are formed and applying pressure, wherein each of the two substrates has an electrode coating formed on its surface.
[0013] Transferring an electrode coating onto a perforated metal foil can include transferring the electrode coating onto the perforated metal foil using a calender, which applies pressure by passing a stacked substrate and the perforated metal foil between metal rolls.
[0014] A second aspect of the invention provides a method for manufacturing a rechargeable battery, comprising the steps of: forming a cathode comprising (i) a cathode active material and (ii) amorphous carbon or carbon fibers; forming an anode comprising (i) an anode active material and (ii) amorphous carbon or carbon fibers; and sealing the cathode, anode, and a predetermined electrolyte in a predetermined container and sealing the container, wherein forming at least one of the cathode or forming the anode comprises each step of the method for manufacturing an electrode of a rechargeable battery according to the first aspect of the invention.
[0015] A third aspect of the present invention provides a rechargeable battery comprising: a cathode comprising a cathode material containing (i) a cathode active material and (ii) amorphous carbon or carbon fibers; an anode comprising an anode material containing (i) an anode active material and (ii) amorphous carbon or carbon fibers; and an electrolyte, wherein at least one of the cathode or anode further comprises a perforated metal foil having a plurality of through holes, and the cathode material or anode material covers at least one surface of the perforated metal foil while filling the plurality of through holes of the perforated metal foil.
[0016] Technical effect
[0017] According to the present invention, electrodes for rechargeable batteries can be easily manufactured using perforated metal foil. Attached Figure Description
[0018] Figure 1 An example of a schematic configuration of a lithium iron phosphate battery 10 according to this embodiment is shown.
[0019] Figure 2 An example of a perforated metal foil 5 according to this embodiment is shown.
[0020] Figure 3 An example of the manufacturing process of the lithium iron phosphate battery 10 according to this embodiment is shown.
[0021] Figure 4 An example of transferring an electrode coating onto a perforated metal foil 5 according to this embodiment is shown.
[0022] Figure 5 An example configuration of the lithium iron phosphate battery 10 according to this embodiment is shown.
[0023] Figure 6 An example of the assembly process of the lithium iron phosphate battery 10 according to this embodiment is shown.
[0024] Figure 7 An example of the charge-discharge characteristics of the lithium iron phosphate battery 10 according to this embodiment is shown.
[0025] Figure 8 An example of the charge-discharge cycle characteristics of the lithium iron phosphate battery 10 according to this embodiment is shown. Detailed Implementation
[0026] <Illustrative configuration of lithium iron phosphate battery 10>
[0027] In this example, lithium iron phosphate batteries will be described as an example of rechargeable batteries. Figure 1 An example of a schematic configuration of a lithium iron phosphate battery 10 according to this embodiment is shown. The lithium iron phosphate battery 10 is a rechargeable secondary battery. The lithium iron phosphate battery 10 includes a cathode 20, an anode 30, a separator 40, an electrolyte 50, and a casing 60.
[0028] Cathode 20 comprises lithium, iron, phosphorus, and conductive materials. The active material of cathode 20 is lithium iron phosphate. Cathode 20 is an electrode formed from, for example, lithium iron phosphate, amorphous carbon, and a binder as cathode materials. Here, amorphous carbon is a conductive additive, such as Ketjenblack or acetylene black. Amorphous carbon can be carbon fiber. The conductive additive is a material used to reduce the resistance of the electrode when forming the electrode of a lithium-ion battery. The binder is PVDF (polyvinylidene fluoride), SBR (styrene-butadiene rubber), etc.
[0029] Anode 30 comprises graphite and a conductive material. The active material of anode 30 is graphite. Anode 30 is an electrode formed from amorphous carbon, a thickener such as CMC (carboxymethyl cellulose), or a binder as the anode material. Amorphous carbon can be carbon fiber. Examples of binders include PVDF (polyvinylidene fluoride) and SBR (styrene-butadiene rubber).
[0030] The separator 40 separates the cathode 20 and the anode 30 while allowing lithium ions to move between them. The separator 40 is, for example, a membrane with a thickness of about tens of μm and having multiple pores of 1 μm or smaller. The separator 40 is formed of, for example, polyethylene, polypropylene, etc.
[0031] Electrolyte 50 converts lithium ions into cations and anions, allowing ion migration. Electrolyte 50 can be a solvent, solution, gel, etc. For example, electrolyte 50 is an organic electrolyte solution in which approximately 1 mol of a lithium salt (LiPF6, LiBF4, LiClO4, etc.) is dissolved in an organic solvent. Examples of organic solvent materials include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl ethyl carbonate (EMC).
[0032] The housing 60 houses the cathode 20, anode 30, diaphragm 40, and electrolyte 50. The housing 60 is preferably a container that seals the cathode 20, anode 30, diaphragm 40, and electrolyte 50. The housing 60 includes a positive terminal 61 electrically connected to the cathode 20 and a negative terminal 62 electrically connected to the anode 30.
[0033] When a power source is connected to the positive terminal 61 and the negative terminal 62, the lithium iron phosphate battery 10 is charged. When the lithium iron phosphate battery 10 is charged, electrons migrate from the cathode 20 to the anode 30, and lithium ions migrate from the cathode 20 through the electrolyte 50 and accumulate in the anode 30, thereby creating a potential difference between the cathode 20 and the anode 30.
[0034] On the other hand, when a discharge circuit, such as a load, is connected to the positive terminal 61 and the negative terminal 62, the lithium iron phosphate battery 10 discharges. When the lithium iron phosphate battery 10 discharges, electrons flow from the anode 30 to the cathode 20 through the discharge circuit, and lithium ions that have accumulated in the anode 30 migrate to the cathode 20 through the electrolyte 50 and are reduced to lithium oxide by combining with electrons in the cathode 20.
[0035] In the lithium iron phosphate battery 10 according to this embodiment, a perforated metal foil is used as the electrode material for at least one of the cathode 20 or the anode 30. The perforated metal foil is a metal foil in which multiple through-holes are formed, and it is a material that can reduce the weight of the metal foil while maintaining strength. The metal foil is copper foil, aluminum foil, etc.
[0036] Figure 2An example of a perforated metal foil 5 according to this embodiment is shown. The perforated metal foil 5 may have a plurality of through holes having the same shape, or conversely, it may have a plurality of through holes having different shapes. Furthermore, the perforated metal foil 5 may have polygonal through holes formed in a mesh pattern. Preferably, the through holes of the perforated metal foil 5 are formed in a complex shape, allowing electrode material to easily enter and remain therein. Additionally, the metal portion of the perforated metal foil 5 can be formed by weaving metal wires together.
[0037] Conventional methods for manufacturing electrodes involve coating electrode material onto a metal foil. However, when using a perforated metal foil 5, the electrode material leaks through the perforations when coated onto one surface, making it difficult to form an electrode using conventional manufacturing methods. It is also conceivable to coat the electrode material onto both surfaces of the perforated metal foil 5. However, when the perforated metal foil 5 is conveyed after coating, a portion of the coated electrode material flows out, making it difficult to form an electrode even when coating both surfaces.
[0038] Therefore, in the method for manufacturing an electrode according to this embodiment, electrode material is formed on the perforated metal foil 5 by transferring electrode material onto the perforated metal foil 5. As described above, the inventors have discovered a manufacturing method that easily forms an electrode with reduced weight by using the perforated metal foil 5. This method can suppress the reduction of the physical strength of the electrode and can reduce the occurrence of breakage, wrinkle formation, and hole formation in the component during the manufacturing process. Therefore, the method for manufacturing an electrode discovered by the inventors will be described below using a lithium iron phosphate battery 10 as an example.
[0039] <Manufacturing process of lithium iron phosphate battery 10>
[0040] Figure 3 An example of the manufacturing process of the lithium iron phosphate battery 10 according to this embodiment is shown. In the lithium iron phosphate battery 10 according to this embodiment, an example using a perforated metal foil 5 as the anode 30 will be described. In this embodiment, as an example of the lithium iron phosphate battery 10, the manufacturing process of a coin-shaped battery having a diameter of approximately 14 mm will be described.
[0041] First, cathode 20 and anode 30 are formed. For example, cathode 20 and anode 30 are formed separately. Cathode 20 and anode 30 may be formed simultaneously in time, or they may be formed at different times. For example, anode 30 may be formed after cathode 20, or alternatively, cathode 20 may be formed after anode 30. Figure 3 An example is shown where the cathode 20 and anode 30 are formed simultaneously in time.
[0042] First, the formation of the cathode 20, comprising lithium, iron, phosphorus, and amorphous carbon, will be described. As an example of the film composition of the cathode 20, the weight ratio of lithium iron phosphate, amorphous carbon, and PVDF is 91:4:5. The amorphous carbon in the cathode material can be another conductive material. For example, the amorphous carbon in the cathode material is carbon fiber.
[0043] More specifically, firstly, the LFP cathode material, composed of lithium, iron, and phosphorus, is vacuum dried (S81). For example, the LFP cathode material is placed in a vacuum chamber or the like, and the chamber is evacuated by a vacuum pump and then the material is kept at a temperature of about 120°C for about 8 hours to dry it.
[0044] Next, dried LFP cathode material and amorphous carbon are added to a solution in which PVDF is dissolved in a solvent such as N-methylpyrrolidone (NMP) and a dispersant is added, and the resulting mixture is stirred to form a cathode slurry (S82). The amount of dispersant is, for example, about 2 wt% relative to the cathode material. Then, NMP is added to the cathode slurry and stirred until the cathode slurry reaches a predetermined concentration. The predetermined concentration is, for example, a solid content of 45 wt%.
[0045] Next, cathode 20 is formed by applying a cathode paste containing cathode materials (including lithium iron phosphate and amorphous carbon) to a substrate and drying the cathode paste (S83). The substrate is, for example, an aluminum foil coated with graphite. The graphite film thickness is, for example, about 1 μm, and the aluminum foil thickness is about 15 μm. Preferably, only a predetermined amount of cathode paste is applied to the substrate to form a predetermined dry film thickness. The predetermined dry film thickness is, for example, about 80 μm. The cathode paste is preferably applied using a die coater or the like.
[0046] The applied cathode slurry is dried in air at a temperature of about 130°C for about 15 minutes to form a coating of cathode material with a dry film thickness. The cathode material coating is then pressed to form a predetermined thickness, for example, about 70 μm. The cathode 20 is formed by cutting the cathode material coating with this predetermined thickness into a predetermined shape.
[0047] Next, the formation of the anode 30, comprising graphite and amorphous carbon, will be described. As an example of the film composition of the anode 30, the weight ratio of graphite, amorphous carbon, CMC, and SBR is 96.2:2.6:0.6:0.6. The amorphous carbon is carbon black, Ketjen black, acetylene black, etc. The amorphous carbon of the anode material can be another conductive material. For example, the amorphous carbon of the anode material is carbon fiber.
[0048] More specifically, first, an anode slurry (S84) is formed. The anode slurry is an electrode slurry comprising (i) an electrode active material, (ii) amorphous carbon or carbon fibers, (iii) a thickener, and (iv) a binder. The thickener is, for example, 1 wt% or less of CMC. The binder is, for example, 1 wt% or less of SBR.
[0049] For example, a predetermined amount of graphite powder and a predetermined amount of amorphous carbon are added to an aqueous solution of CMC, and the resulting mixture is stirred. Then, a predetermined amount of SBR solution is added and stirred to form an anode slurry. As an example, the aqueous solution of CMC contains 2 wt% CMC. Distilled water is then added to the anode slurry, and the resulting mixture is stirred until the anode slurry reaches a predetermined concentration. The predetermined concentration is, for example, a solids content of 53 wt%. The anode slurry is a high-concentration slurry with a higher concentration than that used in conventional electrodes.
[0050] Next, an electrode coating is formed on the surface of the substrate by applying an anolyte to the substrate and drying the anolyte (S85). The substrate is, for example, a copper foil substrate with a thickness of about 10 μm. Preferably, only a predetermined amount of anolyte is applied to the substrate to form an electrode coating with a predetermined dry film thickness. The predetermined dry film thickness is, for example, about 100 μm. The anolyte is preferably applied using a dip coater or the like. The applied anolyte is dried in air at a temperature of about 80°C for about 10 minutes, for example, to form the electrode coating.
[0051] Next, the electrode coating is transferred onto the perforated metal foil 5 by stacking a substrate with an electrode coating formed on its surface onto one surface of the perforated metal foil 5 having multiple through holes and applying pressure (S86). The perforated metal foil 5 is, for example, a... Figure 2 The perforated copper foil shown has an aperture ratio of 58% and a thickness of 50 μm. For example, the stacked substrate and the perforated metal foil 5 are pressed by a rolling mill, which applies pressure by passing the object to be pressed between two metal rollers.
[0052] Figure 4 An example of transferring an electrode coating onto a perforated metal foil 5 according to this embodiment is shown. It has been found that the electrode coating can be easily transferred from the substrate to the perforated metal foil 5 by applying pressure with a press. Figure 4 The results of calendering performed at room temperature with a gap of 50 μm between the two metal rolls are shown.
[0053] It should be noted that, since there are cases where transfer cannot be achieved when the gap is set to 100 μm, a gap of 40 μm or more and 80 μm or less is preferred. The gap can be 40 μm or more and 60 μm or less. Furthermore, since transfer cannot be achieved in the calender at a linear pressure of approximately 400 kgf / cm, a linear pressure of 450 kgf / cm or higher, or 500 kgf / cm or higher, is preferred.
[0054] The thickness of the anode material formed by transferring the electrode coating onto the perforated metal foil 5 is, for example, about 75 μm. The anode 30 is formed by cutting this anode material into a predetermined shape (S87).
[0055] After forming the cathode 20 and anode 30, the cathode 20, anode 30 and predetermined electrolyte 50 are sealed in a predetermined container, and the container is sealed to assemble the lithium iron phosphate battery 10 (S88). Thus, the lithium iron phosphate battery 10 can be formed.
[0056] <Configuration Example of Lithium Iron Phosphate Battery 10>
[0057] Figure 5 An example configuration of the lithium iron phosphate battery 10 according to this embodiment is shown. Figure 6 An example of the assembly process of the lithium iron phosphate battery 10 according to this embodiment is shown. In other words, Figure 5 and Figure 6 It shows the assembly in detail. Figure 4 The diagram shows the operation of S88 of the lithium iron phosphate battery 10 described in the document.
[0058] The lithium iron phosphate battery 10 also includes a casing 11, a liner 12, a gasket 13, a washer 14, and a cover 15. The casing 60 is formed by assembling the casing 11 and the cover 15 together. Before assembling the lithium iron phosphate battery 10, it is preferable to dry the cathode 20 and anode 30 using a vacuum chamber or similar method. In this case, for example, the cathode 20 is dried at approximately 110°C for approximately 8 hours, and the anode 30 is dried at approximately 90°C for approximately 8 hours. It is assumed that the separator 40 has been cut into a predetermined shape.
[0059] First, the gasket 12 is attached to the housing 11 (S91). Next, the cathode 20 is placed in the housing 11 (S92). Then, the diaphragm 40 is placed on the cathode 20 in the housing 11 (S93). The diaphragm 40 is, for example, a polyolefin microporous membrane. Next, a predetermined amount of electrolyte solution is dripped onto the diaphragm 40 in the housing 11 using a pipette or the like (S94). The electrolyte solution is, for example, an organic electrolyte solution in which approximately 1 mol of lithium salt (LiPF6) is dissolved in EC, DMC, and EMC in a 1:1:1 weight ratio. Preferably, the electrolyte solution is dripped in such a way that the cathode 20, anode 30, and diaphragm 40 are fully immersed in the electrolyte solution.
[0060] Next, the anode 30 is placed on the diaphragm 40 containing the electrolyte solution (S95). Next, the gasket 13 is placed on the anode 30 in the housing 11 (S96). Next, the gasket 14 is placed on the gasket 13 in the housing 11 (S97). Next, the cover 15 is placed on the gasket 12 attached to the housing 11 (S98). Next, the cover 15 is pressed down from above, and the housing 11 and the cover 15 are assembled together via the gasket 12 (S99).
[0061] As a result, a lithium iron phosphate battery 10 can be assembled. Preferably, assembly operations S91 to S99 are performed in an argon atmosphere or a dry atmosphere having a moisture dew point of -50°C or lower. The characteristics of the lithium iron phosphate battery 10 formed as described above will be described.
[0062] <Examples of the characteristics of lithium iron phosphate battery 10>
[0063] Figure 7 An example of the charge-discharge characteristics of the lithium iron phosphate battery 10 according to this embodiment is shown. Figure 7 It shows the reference Figures 4 to 6 The charging and discharging characteristics of the lithium iron phosphate battery 10 manufactured using the described manufacturing and assembly processes are presented. Figure 7 In the diagram, the horizontal axis represents capacitance, and the vertical axis represents voltage and current. From... Figure 7 As can be seen, the charging voltage curve, discharging voltage curve, and charging current curve exhibit characteristics comparable to those of conventional lithium iron phosphate batteries.
[0064] Figure 8 An example of the charge-discharge cycle characteristics of the lithium iron phosphate battery 10 according to this embodiment is shown. The charge-discharge cycle characteristics represent the characteristics under repeated conditions, such as... Figure 7 The charge / discharge cycles shown are plotted simultaneously, with the discharge capacity and charge capacity plotted at the end of each cycle. From Figure 8 As can be seen, the cycle characteristics did not suddenly deteriorate, and the lithium iron phosphate battery 10 fully demonstrated its function as a rechargeable battery.
[0065] As can be seen from the above, the electrode of the lithium iron phosphate battery 10 can be easily manufactured using the perforated metal foil 5 according to this embodiment. Therefore, the weight of the electrode can be reduced while maintaining a thickness comparable to that of conventional electrode components. Furthermore, the perforated metal foil 5 can reduce the occurrence of breakage, wrinkle formation, and hole formation in the component during manufacturing, and can maintain the physical strength of the electrode. Therefore, the electrode using the perforated metal foil 5 allows for a thicker electrode material than that applied in conventional electrodes, and can increase the capacity of the rechargeable battery.
[0066] It should be noted that in conventional electrodes, the solid content is approximately 45% to ensure close contact between the slurry and the substrate. Conversely, when using the perforated metal foil 5, a higher slurry concentration allows the electrode coating to more easily adhere to the perforated metal foil 5. As a result, the solid content of the slurry can be increased to 50% or more. Therefore, when using the perforated metal foil 5, it becomes possible to form an electrode with the same thickness as a conventional electrode while increasing the concentration of the electrode material, thereby enabling the rechargeable battery to have a higher energy density than conventional electrodes.
[0067] In the lithium iron phosphate battery 10 according to this embodiment described above, an example has been provided in which the electrode coating is transferred to one surface of the perforated metal foil 5; however, this embodiment is not limited thereto. Optionally, the electrode coating can be transferred to both surfaces of the perforated metal foil 5.
[0068] For example, in Figure 3 In step S85, two substrates are provided, and an electrode coating is formed on the surface of the respective substrates by applying electrode paste to the two substrates and drying the electrode paste. Then, in Figure 3 In step S86, two substrates, each having an electrode coating formed on its surface, are stacked onto two surfaces (i.e., one surface and the other surface of the perforated metal foil 5) having multiple through holes therein, and pressure is applied to transfer the two electrode coatings to the corresponding surfaces of the perforated metal foil 5. As a result, an electrode having electrode coatings formed on the two surfaces of the perforated metal foil 5 can be formed.
[0069] In the lithium iron phosphate battery 10 according to this embodiment, an example has been provided where the electrode using the perforated metal foil 5 is the anode 30; however, this embodiment is not limited to this. In the lithium iron phosphate battery 10, the electrode using the perforated metal foil 5 can be the cathode 20. Furthermore, in the lithium iron phosphate battery 10, the electrodes using the perforated metal foil 5 can be both the cathode 20 and the anode 30.
[0070] The lithium iron phosphate battery 10 according to this embodiment has been described above as an example of manufacturing a coin-type battery, but this embodiment is not limited thereto. Other structures can be used, as long as electrodes with perforated metal foil 5 are provided on at least one of the cathode or anode.
[0071] The lithium iron phosphate battery 10 according to this embodiment is an example of a rechargeable battery having electrodes using perforated metal foil 5, and the rechargeable battery is not limited to the lithium iron phosphate battery 10. The electrodes using perforated metal foil 5 can be used as electrodes for rechargeable batteries such as ternary lithium-ion batteries using nickel, manganese, and cobalt as cathode materials, as well as electrodes for rechargeable batteries that can be made of various materials.
[0072] This rechargeable battery includes: a cathode 20 having a cathode material comprising (i) a cathode active material and (ii) amorphous carbon or carbon fibers; an anode 30 having an anode material comprising (i) an anode active material and (ii) amorphous carbon or carbon fibers; and an electrolyte 50. At least one of the cathode 20 or anode 30 further includes a perforated metal foil 5 having a plurality of through-holes. Here, the cathode material or anode material covers at least one surface of the perforated metal foil 5 while filling the plurality of through-holes of the perforated metal foil 5.
[0073] This disclosure is explained based on exemplary embodiments. The technical scope of this disclosure is not limited to the scope explained in the above embodiments, and various changes and modifications can be made within the scope of this disclosure. For example, all or part of the apparatus may be configured with any functionally or physically distributed or integrated units. Furthermore, new exemplary embodiments resulting from any combination thereof are included in the exemplary embodiments. Moreover, the effects of new exemplary embodiments resulting from combinations also have the effects of the original exemplary embodiments.
[0074] [Symbol Description]
[0075] 5. Perforated metal foil
[0076] 10. Lithium iron phosphate batteries
[0077] 11. Shell
[0078] 12 Padding
[0079] 13 Gaskets
[0080] 14 Washers
[0081] 15 lids
[0082] 20 Cathode
[0083] 30 Anode
[0084] 40 Diaphragm
[0085] 50 Electrolytes
[0086] 60. Outer shell
[0087] 61 Positive extremes
[0088] 62 Negative extremes
Claims
1. A method for manufacturing electrodes for a rechargeable battery, the method comprising the following steps: Forming an electrode slurry comprising (i) an electrode active material, (ii) amorphous carbon or carbon fiber, (iii) a thickener and (iv) a binder; An electrode coating is formed on the surface of the substrate by applying the electrode paste to the substrate and drying the electrode paste. as well as The electrode coating is transferred onto the perforated metal foil by stacking the substrate on which the electrode coating is formed on the surface onto a surface of a perforated metal foil having multiple through holes and applying pressure thereon.
2. The method for manufacturing electrodes for a rechargeable battery according to claim 1, wherein, The thickener is 1 wt% or less carboxymethyl cellulose (CMC).
3. The method for manufacturing electrodes for a rechargeable battery according to claim 1, wherein, The adhesive is 1 wt% or less styrene-butadiene rubber (SBR).
4. The method for manufacturing electrodes for a rechargeable battery according to claim 1, wherein, Forming the electrode coating on the surface of the substrate includes: providing two substrates; and forming the electrode coating on the surfaces of the two substrates by applying the electrode paste to the respective substrates and drying the electrode paste. Transferring the electrode coating onto the perforated metal foil includes: transferring two electrode coatings onto two surfaces of the perforated metal foil by stacking the two substrates onto one surface and the other surface of the perforated metal foil in which the plurality of through holes are formed and applying pressure, wherein each of the two substrates has the electrode coating formed on its surface.
5. The method for manufacturing electrodes for a rechargeable battery according to claim 1, wherein, Transferring the electrode coating onto the perforated metal foil includes transferring the electrode coating onto the perforated metal foil using a calender, the calender applying pressure by passing the stacked substrate and the perforated metal foil between metal rollers.
6. A method for manufacturing a rechargeable battery, comprising the following steps: The cathode is formed comprising (i) a cathode active material and (ii) amorphous carbon or carbon fiber; Forming an anode comprising (i) an anode active material and (ii) amorphous carbon or carbon fiber; as well as The cathode, the anode, and the predetermined electrolyte are sealed in a predetermined container, and the container is sealed, wherein forming at least one of the cathode or the anode includes each step of the method for manufacturing the electrode of the rechargeable battery according to any one of claims 1 to 5.
7. A rechargeable battery, comprising: Cathode, including cathode materials containing (i) cathode active material and (ii) amorphous carbon or carbon fiber; Anodes include anode materials containing (i) anodic active materials and (ii) amorphous carbon or carbon fibers; as well as The electrolyte, wherein at least one of the cathode or the anode further comprises a perforated metal foil having a plurality of through holes, and The cathode material or the anode material covers at least one surface of the perforated metal foil and fills the plurality of through holes in the perforated metal foil.
Citation Information
Patent Citations
Battery
JP2017212045A