A method for preparing sulfonated COF ion transport tubular uniformly porous ceramic membrane and its application

By constructing a ring-shaped radial electric field structure with an internal cathode and an external anode, and an STCOF functional layer induced by an LDH template, the problems of complex ion composition and competitive migration of multiple metal ions in lithium-ion leachate are solved, achieving efficient recovery of lithium resources and removal of impurities, and making it suitable for separation processes in complex environments.

CN123102167APending Publication Date: 2026-11-17SHANDONG JIANZHU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611421729.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion leachate recycling processes suffer from problems such as complex ion composition, low lithium-ion concentration, competitive migration of multiple metal ions, and the difficulty of traditional membrane separation systems to balance selectivity, stability, and continuous operation. In particular, the functional layer suffers from insufficient stability, reduced transport performance, and limited removal efficiency of impurity ions.

Method used

A sulfonated COF ion transport tubular uniform porous ceramic membrane is used. By constructing an annular radial electric field structure with an internal cathode and an external anode, and combining it with LDH template induction to build an STCOF functional layer of a certain thickness on the surface of the ceramic substrate, the sulfonic acid groups are used to adjust the interfacial charge environment and ion transport behavior of the membrane, so as to achieve directional ion migration and simultaneous removal of impurities.

Benefits of technology

It improves the enrichment efficiency and recovery purity of lithium resources, reduces separation costs, and realizes efficient resource recycling of lithium resources in complex lithium-containing waste liquids. It is suitable for separation processes under high temperature, high pressure and strong acid and strong alkali environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102167A_ABST
    Figure CN123102167A_ABST
Patent Text Reader

Abstract

A method for preparing a sulfonated COF ion transport tubular uniform-pore ceramic membrane and its application are disclosed. This invention belongs to the field of high-precision inorganic membrane material preparation technology. This invention aims to solve the problems existing in the resource recovery process of lithium-containing leachate, such as complex ion composition, low lithium-ion concentration, competitive migration of multiple metal ions, and the difficulty of traditional membrane separation systems in simultaneously achieving selectivity, stability, and continuous operation. Method: 1. Preparation of an inorganic ceramic membrane dispersion; 2. Spraying the inorganic ceramic membrane dispersion onto the surface of a tubular ceramic substrate and sintering; 3. Preparation of a hydroxylated LDH template; 4. Preparation of a sulfonated COF layer. Application: It is used to prepare an electrodialysis reactor for treating battery leachate and separating Li from the battery leachate. + And divalent metal ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-precision inorganic membrane material preparation technology. Background Technology

[0002] The rapid development of new energy vehicles, energy storage, and portable electronic devices has led to a surge in demand for lithium batteries, resulting in a corresponding increase in the emissions of waste lithium batteries. Waste batteries are rich in high-value metals such as lithium, cobalt, nickel, and manganese, but also contain pollutants such as electrolytes and heavy metals. Improper disposal not only wastes resources but also severely pollutes water, soil, and the ecological environment, making the development of green and efficient recycling technologies essential. Current recycling methods mainly include pyrometallurgy, hydrometallurgy, and biometallurgy, with hydrometallurgy being the most widely used due to its high recovery rate, low energy consumption, and strong adaptability. After acid leaching, the cathode material forms a mixed system of multiple metal ions. However, since the metal ions have similar properties, traditional precipitation, extraction, and adsorption methods suffer from poor selectivity, high reagent consumption, and are prone to secondary pollution, making it difficult to achieve efficient and selective separation and recovery of lithium.

[0003] Membrane separation technology has attracted widespread attention in the field of lithium resource recycling due to its advantages such as low energy consumption, mild operating conditions, ease of continuous operation, and environmental friendliness. However, in complex lithium-containing systems such as leachate from spent lithium-ion batteries, Li... + Low concentration, and often accompanied by Co 2+ Ni 2+ Mn 2+ The coexistence of multiple metal ions makes traditional membrane separation processes susceptible to competitive migration, concentration polarization, and membrane fouling, limiting lithium recovery efficiency and separation purity. While ceramic membranes possess excellent acid and alkali resistance, high-temperature resistance, and mechanical stability, their ion selectivity is insufficient, making it difficult to meet the fine separation requirements of complex multi-ion systems. Covalent organic frameworks (COFs) possess tunable structures and abundant functional groups; combining them with ceramic substrates to construct composite membranes can enhance the ion transport control capabilities of the membrane interface. However, existing COF / ceramic composite membranes primarily focus on thin-layer structure construction and the sieving performance of the membrane material itself, still suffering from insufficient functional layer stability, limited resistance to interference in complex systems, and the difficulty of simultaneously removing impurities relying solely on membrane separation.

[0004] Therefore, existing lithium-containing leachate resource recovery processes suffer from problems such as complex ion composition, low lithium-ion concentration, competitive migration of multiple metal ions, and the difficulty of traditional membrane separation systems in simultaneously achieving selectivity, stability, and continuous operation. In particular, existing functionalized membrane materials are prone to insufficient interfacial bonding, degraded transport performance, and limited impurity ion removal efficiency under long-term electric fields. There is an urgent need to develop a novel membrane separation system with a highly stable ion transport interface, combined with electric field-driven ion directional migration and simultaneous impurity removal, to improve lithium resource recovery efficiency from complex lithium-containing wastewater, reduce separation costs, and achieve green and efficient resource recycling. Summary of the Invention

[0005] This invention aims to address the problems existing in the resource recovery process of lithium-containing leachate, such as complex ion composition, low lithium ion concentration, competitive migration of multiple metal ions, and the difficulty of traditional membrane separation systems in achieving selectivity, stability, and continuous operation. It provides a method for preparing sulfonated COF ion transport tubular uniform porous ceramic membrane and its application.

[0006] A method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane, comprising the following steps:

[0007] 1. Add nano-titanium dioxide ethanol dispersion and nano-alumina ethanol dispersion to anhydrous ethanol and ultrasonically disperse to obtain inorganic ceramic membrane dispersion.

[0008] 2. The inorganic ceramic membrane dispersion is sprayed onto the surface of the tubular ceramic substrate and then dried. The spraying and drying are repeated multiple times to obtain a ceramic membrane substrate with a uniform surface coating. The ceramic membrane substrate with a uniform surface coating is sintered to obtain the sintered ceramic membrane substrate.

[0009] 3. Co(NO3)2·6H2O, Al(NO3)3·9H2O, urea and NH4F are dissolved in deionized water to obtain a precursor solution. The sintered ceramic membrane substrate is immersed in the precursor solution and heated to react. Then it is taken out and cooled naturally to obtain an LDH template. The LDH template is hydroxylated to obtain a hydroxylated LDH template.

[0010] IV. Add 2,5-diaminobenzenesulfonic acid, 1,3,5-trialdehyde phloroglucinol and acetic acid to a mixed solvent to obtain a treatment solution. Immerse the hydroxylated LDH template in the treatment solution and heat it to react. Then remove it and let it cool naturally to obtain a sulfonated COF ion transport tubular uniform porous ceramic membrane.

[0011] An application of a sulfonated COF ion transport tubular uniform-pore ceramic membrane: utilizing it to prepare an electrodialysis reactor for treating battery leachate and separating Li from the battery leachate. + and divalent metal ions; the divalent metal ions are Co 2+ Ni 2+ and Mn 2+ One or a combination of several of them.

[0012] The beneficial effects of this invention are:

[0013] The STCOF tubular uniform-pore ceramic membrane provided by this invention possesses excellent mechanical strength and a relatively uniform pore size distribution, making it suitable for separation processes under complex environments such as high temperature, high pressure, and strong acids and alkalis. Compared with the prior art, this invention has the following advantages:

[0014] ① This invention constructs a ring-shaped radial electric field structure with an internal cathode and an external anode. Compared with traditional flat-plate electrodialysis, the ring-shaped electric field can shorten the ion migration path and improve the electric field utilization efficiency. Because divalent ions (Co... 2+ Ni 2+ Mn 2+ The electric driving force on (etc.) is greater than that of the unit price Li + It is easier to migrate through STCOF nanochannels; while Li + Due to the influence of higher hydration energy and larger hydration radius, its migration is suppressed, thereby achieving preferential permeation of divalent ions and selective retention of Li+, thus improving the efficiency of lithium resource enrichment.

[0015] ② This invention utilizes the induction effect of an LDH template to construct a STCOF functional layer of a certain thickness on the surface of a ceramic substrate. The LDH template not only provides a uniform heterogeneous nucleation interface, promoting the in-situ growth of STCOF precursors on the ceramic substrate surface, but also facilitates the formation of a fully covered functional transport layer. The formed STCOF layer can effectively regulate the ion transport path within the membrane. By increasing the ion transmembrane migration distance, extending the mass transfer process, and adjusting the local ion transport environment within the membrane, it enhances the transport resistance during lithium ion migration, achieving selective enrichment of lithium ions in complex lithium-containing systems. Unlike traditional ultrathin COF sieving membranes that mainly rely on extremely thin functional layers for rapid ion transfer, this invention constructs a STCOF functional layer structure of a certain thickness, allowing ions to undergo a more thorough transport regulation process within the membrane, reducing the transmembrane migration rate of lithium ions under electric field drive, thereby reducing direct lithium ion loss. Simultaneously, the introduction of sulfonic acid groups improves the hydrophilicity and ion exchange capacity of the membrane layer, improving the mass transfer conditions at the membrane-liquid interface, enabling the membrane structure to maintain good ion selection regulation performance while retaining lithium ion barrier capabilities.

[0016] ③ This invention uses a tubular ceramic membrane as the supporting substrate. Ceramic materials possess excellent mechanical strength, resistance to acid and alkali corrosion, high-temperature resistance, and long-term operational stability, enabling them to adapt to complex working conditions such as acid leaching solutions from spent lithium-ion batteries. Simultaneously, the tubular structure has a high packing density and specific surface area, allowing for large-scale integration of membrane modules; its through-flow channel structure helps reduce fluid resistance, enhance mass transfer processes, and improve membrane flux and processing capacity, demonstrating promising prospects for engineering applications.

[0017] ④ This invention deeply couples STCOF tubular uniform-pore ceramic membranes with electrodialysis technology, achieving synergistic enhancement of membrane selective separation and electric field-driven migration. The applied electric field provides a continuous driving force for ion transport, promoting the directional migration and enrichment of target ions, effectively overcoming the problems of low mass transfer rate and severe concentration polarization in traditional pressure-driven membrane processes. Simultaneously, this system can achieve continuous separation and resource recovery without additional chemical reagents, offering advantages such as low energy consumption, green process, simple operation, and ease of continuous operation. It is suitable for the efficient recovery of lithium resources from waste lithium-ion battery leachates, salt lake brines, and other complex multi-ion systems.

[0018] ⑤ This invention utilizes functional groups in the STCOF membrane layer to regulate the interfacial charge environment and ion transport behavior, promoting Co under the action of an electric field. 2+ Ni 2+ Mn 2+ This allows divalent metal ions to migrate directionally to the electrode region, reducing their competitive impact on the lithium-ion enrichment process. During electrodialysis, OH- ions generated at the cathode... - A localized alkaline environment is created, causing the migrated divalent metal ions to precipitate as hydroxides in situ, thus achieving simultaneous removal of impurity ions. Through the synergistic effect of electromigration and precipitation reaction, the content of divalent metal ions in the leachate can be effectively reduced, improving the purity of lithium resource recovery and achieving integrated lithium enrichment and impurity removal in complex lithium-containing systems. Attached Figure Description

[0019] Figure 1 SEM images of the surface and cross-section of the STCOF tubular uniformly porous ceramic membrane prepared in Example 1: (a) Surface morphology of STCOF functional layer, (b) Cross-sectional morphology of STCOF functional layer, (c) Overall cross-sectional structure of STCOF tubular uniformly porous ceramic membrane, (d) Interface bonding structure between STCOF functional layer and tubular ceramic substrate.

[0020] Figure 2 The image shows the XRD pattern of the STCOF layer in the STCOF tubular uniformly porous ceramic membrane prepared in Example 1.

[0021] Figure 3 Fourier transform infrared spectra of 1,3,5-trialdehyde phloroglucinol, 2,5-diaminobenzenesulfonic acid monomers, and the STCOF functional layer in Example 1.

[0022] Figure 4 The attached figures and pore size distribution diagrams of the STCOF tubular uniform porous ceramic membrane prepared in Example 1 are shown. (a) N2 adsorption-desorption isotherm, (b) pore size distribution curve.

[0023] Figure 5 This is a schematic diagram of the electrodialysis reactor structure in Example 2;

[0024] Figure 6 for Figure 5 Sectional view at CC;

[0025] Figure 7 for Figure 6 Sectional view at point AA;

[0026] Figure 8 for Figure 6 Sectional view at point BB;

[0027] Figure 9 This is a three-dimensional structural diagram of the electrodialysis reactor in Example 2;

[0028] Figure 10 This is the operating system of the electrodialysis reactor in Example 2;

[0029] Figure 11 Example 2 illustrates the effect of STCOF tubular uniform-pore ceramic membrane on Li under different pH and voltage conditions of 4.5V. + Retention rate and Co 2+ Transmittance variation curve (a) and the effect of STCOF tubular uniform-pore ceramic membrane on Li under different voltages and pH 7 conditions. + and Co 2+ Comparison of permeation rates (b);

[0030] Figure 12 In Example 3, under the condition of an applied voltage, Li + Co 2+ K + and Na + A comparison of the changes in the concentration of each ion in the electrolyte in the mixed system as the operating time increases;

[0031] Figure 13 Example 4 shows a single Co under an applied voltage. 2+ System and single Li + A comparison chart of ion permeation rates in the system;

[0032] Figure 14 This is a stability test graph for Example 5 during continuous operation for 24 hours at pH 7 and voltage 4.5V. Detailed Implementation

[0033] The technical solution of the present invention is not limited to the specific embodiments listed below, but also includes any combination of the specific embodiments.

[0034] Specific Implementation Method 1: This implementation method describes a method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane, which is carried out according to the following steps:

[0035] 1. Add nano-titanium dioxide ethanol dispersion and nano-alumina ethanol dispersion to anhydrous ethanol and ultrasonically disperse to obtain inorganic ceramic membrane dispersion.

[0036] 2. The inorganic ceramic membrane dispersion is sprayed onto the surface of the tubular ceramic substrate and then dried. The spraying and drying are repeated multiple times to obtain a ceramic membrane substrate with a uniform surface coating. The ceramic membrane substrate with a uniform surface coating is sintered to obtain the sintered ceramic membrane substrate.

[0037] 3. Co(NO3)2·6H2O, Al(NO3)3·9H2O, urea and NH4F are dissolved in deionized water to obtain a precursor solution. The sintered ceramic membrane substrate is immersed in the precursor solution and heated to react. Then it is taken out and cooled naturally to obtain an LDH template. The LDH template is hydroxylated to obtain a hydroxylated LDH template.

[0038] IV. Add 2,5-diaminobenzenesulfonic acid, 1,3,5-trialdehyde phloroglucinol and acetic acid to a mixed solvent to obtain a treatment solution. Immerse the hydroxylated LDH template in the treatment solution and heat it to react. Then remove it and let it cool naturally to obtain a sulfonated COF ion transport tubular uniform porous ceramic membrane.

[0039] This specific implementation differs from traditional flat-plate electrodialysis membrane modules. It uses sulfonated COF (STCOF) tubular ceramic membranes as ion transport units. A radial electric field is constructed by setting a cathode inside the membrane and an anode outside the membrane, causing ions in the solution to migrate directionally along the membrane thickness, thus achieving coupling between the electric field-driven process and the membrane separation process.

[0040] The STCOF tubular uniformly porous ceramic membrane uses a uniformly porous ceramic membrane as the supporting substrate, forming a uniformly porous structure after coating in step two. An LDH template-induced strategy promotes the in-situ growth of the STCOF functional layer on the ceramic substrate surface, forming a continuous ion transport interface with a certain thickness. This structure enhances the bonding stability between the STCOF layer and the ceramic substrate, and achieves migration regulation in complex multi-ion systems by extending the ion transmembrane transport path, controlling the interfacial charge environment, and regulating ion exchange behavior. Simultaneously, the sulfonic acid groups introduced into the membrane layer improve the hydrophilicity and ion transport capacity of the membrane material, improve the mass transfer process at the membrane / solution interface, and enhance the membrane's operational stability.

[0041] During electrodialysis, an applied radial electric field drives the directional migration of metal ions in the solution to be treated, Co 2+ Ni 2+ Mn 2+Divalent metal ions migrate towards the cathode region under the influence of an electric field and the interface regulation of the STCOF functional layer. The transmembrane migration of lithium ions is regulated by membrane transport resistance and ion competition, thus achieving lithium ion enrichment and recovery. The divalent metal ions that migrate to the cathode region react with OH- produced by the reduction of cathode water. - The reaction occurs, generating the corresponding hydroxide precipitate, thus achieving in-situ removal of impurity ions.

[0042] Through the synergistic effect of the above-mentioned membrane interface regulation, electric field enhanced migration and electrochemical precipitation process, this specific embodiment realizes the integrated treatment of lithium resource enrichment and impurity removal, and improves the separation efficiency and recovery purity in complex lithium-containing leachate systems.

[0043] Principle: This implementation uses an Al2O3 tubular ceramic membrane as the supporting substrate. A sulfonated COF functional layer with a continuous covering structure and stable bonding performance is constructed in situ on its surface using an LDH template-induced strategy, forming a composite membrane interface with both mechanical stability and ion transport regulation capabilities. The LDH template not only promotes the uniform growth of the STCOF layer on the ceramic substrate surface, improving membrane integrity, but also extends the ion transmembrane transport path and enhances the membrane's regulatory effect on ion migration behavior by constructing an organic functional layer of a certain thickness. The STCOF tubular uniform-pore ceramic membrane is assembled inside the electrodialysis reactor, with the solution to be treated located outside the tubular ceramic membrane and the catholyte located inside. A ring-shaped radial electric field is formed through the external anode and the internal cathode. Compared to the traditional planar electrodialysis structure, this radial electric field can shorten the ion migration distance, improve the efficiency of the electric field, promote the rapid migration of ions near the membrane surface, and reduce concentration polarization. Under the action of the applied electric field, different metal ions in the lithium-containing solution undergo directional migration driven by the electric field. The sulfonic acid groups in the STCOF membrane serve as fixed functional sites, regulating the charge environment and ion exchange behavior at the membrane / solution interface, and promoting Co... 2+ Ni 2+ Mn 2+ The migration and transport of divalent metal ions reduces their competitive role in the lithium enrichment process. Simultaneously, lithium ions are affected by the transport resistance of the STCOF functional layer and the competitive migration behavior of ions within the membrane, resulting in a reduced transmembrane migration rate and thus achieving lithium ion enrichment on the side of the untreated liquid. During electrodialysis, OH- is continuously generated in the cathode region due to the electroreduction reaction of water molecules. - This creates a localized alkaline environment, allowing Co to migrate to the cathode region. 2+ Ni 2+ Mn 2+Divalent metal ions are precipitated in situ to form hydroxides, achieving simultaneous removal of impurity metal ions. This process combines membrane ion regulation, electric field migration, and electrochemical precipitation to construct a synergistic separation mechanism of "ion migration regulation—in-situ impurity removal—lithium enrichment and recovery".

[0044] The beneficial effects of this embodiment are:

[0045] The STCOF tubular uniform-pore ceramic membrane provided in this embodiment possesses excellent mechanical strength and a relatively uniform pore size distribution, making it suitable for separation processes under complex environments such as high temperature, high pressure, and strong acids and alkalis. Compared with the prior art, this embodiment has the following advantages:

[0046] ① This embodiment constructs a ring-shaped radial electric field structure with an internal cathode and an external anode. Compared with traditional flat-plate electrodialysis, the ring-shaped electric field can shorten the ion migration path and improve the electric field utilization efficiency. Because divalent ions (Co... 2+ Ni 2+ Mn 2 + The electric driving force on (etc.) is greater than that of the unit price Li + It is easier to migrate through STCOF nanochannels; while Li + Due to the influence of higher hydration energy and larger hydration radius, its migration is suppressed, thereby achieving preferential permeation of divalent ions and selective retention of Li+, thus improving the efficiency of lithium resource enrichment.

[0047] ② In this embodiment, an STCOF functional layer of a certain thickness is constructed on the surface of a ceramic substrate through the induction effect of an LDH template. The LDH template not only provides a uniform heterogeneous nucleation interface, promoting the in-situ growth of STCOF precursors on the ceramic substrate surface, but also facilitates the formation of a fully covered functional transport layer. The formed STCOF layer can effectively regulate the ion transport path within the membrane. By increasing the ion transmembrane migration distance, extending the mass transfer process, and adjusting the local ion transport environment within the membrane, it enhances the transport resistance during lithium ion migration, achieving selective enrichment of lithium ions in complex lithium-containing systems. Unlike traditional ultrathin COF sieving membranes that mainly rely on extremely thin functional layers to achieve rapid ion transfer, this embodiment constructs an STCOF functional layer structure of a certain thickness, allowing ions to undergo a more thorough transport regulation process within the membrane, reducing the transmembrane migration rate of lithium ions under electric field drive, thereby reducing direct lithium ion loss. At the same time, the introduction of sulfonic acid groups improves the hydrophilicity and ion exchange capacity of the membrane layer, improving the mass transfer conditions at the membrane-liquid interface, enabling the membrane structure to maintain good ion selection regulation performance while retaining lithium ion barrier capabilities.

[0048] ③ This embodiment uses a tubular ceramic membrane as the supporting substrate. Ceramic materials possess excellent mechanical strength, resistance to acid and alkali corrosion, high-temperature resistance, and long-term operational stability, enabling them to adapt to complex working environments such as acid leaching solutions from spent lithium-ion batteries. Simultaneously, the tubular structure has a high packing density and specific surface area, allowing for large-scale integration of membrane modules; its through-flow channel structure helps reduce fluid resistance, enhance mass transfer processes, and improve membrane flux and processing capacity, demonstrating promising prospects for engineering applications.

[0049] ④ This embodiment deeply couples STCOF tubular uniform-pore ceramic membranes with electrodialysis technology, achieving synergistic enhancement of membrane selective separation and electric field-driven migration. The applied electric field provides a continuous driving force for ion transport, promoting the directional migration and enrichment of target ions, effectively overcoming the problems of low mass transfer rate and severe concentration polarization in traditional pressure-driven membrane processes. Simultaneously, this system can achieve continuous separation and resource recovery without additional chemical reagents, offering advantages such as low energy consumption, green process, simple operation, and ease of continuous operation. It is suitable for the efficient recovery of lithium resources from waste lithium-ion battery leachates, salt lake brines, and other complex multi-ion systems.

[0050] ⑤ This embodiment utilizes functional groups in the STCOF film layer to regulate the interfacial charge environment and ion transport behavior, promoting Co under the action of an electric field. 2+ Ni 2+ Mn 2+ This allows divalent metal ions to migrate directionally to the electrode region, reducing their competitive impact on the lithium-ion enrichment process. During electrodialysis, OH- ions generated at the cathode... - A localized alkaline environment is created, causing the migrated divalent metal ions to precipitate as hydroxides in situ, thus achieving simultaneous removal of impurity ions. Through the synergistic effect of electromigration and precipitation reaction, the content of divalent metal ions in the leachate can be effectively reduced, improving the purity of lithium resource recovery and achieving integrated lithium enrichment and impurity removal in complex lithium-containing systems.

[0051] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that: the nano-titanium dioxide ethanol dispersion mentioned in step one is specifically obtained by ultrasonically dispersing nano-titanium dioxide in anhydrous ethanol, and the particle size of the nano-titanium dioxide is 5nm~20nm; the nano-alumina ethanol dispersion mentioned in step one is specifically obtained by ultrasonically dispersing nano-alumina in anhydrous ethanol, and the particle size of the nano-alumina is 5nm~20nm. Everything else is the same as in Specific Implementation Method One.

[0052] Specific Implementation Method 3: This implementation method differs from Specific Implementation Method 1 or 2 in that: the mass ratio of nano-titanium dioxide to nano-alumina in the inorganic ceramic membrane dispersion in step 1 is 1:(1~5); the total mass concentration of nano-titanium dioxide and nano-alumina in the inorganic ceramic membrane dispersion in step 1 is 10%~30%. Everything else is the same as in Specific Implementation Method 1 or 2.

[0053] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that: the outer diameter of the tubular ceramic substrate described in step two is 8mm~20mm, the inner diameter is 4mm~12mm, and the wall thickness is 1mm~3mm. Furthermore, the tubular ceramic substrate has a multi-level porous structure, consisting of a macroporous framework layer and a microporous transport layer uniformly distributed on the surface. The pore size of the macroporous framework layer is 0.1μm~1μm, and the porosity of the macroporous framework layer is 30%~50%. The pore size of the microporous transport layer is 0.1μm~0.3μm. In step two, the inorganic ceramic membrane dispersion is sprayed onto the surface of the tubular ceramic substrate, and then dried at a temperature of 60℃~80℃ for 1min~2min. This spraying and drying process is repeated multiple times until the coating thickness reaches 0.1μm~1μm, resulting in a uniformly coated ceramic membrane substrate. The uniformly coated ceramic membrane substrate is then heated to 900℃~1100℃ at a heating rate of 5℃ / min~10℃ / min, and sintered at 900℃~1100℃ for 2h~3h. Other steps are the same as in specific embodiments one to three.

[0054] Specific Implementation Method Five: This implementation method differs from Specific Implementation Methods One to Four in that the concentrations of Co(NO3)2·6H2O in the precursor solution described in step three are 0.03 mol / L to 0.1 mol / L, the concentrations of Al(NO3)3·9H2O are 0.008 mol / L to 0.02 mol / L, the concentration of urea is 0.08 mol / L to 0.2 mol / L, and the concentration of NH4F is 0.1 mol / L to 0.2 mol / L. Everything else is the same as in Specific Implementation Methods One to Four.

[0055] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One to Five in that: in step three, the sintered ceramic film substrate is immersed in the precursor solution and heated for 12 to 72 hours at a temperature of 100℃ to 140℃; the hydroxylation treatment in step three is specifically carried out as follows: the LDH template is immersed in toluene, and then 3-aminopropyltriethoxysilane is added, and soaked at room temperature for 5 to 24 hours; the volume ratio of 3-aminopropyltriethoxysilane to toluene is 1:(280 to 290). Everything else is the same as in Specific Implementation Methods One to Five.

[0056] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One to Six in that: in step four, the concentration of 2,5-diaminobenzenesulfonic acid in the treatment solution is 0.01 mol / L to 0.05 mol / L, the concentration of 1,3,5-trialdehyde phloroglucinol is 0.001 mol / L to 0.005 mol / L, and the concentration of acetic acid is 3 mol / L to 5 mol / L; the mixed solvent in step four is a combination of dioxane and mesitylene in a volume ratio of 1:(1~2); in step four, the hydroxylated LDH template is immersed in the treatment solution and heated for 12 h to 72 h at a temperature of 100℃ to 140℃. Everything else is the same as in Specific Implementation Methods One to Six.

[0057] Specific Implementation Method Eight: This implementation method describes the application of a sulfonated COF ion transport tubular uniform-pore ceramic membrane. It utilizes this membrane to prepare an electrodialysis reactor for treating battery leachate and separating Li from the battery leachate. + and divalent metal ions; the divalent metal ions are Co 2+ Ni 2+ and Mn 2+ One or a combination of several of them.

[0058] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method Eight in that: the electrodialysis reactor comprises a resin shell 1, an adjustable voltage regulator 2, a sulfonated COF ion transport tubular ceramic membrane 3, a cathode rod 4, and an anode mesh 5; a main channel 6 is arranged along the length direction at the center of the resin shell 1, and multiple tubular membrane mounting chambers are arranged along the circumferential and length directions inside the resin shell 1, with the tubular membrane mounting chambers connected to the main channel 6 via branch channels 7; the anode mesh 5 is evenly distributed on the sidewalls of the tubular membrane mounting chambers, and a sulfonated COF ion transport tubular membrane is arranged along the length direction at the center of the tubular membrane mounting chamber. An ion transport tube-type uniformly porous ceramic membrane 3 is sealed and fixed using a sealing ring 8. A cathode rod 4 is arranged along the length of the center of the sulfonated COF ion transport tube-type uniformly porous ceramic membrane 3, and an annular gap of 8mm~10mm is provided between the sulfonated COF ion transport tube-type uniformly porous ceramic membrane 3 and the anode mesh 5, and an annular gap of 2mm~6mm is provided between the sulfonated COF ion transport tube-type uniformly porous ceramic membrane 3 and the cathode rod 4. The cathode rod 4 and the anode mesh 5 are respectively connected to an adjustable regulated power supply 2. The cathode rod 4 is a titanium rod with a diameter of 1mm~3mm; the anode mesh 5 is a titanium mesh. Other aspects are the same as in specific embodiment eight.

[0059] The specific implementation method uses multiple COF tubular ceramic membranes connected in parallel to form a modular reactor, which can significantly improve the membrane area utilization rate and ion treatment flux. Combined with the excellent mechanical strength and acid and alkali corrosion resistance of the ceramic membrane and the stable ion transport characteristics of the STCOF functional layer, the device is suitable for continuous and large-scale resource recycling of complex systems such as waste lithium-ion battery leachate and lithium-containing industrial waste liquid, and has good industrial application prospects.

[0060] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Method Eight or Nine in that the electrodialysis reactor is used according to the following steps:

[0061] 1. Under the condition of a circulation flow rate of 50 mL / min to 100 mL / min, the solution to be treated is introduced into the main channel 6 of the resin shell 1. The solution to be treated flows into the annular gap between each sulfonated COF ion transport tubular uniform porous ceramic membrane 3 and the anode mesh 5. Under the condition of a circulation flow rate of 50 mL / min to 100 mL / min, the catholyte is introduced into the interior of each sulfonated COF ion transport tubular uniform porous ceramic membrane 3.

[0062] The solution to be treated is Li-containing + The battery leaching solution contains divalent ions; the cathode solution is a 0.01 mol / L to 0.2 mol / L sodium chloride solution.

[0063] II. By adjusting the applied voltage to 4V~5V or the current to 0.01A~0.05A, a stable annular radial electric field is formed on both sides of the sulfonated COF ion transport tube type uniform porous ceramic membrane 3 for electrodialysis. Divalent metal ions in the solution to be treated migrate to the cathode region through the sulfonated COF ion transport tube type uniform porous ceramic membrane 3, and form hydroxide precipitates in the cathode region, which flow out with the catholyte, thus achieving the removal of impurity ions; Li + Without passing through the sulfonated COF ion transport tubular uniform porous ceramic membrane 3, it flows out with the desalination solution, realizing Li + The recycling process is the same as in one of the specific implementation methods eight or nine.

[0064] The beneficial effects of the present invention are verified using the following embodiments:

[0065] Example 1:

[0066] A method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane, comprising the following steps:

[0067] 1. Under a power of 150W, nano-titanium dioxide ethanol dispersion and nano-alumina ethanol dispersion were added to anhydrous ethanol and ultrasonically dispersed for 1 hour to obtain inorganic ceramic membrane dispersion.

[0068] The nano-titanium dioxide ethanol dispersion is specifically obtained by ultrasonically dispersing nano-titanium dioxide in anhydrous ethanol for 1 hour at a power of 150W, and the average particle size of the nano-titanium dioxide is 10nm; the nano-alumina ethanol dispersion is specifically obtained by ultrasonically dispersing nano-alumina in anhydrous ethanol for 1 hour at a power of 150W, and the average particle size of the nano-alumina is 10nm.

[0069] The inorganic ceramic membrane dispersion contains a 1:4 mass ratio of nano-titanium dioxide to nano-alumina; the total mass concentration of nano-titanium dioxide and nano-alumina in the inorganic ceramic membrane dispersion is 10%.

[0070] 2. The inorganic ceramic membrane dispersion was sprayed onto the surface of a tubular ceramic substrate, and then dried at 60℃ for 1 min. The spraying and drying were repeated 4 times until the coating thickness was 0.5 μm, resulting in a ceramic membrane substrate with a uniform surface coating. The ceramic membrane substrate with a uniform surface coating was heated to 1050℃ at a heating rate of 10℃ / min, and sintered at 1050℃ for 3 h to obtain the sintered ceramic membrane substrate.

[0071] The tubular ceramic substrate is an Al2O3 tubular ceramic substrate with an outer diameter of 10 mm, an inner diameter of 7 mm, an effective film length of 150 mm, and a wall thickness of 1.5 mm. The tubular ceramic substrate has a multi-level porous structure, consisting of a macroporous framework layer and a microporous transport layer uniformly distributed on the surface. The macroporous framework layer has a pore size of 1 μm and a porosity of 35%, while the microporous transport layer has a pore size of 0.3 μm.

[0072] 3. Co(NO3)2·6H2O, Al(NO3)3·9H2O, urea and NH4F were dissolved in deionized water to obtain a precursor solution. The sintered ceramic film substrate was immersed in the precursor solution and heated for 72 h at 120 °C. Then it was taken out and cooled naturally to obtain an LDH template. The LDH template was immersed in toluene and then added to 3-aminopropyltriethoxysilane. It was soaked at room temperature for 24 h to obtain the hydroxylated LDH template, which is the substrate with an LDH layer grown.

[0073] The precursor solution contains 0.03 mol / L Co(NO3)2·6H2O, 0.008 mol / L Al(NO3)3·9H2O, 0.08 mol / L urea, and 0.1 mol / L NH4F.

[0074] The volume ratio of 3-aminopropyltriethoxysilane to toluene is 1:285;

[0075] IV. 2,5-Diaminobenzenesulfonic acid (Pa-SO3H), 1,3,5-trialdehyde phloroglucinol (Tp) and acetic acid (HOAc) were added to a mixed solvent to obtain a treatment solution. The hydroxylated LDH template was immersed in the treatment solution and heated for 72 hours at a temperature of 120°C. Then it was taken out and cooled naturally to obtain a sulfonated COF ion transport tubular uniform porous ceramic membrane, named STCOF tubular uniform porous ceramic membrane. The sulfonated COF layer on the surface of the tubular uniform porous ceramic membrane was named STCOF functional layer.

[0076] The concentration of 2,5-diaminobenzenesulfonic acid in the treatment solution is 0.01 mol / L, the concentration of 1,3,5-trialdehyde phloroglucinol is 0.001 mol / L, and the concentration of acetic acid is 3 mol / L; the mixed solvent is a combination of dioxane and mesitylene in a volume ratio of 1:1.

[0077] The tubular ceramic substrate described in this embodiment was purchased from Guizhou Membrane New Material Technology Co., Ltd.

[0078] Figure 1 Figures (a) and (b) show the surface and cross-sectional SEM images of the STCOF tubular uniformly porous ceramic membrane prepared in Example 1. The images show the surface morphology of the STCOF functional layer, the cross-sectional morphology of the STCOF functional layer, the overall cross-sectional structure of the STCOF tubular uniformly porous ceramic membrane, and the interface bonding structure between the STCOF functional layer and the tubular ceramic substrate. As shown in Figures (a) and (b), the surface of the prepared STCOF tubular uniformly porous ceramic membrane is continuous, uniform, and free of obvious cracks and defects, indicating that the STCOF layer achieves good coverage on the ceramic substrate surface. Figure (c) shows the overall cross-sectional SEM image of the tubular ceramic substrate, indicating that the substrate has a continuous porous structure. Figure (d) shows that the STCOF functional layer grows uniformly on the surface of the tubular ceramic substrate and forms a tight interface with the substrate. The lower ceramic support retains a rich pore structure, which can provide low-resistance channels for the mass transfer process, while the surface STCOF functional layer endows the membrane with selective separation function.

[0079] Figure 2 The image shows the XRD pattern of the STCOF layer in the STCOF tubular uniformly porous ceramic membrane prepared in Example 1. The experimental diffraction peaks and simulated diffraction peaks show a good correspondence, indicating that 1,3,5-trialdehyde phloroglucinol successfully underwent a condensation reaction with the Pa-SO3H monomer to form a COF material with a regular crystal structure. The resulting COF material exhibits high crystallinity and a well-ordered interlayer stacking structure.

[0080] Figure 3The Fourier transform infrared spectra of 1,3,5-trialdehyde phloroglucinol, 2,5-diaminobenzenesulfonic acid monomers, and the STCOF functional layer in Example 1 are shown. Compared with the monomer 1,3,5-trialdehyde phloroglucinol, its Fourier transform infrared spectrum at 1609 cm⁻¹ is significantly higher. -1 The characteristic peak attributable to the C=O stretching vibration of the aldehyde group almost disappears in the product; simultaneously, the characteristic absorption peak of -NH2 in the 2,5-diaminobenzenesulfonic acid monomer is significantly weakened, indicating that an effective condensation reaction occurred between the aldehyde and amino groups. The product at 1618 cm⁻¹... -1 The characteristic absorption peak of the C=C bond in the β-ketoenamine structure appears nearby, at 1226 cm⁻¹. -1 The presence of a CN stretching vibration peak nearby is important evidence of the successful formation of a conjugated organic framework structure by the 1,3,5-trialdehyde phloroglucinol series of COFs. Furthermore, at 1180 cm⁻¹... -1 and 1030cm -1 The characteristic absorption peaks nearby correspond to the asymmetric and symmetric stretching vibrations of O=S=O in the sulfonic acid group, indicating that the -SO3H group was retained during the reaction. FTIR results confirmed that 1,3,5-trialdehyde phloroglucinol and 2,5-diaminobenzenesulfonic acid successfully underwent a condensation reaction to form the target STCOF material.

[0081] Figure 4 Figure 1 shows the adsorption-desorption isotherm and pore size distribution of the STCOF tubular uniformly porous ceramic membrane prepared in Example 1. (a) N2 adsorption-desorption isotherm, (b) pore size distribution curve. As shown in Figure (a), the N2 adsorption-desorption isotherm of the prepared composite membrane material exhibits Type IV isotherm characteristics. Within the relative pressure P / P0 range of 0.8 to 1.0, the adsorption amount increases significantly, and a hysteresis loop exists between the adsorption and desorption branches, indicating that the material has a mesoporous structure. As shown in Figure (b), the pore size of the composite membrane material is mainly distributed in the range of 2 nm to 15 nm, with the most visible pore size being approximately 3.3 nm, and a significant distribution peak appears at 3 nm to 4 nm. Simultaneously, a certain number of pore structures still exist in the range of 5 nm to 40 nm, indicating that the material has a hierarchical pore structure composed of both small and larger mesopores. This structure allows the membrane material to maintain high porosity while forming continuous transport channels.

[0082] Comparative Experiment 1: This comparative experiment differs from Example 1 in that the LDH template construction step was omitted in this comparative example. Instead, the STCOF layer was grown directly on the surface of the sintered ceramic film substrate. That is, step 3 was omitted, and the sintered ceramic film substrate prepared in step 2 was directly subjected to step 4. Everything else was the same as in Example 1.

[0083] The results show that, due to the lack of LDH template to regulate the nucleation and growth process of STCOF crystals, the growth uniformity of the STCOF layer on the ceramic substrate surface is poor, the film continuity is insufficient, and structural defects are easily generated, affecting the ion selective transport performance of the film. In contrast, Example 1, by pre-constructing an LDH template layer on the ceramic substrate surface, provides uniform active sites for STCOF growth, which promotes the ordered arrangement of STCOF crystals, improves the film density and structural stability, and thus obtains a superior STCOF tubular uniformly porous ceramic film.

[0084] Example 2: An electrodialysis reactor was prepared using the sulfonated COF ion transport tubular uniform-pore ceramic membrane (STCOF tubular uniform-pore ceramic membrane) prepared in Example 1.

[0085] The electrodialysis reactor comprises a resin shell 1, an adjustable voltage regulator 2, a sulfonated COF ion transport tubular uniform-pore ceramic membrane 3, a cathode rod 4, and an anode mesh 5. A main channel 6 is arranged along the length of the center of the resin shell 1. Multiple tubular membrane mounting chambers are arranged along the circumferential and length directions inside the resin shell 1, and these chambers are connected to the main channel 6 via branch channels 7. Anode mesh 5 is evenly distributed on the sidewalls of each tubular membrane mounting chamber, and a sulfonated COF ion transport tubular uniform-pore ceramic membrane 3 is arranged along the length of the center of each chamber. A porous ceramic membrane 3 is sealed and fixed using a sealing ring 8. A cathode rod 4 is arranged along the length of the center of the sulfonated COF ion transport tube type porous ceramic membrane 3, and an 8mm annular gap is set between the sulfonated COF ion transport tube type porous ceramic membrane 3 and the anode mesh 5, and a 3.5mm annular gap is set between the sulfonated COF ion transport tube type porous ceramic membrane 3 and the cathode rod 4. The cathode rod 4 and the anode mesh 5 are respectively connected to an adjustable regulated power supply 2. The cathode rod 4 is a titanium rod with a diameter of 2mm. The anode mesh 5 is a titanium mesh.

[0086] The resin shell 1 is made of corrosion-resistant and insulating resin material, specifically polytetrafluoroethylene (PTFE);

[0087] The sulfonated COF ion transport tubular uniform porous ceramic membrane 3 is fixed by a sealing structure, forming an independent internal flow channel and an external reaction zone.

[0088] The electrodialysis reactor is used in the following steps:

[0089] 1. Under the condition of a circulation flow rate of 50 mL / min, the solution to be treated is introduced into the main channel 6 of the resin shell 1. The solution to be treated flows into the annular gap between each sulfonated COF ion transport tubular uniform porous ceramic membrane 3 and the anode mesh 5. Under the condition of a circulation flow rate of 50 mL / min, the catholyte is introduced into the interior of each sulfonated COF ion transport tubular uniform porous ceramic membrane 3.

[0090] The solution to be treated is Li-containing + and Co 2+ The simulated liquid, and Li + The concentration was 0.1 mol / L, Co 2+ The concentration of the solution is 0.1 mol / L, and the pH of the solution to be treated is 2, 3, 4, 5, 6 or 7; the catholyte is a 0.2 mol / L sodium chloride solution.

[0091] 2. At room temperature, by adjusting the applied voltage to 3V, 4.5V or 6V, a stable annular radial electric field is formed on both sides of the sulfonated COF ion transport tubular uniform porous ceramic membrane 3 for electrodialysis for 4 hours.

[0092] In this embodiment, during the electrodialysis operation, the feed solution to be treated enters each membrane chamber through the main channel 6 and circulates. A low concentration of supporting electrolyte (0.01 mol·L⁻¹) is initially added to the receiving side. -1 NaNO3 solution was used to reduce the system resistance, improve ion migration efficiency, and alleviate concentration polarization.

[0093] Under the action of an applied electric field, Co 2+ Driven by an electric field, it preferentially migrates through the STCOF membrane channels and toward the cathode, while Li + Due to the sieving effect of the STCOF membrane pore size and the electrostatic interaction of the sulfonic acid groups on the membrane surface, its migration rate is suppressed, thereby achieving Li + Selective retention and Co 2+ Preferential permeation. Therefore, under the action of an applied DC electric field, the target ions in the solution undergo directional migration driven by the electric field and the selective permeation of the membrane, achieving selective separation and enrichment of different ions.

[0094] Figure 5 This is a schematic diagram of the electrodialysis reactor structure in Example 2;

[0095] Figure 6 for Figure 5 Sectional view at CC;

[0096] Figure 7 for Figure 6 Sectional view at point AA;

[0097] Figure 8 for Figure 6 Sectional view at point BB;

[0098] Figure 9 This is a three-dimensional structural diagram of the electrodialysis reactor in Example 2;

[0099] Figure 10The operating system of the electrodialysis reactor in Example 2 includes an electrolyte supply tank 9, a transfer pump 10, a solution to be treated supply tank 11, a lithium ion collection tank 12, a Co ion collection tank 13, an adjustable voltage regulator 2, an electrodialysis reactor 16, and a pretreatment filter 15.

[0100] The electrolyte supply tank 9 is connected to the delivery pump 10 via a delivery pipeline. The outlet of the delivery pump 10 is connected to the electrode liquid flow channel of the electrodialysis reactor 16, for supplying electrolyte into the electrodialysis reactor 16. The electrolyte returns to the electrolyte supply tank 9 after circulation, forming an electrode liquid circulation loop. The solution to be treated supply tank 11 is connected to the delivery pump 10 via a delivery pipeline and is delivered by the delivery pump 10 to the pretreatment filter 15 to filter particulate impurities in the lithium-containing solution to be treated, and then enters the main flow channel of the electrodialysis reactor 16. The electrodialysis reactor 16 is an ion-selective separation unit, which is equipped with a sulfonated COF ion transport tubular porous ceramic membrane and corresponding electrode components. The solution to be treated flows outside the sulfonated COF ion transport tubular porous ceramic membrane. Under the action of an applied electric field, Co 2+ Migrating through the ceramic membrane to the enrichment side, while Li + Selective retention occurs. The adjustable regulated power supply 2 is connected to the electrodes at both ends of the electrodialysis reactor 16 via wires to provide a stable and adjustable DC electric field to drive the directional migration of ions in the solution. The Li⁺ enrichment outlet of the electrodialysis reactor 16 is connected to the lithium ion collection tank 12 to collect the lithium-enriched solution after selective migration; the other outlet is connected to the Co ion collection tank 13 to collect high-valence metal ions and other impurity ions that have not permeated the membrane. The Co ion collection tank 13 is connected to the electrodialysis reactor 16 via the transfer pump 10 and the electrolyte supply tank 9 to form a concentrate circulation loop, allowing the concentrate that has not permeated the membrane to circulate and improving ion separation efficiency; when the concentrate reaches the set concentration, it is discharged through the concentrate discharge port.

[0101] Figure 11 Example 2 illustrates the effect of STCOF tubular uniform-pore ceramic membrane on Li under different pH and voltage conditions of 4.5V. + Retention rate and Co 2+ Transmittance variation curve (a) and the effect of STCOF tubular uniform-pore ceramic membrane on Li under different voltages and pH 7 conditions. + and Co 2+Figure (b) shows a comparison of permeation rates. The prepared STCOF tubular uniform-pore ceramic membrane exhibits good ion separation performance under different pH conditions. At pH 5, both Li⁺ rejection and Co²⁺ permeability reach their highest values, approximately 96% and 95%, respectively; within the pH range of 4–6, both indicators remain above 90%, indicating that the membrane has a wide applicable pH range. As shown in Figure (b), at 3V, Co… 2+ and Li + No significant permeation occurred, indicating that the driving force was insufficient to overcome the resistance to ion transmembrane transport. When the voltage was increased to 4.5V, divalent Co... 2+ The driving force is greater than the unit price of Li⁺, only Co 2+ Permeation occurs through the membrane at a rate of approximately 3.5 mol·h⁻¹. -1 ·m -2 While Li⁺ showed no significant migration, this indicates that the membrane can achieve Co… 2+ With Li + Effective separation. Further increasing the voltage to 6V, Co... 2+ The permeation rate increased significantly to approximately 8.2 mol·h⁻¹. -1 ·m -2 Li + The permeation rate is only about 3.2 mol·h⁻¹ -1 ·m -2 Co 2+ / Li + The permeation rate ratio reached 2.6. The results indicate that the STCOF nanochannels constructed in this embodiment can preferentially promote Co permeation. 2+ Transmission, while effectively suppressing Li + Migration, thereby achieving efficient and selective separation and enrichment of lithium and cobalt ions in battery leachate.

[0102] Example 3: This example differs from Example 2 in that the lithium-containing solution to be treated in step 1 is Co-containing. 2+ / Li + / K + / Na + A mixed system, and Li + The concentration was 0.1 mol / L, Co 2+ The concentration is 0.1 mol / L, K + The concentration is 0.1 mol / L, Na + The concentration was 0.1 mol / L, and the pH was 7. In step two, at room temperature, a stable annular radial electric field was formed on both sides of the sulfonated COF ion transport tubular uniform porous ceramic membrane 3 by adjusting the applied voltage to 4.5V, and electrodialysis was performed for 4 hours. Other procedures were the same as in Example 2.

[0103] Example 4: This example differs from Example 2 in that the liquid to be treated in step 1 contains Co. 2+ Single ion solution, and Co 2+ The concentration is 0.1 mol / L, and the pH is 7; or the solution to be treated in step one is Li-containing... + Single ion solution, and Li + The concentration was 0.1 mol / L, and the pH was 7. In step two, at room temperature, a stable electric field was formed across the sulfonated COF ion transport tubular porous ceramic membrane 3 by adjusting the applied voltage to 4.5V, and electrodialysis was performed for 4 hours. Everything else was the same as in Example 2.

[0104] Figure 12 In Example 3, under the condition of an applied voltage, Li + Co 2+ K + and Na + A comparison of the changes in the concentration of each ion in the mixed system with the increase of electrolyte concentration over time; as shown in the figure, in Co 2+ / Li + / K + / Na + In the mixed system, the ions exhibited significantly different transport behaviors. After 60 minutes of operation, Na... + K + and Co 2+ The concentrations increased by approximately 7.0 μM, 5.9 μM, and 5.5 μM, respectively, while Li + The concentration remained consistently low, indicating that the membrane was effective against Li. + It has a significant retention effect.

[0105] Figure 13 Example 4 shows a single Co under an applied voltage. 2+ System and single Li + A comparison of ion permeation rates in the system. As shown in the figure, in the single-ion system, Co... 2+ The permeation rate is approximately 2.6 mol·h⁻¹. -1 ·m -2 The permeation rate of Li⁺ is close to 0, while that of Co is... 2+ / Li + The penetration rate ratio exceeds 100.

[0106] The results show that the STCOF tubular uniformly porous ceramic membrane prepared in the examples has excellent ion selectivity and can effectively promote Co 2+ Migrate and suppress Li + The transfer process can be used for the enrichment of lithium ions and the selective separation of metal ions in battery leachate.

[0107] Example 5: This example differs from Example 2 in that, in step 2, at room temperature, a stable electric field is formed across the sulfonated COF ion transport tubular porous ceramic membrane 3 by adjusting the applied voltage to 4.5V, and electrodialysis is performed for 24 hours. Everything else is the same as in Example 2.

[0108] Figure 14 This is a stability test graph for Example 5, performed continuously for 24 hours at pH 7 and voltage 4.5V. As shown in the graph, at 0.1 mol·L⁻¹... -1 Co 2+ and 0.1 mol·L -1 Li + In a mixed system, the STCOF tubular uniform-pore ceramic membrane maintained stable separation performance throughout 24 hours of continuous operation. 2+ The permeation rate is between 2.3 and 2.6 mol·h⁻¹. -1 ·m -2 It fluctuates within a certain range, with an average value of approximately 2.4 mol·h⁻¹. -1 ·m -2 The fluctuation range within 24 hours was less than 10%; meanwhile, the Li⁺ permeation rate remained close to 0, showing no significant change. This indicates that the membrane exhibits excellent operational stability and ion selectivity.

[0109] Comparative Experiment 2: This comparative experiment differs from Example 3 in that it utilizes the sintered ceramic membrane substrate prepared in step two of Example 1 for electrodialysis separation. Specifically, this comparative experiment uses a uniformly porous ceramic membrane without an STCOF functional layer for electrodialysis separation, without LDH template construction or STCOF functional layer modification. Everything else is the same as in Example 3.

[0110] The results show that, due to the lack of an STCOF functional layer, the uniformly porous ceramic membrane mainly relies on the inorganic pore size for ion transport, lacking an ordered nanoporous structure and ion recognition sites, resulting in weak sieving ability for different ions. Under the action of an external electric field, Li... + Na + K + Co 2+ All plasmas undergo non-selective migration.

[0111] Under conditions of 4.5V and 60 min of electrodialysis, the unmodified uniformly porous ceramic membrane permeates Li on the permeation side. + The concentration increased by 6.2 μM, Co 2+ The concentration increased by 5.6 μM, Na + and K + The concentrations increased by 6.8 μM and 6.3 μM, respectively, where Li + The migration difference between Li and divalent ions is relatively small. + / Co 2+With a selectivity coefficient of only 1.11, it is impossible to achieve effective separation of lithium ions and transition metal ions.

[0112] In contrast, Example 3, by inducing the growth of an STCOF functional layer using a Li-Al LDH template, formed a composite film structure with regularly confined nanopores and ion recognition sites. Because the STCOF channels are conducive to the growth of Li... + Hydrated structures have a strong hindering effect on migration, while Co... 2+ Plasma has a high transport capacity, which causes different ions to exhibit significantly different migration behaviors.

[0113] Under the same test conditions, in Example 3, the permeable side Co 2+ The concentration increased by approximately 5.5 μM, while the Li⁺ concentration increased by only 0.05 μM, resulting in a Li⁺ rejection rate exceeding 99%. Co 2+ / Li + The selectivity coefficient has been increased to 110.

[0114] This demonstrates that the STCOF functional layer induced by the LDH template can significantly enhance the ion sieving ability of the ceramic membrane, achieving Li ion sieving through the nanopore confinement effect and ion recognition. + With Co 2+ The efficient separation by plasma improves the selective separation performance of membranes in complex lithium-containing systems.

[0115] Comparative Experiment 3: This comparative experiment differs from Example 3 in that the electrodialysis process was not coupled during membrane separation in this example; instead, only a simple STCOF tubular uniform-pore ceramic membrane was used for pressure-driven separation. Everything else is the same as in Example 3.

[0116] The results show that, under conditions without an external electric field, the STCOF tubular uniformly porous ceramic membrane mainly relies on the concentration gradient for ion diffusion transport. Although the nanopore structure within the membrane can provide some spatial confinement, the lack of an electric field to drive the directional migration of ions limits the Li... + Co 2+ Plasma exhibits low and similar transport behavior, making effective selective separation impossible.

[0117] Under the same separation time (60 min), the permeable side Li in pressure-driven mode + The concentration increased by approximately 1.1 μM, Co 2+ With a concentration increase of 1.3 μM, the migration rates of the two ions remained essentially the same, Li + / Co 2+ The selectivity coefficient is only 0.85, indicating that pressure-driven operation alone cannot achieve Li + Efficient separation from divalent metal ions.

[0118] In contrast, Example 3 couples the STCOF tubular uniform-pore ceramic membrane with the electrodialysis process. Under an applied electric field, ions are driven by electromigration, resulting in differentiated migration behaviors based on ion size, hydration energy, and the effects of functional groups within the membrane. Co... 2+ Plasma migrates preferentially, while Li + It is effectively blocked by the STCOF confined channel effect.

[0119] Under the same conditions, Co in the electrodialysis coupling system 2+ The concentration increased by 5.5 μM, while Li + The concentration remained below 0.05 μM, Co 2+ / Li + The selectivity reaches over 100, which is significantly higher than that of a purely pressure-driven process.

[0120] The above results show that although the STCOF membrane alone has a certain ability to regulate ion transport, it is difficult to achieve efficient ion separation without an electric field. The introduction of electrodialysis technology can enhance the directional migration process of ions, give full play to the ion sieving effect of STCOF nanopores, and achieve efficient and selective separation.

Claims

1. A method for preparing a sulfonated COF ion transport tubular uniformly porous ceramic membrane, characterized in that... It is done in the following steps:

1. Add nano-titanium dioxide ethanol dispersion and nano-alumina ethanol dispersion to anhydrous ethanol and ultrasonically disperse to obtain inorganic ceramic membrane dispersion.

2. The inorganic ceramic membrane dispersion is sprayed onto the surface of the tubular ceramic substrate and then dried. The spraying and drying are repeated multiple times to obtain a ceramic membrane substrate with a uniform surface coating. The ceramic membrane substrate with a uniform surface coating is sintered to obtain the sintered ceramic membrane substrate.

3. Co(NO3)2·6H2O, Al(NO3)3·9H2O, urea and NH4F are dissolved in deionized water to obtain a precursor solution. The sintered ceramic membrane substrate is immersed in the precursor solution and heated to react. Then it is taken out and cooled naturally to obtain an LDH template. The LDH template is hydroxylated to obtain a hydroxylated LDH template. IV. Add 2,5-diaminobenzenesulfonic acid, 1,3,5-trialdehyde phloroglucinol and acetic acid to a mixed solvent to obtain a treatment solution. Immerse the hydroxylated LDH template in the treatment solution and heat it to react. Then remove it and let it cool naturally to obtain a sulfonated COF ion transport tubular uniform porous ceramic membrane.

2. The method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 1, characterized in that... The nano-titanium dioxide ethanol dispersion mentioned in step one is specifically obtained by ultrasonically dispersing nano-titanium dioxide in anhydrous ethanol, wherein the particle size of the nano-titanium dioxide is 5nm~20nm; the nano-alumina ethanol dispersion mentioned in step one is specifically obtained by ultrasonically dispersing nano-alumina in anhydrous ethanol, wherein the particle size of the nano-alumina is 5nm~20nm.

3. The method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 1, characterized in that... The mass ratio of nano-titanium dioxide to nano-alumina in the inorganic ceramic membrane dispersion in step one is 1:(1~5); the total mass concentration of nano-titanium dioxide and nano-alumina in the inorganic ceramic membrane dispersion in step one is 10%~30%.

4. The method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 1, characterized in that... The tubular ceramic substrate described in step two has an outer diameter of 8mm~20mm, an inner diameter of 4mm~12mm, and a wall thickness of 1mm~3mm. The tubular ceramic substrate has a multi-level porous structure, consisting of a macroporous framework layer and a microporous transport layer uniformly distributed on the surface. The macroporous framework layer has a pore size of 0.1μm~1μm and a porosity of 30%~50%. The microporous transport layer has a pore size of 0.1μm~0.3μm. In step two, the inorganic ceramic membrane dispersion is sprayed onto the surface of the tubular ceramic substrate, and then dried at 60℃~80℃ for 1min~2min. This spraying and drying process is repeated multiple times until the coating thickness reaches 0.1μm~1μm, resulting in a uniformly coated ceramic membrane substrate. The uniformly coated ceramic membrane substrate is then heated to 900℃~1100℃ at a heating rate of 5℃ / min~10℃ / min, and sintered at 900℃~1100℃ for 2h~3h.

5. The method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 1, characterized in that... In step three, the concentrations of Co(NO3)2·6H2O in the precursor solution are 0.03 mol / L to 0.1 mol / L, the concentrations of Al(NO3)3·9H2O are 0.008 mol / L to 0.02 mol / L, the concentrations of urea are 0.08 mol / L to 0.2 mol / L, and the concentrations of NH4F are 0.1 mol / L to 0.2 mol / L.

6. The method for preparing a sulfonated COF ion transport tubular uniformly porous ceramic membrane according to claim 1, characterized in that... In step three, the sintered ceramic film substrate is immersed in the precursor solution and heated for 12-72 hours at a temperature of 100℃~140℃. The hydroxylation treatment in step three is carried out in the following steps: the LDH template is immersed in toluene, and then 3-aminopropyltriethoxysilane is added and soaked at room temperature for 5-24 hours. The volume ratio of 3-aminopropyltriethoxysilane to toluene is 1:(280-290).

7. The method for preparing a sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 1, characterized in that... In step four, the concentration of 2,5-diaminobenzenesulfonic acid in the treatment solution is 0.01 mol / L to 0.05 mol / L, the concentration of 1,3,5-trialdehyde phloroglucinol is 0.001 mol / L to 0.005 mol / L, and the concentration of acetic acid is 3 mol / L to 5 mol / L. The mixed solvent in step four is a combination of dioxane and mesitylene in a volume ratio of 1:(1~2). In step four, the hydroxylated LDH template is immersed in the treatment solution and heated for 12 h to 72 h at a temperature of 100℃ to 140℃.

8. The application of the sulfonated COF ion transport tubular uniform porous ceramic membrane prepared according to claim 1, characterized in that... It was used to prepare an electrodialysis reactor for treating battery leachate and separating Li from the battery leachate. + and divalent metal ions; the divalent metal ions are Co 2+ Ni 2+ and Mn 2+ One or a combination of several of them.

9. The application of the sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 8, characterized in that... The electrodialysis reactor consists of a resin shell (1), an adjustable voltage regulator (2), a sulfonated COF ion transport tubular uniform-pore ceramic membrane (3), a cathode rod (4), and an anode mesh (5). A main channel (6) is arranged along the length direction at the center of the resin shell (1). Multiple tubular membrane mounting chambers are arranged along the circumferential and length directions inside the resin shell (1), and these chambers are connected to the main channel (6) via branch channels (7). Anode meshes (5) are evenly distributed on the sidewalls of the tubular membrane mounting chambers. A sulfonated COF ion transport tubular uniform-pore ceramic membrane (3) is arranged along the length direction at the center of the tubular membrane mounting chamber. The sulfonated COF ion transport tube type uniform porous ceramic membrane (3) is sealed and fixed by a sealing ring (8). A cathode rod (4) is set along the length direction at the center of the sulfonated COF ion transport tube type uniform porous ceramic membrane (3). An annular gap of 8mm~10mm is set between the sulfonated COF ion transport tube type uniform porous ceramic membrane (3) and the anode mesh (5). An annular gap of 2mm~6mm is set between the sulfonated COF ion transport tube type uniform porous ceramic membrane (3) and the cathode rod (4). The cathode rod (4) and the anode mesh (5) are respectively connected to an adjustable regulated power supply (2). The cathode rod (4) is a titanium rod with a diameter of 1mm~3mm. The anode mesh (5) is a titanium mesh.

10. The application of the sulfonated COF ion transport tubular uniform porous ceramic membrane according to claim 9, characterized in that... The electrodialysis reactor is used in the following steps:

1. Under the condition of a circulation flow rate of 50 mL / min to 100 mL / min, the solution to be treated is introduced into the main channel (6) of the resin shell (1). The solution to be treated flows into the annular gap between each sulfonated COF ion transport tube type uniform porous ceramic membrane (3) and the anode mesh (5). Under the condition of a circulation flow rate of 50 mL / min to 100 mL / min, the catholy liquid is introduced into the interior of each sulfonated COF ion transport tube type uniform porous ceramic membrane (3). The solution to be treated is Li-containing + The battery leaching solution contains divalent ions; the cathode solution is a sodium chloride solution of 0.01 mol / L to 0.2 mol / L.

2. By adjusting the applied voltage to 4V~5V or the current to 0.01A~0.05A, a stable annular radial electric field is formed on both sides of the sulfonated COF ion transport tube type uniform porous ceramic membrane (3) for electrodialysis. Divalent metal ions in the solution to be treated migrate to the cathode region through the sulfonated COF ion transport tube type uniform porous ceramic membrane (3) and form hydroxide precipitates in the cathode region, which flow out with the cathode liquid, thus achieving the removal of impurity ions; Li + Without passing through the sulfonated COF ion transport tubular uniform porous ceramic membrane (3), it flows out with the desalination solution, realizing Li + Recycling.