Preparation method of copper chloride modified activated carbon desulfurizer, its desulfurizing agent and application

By introducing acidic oxygen-containing functional groups and carbon defects on the surface of activated carbon through room temperature oxidation with concentrated nitric acid and hydrothermal treatment, combined with the coordination and intercalation of Cu2+, the problems of limited CuCl2 loading and agglomeration are solved, and the desulfurization performance is improved by achieving high efficiency.

CN123102115APending Publication Date: 2026-11-17TAIYUAN UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611439640.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing CuCl2-modified activated carbon desulfurization technologies, the CuCl2 loading is limited, and high-temperature treatment leads to agglomeration, failing to effectively utilize the acidic oxygen-containing functional groups on the activated carbon surface, making it difficult to improve desulfurization performance.

Method used

Acidic oxygen-containing functional groups are introduced on the surface of activated carbon by room temperature oxidation with concentrated nitric acid and carbon defects are etched. Combined with hydrothermal treatment, Cu2+ coordinates with carboxyl groups and/or embeds into carbon defects, avoiding high-temperature calcination and achieving high dispersion of CuCl2 over a wide loading range.

Benefits of technology

The breakthrough sulfur capacity of the copper chloride-modified activated carbon desulfurizer is much higher than that of the traditional Cu2+ oxidation mechanism, resulting in a significant improvement in desulfurization effect. The loading can reach 5wt.%~30wt.%, and the dispersibility is good.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102115A_ABST
    Figure CN123102115A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing copper chloride-modified activated carbon (OCA) desulfurizing agent, as well as the desulfurizing agent and its application, belonging to the field of adsorption-oxidation desulfurization technology. The method includes: grinding coal-based activated carbon; adding concentrated nitric acid (60-65% by volume) and allowing it to stand at room temperature for oxidation treatment; washing until neutral and drying to obtain OAC; preparing a copper chloride aqueous solution and loading copper chloride onto the OAC using a wet impregnation method; transferring it to a hydrothermal reactor for hydrothermal treatment to allow the Cu... 2+ Coordination interactions occur with acidic oxygen-containing functional groups on the surface of coal-based activated carbon and / or Cu... 2+ Embedded into surface carbon defects to allow partial Cu 2+ Reduced to form Cu + After drying at room temperature, a desulfurizing agent is obtained, with a copper chloride mass loading of 5-30 wt.%. This invention achieves high dispersion of copper chloride under high loading, oxidation of acidic oxygen-containing functional groups, and Cu... 2+ Synergistic desulfurization through coordination / oxidation mechanisms significantly improves the sulfur penetration capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of adsorption-oxidation desulfurization, and particularly to a method for preparing a copper chloride-modified activated carbon desulfurizer, as well as the desulfurizer and its application. Background Technology

[0002] Propylene mercaptan is a typical malodorous sulfur-containing organic compound found in fermentation waste gas. It is characterized by a low odor threshold and high toxicity, making its efficient removal a crucial issue in waste gas treatment. Activated carbon, due to its well-developed pore structure and large specific surface area, is widely used for the adsorption and removal of mercaptan pollutants.

[0003] In existing technologies, CuCl2 impregnation and modification of activated carbon is a common method to improve the removal performance of thiols. Studies have shown that the introduction of CuCl2 can form selective adsorption sites with strong affinity for thiols on the surface of activated carbon, thereby significantly enhancing the adsorption capacity of activated carbon for thiols. However, existing CuCl2-modified activated carbon desulfurization technologies still have the following shortcomings:

[0004] First, in existing technologies, activated carbon loaded with CuCl2 typically requires high-temperature calcination (e.g., 150-300℃ or even higher) to solidify the active components. However, high-temperature treatment easily leads to thermally driven agglomeration or grain growth of CuCl2, reducing its dispersion on the activated carbon surface and thus limiting the number of effective active sites. Simultaneously, the inherent pore structure of activated carbon restricts the effective loading of CuCl2; when the CuCl2 loading exceeds a certain threshold, the desulfurization performance decreases instead of increasing.

[0005] Second, the main purpose of using nitric acid oxidation to treat activated carbon in existing technologies is to provide anchoring sites for the dispersion of CuCl2. However, it fails to recognize that the acidic oxygen-containing functional groups (such as carboxyl groups and acid anhydrides) on the surface of activated carbon can participate in the desulfurization reaction, and also fails to utilize the interaction between oxygen-containing species and Cu. 2+ The synergistic effect between CuCl2 and activated carbon enhances desulfurization performance. Current research on desulfurization mechanisms generally suggests that the desulfurization process of CuCl2-modified activated carbon primarily relies on CuCl2. 2+ Redox reaction with thiols (2RSH + 2Cu) 2+ →RSSR+2Cu + +2H + Desulfurization capacity is limited by Cu 2+ The quantity.

[0006] In summary, existing technologies suffer from limitations such as limited effective CuCl2 loading, agglomeration of active components due to high-temperature processing, and failure to utilize oxygen-containing functional groups in conjunction with Cu. 2+ Problems such as synergistic desulfurization make it difficult to further improve desulfurization performance.

[0007] In view of this, a novel method for preparing copper chloride-modified activated carbon desulfurizing agent, as well as its desulfurizing agent and application, are proposed to solve all or part of the above problems. Summary of the Invention

[0008] To address at least one of the aforementioned problems and deficiencies in the prior art, embodiments of the present invention provide a method for preparing a copper chloride-modified activated carbon desulfurizing agent, as well as the desulfurizing agent and its application. Acidic oxygen-containing functional groups are introduced onto the surface of coal-based activated carbon through room temperature oxidation with concentrated nitric acid, followed by etching to generate carbon defects. This is combined with hydrothermal treatment to... 2+ By coordinating with carboxyl groups and / or embedding into carbon defects, and avoiding high-temperature calcination by using only low-temperature drying, high dispersion of CuCl2 was achieved over a wide loading range of 5 wt.% to 30 wt.%. Based on this, the present invention discloses the oxidation of acidic oxygen-containing functional groups and Cu... 2+ Coordination adsorption and Cu 2+ The synergistic effect of the three removal mechanisms of oxidation results in a significantly higher sulfur penetration capacity (240~489 mg / g) for copper chloride-modified activated carbon desulfurizer compared to traditional Cu chloride. 2+ The theoretical values ​​for the oxidation mechanism (57~339 mg / g) were achieved, resulting in outstanding desulfurization performance. The technical solution is as follows:

[0009] According to one aspect of the present invention, a method for preparing a copper chloride-modified activated carbon desulfurizing agent is provided. The preparation method includes the following steps:

[0010] Step S110: Grind the coal-based activated carbon to 40-80 mesh;

[0011] Step S120: Place the ground coal-based activated carbon in a container, add concentrated nitric acid with a volume fraction of 60%~65%, and let it stand for 10~12 hours for room temperature oxidation treatment. The amount of concentrated nitric acid added is 3~5 mL per gram of coal-based activated carbon.

[0012] Step S130: Wash the coal-based activated carbon treated with concentrated nitric acid with deionized water until neutral, and dry it at 100~120℃ for 2~3 hours to obtain oxidized modified activated carbon;

[0013] Step S140: Dissolve copper chloride dihydrate in deionized water to prepare copper chloride aqueous solution, and load copper chloride onto oxidized modified activated carbon by wet impregnation method, wherein the amount of deionized water is 1.3~1.6 mL per gram of coal-based activated carbon;

[0014] Step S150: Transfer the activated carbon sample loaded with copper chloride to a hydrothermal reactor and perform hydrothermal treatment at 100-120℃ for 10-12 hours to allow the Cu chloride to settle. 2+ Coordination interactions occur with acidic oxygen-containing functional groups on the surface of coal-based activated carbon and / or Cu...2+ Embedded into carbon defects on the surface of coal-based activated carbon, so that some Cu 2+ Reduced to form Cu + ;

[0015] Step S160: Dry the hydrothermally treated sample at 25~35℃ for 10~12h to obtain copper chloride modified activated carbon desulfurizer, wherein the mass loading of CuCl2 in the copper chloride modified activated carbon desulfurizer is 5wt.%~30wt.%.

[0016] According to another aspect of the present invention, a copper chloride-modified activated carbon desulfurizer is provided. This copper chloride-modified activated carbon desulfurizer is prepared according to the preparation method described above. In this copper chloride-modified activated carbon desulfurizer, CuCl2 is loaded onto the coal-based activated carbon in the following manner:

[0017] Cu coordinated with acidic oxygen-containing functional groups on the surface of coal-based activated carbon 2+ Cu in carbon defects embedded on the surface of coal-based activated carbon + / Cu 2+ Cu exists in the form of CuCl2·2H2O crystals 2+ Any one of them or any combination thereof.

[0018] According to another aspect of the present invention, an application of a copper chloride-modified activated carbon desulfurizer in the removal of propanethiol from fermentation waste gas is provided. The copper chloride-modified activated carbon desulfurizer is either the copper chloride-modified activated carbon desulfurizer described above or prepared by the preparation method described above.

[0019] In some embodiments, a copper chloride-modified activated carbon desulfurizer is loaded into a fixed-bed reactor, and fermentation waste gas containing propanethiol is passed through the copper chloride-modified activated carbon desulfurizer at 20-40°C, wherein propanethiol is removed by any one or any combination of the following removal mechanisms:

[0020] The first removal mechanism involves the oxidative removal of propanethiol by acidic oxygen-containing functional groups on the surface of coal-based activated carbon, generating RSO3H.

[0021] The second removal mechanism, Cu 2+ Coordination adsorption with propanethiol for removal;

[0022] The third removal mechanism, Cu 2+ The oxidative removal of propanethiol yields dipropyl disulfide.

[0023] The preparation method of the copper chloride-modified activated carbon desulfurizer provided in the embodiments of the present invention, as well as the desulfurizer and its application, have at least one or a portion of the following advantages:

[0024] (1) Acidic oxygen-containing functional groups (carboxyl groups, acid anhydrides) are introduced onto the surface of coal-based activated carbon by concentrated nitric acid oxidation at room temperature, and carbon defects are generated by etching the carbon skeleton, providing sufficient anchoring points for CuCl2 loading; CuCl2 is then subjected to hydrothermal treatment. 2+ Coordination interactions with acidic oxygen-containing functional groups and / or Cu 2+ By embedding itself within carbon defects and avoiding high-temperature calcination while employing only low-temperature drying, thermally driven agglomeration of CuCl2 is prevented. The desulfurizer prepared by this method can achieve a CuCl2 mass loading of 5wt.%~30wt.%, and maintains good dispersion even at high loading levels, achieving significantly higher performance than traditional CuCl2 methods. 2+ The theoretical value of the breakthrough sulfur capacity based on the oxidation mechanism;

[0025] (2) Oxidation treatment of activated carbon with concentrated nitric acid at room temperature with a volume fraction of 60%~65% can introduce acidic oxygen-containing functional groups, including carboxyl groups and acid anhydrides, onto the surface of activated carbon, while simultaneously etching the carbon skeleton structure to generate carbon defects (confirmed by Raman spectroscopy). D / I G (From 1.1 to 1.2), providing dual protection for the dispersion of CuCl2 by chemical anchoring points and structural anchoring points;

[0026] (3) During the hydrothermal treatment process, some Cu 2+ It is embedded in carbon defects and reduced to form Cu. + This makes the surface of coal-based activated carbon electron-deficient, thereby endowing its surface acidic oxygen-containing functional groups with the ability to oxidize propanethiol, realizing a new mechanism for desulfurization by acidic oxygen-containing functional group oxidation.

[0027] (4) When the CuCl2 mass loading is 10 wt.%, the desulfurizer's breakthrough sulfur capacity for propanethiol reaches 310 mg / g, which is higher than that of traditional CuCl2. 2+ The oxidation mechanism theory shows that the sulfur capacity (113 mg / g) is 2.7 times that of sulfur, and the desulfurization process simultaneously includes the oxidative removal of acidic oxygen-containing functional groups and Cu. 2+ Two mechanisms: coordination adsorption and removal;

[0028] (5) When the CuCl2 mass loading is 20wt.%~30wt.%, the desulfurizing agent's breakthrough sulfur capacity for propanethiol reaches 402mg / g and 489mg / g, respectively, which are 1.8 times and 1.4 times the traditional theoretical sulfur capacity (226mg / g and 339mg / g), respectively. The desulfurization process simultaneously includes the oxidative removal of acidic oxygen-containing functional groups and Cu 2+ Coordination adsorption removal and Cu 2+ The synergistic effect of three mechanisms of oxidative removal;

[0029] (6) The CuCl2-modified activated carbon desulfurizer prepared by the method of the present invention has the characteristics of high CuCl2 loading (5wt.%~30wt.%), good dispersibility, and excellent desulfurization performance; CuCl2 is loaded on activated carbon in multiple forms: CuCl2 coordinated with acidic oxygen-containing functional groups on the surface of activated carbon. 2+ Cu embedded in carbon defects + / Cu 2+ Cu, and Cu existing in the form of CuCl2·2H2O crystals 2+ The form of Cu varies under different loading levels (as confirmed by XRD and XPS characterization), enabling on-demand control of the desulfurization mechanism.

[0030] (7) The desulfurizing agent of this invention can be effectively applied to remove propanethiol from fermentation waste gas. When removing propanethiol in a fixed-bed reactor at 20~40℃, it is removed by oxidation of acidic oxygen-containing functional groups (generating RSO3H) and Cu. 2+ Coordination adsorption removal and Cu 2+ The synergistic effect of three mechanisms—oxidative removal (generating dipropyl disulfide RSSR)—achieves highly efficient desulfurization, with desulfurization performance significantly superior to that of a single mechanism.

[0031] (8) When the CuCl2 mass loading is 5 wt.%, the desulfurization process is mainly based on the oxidation removal of acidic oxygen-containing functional groups (the RSO3H peak in XPS is absolutely dominant); when the loading is 10 wt.%, it includes both oxidation removal and coordination adsorption removal; when the loading is 20 wt.%~30 wt.%, it includes the synergistic effect of the three mechanisms; thus achieving the effect of controlling the desulfurization path according to the loading. Attached Figure Description

[0032] These and / or other aspects and advantages of the present invention will become apparent and readily understood from the following description of preferred embodiments taken in conjunction with the accompanying drawings, in which:

[0033] Figure 1 A flowchart illustrating the preparation method of CuCl2 modified activated carbon desulfurizer according to an embodiment of the present invention;

[0034] Figure 2 The Cu 2p content of the sample (10 wt.% CuCl2 loading) before and after desulfurization in Example 1 of the present invention is shown. 3 / 2 XPS spectrum;

[0035] Figure 3 The image shows the S 2p XPS spectrum of the sample after desulfurization according to Example 1 of the present invention.

[0036] Figure 4 The image shows the S 2p XPS spectrum of the sample (5 wt.% CuCl2 loading) after desulfurization according to Example 2 of the present invention.

[0037] Figure 5 To illustrate the Cu 2p content of the sample (30 wt.% CuCl2 loading) before and after desulfurization in Example 4 of the present invention 3 / 2 XPS spectrum;

[0038] Figure 6 The image shows the S 2p XPS spectrum of the sample after desulfurization according to Example 4 of the present invention.

[0039] Figure 7 The N2 adsorption-desorption curves of the coal-based activated carbon support before and after oxidation with concentrated nitric acid according to the present invention are shown.

[0040] Figure 8 The images show the Raman spectra of coal-based activated carbon before and after oxidation with concentrated nitric acid according to the present invention.

[0041] Figure 9 The XRD patterns of coal-based activated carbon oxidized with concentrated nitric acid according to the present invention, as well as samples from Example 1, Example 3, and Example 4;

[0042] Figure 10 The XRD patterns of the samples after desulfurization according to Examples 1-4 of the present invention are shown. Detailed Implementation

[0043] The technical solution of the present invention will be further described in detail below through embodiments and in conjunction with the accompanying drawings. In this specification, the same or similar reference numerals indicate the same or similar components. The following description of the embodiments of the present invention with reference to the accompanying drawings is intended to explain the overall inventive concept of the present invention and should not be construed as a limitation thereof.

[0044] The present invention provides a method for preparing a CuCl2 modified activated carbon desulfurizer for removing propanethiol from fermentation waste gas. The present invention will be further described in detail below with reference to specific operation steps and embodiments.

[0045] See Figure 1 The process flow of the preparation method of the CuCl2 modified activated carbon desulfurizer is shown, which mainly includes the following steps:

[0046] Step S110: Grind the coal-based activated carbon to 40-80 mesh, the specific surface area of ​​the coal-based activated carbon being ≥900m². 2 / g, total pore volume ≥0.5mL / g, and the proportion of mesopore volume to total pore volume is not less than 20%;

[0047] Step S120: Place the ground coal-based activated carbon in a container, add concentrated nitric acid with a volume fraction of 60%~65%, and let it stand for 10~12 hours for room temperature oxidation treatment. The amount of concentrated nitric acid added is 3~5 mL per gram of coal-based activated carbon.

[0048] Step S130: Wash the coal-based activated carbon treated with concentrated nitric acid with deionized water until neutral, and dry it at 100~120℃ for 2~3h to obtain oxidized modified activated carbon (OAC).

[0049] Step S140: Dissolve copper chloride dihydrate (CuCl2·2H2O) in deionized water to prepare a copper chloride aqueous solution. Load the copper chloride onto the oxidized modified activated carbon using the wet impregnation method. The amount of deionized water used is 1.3~1.6 mL per gram of coal-based activated carbon.

[0050] Step S150: Transfer the coal-based activated carbon sample loaded with copper chloride to a hydrothermal reactor and perform hydrothermal treatment at 100-120℃ for 10-12 hours to allow the Cu chloride to be absorbed and dissolved. 2+ Coordination interactions occur with acidic oxygen-containing functional groups on the surface of coal-based activated carbon and / or Cu... 2+ Embedded into carbon defects on the surface of coal-based activated carbon;

[0051] Step S160: After hydrothermal treatment in step S150, dry at 25~35℃ for 10~12h to obtain CuCl2 modified activated carbon desulfurizer. The mass loading of CuCl2 in CuCl2 modified activated carbon desulfurizer is 5wt.%~30wt.%.

[0052] In a specific embodiment, steps S110-S130 are pretreatment steps for the coal-based activated carbon carrier. The coal-based activated carbon with the texture parameters defined in step S110 can provide sufficient structural space for the subsequent high-loading dispersion of CuCl2.

[0053] Then, the ground coal-based activated carbon is placed in a glass container, and concentrated nitric acid with a volume fraction of 60%~65% (preferably 63%) is added. The mixture is allowed to stand for 10~12 hours for room temperature oxidation treatment. The amount of concentrated nitric acid added is 3~5 mL per gram of coal-based activated carbon. It should be noted that too little concentrated nitric acid will result in insufficient oxygen-containing species on the surface of the coal-based activated carbon, failing to provide sufficient anchoring points for the dispersion of CuCl2; too much concentrated nitric acid will lead to over-oxidation of the coal-based activated carbon surface, causing the pore structure to collapse. The purpose of using concentrated nitric acid for room temperature oxidation treatment is twofold: firstly, room temperature oxidation can generate more acidic oxygen-containing functional groups, such as carboxyl groups and anhydrides; secondly, concentrated nitric acid can etch the carbon skeleton structure, thereby generating more structural defects.

[0054] Next, the coal-based activated carbon oxidized by concentrated nitric acid is washed with deionized water until neutral, and then dried in a forced-air drying oven at 100~120℃ for 2~3 hours to obtain oxidized modified activated carbon (OAC).

[0055] In one specific embodiment, steps S140-S160 are steps involving loading CuCl2 and hydrothermal treatment.

[0056] First, a certain amount of copper chloride dihydrate (CuCl2·2H2O) is weighed and dissolved in deionized water to prepare a copper chloride aqueous solution. The copper chloride is then impregnated onto the OAC using the wet impregnation method. The amount of deionized water added is 1.3~1.6 mL per gram of activated carbon.

[0057] Then, the activated carbon sample loaded with copper chloride was transferred to a hydrothermal reactor and subjected to hydrothermal treatment at 100-120℃ for 10-12 hours. The purpose of the hydrothermal treatment was to allow the Cu adsorbed on the surface of the coal-based activated carbon to react. 2+ It exhibits a strong interaction with the carboxyl groups on the surface of coal-based activated carbon, and this strong interaction includes Cu 2+ Coordinate with acidic functional groups on the surface of coal-based activated carbon, and / or incorporate Cu 2+ It is embedded in the carbon defects on the surface of coal-based activated carbon.

[0058] Next, the hydrothermally treated sample is dried at 25-35℃ (preferably 30℃) for 10-12 hours to obtain the CuCl2-modified activated carbon desulfurizer. The mass loading of CuCl2 in this desulfurizer is 5wt.%~30wt.%. It should be emphasized that in this embodiment of the invention, the activated carbon loaded with CuCl2 is dried only at low temperature, without any high-temperature heat treatment, thus avoiding thermally driven agglomeration or grain growth of metal salt species.

[0059] The role of oxygen-containing functional groups and the desulfurization mechanism of the CuCl2-modified activated carbon desulfurizer in this invention are further elaborated below:

[0060] In this invention, the acidic oxygen-containing functional groups on the surface of coal-based activated carbon have the following three functions: First, they provide anchoring sites for CuCl2, promoting its dispersion; second, they coordinate with CuCl2 during the hydrothermal process, regulating the electronic structure of copper species; third, they act as an oxidant to oxidize propanethiol to generate RSO3H species. It should be noted that the oxidation effect of the acidic oxygen-containing functional groups is only under hydrothermal conditions and on a portion of the Cu... 2+ It can only be generated after it is embedded in the carbon defects on the surface of coal-based activated carbon.

[0061] In this invention, the desulfurization performance is mainly related to the loading of CuCl2, the number of acidic oxygen-containing functional groups, and the relationship between the acidic functional groups and Cu. 2+ It is related to coordination / strong interaction.

[0062] The reasons why the CuCl2 loading in this invention is significantly higher than that in existing desulfurizers include: 1) The use of concentrated nitric acid treatment increases the number of oxygen-containing species on the surface of the coal-based activated carbon, providing sufficient anchoring points for the dispersion of CuCl2; 2) After loading CuCl2, the coal-based activated carbon is dried at low temperature without undergoing high-temperature heat treatment, thus avoiding the agglomeration or grain growth of heat-driven metal salt species; 3) Oxidation by concentrated nitric acid will etch the skeleton structure of the activated carbon, generating more defect sites, which can also serve as anchoring points to promote its dispersion; 4) The selected coal-based activated carbon itself has a well-developed texture.

[0063] Regarding the desulfurization mechanism, current technologies generally believe that the desulfurization mechanism of CuCl2 modified activated carbon mainly depends on Cu. 2+ The reaction equation is: 2RSH + 2Cu 2+ →RSSR+2Cu + +2H + RSH+Cu + →RSCu+H + That is, 1 mole of Cu 2+ It can remove 2 moles of mercaptan; the desulfurization performance mainly depends on Cu. 2+ The quantity.

[0064] The desulfurization mechanism of this invention is mainly the synergistic oxidation of acidic oxygen-containing functional groups with Cu. 2+ Coordination adsorption with propanethiol. The desulfurization mechanism varies significantly depending on the CuCl2 loading, as detailed below:

[0065] When the CuCl2 loading is low (e.g., 5 wt.%), the loaded Cu... 2+ During hydrothermal processes, it is easily embedded into the carbon skeleton of coal-based activated carbon and reduced to form Cu. + At this time, the surface of coal-based activated carbon tends to be electron-deficient, which makes the acidic oxygen-containing functional groups on the surface of coal-based activated carbon capable of oxidizing propanethiol. Therefore, when the CuCl2 loading is at a low level, the desulfurization process is mainly based on the oxidative desulfurization of acidic functional groups.

[0066] Then, with the increase of CuCl2 loading (e.g., 10 wt.%), a portion of Cu... 2+ During the hydrothermal process, it will be embedded in carbon defects, and another part of Cu will be embedded in them. 2+ It then coordinates with the acidic functional groups on the surface of coal-based activated carbon, at which point the desulfurization process simultaneously includes oxidative desulfurization of the acidic oxygen-containing functional groups and Cu. 2+ Coordination adsorption removal.

[0067] Furthermore, as the CuCl2 loading continues to increase (e.g., 20 wt.%~30 wt.%), the Cu...2+ Some are embedded in the carbon defects of coal-based activated carbon, another part coordinates with the acidic oxygen-containing functional groups on the surface of coal-based activated carbon, and a portion of Cu... 2+ It exists on the surface of coal-based activated carbon in the form of CuCl2·2H2O. Therefore, the desulfurization process at this time involves both the oxidative removal of oxygen-containing functional groups and the removal of Cu. 2+ Coordination adsorption and removal, and Cu 2+ Oxidative adsorption removal.

[0068] In one specific embodiment, the desulfurization performance of the CuCl2-modified activated carbon desulfurizer (hereinafter referred to as the desulfurizer) obtained in the embodiments of the present invention was determined and evaluated through a micro-fixed bed experiment. The specific process is as follows:

[0069] The prepared desulfurizing agent was loaded into a U-shaped tube (inner diameter 5-8 mm, usually 6 mm) to a height of 1.5-3.5 cm (usually 2 cm), and both ends of the sample were fixed with quartz wool. A water bath heating method was used to control the desulfurization temperature at 25-35℃. A mixture of methane and propane mercaptan was bubbled through a water saturator (the temperature of the water saturator was controlled at 25-35℃ using a water bath), and then introduced into the U-shaped tube reactor for reaction. The inlet concentration of propane mercaptan was 3000 ppm, and the total gas flow rate was 50 mL / min. The outlet concentration of propane mercaptan was detected by a gas chromatograph equipped with a flame photometric detector (FPD), and the outlet concentration was measured every ten minutes. The desulfurization experiment was terminated when the outlet concentration of propane mercaptan reached 1 ppm. The breakthrough sulfur capacity was calculated as the total amount of propane mercaptan adsorbed by the desulfurizing agent before breakthrough divided by the mass of the desulfurizing agent.

[0070] The following examples and comparative examples further verify and illustrate the desulfurizing agent prepared in this invention and its desulfurization performance.

[0071] Example 1:

[0072] In Example 1, the loading of CuCl2 was 10 wt.%.

[0073] The initial coal-based activated carbon was ground into 40-80 mesh particles. The ground activated carbon was placed in a glass container, and then concentrated nitric acid (63% by volume) was added. The mixture was allowed to stand for 12 hours. The amount of concentrated nitric acid added was 5 mL per gram of coal-based activated carbon. The activated carbon oxidized by concentrated nitric acid was washed with deionized water until neutral and dried in a forced-air oven at 120°C for 2 hours to obtain OAC. A certain amount of copper chloride dihydrate (CuCl2·2H2O) was weighed and dissolved in deionized water to prepare a copper chloride aqueous solution. The copper chloride was impregnated onto the OAC using a wet impregnation method. The obtained sample was then transferred to a hydrothermal reactor and allowed to stand at 100-120°C for 10-12 hours. The obtained sample was then dried in an oven at 30°C for 10-12 hours to obtain the sample of Example 1, in which the mass loading of CuCl2 was 10 wt.%.

[0074] Based on the existing CuCl2-supported activated carbon desulfurization mechanism, the theoretical sulfur capacity for removing propanethiol with 10 wt.% CuCl2 is 113 mg / g.

[0075] The above micro-fixed bed experiments verified that the desulfurization breakthrough time of the desulfurizing agent designed in Example 1 of this invention is 190 min, and the breakthrough sulfur capacity is 310 mg / g, which is much higher than the theoretical value.

[0076] See Figure 2 This demonstrates the Cu 2p content of the sample from Example 1 (10 wt.% CuCl2 loading) before and after desulfurization. 3 / 2 XPS spectrum.

[0077] like Figure 2 As shown, the Cu ions exist in the form of Cu before desulfurization. 2+ Mainly composed of Cu, with a small amount of Cu. + The presence of satellite peaks further confirms the presence of Cu in the sample of Example 1. 2+ The existence of Cu. + The presence of Cu is due to the hydrothermal process 2+ It is generated by the reduction of carbon defects embedded in the surface of coal-based activated carbon. Before and after desulfurization, Cu... + and Cu 2+ The peak position and intensity ratio did not change significantly, indicating that the desulfurization process of the sample in Example 1 did not follow the traditional Cu 2+ Oxidative desulfurization route (Cu 2+ →Cu + Instead of the redox route, coordination desulfurization is the main method.

[0078] See Figure 3 The S 2p XPS spectrum of the sample after desulfurization in Example 1 is shown.

[0079] like Figure 3As shown, the desulfurization products include both RSO3H (oxidation product) and RSH or RSSR (adsorption product). Since the sample in Example 1 was tested under an oxygen-free N2 atmosphere, the oxidant required for oxidative desulfurization originates from the acidic oxygen-containing functional groups on the surface of the coal-based activated carbon. Combined with... Figure 1 The oxidation state of Cu did not change significantly, indicating that propanethiol mainly interacts with Cu in a coordinated manner during the desulfurization process. 2+ The desulfurization process involves the combination and removal of these substances, while also incorporating oxidative desulfurization contributed by the acidic oxygen-containing functional groups on the surface of the coal-based activated carbon. Therefore, the desulfurization process of the sample in Example 1 simultaneously involves oxidative desulfurization and coordination adsorption desulfurization, i.e., it simultaneously includes the oxidative removal of acidic oxygen-containing functional groups (the first removal mechanism) and Cu... 2+ Coordination adsorption with propanethiol for removal (second removal mechanism).

[0080] Example 2:

[0081] In Example 2, the loading of CuCl2 was 5 wt.%.

[0082] The initial coal-based activated carbon was ground into 40-80 mesh particles. The ground activated carbon was placed in a glass container, and then concentrated nitric acid (63% by volume) was added. The mixture was allowed to stand for 12 hours. The amount of concentrated nitric acid added was 5 mL per gram of activated carbon. The activated carbon oxidized by concentrated nitric acid was washed with deionized water until neutral and dried in a forced-air oven at 120°C for 2 hours to obtain OAC. A certain amount of copper chloride dihydrate (CuCl2·2H2O) was weighed and dissolved in deionized water to prepare a copper chloride aqueous solution. The copper chloride was impregnated onto the OAC using a wet impregnation method. The sample was then transferred to a hydrothermal reactor and allowed to stand at 100-120°C for 10-12 hours. The resulting sample was then dried in an oven at 30°C for 10-12 hours to obtain the sample of Example 2, in which the mass loading of CuCl2 was 5 wt.%.

[0083] Based on the existing CuCl2-supported activated carbon desulfurization mechanism, the theoretical sulfur capacity for removing propanethiol with 5wt.% CuCl2 is 57mg / g.

[0084] The above micro-fixed bed experiments verified that the desulfurization breakthrough time of the desulfurizing agent designed in Example 2 of this invention is 130 min and the breakthrough sulfur capacity is 240 mg / g, which is much higher than the theoretical value.

[0085] See Figure 4 The S 2p XPS spectrum of the sample (5 wt.% loading) after desulfurization in Example 2 is shown.

[0086] like Figure 4As shown, when the CuCl2 loading is 5 wt%, the RSO3H peak is absolutely dominant, while the RSH or RSSR peaks are extremely weak. This confirms that when the CuCl2 loading is low, Cu... 2+ It is easily embedded in the carbon defects on the surface of coal-based activated carbon and reduced to Cu. + The surface of coal-based activated carbon tends to be electron-deficient, and the desulfurization process is mainly oxidative desulfurization by acidic oxygen-containing functional groups. Therefore, the desulfurization process of the sample in Example 2 is mainly oxidative removal by acidic oxygen-containing functional groups (the first removal mechanism).

[0087] Example 3:

[0088] In Example 3, the CuCl2 loading was 20 wt.%.

[0089] The initial coal-based activated carbon was ground into 40-80 mesh particles. The ground activated carbon was placed in a glass container, and then concentrated nitric acid (63% by volume) was added. The mixture was allowed to stand for 12 hours. The amount of concentrated nitric acid added was 5 mL per gram of activated carbon. The activated carbon oxidized by concentrated nitric acid was washed with deionized water until neutral and dried in a forced-air oven at 120°C for 2 hours to obtain OAC. A certain amount of copper chloride dihydrate (CuCl2·2H2O) was weighed and dissolved in deionized water to prepare a copper chloride aqueous solution. The copper chloride was impregnated onto the OAC using a wet impregnation method. The sample was then transferred to a hydrothermal reactor and allowed to stand at 100-120°C for 10-12 hours. The resulting sample was then dried in an oven at 30°C for 10-12 hours to obtain the sample of Example 3, in which the mass loading of CuCl2 was 20 wt.%.

[0090] Based on the existing CuCl2-supported activated carbon desulfurization mechanism, the theoretical sulfur capacity for removing propanethiol with 20wt.% CuCl2 is 226mg / g.

[0091] The above micro-fixed bed experiments verified that the desulfurization breakthrough time of the desulfurizing agent designed in Example 3 of this invention is 280 min, and the breakthrough sulfur capacity is 402 mg / g, which is much higher than the theoretical value.

[0092] The desulfurization process in Example 3 simultaneously includes the oxidative removal of acidic oxygen-containing functional groups (the first removal mechanism) and Cu. 2+ Coordination adsorption removal (second removal mechanism) and Cu 2+ The synergistic effect of oxidative removal (the third removal mechanism).

[0093] Example 4:

[0094] In Example 4, the CuCl2 loading was 30 wt.%.

[0095] The initial coal-based activated carbon was ground into 40-80 mesh particles. The ground activated carbon was placed in a glass container, and then concentrated nitric acid (63% by volume) was added. The mixture was allowed to stand for 12 hours. The amount of concentrated nitric acid added was 5 mL per gram of activated carbon. The activated carbon oxidized by concentrated nitric acid was washed with deionized water until neutral and dried in a forced-air oven at 120°C for 2 hours to obtain OAC. A certain amount of copper chloride dihydrate (CuCl2·2H2O) was weighed and dissolved in deionized water to prepare a copper chloride aqueous solution. The copper chloride was impregnated onto the OAC using a wet impregnation method. The sample was then transferred to a hydrothermal reactor and allowed to stand at 100-120°C for 10-12 hours. The resulting sample was then dried in an oven at 30°C for 10-12 hours to obtain the sample of Example 4, in which the mass loading of CuCl2 was 30 wt.%.

[0096] Based on the existing CuCl2-supported activated carbon desulfurization mechanism, the theoretical sulfur capacity for removing propanethiol with 30wt.% CuCl2 is 339mg / g.

[0097] The above micro-fixed bed experiments verified that the desulfurization breakthrough time of the desulfurizing agent designed in Example 4 of this invention is 400 min and the breakthrough sulfur capacity is 489 mg / g, which is much higher than the theoretical value.

[0098] See Figure 5 This demonstrates the Cu 2p content of the sample (30 wt% loading) in Example 4 before and after desulfurization. 3 / 2 XPS spectrum.

[0099] like Figure 5 As shown, Cu in the sample of Example 4 after desulfurization + The content of Cu increased significantly, indicating that some Cu was produced during the desulfurization process. 2+ It participates in the oxidative removal of propanethiol, that is, to generate dipropyl disulfide (RSSR, CH3CH2CH2SSCH2CH2CH3).

[0100] See Figure 6 The S 2p XPS spectrum of the sample after desulfurization in Example 4 is shown.

[0101] like Figure 6 As shown, the RSH or RSSR peak (approximately 164 eV) is very strong, while the RSO3H peak is relatively weak, indicating that this sample mainly reacts with Cu during the desulfurization process. 2+ Related to oxidative desulfurization, which simultaneously involves oxygen-containing functional groups. Combined with... Figure 5 Cu 2p 3 / 2 The XPS spectra show that the desulfurization process involves Cu. 2+ The oxidation of propanethiol to form RSSR also involves Cu. 2+Desulfurization occurs through coordination adsorption with propanethiol. Therefore, the desulfurization process of the sample in Example 4 simultaneously includes the oxidative removal of oxygen-containing functional groups (the first removal mechanism) and Cu... 2+ Coordination adsorption removal (second removal mechanism) and Cu 2+ The synergistic effect of three mechanisms: oxidative removal (the third removal mechanism).

[0102] Comparative Example 1:

[0103] Comparative Example 1 is a control experiment, which is coal-based activated carbon without nitric acid oxidation loaded with 10 wt.% CuCl2.

[0104] Untreated coal-based activated carbon was ground into 40-80 mesh particles. 10 wt.% of copper chloride dihydrate (CuCl2·2H2O) was dissolved in deionized water to prepare a copper chloride aqueous solution. The coal-based activated carbon was then impregnated into this solution using a wet impregnation method. The sample was then transferred to a hydrothermal reactor and allowed to stand at 100-120°C for 10-12 hours. The resulting sample was then dried in an oven at 30°C for 10-12 hours to obtain Comparative Example 1 sample, in which the CuCl2 mass loading was 10 wt.%.

[0105] The above micro-fixed bed experiment verified that the desulfurization breakthrough time of the comparative example 1 sample was 97 min and the breakthrough sulfur capacity was 170 mg / g.

[0106] Compared with Example 1, the coal-based activated carbon in Comparative Example 1 was not treated with concentrated nitric acid oxidation. The purpose of this example is to illustrate that the number of acidic oxygen-containing species on the surface of coal-based activated carbon significantly affects desulfurization performance, thus demonstrating the necessity of concentrated nitric acid oxidation treatment to improve desulfurization performance.

[0107] Comparative Example 2:

[0108] Comparative Example 2 was a control experiment, which was a 10wt.% CuCl2 / OAC sample that had not undergone hydrothermal treatment.

[0109] Initially, coal-based activated carbon was ground into 40-80 mesh particles. The ground activated carbon was placed in a glass container, and then concentrated nitric acid (63% by volume) was added. The mixture was allowed to stand for 12 hours. The amount of concentrated nitric acid added was 5 mL per gram of coal-based activated carbon. The activated carbon oxidized by concentrated nitric acid was washed with deionized water until neutral and dried in a forced-air oven at 120°C for 2 hours to obtain OAC. A certain amount of copper chloride dihydrate (CuCl2·2H2O) was weighed and dissolved in deionized water to prepare a copper chloride aqueous solution. The copper chloride was impregnated onto the OAC using a wet impregnation method. The impregnated sample was then placed in a forced-air oven at 30°C and allowed to stand for 12 hours to obtain Comparative Example 2 sample, in which the mass loading of CuCl2 was 10 wt.%.

[0110] The above micro-fixed bed experiment verified that the desulfurization breakthrough time of the comparative example 2 sample was 85 min and the breakthrough sulfur capacity was 131 mg / g.

[0111] Compared to Example 1, the sample in Control Example 2 was not subjected to hydrothermal treatment. This is intended to illustrate that for acidic oxygen-containing species on the surface of coal-based activated carbon to exert their effect of oxidizing propanethiol, Cu... 2+ Cu needs to be embedded into the carbon defects on the surface of coal-based activated carbon through a hydrothermal process to form Cu. + This further demonstrates the crucial role of hydrothermal treatment in realizing the oxidative desulfurization mechanism of acidic oxygen-containing functional groups.

[0112] See Figure 7 The N2 adsorption-desorption curves of the coal-based activated carbon carrier before and after oxidation with concentrated nitric acid are shown.

[0113] like Figure 7 As shown, the nitrogen adsorption volume of coal-based activated carbon decreased after oxidation with concentrated nitric acid, indicating that more acidic oxygen-containing functional groups were generated on the surface of the activated carbon after nitric acid oxidation, leading to a reduction in effective pore volume. Furthermore, the shape of the curve did not fundamentally change, indicating that the oxidation with concentrated nitric acid did not destroy the carbon skeleton structure of the coal-based activated carbon.

[0114] See Figure 8 The Raman spectra of coal-based activated carbon before and after oxidation with concentrated nitric acid are shown.

[0115] like Figure 8 As shown, the D peak in the Raman spectrum (approximately 1350 cm⁻¹) -1 ) and G peak (approximately 1580cm) -1 The strength ratio of (I) D / I G () represents the number of carbon defects on the surface of coal-based activated carbon. The initial I of the coal-based activated carbon D / I G The strength ratio was 1.1, which became 1.2 after oxidation with concentrated nitric acid. The increase in strength ratio indicates that oxidation with concentrated nitric acid etched more structural defect sites into the carbon skeleton, which provided more anchoring points for the subsequent anchoring and dispersion of CuCl2.

[0116] See Figure 9 The XRD patterns of coal-based activated carbon after oxidation with concentrated nitric acid, as well as samples from Example 1, Example 3, and Example 4, are shown.

[0117] XRD patterns are used to analyze phases, such as Figure 9As shown, when the CuCl2 loading is below 20 wt.% (e.g., in Examples 1 and 3), the XRD pattern only shows broad diffraction peaks of coal-based activated carbon, without the characteristic diffraction peaks of CuCl2·2H2O, indicating that CuCl2 is highly dispersed on the surface of the coal-based activated carbon. However, when the CuCl2 content reaches 30 wt.% (e.g., in Example 4), obvious characteristic diffraction peaks of CuCl2·2H2O appear, indicating the formation of a crystalline phase. The XRD patterns can intuitively explain the significant differences in desulfurization mechanisms caused by different loading amounts.

[0118] See Figure 10 The XRD patterns of the samples after desulfurization in Examples 1-4 are shown.

[0119] like Figure 10 As shown, no obvious characteristic diffraction peaks of sulfides (such as Cu2S, CuS, etc.) were observed in the desulfurized sample, indicating that the desulfurization products mainly existed in an amorphous or highly dispersed state, without causing pore blockage. Furthermore, comparing the XRD patterns of the sample before desulfurization (see...) Figure 9 In Example 4, the characteristic diffraction peak of CuCl2·2H2O disappeared after desulfurization, indicating that this species participated in the reaction during the desulfurization process, further proving that CuCl2·2H2O was involved in the desulfurization process. 2+ It participated in the oxidation reaction of propanethiol to generate RSSR.

[0120] pass Figures 2 to 10 Based on the desulfurization performance data of various embodiments and comparative examples, it can be seen that through N2 adsorption-desorption (… Figure 7 ) and Raman spectroscopy ( Figure 8 This demonstrated the role of carrier pretreatment (concentrated nitric acid oxidation); XRD before desulfurization ( Figure 9 The dispersion state of CuCl2 under different loadings was demonstrated; XPS ( Figures 2 to 6 ) and XRD after desulfurization ( Figure 10 This reveals the relationship between "acidic functional group oxidation" and "CuCl2 oxidation" under different CuCl2 loadings. 2+ The dynamic mechanism of coordination / oxidation synergy enables the desulfurizer of this invention to have a sulfur penetration capacity that is much higher than the theoretical value.

[0121] In summary, the desulfurizing agent of this invention achieves high-efficiency desulfurization in removing propanethiol from fermentation waste gas through the synergistic effect of the following three mechanisms:

[0122] The first removal mechanism: the acidic oxygen-containing functional groups on the surface of coal-based activated carbon oxidize and remove propanethiol, generating RSO3H;

[0123] Second removal mechanism: Cu 2+ Coordination adsorption with propanethiol for removal;

[0124] Third removal mechanism: Cu 2+ The oxidative removal of propanethiol yields dipropyl disulfide (RSSR).

[0125] Under different CuCl2 loading conditions, the contribution of the above three mechanisms varies: when the CuCl2 loading is 5 wt.%, the first removal mechanism is dominant; when it is 10 wt.%, both the first and second removal mechanisms are included; and when it reaches 20 wt.% to 30 wt.%, the synergistic effect of the first, second, and third removal mechanisms is included.

[0126] The preparation method of the copper chloride-modified activated carbon desulfurizer provided in the embodiments of the present invention, as well as the desulfurizer and its application, have at least one or a portion of the following advantages:

[0127] (1) Acidic oxygen-containing functional groups (carboxyl groups, acid anhydrides) are introduced onto the surface of coal-based activated carbon by concentrated nitric acid oxidation at room temperature, and carbon defects are generated by etching the carbon skeleton, providing sufficient anchoring points for CuCl2 loading; CuCl2 is then subjected to hydrothermal treatment. 2+ Coordination interactions with acidic oxygen-containing functional groups and / or Cu 2+ By embedding itself within carbon defects and avoiding high-temperature calcination while employing only low-temperature drying, thermally driven agglomeration of CuCl2 is prevented. The desulfurizer prepared by this method can achieve a CuCl2 mass loading of 5wt.%~30wt.%, and maintains good dispersion even at high loading levels, achieving significantly higher performance than traditional CuCl2 methods. 2+ The theoretical value of the breakthrough sulfur capacity based on the oxidation mechanism;

[0128] (2) Oxidation treatment of activated carbon with concentrated nitric acid at room temperature with a volume fraction of 60%~65% can introduce acidic oxygen-containing functional groups, including carboxyl groups and acid anhydrides, onto the surface of activated carbon, while simultaneously etching the carbon skeleton structure to generate carbon defects (confirmed by Raman spectroscopy). D / I G (From 1.1 to 1.2), providing dual protection for the dispersion of CuCl2 by chemical anchoring points and structural anchoring points;

[0129] (3) During the hydrothermal treatment process, some Cu 2+ It is embedded in carbon defects and reduced to form Cu. + This makes the surface of coal-based activated carbon electron-deficient, thereby endowing its surface acidic oxygen-containing functional groups with the ability to oxidize propanethiol, realizing a new mechanism for desulfurization by acidic oxygen-containing functional group oxidation.

[0130] (4) When the CuCl2 mass loading is 10 wt.%, the desulfurizer's breakthrough sulfur capacity for propanethiol reaches 310 mg / g, which is higher than that of traditional CuCl2. 2+The oxidation mechanism theory shows that the sulfur capacity (113 mg / g) is 2.7 times that of sulfur, and the desulfurization process simultaneously includes the oxidative removal of acidic oxygen-containing functional groups and Cu. 2+ Two mechanisms: coordination adsorption and removal;

[0131] (5) When the CuCl2 mass loading is 20wt.%~30wt.%, the desulfurizing agent's breakthrough sulfur capacity for propanethiol reaches 402mg / g and 489mg / g, respectively, which are 1.8 times and 1.4 times the traditional theoretical sulfur capacity (226mg / g and 339mg / g), respectively. The desulfurization process simultaneously includes the oxidative removal of acidic oxygen-containing functional groups and Cu 2+ Coordination adsorption removal and Cu 2+ The synergistic effect of three mechanisms of oxidative removal;

[0132] (6) The CuCl2-modified activated carbon desulfurizer prepared by the method of the present invention has the characteristics of high CuCl2 loading (5wt.%~30wt.%), good dispersibility, and excellent desulfurization performance; CuCl2 is loaded on activated carbon in multiple forms: CuCl2 coordinated with acidic oxygen-containing functional groups on the surface of activated carbon. 2+ Cu embedded in carbon defects + / Cu 2+ Cu, and Cu existing in the form of CuCl2·2H2O crystals 2+ The form of Cu varies under different loading levels (as confirmed by XRD and XPS characterization), enabling on-demand control of the desulfurization mechanism.

[0133] (7) The desulfurizing agent of this invention can be effectively applied to remove propanethiol from fermentation waste gas. When removing propanethiol in a fixed-bed reactor at 20~40℃, it is removed by oxidation of acidic oxygen-containing functional groups (generating RSO3H) and Cu. 2+ Coordination adsorption removal and Cu 2+ The synergistic effect of three mechanisms—oxidative removal (generating dipropyl disulfide RSSR)—achieves highly efficient desulfurization, with desulfurization performance significantly superior to that of a single mechanism.

[0134] (8) When the CuCl2 mass loading is 5 wt.%, the desulfurization process is mainly based on the oxidation removal of acidic oxygen-containing functional groups (the RSO3H peak in XPS is absolutely dominant); when the loading is 10 wt.%, it includes both oxidation removal and coordination adsorption removal; when the loading is 20 wt.%~30 wt.%, it includes the synergistic effect of the three mechanisms; thus achieving the effect of controlling the desulfurization path according to the loading.

[0135] While some embodiments of the present general inventive concept have been shown and described, those skilled in the art will understand that changes may be made to these embodiments without departing from the principles and spirit of the present general inventive concept, the scope of which is defined by the claims and their equivalents.

Claims

1. A method for preparing a copper chloride-modified activated carbon desulfurizing agent, characterized in that, The preparation method includes the following steps: Step S110: Grind the coal-based activated carbon to 40-80 mesh; Step S120: Place the ground coal-based activated carbon in a container, add concentrated nitric acid with a volume fraction of 60%~65%, and let it stand for 10~12 hours for room temperature oxidation treatment, wherein the amount of concentrated nitric acid added is 3~5 mL per gram of coal-based activated carbon. Step S130: Wash the coal-based activated carbon treated with concentrated nitric acid with deionized water until neutral, and dry it at 100~120℃ for 2~3 hours to obtain oxidized modified activated carbon; Step S140: Dissolve copper chloride dihydrate in deionized water to prepare a copper chloride aqueous solution, and load the copper chloride onto the oxidized modified activated carbon using a wet impregnation method, wherein the amount of deionized water used is 1.3~1.6 mL per gram of coal-based activated carbon; Step S150: transferring the activated carbon sample loaded with copper chloride into a hydrothermal reactor, and standing for 10-12 h at 100-120℃ for hydrothermal treatment, so that Cu 2+ is coordinated with the acidic oxygen-containing functional groups on the surface of the coal-based activated carbon and / or embedded into the carbon defects on the surface of the coal-based activated carbon, so that part of the Cu 2+ is reduced to generate Cu 2+ ; and + ​ Step S160: Dry the hydrothermally treated sample at 25~35℃ for 10~12h to obtain the copper chloride modified activated carbon desulfurizer, wherein the mass loading of CuCl2 in the copper chloride modified activated carbon desulfurizer is 5wt.%~30wt.%.

2. The preparation method according to claim 1, characterized in that, The specific surface area of the coal-based activated carbon is greater than or equal to 900 m 2 / g, the total pore volume is greater than or equal to 0.5 mL / g, and the ratio of mesopore volume to total pore volume is not less than 20%.

3. The preparation method according to claim 2, characterized in that, In step S120, The room temperature oxidation treatment with concentrated nitric acid introduces acidic oxygen-containing functional groups on the surface of the coal-based activated carbon, including carboxyl groups and acid anhydrides. Simultaneously, the concentrated nitric acid etches the carbon skeleton structure of the coal-based activated carbon to generate carbon defects on the surface of the coal-based activated carbon.

4. The preparation method according to claim 2, characterized in that, In step S150, During the hydrothermal treatment process, some Cu 2+ The carbon defects embedded in the surface of the coal-based activated carbon are reduced to form Cu. + This makes the surface of the coal-based activated carbon electron-deficient, enabling the acidic oxygen-containing functional groups on the surface of the coal-based activated carbon to acquire the ability to oxidize propanethiol.

5. The preparation method according to any one of claims 1-4, characterized in that, In the copper chloride modified activated carbon desulfurizer, the mass loading of CuCl2 is 10 wt.%.

6. The preparation method according to any one of claims 1-4, characterized in that, In the copper chloride modified activated carbon desulfurizer, the mass loading of CuCl2 is 20wt.%~30wt.%.

7. A copper chloride-modified activated carbon desulfurizing agent, wherein the copper chloride-modified activated carbon desulfurizing agent is prepared by the preparation method according to any one of claims 1-6, characterized in that, In the copper chloride-modified activated carbon desulfurizer, CuCl2 is loaded onto the coal-based activated carbon in the following ways: Cu coordinated to acidic oxygen-containing functional groups on the surface of the coal-based activated carbon 2+ , Cu embedded in carbon defects on the surface of the coal-based activated carbon + / Cu 2+ , Cu in the form of CuCl2-2H2O crystals 2+ any one of the foregoing or any combination thereof.

8. The copper chloride-modified activated carbon desulfurizer according to claim 7, characterized in that, When the CuCl2 mass loading is 5 wt.%, Cu mainly exists as Cu embedded in the carbon defects on the surface of the coal-based activated carbon. + It exists in the form of; When the CuCl2 mass loading is 10 wt.%, Cu simultaneously exists as Cu coordinated with acidic oxygen-containing functional groups. 2+ and Cu embedded in carbon defects + It exists in the form of; When the CuCl2 mass loading is 20 wt.%~30 wt.%, Cu simultaneously exists as Cu coordinated with acidic oxygen-containing functional groups. 2+ Cu embedded in carbon defects + It exists in the form of CuCl2·2H2O crystals.

9. The application of a copper chloride-modified activated carbon desulfurizer in the removal of propanethiol from fermentation waste gas, wherein the copper chloride-modified activated carbon desulfurizer is the copper chloride-modified activated carbon desulfurizer according to claim 7 or 8, or the copper chloride-modified activated carbon desulfurizer prepared by the preparation method according to any one of claims 1-6, characterized in that... The applications include: The copper chloride-modified activated carbon desulfurizer is loaded into a fixed-bed reactor, and fermentation waste gas containing propanethiol is passed through the copper chloride-modified activated carbon desulfurizer at 20-40°C, wherein propanethiol is removed by any one or any combination of the following removal mechanisms: The first removal mechanism involves the oxidative removal of propanethiol by acidic oxygen-containing functional groups on the surface of coal-based activated carbon, generating RSO3H. The second removal mechanism, Cu 2+ Coordination adsorption with propanethiol for removal; The third removal mechanism, Cu 2+ The oxidative removal of propanethiol yields dipropyl disulfide.

10. The application according to claim 9, characterized in that, When the mass loading of CuCl2 in the copper chloride modified activated carbon desulfurizer is 5 wt.%, desulfurization is completed by the first removal mechanism. When the mass loading of CuCl2 in the copper chloride modified activated carbon desulfurizer is 10 wt.%, desulfurization is completed simultaneously by the first removal mechanism and the second removal mechanism. When the mass loading of CuCl2 in the copper chloride modified activated carbon desulfurizer is 20wt.%~30wt.%, desulfurization is completed simultaneously by the first removal mechanism, the second removal mechanism and the third removal method.