A defoamer for high weather-resistant coatings and its preparation method
By combining modified polysiloxane with nano-titanium dioxide, a defoamer for high weather-resistant coatings with a SiO2 coating layer is formed, solving the problems of uneven dispersion and interface migration of defoamers in high weather-resistant coatings, and achieving the effects of rapid defoaming, continuous foam suppression and high gloss maintenance.
Patent Information
- Application Number
- CN202611623413.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing defoamers are difficult to use in high weather-resistant coatings while maintaining high defoaming and foam-suppressing capabilities, as well as controlling the dispersion state and interfacial migration after film formation, which affects the long-term stability and gloss retention of the coating film.
A modified polysiloxane was prepared by reacting a side-containing hydrogen polysiloxane with allyl polyether and allyl glycidyl ether, followed by ring-opening with 1-octyl mercaptan to form a SiO2 coating layer on the surface of nano-titanium dioxide. The system's fluidity and dispersibility were then adjusted by combining silicone oil, polypropylene glycol, and nonionic surfactants.
It achieves uniform dispersion of modified polysiloxane in coatings, maintains rapid defoaming and continuous foam suppression performance, while reducing adverse effects on the coating film and improving the aging gloss retention rate and storage stability of the coating film.
Smart Images

Figure CN123102008A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of defoamer technology, specifically to a defoamer for high weather-resistant coatings and its preparation method. Background Technology
[0002] During the production, formulation, and application of coatings, high-speed stirring, pumping, spraying, and the presence of surface-active components such as wetting agents and dispersants can easily introduce air into the system, forming stable foam. If this foam is not eliminated promptly, it not only reduces production and application efficiency but may also create defects such as pinholes, craters, and craters in the coating film, thus affecting its appearance, density, and protective performance. Existing defoamers for coatings mainly include mineral oil-based, polyether-based, organosilicon-based, and polyether-modified organosilicon defoamers. Among them, polyether-modified organosilicon defoamers combine the low surface tension of organosilicon segments with the good system adaptability of polyether segments, and are therefore widely used in the coatings industry. To further improve defoaming performance, existing technologies often combine hydrophobic silica and other inorganic particles with polysiloxanes. The hydrophobic particles disturb the structure of the foam film after entering it, thereby enhancing the foam-breaking effect.
[0003] However, for high-weather-resistant coatings such as architectural exterior wall coatings that require long-term exposure to ultraviolet light, heat, oxygen, and moisture, defoamers, in addition to meeting initial defoaming and continuous foam suppression requirements, also need to minimize their adverse effects on the long-term weather resistance of the coating film. Therefore, how to maintain high defoaming and foam suppression capabilities while controlling the dispersion state of the defoamer in the coating and its interfacial migration after film formation, and maintaining the gloss retention and long-term stability of the coating film after aging, remains a key technical problem that defoamers for high-weather-resistant coatings need to solve. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the purpose of this invention is to provide a defoamer for high weather resistance coatings and its preparation method.
[0005] A method for preparing a defoamer for high weather resistance coatings includes the following steps:
[0006] (1) The side-containing hydrogen polysiloxane is first reacted with allyl polyether and allyl glycidyl ether by hydrosilylation reaction, and then reacted with 1-octyl mercaptan to undergo ring-opening reaction to obtain modified polysiloxane.
[0007] (2) Nano titanium dioxide and sodium silicate are aged under alkaline conditions to obtain coated titanium dioxide; methyltriethoxysilane and hexadecyltrimethoxysilane are mixed and the pH is adjusted to 4-5, coated titanium dioxide is added to carry out a condensation reaction to obtain modified titanium dioxide;
[0008] (3) Mix the modified polysiloxane, silicone oil and stabilizer, add the modified titanium dioxide and disperse at high speed, then add the nonionic surfactant and mix well, and degas under vacuum to obtain a defoamer for high weather resistance coatings.
[0009] In step (1), the allyl polyether is allyl polyoxyethylene polyoxypropylene methyl ether; the mass ratio of the side-containing hydrogen polysiloxane, allyl polyether, allyl glycidyl ether, and 1-octyl mercaptan is 100:(50-60):(13.5-15):(17.5-19).
[0010] In step (1), the temperature of the hydrosilylation reaction is 70-80℃ and the time is 4-6h.
[0011] In step (1), the ring-opening reaction is carried out at a temperature of 40-50°C for 5-7 hours.
[0012] In step (2), the mass ratio of nano-titanium dioxide, sodium silicate, methyltriethoxysilane and hexadecyltrimethoxysilane is 1:(0.3-0.5):(0.06-0.1):(0.03-0.05).
[0013] In step (2), the aging reaction is carried out at a temperature of 85-95℃ for 1-2 hours; the condensation reaction is carried out at a temperature of 60-70℃ for 3-5 hours.
[0014] In step (3), the mass ratio of the modified polysiloxane, silicone oil, stabilizer, modified titanium dioxide, and nonionic surfactant is (60-75):(8-15):(5-12):(6-10):2.
[0015] In step (3), the nonionic surfactant is fatty alcohol polyoxyethylene ether.
[0016] In step (3), the stabilizer is polypropylene glycol.
[0017] A defoamer for high weather resistance coatings is prepared by the above method.
[0018] Due to the adoption of the above technical solutions, the beneficial effects of the present invention include:
[0019] (1) This invention uses a side-containing hydrogen-containing polysiloxane as a backbone, and introduces EO (polyoxyethylene ether) / PO (polyoxypropylene ether) polyether segments and β-hydroxy octyl sulfide structures into the side chains, so that hydrophilic and hydrophobic functional groups are distributed at multiple points along the polysiloxane backbone, reducing the local enrichment and phase separation of low polar siloxane segments. Among them, the polysiloxane backbone has low surface tension, which is conducive to migration and spreading to the gas-liquid interface; the EO segment improves the compatibility and water dispersion stability of the system, the PO segment maintains moderate hydrophobicity, and reduces the tendency of polyether overhydration and foam stabilization; the β-hydroxy octyl sulfide regulates the interfacial properties through the polar effect of hydroxyl and the hydrophobic effect of octyl; the synergistic effect of each functional group enables the modified polysiloxane to maintain good interfacial migration, rapid defoaming and continuous foam suppression performance while improving dispersion stability.
[0020] (2) In this invention, a SiO2 coating layer is formed on the surface of nano-titanium dioxide, and the surface is further modified by methyltriethoxysilane and hexadecyltrimethoxysilane. The SiO2 coating layer can isolate the photocatalytic active sites on the TiO2 surface, reducing the adverse effect of its photocatalytic activity on the long-term stability of the organic components of the coating film; methylsilane and long-chain alkylsilane synergistically regulate the hydrophobicity and interfacial compatibility of the particle surface, reduce particle agglomeration, promote the entry of modified titanium dioxide into the bubble film region, promote local dewetting and drainage, and thus play an auxiliary role in bubble breaking and weather resistance enhancement.
[0021] (3) The present invention adjusts the fluidity, dispersibility and interfacial wettability of the system by using silicone oil, polypropylene glycol stabilizer and nonionic surfactant, so that the modified polysiloxane and modified titanium dioxide are kept relatively uniformly dispersed, reducing floating oil, flocculation and sedimentation during storage, and obtaining a high weather-resistant defoamer for coatings that has the advantages of rapid defoaming, continuous foam suppression, good storage stability and high gloss retention rate after aging. Attached Figure Description
[0022] Figure 1 Fourier transform infrared spectra of allyl polyoxyethylene polyoxypropylene methyl ether, side-containing hydrogen polysiloxane, and the modified polysiloxane prepared in Example 2.
[0023] Figure 2 Fourier transform infrared spectra of unmodified titanium dioxide, coated titanium dioxide prepared in Example 5, and modified titanium dioxide.
[0024] Figure 3 This is a transmission electron microscope (TEM) image of the modified titanium dioxide prepared in Example 5. Detailed Implementation
[0025] The following description, in conjunction with specific embodiments, provides further details, but the present invention is not limited to these embodiments.
[0026] Example 1: Preparation of modified polysiloxane
[0027] Under nitrogen protection, 100g of hydrogen-containing polysiloxane and 0.4g of Karstedt platinum catalyst (Pt content 0.2wt%) were added to a reaction flask. The mixture was stirred at 300rpm and heated to 60℃. A mixture of 50g of allyl polyoxyethylene polyoxypropylene methyl ether (number average molecular weight 1000) and 15g of allyl glycidyl ether was added dropwise over 60min. The mixture was then heated to 70℃ and reacted for 6h. The temperature was lowered to 40℃, and 0.08g of triethylamine was added and stirred until homogeneous. 19g of 1-octyl mercaptan was added dropwise over 10min. The mixture was kept at this temperature for 7h. The mixture was then distilled under reduced pressure at 90℃ and a gauge pressure of -0.09MPa to constant weight. After cooling to room temperature, the modified polysiloxane was obtained. In the above reaction process, the hydrogen-containing polysiloxane undergoes hydrosilylation with allyl polyoxyethylene polyoxypropylene methyl ether and allyl glycidyl ether under the action of Karstedt platinum catalyst, so that the polyether segment and epoxy side link are branched onto the polysiloxane chain; then 1-octyl mercaptan undergoes ring-opening reaction with epoxy group under the action of triethylamine, introducing β-hydroxy octyl sulfide structure, and obtaining modified polysiloxane.
[0028] Example 2 Preparation of modified polysiloxane
[0029] Under nitrogen protection, 100g of hydrogen-containing polysiloxane and 0.4g of Karstedt platinum catalyst (Pt content 0.2wt%) were added to a reaction flask. The mixture was stirred at 300rpm and heated to 60℃. A mixture of 55g of allyl polyoxyethylene polyoxypropylene methyl ether (number average molecular weight 1000) and 14.5g of allyl glycidyl ether was added dropwise over 60min. The mixture was then heated to 75℃ and reacted for 5h. The temperature was lowered to 45℃, and 0.08g of triethylamine was added and stirred until homogeneous. 18.5g of 1-octyl mercaptan was added dropwise over 10min. The mixture was kept at this temperature for 6h. The mixture was then distilled under reduced pressure at 80℃ and a gauge pressure of -0.09MPa to constant weight. After cooling to room temperature, the modified polysiloxane was obtained.
[0030] Figure 1 Fourier transform infrared spectra of allyl polyoxyethylene polyoxypropylene methyl ether, hydrogen-containing polysiloxane, and modified polysiloxane are shown. As can be seen from the figure, compared with the raw material, the modified polysiloxane has a higher concentration at 1640 cm⁻¹. -1 The allyl characteristic peaks in the vicinity have basically disappeared, 2160 cm⁻¹ -1 The Si-H characteristic peaks in the vicinity are significantly reduced, while those at 3400 cm⁻¹ are also significantly reduced. -1 A broad absorption peak for hydroxyl groups appeared nearby, at 1260 cm⁻¹. -1 and 1100-1020cm -1 The characteristic absorption peaks of Si-CH3 and Si-O-Si were retained nearby, respectively; the above results indicate that polyether segments and hydroxyl-containing octyl sulfide side chains were introduced into the modified polysiloxane.
[0031] Example 3 Preparation of modified polysiloxane
[0032] Under nitrogen protection, 100g of hydrogen-containing polysiloxane and 0.4g of Karstedt platinum catalyst (Pt content 0.2wt%) were added to a reaction flask. The mixture was stirred at 300rpm and heated to 60℃. A mixture of 60g of allyl polyoxyethylene polyoxypropylene methyl ether (number average molecular weight 1000) and 13.5g of allyl glycidyl ether was added dropwise over 60min. The mixture was then heated to 80℃ and reacted for 4h. The temperature was lowered to 50℃, and 0.08g of triethylamine was added and stirred until homogeneous. 17.5g of 1-octyl mercaptan was added dropwise over 10min. The mixture was kept at this temperature for 5h. The mixture was then distilled under reduced pressure at 80℃ and a gauge pressure of -0.09MPa to constant weight. After cooling to room temperature, the modified polysiloxane was obtained.
[0033] Example 4 Preparation of modified titanium dioxide
[0034] Add 200 mL of deionized water, 10 g of nano-titanium dioxide, and 0.10 g of sodium hexametaphosphate to a reaction flask. Disperse the mixture ultrasonically at 30 kHz and 300 W for 30 min. Heat to 85 °C with stirring at 500 rpm. Adjust the pH to 9 using 1 mol / L sodium hydroxide aqueous solution. Add 15 g of 20 wt% sodium silicate aqueous solution dropwise over 60 min. During the addition, maintain the pH at 9 ± 0.2 using 5 wt% sulfuric acid aqueous solution. Incubate for 2 h, cool to room temperature, centrifuge at 8000 rpm for 10 min, collect the precipitate, and wash successively with deionized water (3 × 50 mL) and 50 mL of 90 wt% ethanol aqueous solution to obtain coated titanium dioxide. Add 0.6 g of methyltriethoxysilane and 0.3 g of hexadecyltrimethoxysilane to 100 g of... In a 90wt% ethanol aqueous solution, the pH was adjusted to 4 using 1mol / L hydrochloric acid aqueous solution, and the mixture was stirred for 30 min. All of the above-mentioned coated titanium dioxide was then added, and the mixture was ultrasonically dispersed at 30 kHz and 200 W for 15 min. The temperature was raised to 60℃, and the mixture was stirred at 500 rpm for 5 h. After cooling to room temperature, the mixture was centrifuged at 8000 rpm for 10 min, and the precipitate was collected. The precipitate was washed with anhydrous ethanol (3 × 50 mL) and dried at 100℃ and a gauge pressure of -0.09 MPa for 6 h to obtain modified titanium dioxide.
[0035] Example 5 Preparation of modified titanium dioxide
[0036] 200 mL of deionized water, 10 g of nano-titanium dioxide, and 0.10 g of sodium hexametaphosphate were added to a reaction flask and ultrasonically dispersed at 30 kHz and 300 W for 30 min. The mixture was then heated to 90 °C with stirring at 500 rpm. The pH was adjusted to 9.5 using a 1 mol / L sodium hydroxide aqueous solution. 20 g of 20 wt% sodium silicate aqueous solution was added dropwise over 60 min. During the addition, the pH was maintained at 9.5 ± 0.2 using a 5 wt% sulfuric acid aqueous solution. The mixture was aged at this temperature for 1.5 h, cooled to room temperature, and centrifuged at 8000 rpm for 10 min. The precipitate was collected and washed successively with deionized water (3 × 50 mL) and 50 mL of 90 wt% ethanol aqueous solution to obtain coated titanium dioxide. 0.8 g of methyltriethoxysilane and 0.4 g of hexadecyltrimethoxysilane were added to 100 g of... In a 90wt% ethanol aqueous solution, the pH was adjusted to 4.5 using 1mol / L hydrochloric acid aqueous solution, and the mixture was stirred for 30 min. All of the above-mentioned coated titanium dioxide was then added, and the mixture was ultrasonically dispersed at 30 kHz and 200 W for 15 min. The temperature was raised to 65 °C, and the mixture was stirred at 500 rpm for 4 h. After cooling to room temperature, the mixture was centrifuged at 8000 rpm for 10 min, and the precipitate was collected. The precipitate was washed with anhydrous ethanol (3 × 50 mL) and dried at 100 °C and a gauge pressure of -0.09 MPa for 6 h to obtain modified titanium dioxide.
[0037] Figure 2 The figures show the Fourier transform infrared spectra of unmodified titanium dioxide, coated titanium dioxide, and modified titanium dioxide. As can be seen from the figures, coated titanium dioxide exhibits the best performance at 1080 cm⁻¹. -1 800cm -1 The characteristic absorption peaks appearing nearby are attributed to the Si-O-Si asymmetric stretching vibration and the Si-O-Si symmetric stretching vibration, in the range of 950-970 cm⁻¹. -1 The nearby absorption peaks are related to Si-O-Ti and surface Si-OH vibrations, indicating the formation of a SiO2 coating layer on the titanium dioxide surface. Modified titanium dioxide, while retaining the relevant absorption peaks of coated titanium dioxide, exhibits a peak at 2924 cm⁻¹. -1 and 2854cm -1 An aliphatic -CH2- stretching vibration absorption peak appeared nearby, at 1460 cm⁻¹. -1 An absorption peak for the -CH2- bending vibration appeared nearby, at 720 cm⁻¹. -1 A long-chain alkyl rocking vibration absorption peak appeared nearby, along with a peak at 3400 cm⁻¹. -1 The weakening of the broad peak of the nearby hydroxyl group indicates that the organosilane has been grafted onto the surface of the coated titanium dioxide and has consumed some of the surface hydroxyl groups, thus producing modified titanium dioxide.
[0038] Figure 3This is a transmission electron microscope (TEM) image of the modified titanium dioxide. As shown in the image, the modified titanium dioxide particles are generally dispersed at the nanoscale with relatively clear particle boundaries. Inside the particles, a dark core with a lighter outer shell is visible, exhibiting a distinct core-shell structure.
[0039] Example 6 Preparation of modified titanium dioxide
[0040] Add 200 mL of deionized water, 10 g of nano-titanium dioxide, and 0.10 g of sodium hexametaphosphate to a reaction flask. Disperse the mixture ultrasonically at 30 kHz and 300 W for 30 min. Heat to 95 °C with stirring at 500 rpm. Adjust the pH to 10 using 1 mol / L sodium hydroxide aqueous solution. Add 25 g of 20 wt% sodium silicate aqueous solution dropwise over 60 min. During the addition, maintain the pH at 10 ± 0.2 using 5 wt% sulfuric acid aqueous solution. Incubate for 1 h, cool to room temperature, centrifuge at 8000 rpm for 10 min, collect the precipitate, and wash successively with deionized water (3 × 50 mL) and 50 mL of 90 wt% ethanol aqueous solution to obtain coated titanium dioxide. Add 1.0 g of methyltriethoxysilane and 0.5 g of hexadecyltrimethoxysilane to 100 g of... In a 90wt% ethanol aqueous solution, the pH was adjusted to 5 using 1mol / L hydrochloric acid aqueous solution, and the mixture was stirred for 30 min. All of the above-mentioned coated titanium dioxide was then added, and the mixture was ultrasonically dispersed at 30 kHz and 200 W for 15 min. The temperature was raised to 70 °C, and the mixture was stirred at 500 rpm for 3 h. After cooling to room temperature, the mixture was centrifuged at 8000 rpm for 10 min, and the precipitate was collected. The precipitate was washed with anhydrous ethanol (3 × 50 mL) and dried at 100 °C and a gauge pressure of -0.09 MPa for 6 h to obtain modified titanium dioxide.
[0041] Example 7 Preparation of defoamer for high weather-resistant coatings
[0042] (1) Weigh: 60g of modified polysiloxane (prepared in Example 1), 8g of silicone oil, 5g of stabilizer (polypropylene glycol PPG-1000), 6g of modified titanium dioxide (prepared in Example 4), and 2g of nonionic surfactant (fatty alcohol polyoxyethylene ether AEO-5);
[0043] (2) Mix the modified polysiloxane, silicone oil and stabilizer, and stir for 20 min at 50°C and 500 rpm; add the modified titanium dioxide in batches (divided into 4 batches with a 5 min interval between batches), and disperse at 2500 rpm for 30 min; then reduce the speed to 800 rpm, add the nonionic surfactant, and continue stirring for 20 min; finally, degas under vacuum for 15 min at 50°C and a gauge pressure of -0.08 MPa, and cool to room temperature to obtain a defoamer for high weather resistance coatings.
[0044] Example 8 Preparation of defoamer for high weather-resistant coatings
[0045] (1) Weigh: 70g of modified polysiloxane (prepared in Example 2), 12g of silicone oil, 10g of stabilizer (polypropylene glycol PPG-1200), 8g of modified titanium dioxide (prepared in Example 5), and 2g of nonionic surfactant (fatty alcohol polyoxyethylene ether AEO-5);
[0046] (2) Mix the modified polysiloxane, silicone oil and stabilizer, and stir for 20 min at 55℃ and 500 rpm; add modified titanium dioxide in batches (divided into 4 batches with a 5 min interval between batches), and disperse at high speed of 2500 rpm for 30 min; then reduce the speed to 800 rpm, add nonionic surfactant, and continue stirring for 20 min; finally, degas under vacuum for 15 min at 55℃ and gauge pressure of -0.08 MPa, and cool to room temperature to obtain a defoamer for high weather resistance coatings.
[0047] Example 9 Preparation of defoamer for high weather-resistant coatings
[0048] (1) Weigh: 75g of modified polysiloxane (prepared in Example 3), 15g of silicone oil, 12g of stabilizer (polypropylene glycol PPG-1500), 10g of modified titanium dioxide (prepared in Example 6), and 2g of nonionic surfactant (fatty alcohol polyoxyethylene ether AEO-5);
[0049] (2) Mix the modified polysiloxane, silicone oil and stabilizer, and stir for 20 min at 60℃ and 500 rpm; add the modified titanium dioxide in batches (divided into 4 batches with a 5 min interval between batches), and disperse at 2500 rpm for 30 min; then reduce the speed to 800 rpm, add the nonionic surfactant, and continue stirring for 20 min; finally, degas under vacuum for 15 min at 60℃ and gauge pressure -0.08 MPa, and cool to room temperature to obtain a defoamer for high weather resistance coatings.
[0050] Comparative Example 1
[0051] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified polysiloxane added to the components is replaced with an equal weight of the modified polysiloxane prepared by the following method:
[0052] The preparation method of the modified polysiloxane is basically the same as that in Example 2, except that the side-hydrogen-containing polysiloxane is replaced with an equal weight of end-hydrogen-containing polysiloxane (model RH-H518, hydrogen content 0.18wt%, produced by Ningbo Runhe High-tech Materials Technology Co., Ltd.).
[0053] Comparative Example 2
[0054] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified polysiloxane added to the components is replaced with an equal weight of the modified polysiloxane prepared by the following method:
[0055] The preparation method of the modified polysiloxane is basically the same as that in Example 2, except that the allyl polyether (number average molecular weight of 1000) is replaced with an equal weight of allyl polyoxyethylene methyl-terminated polyether (number average molecular weight of 1000).
[0056] Comparative Example 3
[0057] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified polysiloxane added to the components is replaced with an equal weight of the modified polysiloxane prepared by the following method:
[0058] The preparation method of the modified polysiloxane is basically the same as that in Example 2, except that the amount of 55g allyl polyether (number average molecular weight of 1000) is replaced with 70g, the amount of allyl glycidyl ether is replaced with 12.8g, and the amount of 1-octyl mercaptan is replaced with 16.3g.
[0059] Comparative Example 4
[0060] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified polysiloxane added to the components is replaced with an equal weight of the modified polysiloxane prepared by the following method:
[0061] The preparation method of the modified polysiloxane is basically the same as that in Example 2, except that 1-octylthiol is replaced with 11.4g of 1-butyrithiol.
[0062] Comparative Example 5
[0063] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified titanium dioxide added to the components is replaced with an equal weight of modified titanium dioxide prepared by the following method:
[0064] The preparation method of modified titanium dioxide is basically the same as that in Example 5, except that 0.8g of methyltriethoxysilane and 0.4g of hexadecyltrimethoxysilane are replaced with 0.4g of methyltriethoxysilane and 0.8g of hexadecyltrimethoxysilane.
[0065] Comparative Example 6
[0066] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified titanium dioxide added to the components is replaced with an equal weight of modified titanium dioxide prepared by the following method:
[0067] The preparation method of modified titanium dioxide is basically the same as that in Example 5, except that 20g of 20wt% sodium silicate aqueous solution is replaced with 10g of 20wt% sodium silicate aqueous solution.
[0068] Comparative Example 7
[0069] The preparation method of the defoamer for high weather-resistant coatings is basically the same as that in Example 8, except that the modified titanium dioxide added to the components is replaced with an equal weight of modified titanium dioxide prepared by the following method:
[0070] The preparation method of modified titanium dioxide is basically the same as that in Example 5, except that 20g of 20wt% sodium silicate aqueous solution is replaced with 35g of 20wt% sodium silicate aqueous solution.
[0071] The silicone oil used in the embodiments and comparative examples of this application is model QL-201-350, produced by Jiangsu Quanli Chemical Co., Ltd.; the titanium dioxide is model ZC-TiO2-NJ50, with an average particle size of 50nm, produced by Zhejiang Chongchuan New Material Technology Co., Ltd.; the hydrogen-containing polysiloxane is model SH-18, with a hydrogen content of 0.18wt%, produced by Jiangsu Kexing New Material Co., Ltd.; the allyl polyether is allyl polyoxyethylene polyoxypropylene methyl ether, model POLYCERIN® 35PK-210; and the sodium silicate has a modulus of 3.
[0072] The defoaming properties, foam suppression properties, dispersion stability, and weather resistance of the high weather-resistant coatings prepared in the examples and comparative examples were tested. The test results are shown in Table 1.
[0073] Defoaming performance test: Pour 100ml of 2wt% sodium dodecylbenzenesulfonate aqueous solution into a 500ml graduated cylinder, bubble with nitrogen gas at a flow rate of 1L / min until the 500ml mark is reached, stop the gas flow, add 20mg of defoamer, and immediately use an electronic stopwatch to record the time when the residual foam volume above the liquid surface is ≤10ml. Repeat the test 3 times and take the average value as the final defoaming time.
[0074] Defoaming performance test: Pour 100ml of 2wt% sodium dodecylbenzenesulfonate aqueous solution into a 500ml beaker, add 20mg of defoamer, stir at 200rpm for 5min, transfer to a 500ml graduated cylinder, and then start introducing nitrogen gas at a flow rate of 2L / min while simultaneously timing with an electronic stopwatch. Stop timing when the total volume reaches the 500ml mark and record the defoaming time. Repeat the test 3 times and take the average value as the final defoaming time.
[0075] Dispersion stability test: Add 10g of defoamer to 90g of deionized water, stir at 800rpm for 5min, seal and store at 70℃ for 48h, cool to room temperature, and observe whether floating oil, flocculation, or sedimentation occurs.
[0076] Weather resistance test: The experiment used high weather-resistant acrylic paint HF790 (produced by Shenzhen Baoguang Industrial Co., Ltd.) and its matching HF7900 thinner. 200g of high weather-resistant acrylic paint HF790 was weighed, 1.0g of defoamer was added, and the mixture was stirred at 500rpm for 5min, then at 1500rpm for 10min. 100g of HF7900 thinner was added, and the mixture was stirred at 500rpm for another 5min, then allowed to stand for 30min. The resulting paint was then evenly sprayed onto the surface of a 150mm×75mm×2mm 6061 aluminum plate (washed and dried with anhydrous ethanol before use). The spraying pressure was 0.30MPa, the distance between the spray gun and the test plate was 20cm, and the dry film thickness was controlled at 50±2μm. The plate was cured at 23℃ and 50% relative humidity for 7 days. The initial gloss before aging was measured using a 60° precision gloss meter (model DG-60N). The test panel was placed in a fluorescent ultraviolet aging test chamber, using a UVA-340 lamp, and the irradiance at 340nm was controlled at 0.89W / (m²). 2 The UV irradiation was performed at 60°C for 4 hours and condensation at 50°C for 4 hours, with each cycle lasting 1200 hours. The gloss level at 60°C after aging was then measured. The gloss retention rate was calculated using the formula: Gloss retention rate / % = Gloss after aging / Gloss before aging × 100%. Three parallel test plates were used in each group, and the average value of the test results was taken.
[0077] Table 1 Performance Test Data
[0078]
[0079] As can be seen from the data in Table 1, the defoamer for high weather resistance coatings prepared by the present invention has good defoaming, foam suppression and water dispersion stability, and can maintain a high gloss retention rate after artificial accelerated aging.
[0080] In Comparative Example 1, after replacing the side-containing hydrogen polysiloxane with the end-containing hydrogen polysiloxane, the functional groups changed from being distributed at multiple points on the main chain to being concentrated at the chain ends. The middle part still retains a relatively long low-polarity siloxane segment, which is not conducive to taking into account both system compatibility and interfacial migration ability, resulting in a decrease in water dispersion stability and coating weather resistance stability.
[0081] In Comparative Example 2, after replacing the EO / PO type allyl polyether with pure polyoxyethylene methyl-terminated polyether, the hydration of the polyether segments was enhanced, which was not conducive to their migration to the gas-liquid interface and the promotion of bubble film drainage, thus reducing the defoaming and foam suppression performance.
[0082] In Comparative Example 3, increasing the amount of allyl polyether and decreasing the amounts of allyl glycidyl ether and 1-octyl mercaptan increased the proportion of polyether segments and reduced the side chains of β-hydroxyoctyl sulfide, causing the hydrophilic-hydrophobic balance of the modified polysiloxane to shift towards hydrophilicity. This is not conducive to the migration of active components to the gas-liquid interface and the disturbance of the bubble film, thus reducing the overall defoaming performance.
[0083] In Comparative Example 4, after replacing 1-octylthiol with 1-butyrithiol, the hydrophobic alkyl chain was shortened, the hydrophobic affinity to the gas-liquid interface was weakened, and the ability of the modified polysiloxane to enter the gas-liquid interface and the bubble film was reduced, which was not conducive to the drainage and rupture of the bubble film, resulting in a decrease in defoaming and foam suppression performance.
[0084] In Comparative Example 5, increasing the amount of hexadecyltrimethoxysilane and decreasing the amount of methyltriethoxysilane increased the proportion of long-chain hydrophobic groups on the particle surface, enhanced the hydrophobic association and van der Waals effects between long-chain alkyl groups, making the modified titanium dioxide more prone to secondary agglomeration. As a result, the water dispersion stability decreased, and the particle dispersion uniformity was reduced, which reduced the defoaming and weather resistance properties.
[0085] In Comparative Example 6, reducing the amount of sodium silicate aqueous solution reduced the amount of SiO2 deposition on the TiO2 surface, resulting in insufficient coverage and shielding of the active TiO2 surface. Under ultraviolet irradiation, it was easier to generate photoactive species and promote resin photo-oxidation, leading to a decrease in gloss retention after artificial aging.
[0086] In Comparative Example 7, increasing the amount of sodium silicate increased the amount of SiO2 deposition on the TiO2 surface. Although photocatalytic passivation was enhanced, the degree of organic modification on the surface of each particle decreased, the amount of residual Si-OH increased, and the hydrogen bonding and agglomeration tendency between particles were enhanced. At the same time, the excessively thick SiO2 coating layer reduced the TiO2 content per unit mass of particles, and the agglomeration and uneven dispersion of the particles enhanced the light scattering of the coating, thereby reducing the dispersion stability and the gloss retention rate after artificial aging.
[0087] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. However, any modifications, alterations, and variations made by those skilled in the art without departing from the scope of the present invention based on the disclosed technical content are equivalent embodiments of the present invention. Furthermore, any modifications, alterations, and variations made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the present invention.
Claims
1. A method for producing a defoaming agent for high weatherability paint, characterized by, Includes the following steps: (1) The side-containing hydrogen polysiloxane is first reacted with allyl polyether and allyl glycidyl ether by hydrosilylation reaction, and then reacted with 1-octyl mercaptan to undergo ring-opening reaction to obtain modified polysiloxane. (2) Nano titanium dioxide and sodium silicate are aged under alkaline conditions to obtain coated titanium dioxide; methyltriethoxysilane and hexadecyltrimethoxysilane are mixed and the pH is adjusted to 4-5, coated titanium dioxide is added to carry out a condensation reaction to obtain modified titanium dioxide; (3) Mix the modified polysiloxane, silicone oil and stabilizer, add the modified titanium dioxide and disperse at high speed, then add the nonionic surfactant and mix well, and degas under vacuum to obtain a defoamer for high weather resistance coatings.
2. The method for preparing a defoaming agent for a high weather-resistant paint according to claim 1, characterized by, In step (1), the allyl polyether is allyl polyoxyethylene polyoxypropylene methyl ether; the mass ratio of the side-containing hydrogen polysiloxane, allyl polyether, allyl glycidyl ether, and 1-octyl mercaptan is 100:(50-60):(13.5-15):(17.5-19).
3. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (1), the temperature of the hydrosilylation reaction is 70-80℃ and the time is 4-6h.
4. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (1), the ring-opening reaction is carried out at a temperature of 40-50°C for 5-7 hours.
5. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (2), the mass ratio of nano-titanium dioxide, sodium silicate, methyltriethoxysilane and hexadecyltrimethoxysilane is 1:(0.3-0.5):(0.06-0.1):(0.03-0.05).
6. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (2), the aging reaction is carried out at a temperature of 85-95℃ for 1-2 hours; the condensation reaction is carried out at a temperature of 60-70℃ for 3-5 hours.
7. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (3), the mass ratio of the modified polysiloxane, silicone oil, stabilizer, modified titanium dioxide, and nonionic surfactant is (60-75):(8-15):(5-12):(6-10):
2.
8. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (3), the nonionic surfactant is fatty alcohol polyoxyethylene ether.
9. The method for preparing a defoamer for high weather-resistant coatings according to claim 1, characterized in that, In step (3), the stabilizer is polypropylene glycol.
10. A defoaming agent for high weatherability paint, characterized by, It is prepared by the preparation method described in any one of claims 1-9.