A metal vapor reduction furnace and a method for preparing silicon-based nanomaterials
By using an independent temperature control design and airflow series coupling in a metal vapor reduction furnace, the safety hazards and uneven reaction problems of traditional metal thermal reduction have been solved, enabling low-cost and high-efficiency preparation and resource utilization of silicon-based nanomaterials.
Patent Information
- Application Number
- CN202611560963.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional metallothermic reduction processes have safety hazards, uneven reactions, and intense exothermic reactions at high temperatures. They are difficult to effectively utilize the natural nanostructure of clay minerals, and the large temperature difference between carbothermic reduction and metallothermic reduction makes the reaction process uncontrollable.
A metal vapor reduction furnace is used, through an independently temperature-controlled reaction vessel and an evaporation vessel, and by using airflow series coupling, metal vapor is generated to react with silicon-containing precursors, so as to achieve safe, uniform and low-cost preparation of silicon-based materials.
It achieves the preservation of the nanostructure of clay minerals, reduces raw material costs and energy consumption, is adaptable to various metal sources, is suitable for industrial production, allows for the resource utilization of by-products, and reduces environmental pollution.
Smart Images

Figure CN123102290A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of equipment and methods for preparing nanomaterials, and more specifically, to a metal vapor reduction furnace and a method for preparing silicon-based nanomaterials. Background Technology
[0002] Silicon-based materials have wide applications in lithium-ion batteries, semiconductors, and other fields due to their excellent lithium storage performance, microwave absorption properties, and chemical stability. Metallothermic reduction is one of the important methods for preparing high-performance silicon-based materials because of its low cost, mild reaction conditions, and ability to well preserve the original morphology of the precursor.
[0003] However, traditional metallothermic reduction processes generally employ a solid-solid mixing method, where the metal block is first processed into micron-sized metal powder, which is then physically mixed with a silicon-containing precursor. This process not only increases processing steps and raw material costs, but also poses serious safety hazards during storage, transportation, and mixing due to the flammability and explosiveness of the micron-sized metal powder. More critically, the solid-solid interaction between the metal powder and the solid precursor... Solid-state contact reactions are highly exothermic, with heat being released rapidly in a short period of time. This can easily lead to local overheating, uneven reaction, and damage to the microstructure of the precursor, ultimately limiting the performance of the product.
[0004] Furthermore, if metal-containing minerals (such as magnesium oxide) can be directly converted into metal vapor through carbothermic reduction and coupled with a subsequent metallothermic reduction process, the entire intermediate step of "mineral → metal block → metal vapor" can be skipped, achieving a "one-step" preparation from minerals to silicon-based materials. This would significantly reduce raw material costs and energy consumption. Carbothermic reduction of metal vapor is considered one of the most promising industrial routes for metal vapor generation due to the wide availability and low cost of raw materials. However, the reaction temperature required for carbothermic reduction is as high as 1200–1600℃, while the suitable temperature for metallothermic reduction is only 650–800℃, resulting in a huge temperature difference. Simply coupling the carbothermic reduction process with a traditional solid-solid mixture system would lead to an uncontrollable reaction process, failing to meet purity requirements.
[0005] It is worth mentioning that clay minerals possess natural nanostructures (such as the tubular structure of halloysite, the layered structure of montmorillonite, and the fibrous structure of sepiolite), and are abundant, inexpensive, and environmentally friendly. If these original morphologies can be preserved during the reduction reaction, the resulting nano-silicon will inherit its structural advantages and exhibit superior cycle stability in lithium-ion battery anodes. However, traditional solid... Solid metal thermal reduction reactions are violently exothermic, leading to the destruction of the fine microstructure of clay minerals. Therefore, developing a reduction furnace and method capable of gently and uniformly reducing clay minerals is of great significance for the large-scale preparation of low-cost, high-performance silicon-based anode materials.
[0006] In view of this, the present invention is proposed. Summary of the Invention
[0007] The present invention aims to provide a metal vapor reduction furnace and a method for preparing silicon-based nanomaterials, which can achieve spatial independence between the high-temperature metal-producing evaporation vessel and the low-temperature reaction vessel, while simultaneously using airflow series coupling to controllably and directionally introduce metal vapor generated from metal blocks, metal alloys or metal-containing minerals into the silicon-containing precursor reaction zone, thereby achieving safe, uniform and low-cost preparation of silicon-based materials while being compatible with multiple metal sources.
[0008] The embodiments of the present invention can be implemented as follows: In a first aspect, the present invention provides a metal vapor reduction furnace, the metal vapor reduction furnace comprising a reaction vessel, an evaporation vessel, an atmosphere control mechanism, and a condensation mechanism; the reaction vessel and the evaporation vessel are connected by a gas pipeline; the reaction vessel and the evaporation vessel are independently temperature controlled, the evaporation vessel is provided with an evaporation temperature control mechanism, and the reaction vessel is provided with a reaction temperature control mechanism; the atmosphere control mechanism is provided with an exhaust pipe connected to the reaction vessel, and the condensation mechanism is located inside the exhaust pipe; the evaporation vessel is provided with a waiting area, an evaporation area, and a cooling area in sequence along the horizontal direction; the gas pipeline is connected to the evaporation area; a heat-insulating transition area is provided between the gas pipeline and the reaction vessel, and heat-insulating baffles are stacked in the transition area along the airflow direction.
[0009] Secondly, the present invention provides a method for preparing silicon-based nanomaterials, which is carried out using a metal vapor reduction furnace as described in any of the above embodiments, the method comprising: S1. The reactants are placed in the reaction vessel, and the metal raw material is placed in the evaporation zone of the evaporation vessel. The atmosphere control mechanism evacuates the reaction vessel and the evaporation vessel. The reactants include at least one of the following: clay minerals with natural nanostructures or their modified products, silicon-containing precursors, metal-containing minerals, industrial solid waste, or synthetic nanomaterial precursors. S2. After evacuating to <800 Pa, the evaporation temperature control mechanism and the reaction temperature control mechanism are activated respectively to raise the temperature of the evaporation container to 600~1700℃ to generate metal vapor. The metal vapor enters the reaction container through the gas pipeline. The reaction container is then raised to 600~900℃ to allow the metal vapor to undergo a gas-solid reduction reaction with the reactants, yielding a crude reduced product containing byproduct metal oxides. S3. The crude reduced product is post-processed by acid washing, water washing and drying to remove the by-product metal oxides, and a silicon-based material product is obtained. The gas after the reaction is recovered by the condensation mechanism.
[0010] The beneficial effects of the metal vapor reduction furnace and the method for preparing silicon-based nanomaterials provided in this invention include: I. Key Application Advantages: Clay minerals and their modified products possess natural nanostructures, abundant resources, low cost, and environmental friendliness, making them ideal precursors for silicon-based materials. Clay minerals can be transformed into porous silicon with different morphologies (e.g., sheet-like, tubular, fibrous) through morphological inheritance during metallothermic reduction, providing excellent lithium storage performance for lithium-ion battery anodes. Their modified products (including acid treatment, heat treatment, mechanical treatment, organic modification, and inorganic modification) can be further optimized in terms of structural composition, silica content, and reactivity. This invention employs vacuum metal vapor gas-solid reduction, where the metal vapor is uniformly dispersed at the atomic level on the material surface. The reaction is mild, exothermic, and dispersed, effectively preserving the original microstructure of clay minerals and their modified products. Furthermore, this invention is also applicable to other silicon-containing precursors such as artificially synthesized silica, rice husk ash, silica fume, and waste solar panels, allowing for flexible selection based on cost and performance requirements, and offering broad silicon source compatibility.
[0011] II. High process integration, achieving "one-step" series production, significantly saving energy and reducing costs. Taking magnesium vapor as an example, this invention spatially connects and temporally couples the carbothermic reduction or Pidgeon process for magnesium production with the metal vapor reduction process. It eliminates the intermediate steps of preparing magnesium ingots from magnesium-containing minerals and remelting them to obtain metal vapor. The magnesium vapor generated in the magnesium production zone is directly introduced into the material reaction zone to react with the solid precursor. There is no need for separate preparation, cooling, storage, and remelting of magnesium ingots, resulting in reduced energy consumption, lower raw material costs, and a shorter production cycle, making it suitable for industrial production. The reduction furnace is compatible with three magnesium sources: carbothermic reduction (inexpensive carbonaceous reducing agent + magnesium-containing minerals), Pidgeon process (calcined white + ferrosilicon), and direct use of magnesium ingots / magnesium alloys. It can be flexibly switched according to raw material prices and supply, offering strong economic adaptability. Simultaneously, this reduction furnace is also suitable for directly heating and evaporating calcium vapor from elemental calcium or calcium alloys, as well as directly heating and evaporating sodium vapor, potassium vapor, or sodium-potassium alloys to produce sodium vapor or potassium vapor. This achieves series coupling of multiple metal vapor sources with the metal thermal reduction process, resulting in strong equipment versatility.
[0012] Third, the dual-temperature zone independent temperature control and liftable insulation partition design perfectly solve the temperature difference contradiction between high-temperature metal vapor production and low-temperature reduction, and achieve operation without cooling. This invention connects the material reaction system and the metal evaporation system through a transition zone, each equipped with independent heating elements and temperature control systems. The high-temperature zone can operate stably at 1700℃, and the low-temperature zone is precisely controlled at 600~900℃, completely solving the problem that traditional single-temperature zone furnaces cannot simultaneously meet the two temperature requirements. The metal evaporation system is arranged in a horizontal direction with a backup zone, an evaporation zone, and a cooling zone. Adjacent zones are equipped with liftable insulation partitions. When the metal in the evaporation zone is exhausted, there is no need for overall cooling. Simply raise the partition to push the new crucible into the evaporation zone and the empty crucible into the cooling zone, realizing relay-style material replacement, which is suitable for long-cycle industrial production. IV. The combination of automatic feeding and discharging with a dynamic reaction system ensures uniform and thorough reaction and a high degree of automation. The rotary feed pipe, equipped with vanes, pushes powdery or granular reactants from the feed hopper to the reaction chamber, avoiding vacuum disruption and heat loss caused by manual opening. The reaction chamber rotates at a constant speed (1~100 rpm) driven by a rotary motor, with internal turning plates continuously lifting and turning the material, ensuring full contact between solid particles and metal vapor, resulting in a uniform reaction and preventing localized overburning or under-reduction. After the reaction, the furnace tilting system tilts the reaction chamber to the left, and the discharge return plate guides the product to the left pipe and discharges it into the discharge hopper, achieving automated discharge. Incompletely reacted material can be returned to the reaction zone via the return plate, reducing waste. V. A comprehensive vacuum and atmosphere control system, along with a condensation recovery system, ensures reaction quality and enables multi-resource utilization. Equipped with a high-precision vacuum gauge, vacuum pump, and a three-stage filtration system (filter chamber + filter plate + filter), it can achieve a vacuum of less than 20 Pa. Simultaneously, the filtration system effectively captures dust, extending equipment life. A porous condenser is installed on the extraction pipeline, allowing the recovery of condensable vapors generated during the reaction in the condensation zone, yielding high-value-added metal powders or compounds. This makes the invention not only a material preparation tool but also equipment for resource extraction and solid waste value-added utilization. VI. The invention boasts a wide range of applications, covering multiple fields such as key metal extraction, industrial solid waste resource utilization, and the synthesis of nano-alloys and ceramic powders. It utilizes metal vapor to disrupt stable crystal structures, releasing metals in the form of elemental or low-valence oxides. Low-boiling-point metals volatilize, condense, and accumulate, while high-boiling-point metals are enriched in the slag for subsequent magnetic separation or acid leaching. This is a green and low-carbon metallurgical technology. It can also treat industrial solid wastes such as lithium smelting slag, steel dust, electroplating sludge, spent catalysts, waste lithium battery powder, red mud, and fly ash, achieving volume reduction, harmlessness, and valuable metal recovery. Furthermore, by controlling reaction conditions, it can prepare nano-metal powders, nano-silicides / nitrides / carbides / intermetallic compounds, nano-oxides / borides / sulfides / phosphides, and nano-alloys, significantly simplifying traditional preparation processes.
[0013] VII. Environmentally friendly, with full resource utilization of byproducts, near-zero emissions, and significantly reduced energy consumption and carbon emissions. The polymetallic ion solution generated from pickling can replenish corresponding ions and adjust pH, used to prepare high-value-added hydrotalcite; the metal powder recovered by condensation can be sold directly or used in powder metallurgy. Compared with traditional routes, this invention eliminates the two energy-intensive steps of metal block smelting and remelting, saving electricity and correspondingly reducing CO2 emissions. If biochar is used as a carbonaceous reducing agent, carbon negative emissions can also be achieved. The reduction furnace has a compact structure and high integration, with one piece of equipment replacing multiple traditional pieces of equipment, saving factory space and infrastructure investment, reducing manual operation, lowering labor intensity and safety risks, and has extremely high industrial promotion value and economic and social benefits.
[0014] 8. The reduction furnace and method described in this invention have extremely high configuration flexibility. Based on the same series thermal reduction principle, those skilled in the art can freely design the reduction furnace into various physical configurations such as horizontal, vertical, inclined, or even fluidized bed types, depending on factors such as plant conditions, material characteristics, and production capacity, without requiring creative effort. This greatly expands the industrial application scenarios of this invention. Attached Figure Description
[0015] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1 This is a schematic diagram of the metal vapor reduction furnace of the present invention; Figure 2 for Figure 1 Schematic diagram of the structure of the evaporation vessel; Figure 3 This is a schematic diagram of the intermittent horizontal series structure of the present invention; Figure 4 A schematic diagram of a variant of the present invention: an integrated vertical series structure; Figure 5 This is a schematic diagram of the variant, separate, vertical, series structure of the present invention; Figure 6 X-ray diffraction pattern of the sheet-like nano-silicon prepared in Example 2; Figure 7 Cycle performance diagram of micro / nano silicon prepared for application example as a negative electrode material for lithium-ion batteries.
[0017] Icon: 100 - Metal Steam Reduction Furnace; 110 - Reaction vessel; 111 - Gas pipeline; 112 - Gas inlet valve; 113 - Reaction temperature control mechanism; 1131 - First heating element; 1132 - First insulation layer; 114 - Furnace body; 1141 - Feed inlet; 1142 - Discharge outlet; 1143 - Discharge plate; 1144 - Tilting plate; 115 - Transition zone; 1151 - Stainless steel sheet; 1152 - Vacuum sealing flange; 116 - Exhaust port; 120 - Evaporation container; 121 - Evaporation temperature control mechanism; 1211 - Second heating element; 1212 - Second insulation layer; 122 - Backup area; 123 - Evaporation zone; 124 - Cooling zone; 125 - First insulation partition layer; 126 - Second insulation partition layer; 127 - Rolling wheel; 130 - Feeding / Discharging Mechanism; 131 - Feeding Bin; 132 - Feeder; 133 - Discharging Bin; 140 - Atmosphere control mechanism; 141 - Evacuation pipe; 142 - Vacuum pump; 143 - Filter; 144 - Filter chamber; 145 - Filter plate; 146 - Vacuum gauge; 147 - Vacuum meter; 150 - Condensation mechanism; 160 - Hybrid mechanism; 162 - Rotary mechanism; 163 - Movable rotary interface; 170 - Tilting mechanism; 171 - Support body; 172 - Support platform; 173 - Bearing; 174 - Push rod; 201-Heat-resistant steel pipe; 202-Agitator; 203-S-shaped ventilation channel; 204-Removable insulated furnace cover; 205-Material inlet; 206-Impeller. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0019] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.
[0020] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0021] In the description of this invention, it should be noted that if terms such as "upper," "lower," "inner," or "outer" are used to indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship in which the product of this invention is usually placed, they are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.
[0022] Furthermore, the terms "first" and "second" are used only to distinguish descriptions and should not be interpreted as indicating or implying relative importance.
[0023] It should be noted that, where there is no conflict, the features in the embodiments of the present invention can be combined with each other.
[0024] Please see Figure 1 This invention provides a metal vapor reduction furnace 100. The 100, used for the series-connected metal vapor reduction of silicon-based materials, includes a reaction vessel 110, an evaporation vessel 120, a feeding / discharging mechanism 130, an atmosphere control mechanism 140, a condensation mechanism 150, a mixing mechanism 160, and a tilting mechanism 170. The reaction vessel 110 is used to contain the reactants and carry out the metal vapor reduction reaction. The evaporation vessel 120 is used to contain the metal raw materials and generate metal vapor. The reaction vessel 110 and the evaporation vessel 120 are connected by a gas pipe 111, on which a gas pipe 111 is provided with a... Argon gas inlet valve 112, reaction vessel 110 is equipped with reaction temperature control mechanism 113, evaporation vessel 120 is equipped with evaporation temperature control mechanism 121; feeding and discharging mechanism 130 is used to realize the entry or discharge of materials into or out of reaction vessel 110; atmosphere control mechanism 140 is equipped with suction pipe 141, suction pipe 141 is connected to reaction vessel 110, condensation mechanism 150 is set in suction pipe 141, mixing mechanism 160 is used to drive the materials in reaction vessel 110 to fully mix, and tilting mechanism 170 is used to drive reaction vessel 110 to tilt for material discharge.
[0025] In this invention, the reaction vessel 110 and the evaporation vessel 120 are independently set up and connected by a gas pipeline 111. The temperatures of both vessels can be controlled independently, but the atmosphere control mechanism 140 can simultaneously perform vacuuming operations on both vessels, achieving a series-connected and identical gas flow. This invention effectively overcomes the defects of solid-solid mixing by using metal vapor to directly react with the solid precursor. Using a metal block or metal alloy block as the metal source, metal vapor is generated in situ by heating in the evaporation vessel 120, completely eliminating the step of processing the metal block into metal powder and fundamentally eliminating the safety risks and uneven reaction problems associated with metal powder. Especially under low vacuum conditions, the diffusion coefficient of metal vapor is significantly improved compared to atmospheric pressure, enabling rapid and uniform mass transfer. The metal evaporation process achieves differential supply of reactants, effectively dispersing the exothermic reaction on both temporal and spatial scales, thereby fundamentally suppressing thermal runaway and structural sintering.
[0026] Next, this application will describe in detail the structure of the above-mentioned reaction vessel 110, evaporation vessel 120, atmosphere control mechanism 140, condensation mechanism 150, mixing mechanism 160 and tilting mechanism 170.
[0027] (1) Reaction vessel 110.
[0028] The reaction vessel 110 includes a furnace body 114, which is a horizontally placed cylindrical heat-resistant steel container. The furnace body 114 is used to contain the reactants and react with the introduced metal vapor. The furnace body 114 is provided with a feed inlet 1141, a discharge outlet 1142, a discharge plate 1143, a tilting plate 1144, and an insulation layer. There are multiple discharge plates 1143, which are located close to the discharge outlet 1142 of the furnace body 114. The discharge plates 1143 are used to discharge the material from the discharge outlet 1142. When tilted, the discharge plates 1143 are used to discharge the reacted material into the discharge bin 133 through the left-side pipe. There are multiple tilting plates 1144, which are evenly distributed inside the furnace body 114. The tilting plates 1144 are used to make the material evenly rotate inside the furnace body 114 under the action of the mixing mechanism 160. The tilting plate 1144 is a metal plate at a certain angle. When the silo rotates, the tilting plate 1144 continuously lifts and scatters the material, ensuring full contact between solid particles and metal vapor. The reaction temperature control mechanism 113 is located on the outer wall of the furnace body 114, and an insulation layer covers its outer surface. The reaction temperature control mechanism 113 includes a first heating element 1131 and a first insulation layer 1132. The first heating element 1131 is laid on the upper and lower side walls of the furnace body 114. The heating control system controls the heating, cooling, and insulation within the furnace body 114. The first insulation layer 1132 covers the outer side of the furnace body 114. The heating control system can automatically adjust the temperature according to a set curve. The first heating element 1131 of the reaction temperature control mechanism 113 is a medium-temperature type with a maximum operating temperature of 1000℃. The first heating element 1131 is controlled by a programmable logic controller (PLC) or industrial computer, which is electrically connected to the solid-state relay, thermocouple, and motor of the cooling mechanism of the first heating element 1131. Operators can set the heating rate (1~20℃ / min), target temperature, holding time, and cooling rate via the control panel. The system automatically executes the set curve and displays parameters such as temperature and vacuum level in real time.
[0029] Both sides of the furnace body 114 are provided with transition zones 115. The left transition zone 115 connects to the evaporation container 120 and serves as the inlet channel for metal vapor. The right transition zone 115 connects to the feeder 132 and the atmosphere control mechanism 140 and serves as the inlet for reactants and the exhaust port. The gas pipe 111 is inserted into the furnace body 114 through the transition zone 115. The gas pipe 111 is provided with a movable rotating interface 163. The feed port 1141 and the exhaust pipe 141 are arranged side by side and are both inserted into the furnace body 114 through the transition zone 115. Movable rotating interfaces 163 are also provided on the outside of the feeder 132 and the exhaust pipe 141. The movable rotating interfaces 163 are used to keep the gas pipe 111, the feeder 132 and the exhaust pipe 141 stable when the furnace body 114 rotates.
[0030] A gas pipe 111 is located in the left transition zone 115 of the furnace body 114. The gas pipe 111 is used for the inflow of metal vapor into the interior of the furnace body 114. Concentric stainless steel sheets 1151 are arranged around the pipe in the left transition zone 115 for heat insulation, dust blocking and pipe support. These stainless steel sheets 1151 are stacked in concentric circles or spirals and serve three purposes: first, to block dust flowing back from the reaction vessel 110 into the evaporation vessel 120; second, to reduce heat radiation outward along the pipe; and third, to support the gas pipe 111 and keep it in a centered position.
[0031] The leftmost transition zone 115 is connected to a vacuum sealing flange 1152, which is used to ensure the airtightness of the connection and maintain the vacuum required by the furnace body 114.
[0032] A movable rotating interface 163 is installed on the gas pipeline 111 between the reaction vessel 110 and the evaporation vessel 120, allowing the furnace body 114 to rotate relative to the evaporation vessel 120 when it is stationary. The rotating end of the movable rotating interface 163 is rigidly fixedly connected to the gas pipeline 111, which rotates synchronously with the furnace body 114. The stationary end of the movable rotating interface 163 is rigidly fixedly connected to the outside of the evaporation vessel 120 via a fixed pipe section. This configuration ensures that the gas pipeline 111 maintains connectivity and a vacuum or positive pressure seal within the system even when it rotates freely 360° with the furnace body 114 of the reaction vessel 110.
[0033] The right-side transition zone 115 of the furnace body 114 contains a right-side pipe. The right-side pipe has a rotary feed pipe of the feeder 132 and an exhaust pipe 141 of the atmosphere control mechanism 140 in the middle. The rotary feed pipe has internal spiral vanes and is connected to the feed hopper 131 and the feeder 132 via a sealed bearing 173. Its left end extends into the reaction vessel 110. The feeder 132 quantitatively pushes the powdered or granular reactants from the feed hopper 131 into the rotary feed pipe, and the vanes inside transport the materials into the hopper. Similar to the left side, the right-side pipe is also equipped with a stainless steel sheet 1151, a right-side vacuum sealing flange 1152, and a movable rotating interface 163. The outer side of the right-side transition zone 115 is connected to the rotating mechanism 162 for rotating the furnace body 114. The furnace body 114 rotates uniformly at a speed of 1~100 rpm under the drive of the rotating mechanism 162.
[0034] (2) Evaporation container 120.
[0035] Please see Figure 2 The evaporation container 120 includes a reserve area 122, an evaporation area 123 and a cooling area 124 arranged sequentially in a horizontal direction. A first heat-insulating partition layer 125 that can be raised and lowered is provided between the reserve area 122 and the evaporation area 123, and a second heat-insulating partition layer 126 that can be raised and lowered is provided between the evaporation area 123 and the cooling area 124.
[0036] The standby zone 122 is a storage area for spare crucibles; this area is not equipped with heating elements. The evaporation zone 123 is the core working area of the evaporation vessel 120, and its exterior is covered by an evaporation temperature control mechanism 121. The interior of the evaporation zone 123 houses the raw materials for generating metal vapor; depending on the type of metal vapor required, the raw materials are selected from any of the following: carbothermic reduction mixture (carbonaceous reducing agent + magnesium-containing raw material + optional catalyst) for generating magnesium vapor, Pidgeon process mixture (calcined white + ferrosilicon alloy + mineralizer), magnesium ingots or magnesium-containing alloys; elemental calcium or calcium-containing alloys for generating calcium vapor; elemental sodium, elemental potassium, or sodium-potassium alloys for generating sodium or potassium vapor. The cooling zone 124 is used to cool empty crucibles or crucibles that have not yet fully reacted, which are removed from the evaporation zone, for safe removal.
[0037] When the metal raw materials in the evaporation zone 123 are exhausted, the first heat insulation layer 125 and the second heat insulation layer 126 are raised, and a new crucible in the waiting zone 122 is pushed into the evaporation zone 123. At the same time, the empty crucible in the evaporation zone 123 is pushed into the cooling zone 124, and continuous production is carried out under the condition that the evaporation zone 123 and the reaction vessel 110 are not cooled.
[0038] An evaporation temperature control mechanism 121 is disposed in the evaporation zone 123, and a gas pipeline 111 is connected to the evaporation zone 123. The evaporation temperature control mechanism 121 includes a second heating element 1211 and a second insulation layer 1212. The second heating element 1211 is used to heat the metal raw material to generate metal vapor in the evaporation zone 123. The second insulation layer 1212 is wrapped around the evaporation zone 123 and the pipeline to reduce heat loss. When the first thermal insulation layer 125 rises, the waiting area 122 connects with the evaporation area 123, allowing the push rod to push the crucible from the waiting area 122 into the evaporation area 123. When the second thermal insulation layer 126 rises, the evaporation area 123 connects with the cooling area 124, allowing the push rod to push the crucible from the evaporation area 123 into the cooling area 124. When the first thermal insulation layer 125 and the second thermal insulation layer 126 descend, they thermally isolate adjacent areas, maintaining the evaporation container 120 at a high temperature during operation and preventing the high temperature (1150~1700℃) of the evaporation area 123 from being conducted to the waiting area 122. The heating element of the evaporation temperature control mechanism 121 is a high-temperature type with a maximum operating temperature of 1700℃.
[0039] The evaporation vessel 120 is also provided with a sealing flange and rollers 127. The vacuum sealing flange is located at the leftmost end of the evaporation vessel 120 (the side away from the reaction vessel 110) to seal the system and maintain the internal vacuum. The rollers 127 are located below each section of the evaporation vessel 120 to support the weight of the entire evaporation vessel 120 and allow it to move slightly axially to compensate for thermal expansion.
[0040] The gas pipe 111 is connected to both the evaporation zone 123 of the evaporation container 120 and the reaction container 110, so as to guide the generated metal vapor to the reaction container 110.
[0041] (3) Feeding and discharging mechanism 130.
[0042] The feeding and discharging mechanism 130 includes a feeding bin 131, a feeder 132, and a discharging bin 133. The feeder 132 is a screw feeder 132, equipped with a rotary feed pipe and a rotating motor. The discharge port 1142 of the feeder 132 is sealed to the inlet of the rotary feed pipe via a bellows. The other end of the rotary feed pipe passes through the vacuum-sealed flange 1152 and the movable rotating interface 163 of the right-side transition zone 115, ultimately extending into the inlet 1141 of the reaction vessel 110. Helical vanes are welded to the inner wall of the rotary feed pipe. The feeding bin 131 is connected to the feeder 132 and is used to push material from the feeding bin 131 to the furnace body 114. When material falls from the feeder 132 into the inlet of the rotary feed pipe, the vanes rotate with the pipe body, pushing the material forward to achieve feeding. The feeding rate can be controlled collaboratively by adjusting the rotation speed of the feeder 132 and the rotation speed of the rotary feed pipe.
[0043] The discharge bin 133 is located on the gas pipeline 111, on the pipeline bypass below the movable rotary interface 163, and is used to collect the material that has reacted with the metal vapor in the furnace body 114. The material that has completed the reaction falls into the discharge bin 133 through the discharge port 1142, the gas pipeline 111 and the bypass.
[0044] (4) Atmosphere control mechanism 140.
[0045] The atmosphere control mechanism 140 includes a vacuum pump 142, which can be a rotary vane vacuum pump unit, a slide valve Roots pump unit, or a screw Roots pump unit, used to evacuate the system to achieve the required working vacuum level (<800 Pa, preferably <100 Pa) within the reaction vessel 110. One end of the evacuation pipe 141 extends into and communicates with the furnace body 114, while the other end is connected to the vacuum pump 142. A filter 143 is installed at the end of the evacuation pipe 141 located inside the furnace body 114. A filter chamber 144 is installed inside the evacuation pipe 141 on the side closest to the vacuum pump 142. A filter plate 145 is also installed inside the evacuation pipe 141. A vacuum gauge 146 and a high-precision vacuum meter 147 are installed on the evacuation pipe 141 for monitoring the vacuum level. The vacuum gauge 146 is either an analog or digital type, used for coarse measurement and on-site indication; the high-precision vacuum meter 147 is used for precise measurement. In this invention, the filter 143, filter plate 145, and filter chamber 144 sequentially arranged on the extraction pipe 141 can effectively filter the extracted gas, preventing particles or powders from entering the vacuum pump 142 during the reaction process, thus achieving thorough filtration. Furthermore, the atmosphere control mechanism 140 is also equipped with a support body 171 and rollers 127 to support and move the entire vacuum system, and to compensate for thermal expansion and contraction of the pipeline.
[0046] The inlet valve 112 is a mass flow controller, installed on the bypass of the reaction vessel 110 or pipeline, used to introduce high-purity argon gas (purity ≥99.999%). When the system is working, the vacuum pump 142 first evacuates to the set vacuum level.
[0047] In addition, the atmosphere control mechanism 140 also includes a support body 171 and a roller 127. The support body 171 is used to support the entire vacuum pipeline system; the roller 127 is located at the bottom of the support body 171 and can compensate for the displacement of the pipeline caused by thermal expansion and contraction.
[0048] (5) Condensation mechanism 150.
[0049] In this invention, the condensation mechanism 150 includes a porous condenser, which is disposed on the suction pipe 141, between the filter chamber 144 and the vacuum pump 142, or at the front end of the filter chamber 144 (near the reaction vessel 110), for condensing and recovering metal vapor or compound vapor. The porous condenser is filled with porous metal or ceramic packing. When the condensable vapor generated by the reaction passes through the porous condenser with the airflow, it condenses into liquid or solid at a low temperature surface. High-purity nano-metal powder or compound powder can be obtained by periodically collecting the condenser.
[0050] (6) Hybrid mechanism 160.
[0051] The mixing mechanism 160 is either an agitator extending into the furnace body 114 to stir the materials or a rotating mechanism 162 used to drive the furnace body 114 to rotate. When the mixing mechanism 160 is an agitator, the furnace body 114 does not need to rotate; the agitator is used to achieve mixing and tumbling of the materials within the furnace body 114. In this case, a discharge plate 1143 and a tipping plate 1144 can be installed inside the furnace body 114, or they can be omitted. When the mixing mechanism 160 is a rotating mechanism 162, it uses a rotating motor, a reducer, a drive gear, and a driven gear ring to drive the furnace body 114 to rotate. The rotating motor is a variable frequency speed control motor, and its output shaft is connected to the reducer. The reducer's output shaft is fitted with the drive gear. The driven gear ring is fixedly mounted on the outer wall of the furnace body 114 and meshes with the drive gear. The rotational motor is set to a speed (1~100 rpm) via the control panel, which drives the drive gear to rotate the driven gear ring and the entire furnace body 114 at a uniform speed, causing the material inside the furnace body 114 to tumble continuously under the action of the tipping plate 1144.
[0052] (7) Tilting mechanism 170.
[0053] The tilting mechanism 170 includes a support body 171, a support platform 172, a bearing 173, and a push rod 174. In this invention, the support platform 172 serves as the platform for the entire equipment. The reaction vessel 110, evaporation vessel 120, feeding / discharging mechanism 130, and atmosphere control mechanism 140 are all mounted on this support platform 172. One end of the support body 171 is mounted on the support platform 172, and the other end is connected to the furnace body 114. The support body 171 has an internal rotating shaft, allowing the furnace body 114 to tilt around this shaft. The furnace body 114 is rotatably mounted on the surface of the support body 171. One side of the support platform 172 is connected to the bearing 173, and the other side is close to the push rod 174. One end of the push rod 174 is hinged to the bottom of the reaction vessel 110 near the right transition zone 115. The push rod 174 is used to tilt the furnace body 114. The push rod 174 is controlled by a tilt angle adjustment button on the control panel and can drive the furnace body 114 to tilt for material discharge. When the furnace body 114 is tilted, the corresponding evaporation container 120, feeding and discharging mechanism 130 and atmosphere control mechanism 140 are also tilted.
[0054] (8) Cooling mechanism The metal vapor reduction furnace 100 of this invention also includes a cooling mechanism, which comprises a blower and an exhaust port 116. The blower is fixedly installed below or to the side of the reaction vessel 110, with its exhaust port facing the bottom of the reaction vessel 110. The exhaust port 116 is an opening equipped with an electric valve and is located above the chamber wall of the furnace body 114. The exhaust port 116 is used to discharge hot gas to achieve rapid cooling of the reaction vessel 110.
[0055] When the reaction is complete and rapid cooling is required, the heating element is turned off and the cooling mechanism is started. The blower blows cooling gas, such as room temperature or cooled air / nitrogen, into the reaction vessel 110 through the air inlet valve 112. At the same time, the exhaust port 116 is opened and the hot gas is discharged from the exhaust port 116, forming forced convection cooling.
[0056] The aforementioned metal vapor reduction furnace 100, with its horizontal series structure, is a typical but non-limiting example listed in this application. Based on the same series thermal reduction principle, other optional configurations include intermittent horizontal structures, integrated vertical structures, and separate vertical structures.
[0057] For example, the metal vapor reduction furnace 100 of this application can also have a variety of variations: Variant 1: Intermittent horizontal series structure.
[0058] like Figure 3 As shown, this variant is a... Figure 1 The diagram shows a simplified horizontal series structure. (And...) Figure 1 In comparison, this variant omits the feeding and discharging mechanism 130, including the feeding bin 131, the feeder 132, and the rotary feed pipe, and also omits the multi-zone relay structure in the evaporation container 120, including the backup zone 122, the first thermal insulation layer 125, the second thermal insulation layer 126, and the cooling zone 124.
[0059] Specifically, the reaction vessel 110 of this variant and Figure 1 The basic structure is the same, retaining the tilting plate 1144, discharge plate 1143, first heating element 1131, insulation layer, rotating motor, and furnace tilting system. However, feeding and discharging are done manually. The evaporation container 120 retains only one independent evaporation zone 123, without a waiting area or cooling zone. The evaporation zone 123 is equipped with a removable insulated door. The metal is loaded once, and after the reaction, the entire container must be cooled before it can be loaded again. This variant has a simple structure and low equipment investment. Its core "metal vapor generation-metal thermal reduction series" principle and independent temperature zone control, vacuum and atmosphere control structures are similar to those of the previous version. Figure 1 The scheme shown is exactly the same.
[0060] Variant 2: Integrated vertical series structure.
[0061] like Figure 4 As shown, in this invention, the reaction vessel 110 and the evaporation vessel 120 are integrally arranged and connected by a gas pipeline 111. The reaction vessel 110 is disposed inside the evaporation vessel 120 and isolated by a heat insulation layer, ensuring that the reaction vessel 110 and the evaporation vessel 120 are still heated by independent heating mechanisms. The evaporation vessel 120 is provided with an evaporation temperature control mechanism 121, and the reaction vessel 110 is provided with a reaction temperature control mechanism 113. A stirrer 202 is disposed inside the reaction vessel 110. This invention... Figure 4 The diagram shown is only a typical illustration and can be adapted and modified accordingly.
[0062] Variant 3: Separate vertical series structure.
[0063] like Figure 5 As shown, the evaporation vessel 120 (vertical or horizontal furnace) is located below or to the side of the reaction vessel 110 (vertical reduction furnace), and its top is connected to the bottom or lower side of the reaction vessel 110 via a heat-resistant steel pipe 201 with an insulation jacket. The reaction vessel 110 is equipped with a stirrer 202, a side-vented crucible, and an S-shaped ventilation channel 203. A removable insulated furnace cover 204 is installed on the top of the reaction vessel 110. An impeller 206 extends into the reaction vessel 110 from the stirrer 202. The evaporation vessel 120 has a material inlet 205, which can serve as a material inlet 1141, a material outlet 1142, or a gas inlet / outlet. The two furnace bodies 114 share the same atmosphere control mechanism 140, enabling independent heating of the evaporation vessel 120 and the reaction vessel 110. This variant achieves the most thorough physical isolation and independent control of the two temperature zones, avoiding thermal interference from the high-temperature metal vapor zone to the low-temperature reaction zone, and is especially suitable for process scenarios with large temperature differences.
[0064] Based on the aforementioned metal vapor reduction furnace 100, this invention provides a method for preparing silicon-based nanomaterials, which is carried out using the aforementioned metal vapor reduction furnace 100. In this application, the method is described with reference to a horizontal series structure of the metal vapor reduction furnace 100. Other structures also have similar method operations, which will not be described in detail in this application.
[0065] The method of this invention uses safer and lower-cost metal raw materials, eliminating the need for flammable and explosive micron-sized metal powders. Depending on the type of metal vapor, corresponding generation methods are employed: for magnesium vapor, it can be obtained through carbothermic reduction (carbonaceous reducing agent and magnesium-containing minerals), the Pidgeon process (ferrosilicon alloy reduction calcination), or direct heating and evaporation of magnesium ingots / magnesium-containing alloys; for calcium vapor, it is obtained by heating and evaporating elemental calcium or calcium-containing alloys; for sodium or potassium vapor, it is obtained by heating and evaporating elemental sodium, elemental potassium, or sodium-potassium alloys. The resulting metal vapor comes into full contact with the reactants (such as silicon-containing precursors, key metal minerals, or industrial solid waste) and undergoes a reduction reaction to generate the target crude product. The two key reactions of this invention are carried out in two isolated and independently temperature-controlled regions, namely, an evaporation vessel 120 and a reaction vessel 110: when magnesium vapor is generated, the evaporation vessel 120 is independently heated to 650~1700℃ depending on the magnesium source type; when calcium vapor is generated, it is heated to 1000~1300℃; and when sodium or potassium vapor is generated, it is heated to 600~900℃. The reaction vessel 110 is independently heated to 600~1000℃, allowing for the replacement of metal raw materials and reactants without the entire vessel being cooled to room temperature. Because the metal vapor is dispersed at the atomic level, the reduction reaction has a low energy barrier and releases little heat, and the mean free path of gas molecules is significantly increased under vacuum conditions, the contact between the metal vapor and the solid material is more uniform, and the reaction rate is faster. Therefore, this invention can achieve efficient reduction without the addition of heat regulators, completely preserving the original microstructure of the reactants (such as the platy, tubular, and fibrous structures of clay minerals), and significantly reducing or even completely eliminating the formation of unreacted precursors and high-temperature byproducts (such as magnesium silicide, spinel, etc.). The porous condenser installed on the extraction pipe 141 can recover and condense metal vapor, and the pickling waste liquid can be used to replenish magnesium / aluminum sources and adjust pH to prepare hydrotalcite, realizing the resource utilization of the entire process.
[0066] The method includes the following steps: S1. Loading and Pretreatment The reactants are placed in the reaction vessel 110, and the metal raw materials are placed in the evaporation zone 123 of the evaporation vessel 120. The atmosphere control mechanism 140 evacuates the reaction vessel 110 and the evaporation vessel 120.
[0067] Before evacuation, inert gas is introduced into the evaporation container 120 and the reaction container 110 through the gas inlet valve 112.
[0068] The molar ratio of metal raw materials to reactants is 0.3~2.5:1.
[0069] Specifically, the metal raw material is loaded into the crucible in the evaporation zone 123, while a spare crucible and spare metal raw material can be placed in the reserve zone 122. The metal raw material is selected based on the required type of metal vapor and the cost of the raw material. When magnesium vapor is generated, any of the following sources can be used: magnesium ingots or magnesium alloys, heated to 650~1000℃; Pidgeon process raw materials (a mixture of calcined magnesia, ferrosilicon alloy, and fluorite mineralizer, in a mass ratio of 6:0.8~1.2:0.1~0.2), heated to 1100~1300℃; carbothermic reduction process raw materials (a mixture of carbonaceous reducing agent and magnesium-containing raw materials, with the addition of a catalyst), heated to 1150~1700℃. The carbonaceous reducing agent is selected from one or more of coke, coal coke, semi-coke, metallurgical coke, petroleum coke, bituminous coal, anthracite, graphite, activated carbon, and charcoal; the magnesium-containing raw material is selected from one or more of magnesium oxide, calcined magnesite, dolomite, and calcined magnesia; and the catalyst is selected from one or more of fluorite, calcium fluoride, and calcium oxide.
[0070] When calcium vapor is generated, use elemental calcium or calcium-containing alloys, and heat at a temperature of 1000~1300℃.
[0071] When sodium or potassium vapor is generated, elemental sodium, elemental potassium, or sodium-potassium alloy are used, and the heating temperature is 600~900℃.
[0072] The reactants include at least one of the following: clay minerals with natural nanostructures or their modified products, silicon-containing precursors, metal-containing minerals, industrial solid waste, or synthetic nanomaterial precursors.
[0073] The clay minerals include any one or more of montmorillonite, kaolinite, halloysite, palygorskite, talc, black talc, muscovite, soapstone, biotite, lepidolite, illite, chlorite, sepiolite, and pyrophyllite; the modified product is a product obtained by at least one of heat treatment, acid treatment, mechanical treatment, organic modification, or inorganic modification.
[0074] The silicon-containing precursor includes at least one of silica materials, industrial by-products, and silicon-carbon precursors; wherein, the silica materials include any one or more of the following: synthetic silica such as fumed silica, precipitated silica, silica sol, mesoporous silica such as MCM-41 and SBA-15, hollow or core-shell structured silica, and natural minerals such as quartz, silica, and quartz sand; the industrial by-products or wastes include any one or more of the following: waste solar panels, silica ash, rice husk ash, and fly ash; the silicon-carbon precursors include any one or more of the following: rice husk, straw, bamboo leaves, reeds, bagasse, silicon-containing plastics, silicon-containing rubber, and waste clay that adsorbs organic matter; and the modified products of the above precursors, wherein the modification methods include at least one of the following: heat treatment, acid treatment, mechanical treatment, organic modification, and inorganic modification; after metal vapor reduction, the by-product metal oxides are removed by acid washing to obtain nano-silicon or nano-silicon / carbon composite materials, which are used as a negative electrode for lithium-ion batteries.
[0075] Furthermore, a carbon source can be added to the silicon-containing precursor; the carbon source is selected from any one or more of carbon powder, graphite, graphene, carbon nanotubes, carbon fibers, and carbon black; the silicon-containing precursor or its modified product is pre-purified and dried in an oven, and all selected particles are passed through a sieve with a mesh size >100.
[0076] Metal-bearing minerals refer to precursors used for the extraction of critical minerals, minerals containing critical metals, and one or more layered silicate minerals used for the extraction of critical metals (such as lithium).
[0077] Industrial solid waste refers to industrial solid waste or tailings as raw materials, selected from at least one of the following: smelting slag containing a target metal (such as lithium), steel dust, electroplating sludge, spent catalysts, waste battery powder, red mud, and fly ash. Precursors for synthesizing nanomaterials include, but are not limited to, nano-metals, nano-alloys, nano-ceramics, and nano-compounds.
[0078] The reactants can be pre-mixed with inorganic salts (NaCl, KCl, CaCl2, MgCl2, etc.) at a mass ratio of 0~5:1 to absorb the exothermic reaction. The reactants are pushed into the reaction vessel 110 through the feeder 132 and the rotary feed pipe. The rotary motor is started to make the reaction vessel 110 rotate at a constant speed of 1~100 rpm, and the tilting plate 1144 continuously lifts the material. All vacuum sealing flanges 1152 are closed, and the vacuum pump 142 is started to draw a vacuum. At the same time, inert gas can be introduced into the system to replace the air. The vacuum degree during operation is <800 Pa (preferably <100 Pa).
[0079] The heating temperature of the reaction vessel 110 is set according to the type of metal vapor: 600-900℃ for magnesium vapor, 800-1000℃ for calcium vapor, and 600-900℃ for sodium or potassium vapor. The inventors have discovered that the vacuum metal vapor reduction process of this invention, due to the atomic dispersion of the metal vapor, lowers the energy barrier of the reduction reaction and generates less heat. Simultaneously, the mean free path of gas molecules increases significantly under vacuum conditions, resulting in a more uniform and rapid reduction reaction. Therefore, the generation of byproducts can be significantly reduced without the need for inorganic salts to regulate the heat.
[0080] After the furnace body 114 is filled with material, it rotates, and the rotation speed of the furnace body 114 is 1~100 rpm.
[0081] S2, reduction reaction.
[0082] After evacuating to <800 Pa, the evaporation temperature control mechanism 121 and the reaction temperature control mechanism 113 are activated respectively to raise the temperature inside the evaporation container 120 to 650~1700℃ to generate metal vapor. The metal vapor enters the reaction container 110 through the gas pipe 111, raising the temperature inside the reaction container 110 to 600~900℃, causing the metal vapor to undergo a gas-solid reduction reaction with the reactants to obtain a crude reduced product containing byproduct metal oxides.
[0083] The heating temperature of the evaporation container 120 is set differently depending on the selection of the metal raw material; When the metal raw material is a mixture of metal minerals and reducing agents, the evaporation temperature control mechanism can heat the evaporation zone to 1100~1700℃, so that the mixture undergoes carbothermic reduction or metallothermic reduction reaction to generate metal vapor in situ; the metal minerals are selected from one or more of magnesium oxide, calcined magnesite, dolomite, and calcined white metal; the reducing agent is selected from one or more of coke, coal coke, semi-coke, metallurgical coke, petroleum coke, bituminous coal, anthracite, graphite, activated carbon, and charcoal.
[0084] When the metal raw material is magnesium ingot, magnesium alloy, elemental calcium, calcium alloy, elemental sodium, elemental potassium, or sodium-potassium alloy, the evaporation temperature control mechanism can heat the evaporation zone to 600~1300℃, so that the metal raw material evaporates to produce metal vapor.
[0085] The two zones are heated at a rate of 5-15℃ / min. Since the evaporation container 120 requires a higher temperature, the reaction container 110 often reaches the target temperature first. At this point, the program control system automatically enters the heat preservation mode. The total heat preservation time is calculated after the evaporation container 120 reaches the target temperature. The heat preservation time of the reaction container 110 must cover the time difference between the two chambers reaching the predetermined temperature, and continue for an additional 0.5-8 hours (preferably 1-3 hours) on top of this time difference. The heat preservation time of the evaporation container 120 is generally equal to or slightly shorter than that of the reaction container 110, as it continuously generates metal vapor after reaching the target temperature. During the heating process, the metal in the evaporation zone 123 undergoes a thermal reduction reaction to generate metal vapor, which enters the reaction container 110 through the gas pipe 111 and comes into full contact with the material continuously tumbling under the action of the turning plate 1144, resulting in a gas-solid reduction reaction. The gaseous byproducts generated by the reaction, as well as unreacted argon and excess metal vapor, are discharged through the extraction pipe 141. They then pass through the filter chamber 144, filter plate 145, and filter 143 (to remove dust), and are then condensed and recovered by a porous condenser. Non-condensable gases are discharged by the vacuum pump 142. When the metal in the evaporation zone 123 is exhausted, there is no need for overall cooling: the first insulation layer 125 and the second insulation layer 126 are raised, and the new crucible in the waiting area 122 is pushed into the evaporation zone 123 by the external push rod 174. At the same time, the empty crucible is pushed into the cooling zone 124, and production is achieved without cooling the evaporation zone 123 and the reaction vessel 110.
[0086] S3. Post-processing and resource utilization.
[0087] After the reaction is completed, the reaction product is post-processed by acid washing, water washing and drying to remove the by-product metal oxide, and silicon-based material product is obtained. The gas after the reaction is recovered by condensation device 150.
[0088] Specifically, after the reaction is complete, the first heating element 1131 and the second heating element 1211 are turned off, and the argon gas supply is stopped. The cooling mechanism is activated to blow cooling gas (air or nitrogen) into the reaction vessel 110, and the exhaust port 116 is opened simultaneously to form forced convection cooling, reducing the temperature of the chamber to below 50°C. The vacuum pump 142 is turned off, and after the vacuum is broken, the tilting system of the furnace body 114 is activated to tilt the reaction vessel 110 to the left, allowing the crude reaction product to fall into the discharge chamber 133 through the gas channel. The crude product is then removed and post-processed according to the target product type: for silicon-based materials, it is washed sequentially with hydrochloric acid (or sulfuric acid, nitric acid) at a volume concentration of 1-20% for 0.1-10 hours to remove byproducts such as MgO; after solid-liquid separation, it is washed with hydrofluoric acid at a volume concentration of 1-10% for 1-60 minutes to remove unreacted SiO2; finally, it is washed with deionized water until neutral and vacuum dried at 60-80°C for 8-24 hours to obtain nano-silicon or nano-silicon / carbon composite materials. Pickling waste liquid (mainly containing MgCl2, MgSO4 and a small amount of Al) 3+ Fe 3+ After collection, magnesium or aluminum sources are added, and the pH is adjusted to 6-14 (preferably 9-11) with an alkaline solution (such as sodium hydroxide or sodium carbonate). After aging, filtration, and drying, hydrotalcite is prepared, achieving full-element resource utilization of the waste liquid. The condensate recovered from the porous condenser is periodically removed and purified or directly used as nano-metal powder products as needed. By controlling parameters such as metal type, reactant type, metal-to-silicon molar ratio (0.3-2.5:1), and reaction time (0.5-8 hours), various types of materials, including nanoscale and microscale elemental silicon, silicon suboxide, silicon carbide, silicon nitride, metal silicides, nano-metals, nano-alloys, and high-entropy alloys, can be prepared, widely applicable in new energy, key metal extraction, and solid waste resource utilization.
[0089] The following describes in detail the overall structure, working principle, and technical effects of the metal vapor reduction furnace 100 provided by the present invention, as well as the detailed steps, implementation principles, and technical effects of the supporting silicon-based nanomaterial preparation method, through embodiments and in conjunction with the accompanying drawings.
[0090] Example 1 This embodiment uses the horizontal series structure described above as the metal vapor reduction furnace 100 to prepare silicon-based nanomaterials, specifically including the following steps: S1. The bulk mixture and the silicon-containing precursor are respectively added to the evaporation vessel 120 and the reaction vessel 110, with a mass ratio of 180:50 between the bulk mixture and the silicon-containing precursor.
[0091] The bulk mixture is made by mixing magnesium oxide (MgO, purity ≥98%), coke (fixed carbon ≥85%), and calcium fluoride (CaF2, purity ≥95%) in a mass ratio of 100:72:8 and then pressing them together. 18 kg of the bulk mixture is weighed and placed in the crucible in the evaporation zone 123. Simultaneously, a spare bulk mixture is placed in the reserve zone 122 to facilitate non-cooling operation of the evaporation vessel 120.
[0092] The silicon-containing precursor is acid-washed montmorillonite: Montmorillonite ore (montmorillonite content ≥85%) is taken and acid-washed in 1 mol / L hydrochloric acid for 40 h to remove metallic impurities such as iron and aluminum and enrich the silicon content. After acid washing, it is filtered, washed until neutral, dried in an oven at 105℃ for 12 h, and ground through a 200-mesh sieve to obtain relatively pure SiO2. 5 kg of acid-washed montmorillonite is weighed and pushed into the reaction vessel 110 through the feeder 132 and the rotary feed pipe. The rotating motor is started, causing the reaction vessel 110 to rotate at a uniform speed of 5 rpm, and the tipping plate 1144 continuously lifts the material.
[0093] Close all vacuum sealing flanges 1152 and start vacuum pump 142 to evacuate to <800 Pa.
[0094] S2. Start the heating control system to independently control the temperature of evaporation container 120 and reaction container 110. The target temperature of evaporation zone 123 is set to 1500℃; the heating temperature of reaction container 110 is set to 700℃. Due to the higher temperature of evaporation zone 123, the heating time is longer. Reaction container 110 first reaches 700℃ and automatically enters the heat preservation mode. After evaporation zone 123 reaches 1500℃, the total heat preservation time is calculated and set to 2 hours.
[0095] During the heating process, the blocky mixture in evaporation zone 123 undergoes a carbothermic reduction reaction: MgO + C → Mg(g) + CO(g). The generated magnesium vapor enters the reaction vessel 110 through the left-side pipe, where it comes into full contact with the acid-washed montmorillonite, which is continuously tumbling under the action of the turning plate 1144, resulting in a gas-solid reduction reaction: SiO2 + 2Mg → Si + 2MgO. The gaseous byproducts generated in the reaction (CO and unreacted argon) are finally discharged through the extraction pipe 141, and the porous condenser condenses and recovers any condensable metal vapors that may be generated.
[0096] S3. After the reaction is complete, close the first heating element 1131, the second heating element 1211, and the inlet valve 112 to stop the argon gas supply. Start the cooling mechanism to blow cooling air into the reaction vessel 110, and simultaneously open the exhaust port 116 to form forced convection cooling, reducing the chamber temperature to below 30°C. Turn off the vacuum pump 142, break the vacuum, and start the furnace body 114 tilting system to tilt the reaction vessel 110 to the left, allowing the crude reaction product to fall into the discharge hopper 133 through the left-side pipe.
[0097] The crude product was collected and first washed with 5% hydrochloric acid (liquid-solid ratio 10:1) for 10 hours to remove MgO generated in the reaction and soluble impurities from unreacted acid-washed montmorillonite. After solid-liquid separation, a silicon-based crude product was obtained, which was then washed with 1% hydrofluoric acid (liquid concentration) for 15 minutes to remove unreacted SiO2. After solid-liquid separation, the product was repeatedly washed with ultrapure water until the washing solution was neutral (pH≈7). The solid was collected in a tray and placed in a vacuum desiccator, where it was dried with stirring at 60°C for 8 hours to obtain the final product.
[0098] like Figure 6 The image shows the X-ray diffraction patterns of the crude and final products. The crude product exhibits typical diffraction peaks of magnesium oxide (MgO) and elemental silicon (Si), with no other impurity phases observed. The final product shows only characteristic diffraction peaks of elemental silicon, with no MgO or SiO2 residues. According to the Scherrer formula, the silicon grain size is approximately 13 nm.
[0099] Elemental analysis of the final product revealed that the Si content was 94.0 wt%, the O content was 0.8 wt%, and the C content was 5.2 wt% (from the carbon generated by the reaction of carbon monoxide and magnesium silicide).
[0100] The reduction rate of silicon dioxide is calculated using the following formula:
[0101] Calculations show that the reduction rate of silica in this embodiment is as high as 99.3%, indicating that under the conditions of magnesium evaporation temperature of 1500℃, high vacuum of 20Pa and heat preservation for 2 hours, the magnesium vapor generated by carbothermic reduction can almost completely reduce the silica in acid-washed montmorillonite to elemental silicon, and the morphology of the product is completely preserved.
[0102] The nano-silicon obtained in this embodiment has good crystallinity and ultra-small grain size (13 nm), and retains the two-dimensional lamellar morphology of the precursor, making it suitable for use as a negative electrode material for lithium-ion batteries or other nano-silicon-based functional materials.
[0103] Example 2 In this embodiment, calcium ingots are used to directly generate calcium vapor, which is then used to reduce palygorskite to prepare nano-silicon. 58 kg of calcium ingots (Ca≥99.9%) are loaded into evaporation zone 123. 50.0 kg of raw palygorskite ore (purity≥90%) is ground through a 200-mesh sieve and fed into reaction vessel 110 via feeder 132. The vessel rotates at 5 rpm. A vacuum of 20 Pa is applied.
[0104] Heating was initiated, with the evaporation zone (123) heated to 1250℃ and the reaction vessel (110) heated to 850℃, and held at these temperatures for 1.5 hours. Calcium vapor entered the reaction chamber through the gas channel and underwent a reduction reaction with palygorskite (2Ca + SiO2 → Si + 2CaO). After the reaction, the mixture was cooled, tilted, and discharged. The crude product was washed with 5% hydrochloric acid for 6 hours, then with 1% hydrofluoric acid for 10 minutes, and finally washed with water and dried to obtain nano-silicon.
[0105] The crude product contains elemental silicon and CaO; after hydrofluoric acid washing, the final product only shows characteristic peaks of elemental silicon, with no impurity phases. The product is fibrous, completely preserving the original one-dimensional morphology of palygorskite, and the fibers are composed of tightly packed nanoparticles with a diameter of approximately 50-100 nm. Elemental analysis shows that the final product contains approximately 95% Si. This example is simple to operate and the product morphology is well preserved.
[0106] Example 3 In this embodiment, magnesium vapor is generated using the Pidgeon process to reduce precipitated silica and prepare nano-silicon. Calcined white silica (MgO to CaO molar ratio 1), ferrosilicon alloy (78.22% silicon, 0.03% S, 0.09% Al), and fluorite (95.1% CaF2) are uniformly mixed at a mass ratio of 6:1.2:0.2, ball-milled through a 200-mesh sieve, and an appropriate amount is weighed and loaded into evaporation zone 123, ensuring that the mass ratio of generated magnesium vapor to precipitated silica is 0.9:1 (i.e., the mass ratio of elemental magnesium to SiO2). 50 kg of precipitated silica (purity ≥99%, average particle size 10~20 μm) is weighed and pushed into reaction vessel 110 through feeder 132 and a rotary feed pipe. The vessel rotates at 5 rpm, and a vacuum of 20 Pa is applied.
[0107] The heating control system is activated, with evaporation zone 123 heating up to 1180℃ at a rate of 10℃ / min, and reaction vessel 110 heating up to 700℃ at a rate of 10℃ / min. Both chambers are kept at the target temperature for 2 hours. The Pidgeon process raw materials undergo a reduction reaction to generate magnesium vapor, which enters reaction vessel 110 through the left-side pipe and undergoes a gas-solid reduction reaction with the tumbling precipitated silica (SiO2 + 2Mg → Si + 2MgO).
[0108] After the reaction, the mixture was cooled and discharged at an angle. The crude product was washed with 5% hydrochloric acid for 6 h to remove MgO, and then washed with 1% hydrofluoric acid for 10 min to remove unreacted SiO2. After washing with water and drying, nano-silicon was obtained. The final product was elemental silicon; the product consisted of spherical or near-spherical nanoparticles with good dispersibility. Elemental analysis showed that the Si content was approximately 98%.
[0109] Example 4 This embodiment demonstrates the equipment's ability to replace metals and materials without disrupting the vacuum or cooling the equipment. Building upon Embodiment 1, without shutting off the heating, after the reaction is complete and the material is discharged, the first and second insulation layers 125 and 126 are raised. An external push rod 174 pushes a pre-placed spare block-shaped mixing crucible in the waiting area 122 into the evaporation zone, while simultaneously pushing an empty crucible into the cooling zone and lowering the insulation layers. The reaction vessel 110 does not need to be re-vacuumed (the system maintains a vacuum), and the second batch of acid-washed montmorillonite is directly fed into the chamber again via the feeder 132. A 2-hour heat preservation period is initiated to complete the second batch reaction. Throughout the process, the reaction vessel 110 does not undergo a heating-cooling-reheating cycle; only the evaporation zone 123 undergoes a short-term material replacement operation, significantly improving production efficiency. The XRD and SEM results of the second batch of products are consistent with those of Embodiment 2. This embodiment demonstrates that the reduction furnace can achieve long-cycle production with significantly reduced energy consumption and labor time.
[0110] Example 5 The only difference between this embodiment and Example 1 is that acid-washed montmorillonite is replaced with silica fume. 5 kg of silica fume (SiO2 content ≥90%) is weighed and fed into reaction vessel 110 via feeder 132. All other conditions are exactly the same as in Example 2. The final product is elemental silicon with a particle size of 50-150 nm and a reduction rate of approximately 97%.
[0111] Example 6 The difference between this embodiment and Embodiment 1 is that the acid-washed montmorillonite is replaced with optical fiber waste (containing approximately 85% SiO2 and approximately 5-10% GeO2). 5 kg of optical fiber waste (ground through a 200-mesh sieve) is weighed and fed into reaction vessel 110, with all other conditions identical to Embodiment 1. The final product is a mixture of elemental silicon and elemental germanium, with a reduction rate of approximately 96%. This embodiment achieves the synergistic recovery of silicon and germanium from optical fiber waste.
[0112] Example 7 The only difference between this embodiment and Example 1 is that the acid-washed montmorillonite is replaced with spodumene (LiAlSi2O6, purity ≥90%). Spodumene is ball-milled, ground through a 200-mesh sieve, and 5 kg is weighed and fed into reaction vessel 110 via feeder 132. All other conditions are identical to Example 2: 18 kg of carbothermic reduction block mixture, magnesium evaporation zone 1500℃, reaction vessel 110℃, and maintained at this temperature for 2 hours. After magnesium vapor reduction, the spodumene structure is destroyed, lithium is released as Li2O, some of which volatilizes and condenses, while some remains in the slag; silicon oxide is reduced to elemental silicon. The crude product is washed with 5% hydrochloric acid, lithium enters the washing solution (in LiCl form), and MgO is removed simultaneously; then, unreacted SiO2 is removed by washing with 1% hydrofluoric acid, and after washing and drying, nano-silicon (particle size 50~150 nm, reduction rate approximately 94%) is obtained. The pickling solution is supplemented with magnesium and aluminum sources, and the pH is adjusted to 9-11. After aging, filtration, and drying, lithium-containing hydrotalcite is prepared to achieve the synergistic recovery of lithium and silicon.
[0113] Example 8 This embodiment adopts the integrated vertical series structure described in variant two (such as...). Figure 4 As shown in the figure, magnesium vapor is directly generated from magnesium ingots to reduce acid-activated montmorillonite and prepare nano-silicon. The specific steps are as follows: 42 kg of magnesium ingots (Mg≥99.9%) are loaded into evaporation zone 123; 50 kg of acid-washed montmorillonite (the same acid-washed montmorillonite used in Example 2) is loaded into reaction vessel 110 with a side-ventilated crucible. After closing the furnace lid, a vacuum of 20 Pa is drawn. The stirrer is started so that the impeller 206 of the stirrer rotates at 60 rpm, and then the heating control system is started. The temperature of evaporation zone 123 is increased to 800℃ at 10℃ / min, and the temperature of reaction vessel 110 is increased to 700℃ at 10℃ / min; after both zones reach the target temperature, the reaction is maintained at this temperature for 1.5 hours. During the reaction, magnesium vapor enters reaction vessel 110 through S-shaped ventilation channel 203 and undergoes a gas-solid reduction reaction with the continuously stirred acid-activated montmorillonite.
[0114] The product has a lamellar morphology formed by the accumulation of nanoparticles, retaining the original two-dimensional lamellar structure of montmorillonite, with a Si content of 98.8 wt% and an O content of 1.2 wt%.
[0115] Example 9 The difference between this embodiment and Example 1 is that the acid-washed montmorillonite is pre-mixed with inorganic salt at a mass ratio of 1:1 and then fed into the reaction vessel 110 through feeder 132. All other conditions are exactly the same as in Example 2. The final product is elemental silicon with a silicon grain size of approximately 11 nm and a reduction rate of approximately 97%.
[0116] Comparative Example 1 Similar to the steps in Example 1, the only difference is that an automatic feeding and discharging system is not installed; the reactants are added manually by opening the chamber. Each addition requires cooling, breaking the vacuum, opening the chamber, adding material, resealing, vacuuming again, and heating up. The entire process takes approximately 3 hours, and the frequent opening of the chamber increases the risk of leakage and material contamination. Example 1 achieves vacuum feeding through a rotating feed pipe and feeder 132.
[0117] Comparative Example 2 Similar to the steps in Example 1, the only difference is that the rotating motor is not activated during the reaction, and the reaction vessel 110 remains stationary. Because the material accumulates inside the chamber, the magnesium vapor can only contact the surface material, resulting in insufficient reduction of the internal material. After the reaction, the surface product is completely reduced, while the bottom material remains unreacted acid-washed montmorillonite, leading to highly uneven product distribution and an overall reduction rate of only about 55%. This demonstrates that rotation of the furnace body 114 is a necessary condition for achieving sufficient contact between the magnesium vapor and the material.
[0118] Comparative Example 3 Similar to the steps in Example 1, the only difference was that the vacuum was only evacuated to 5000 Pa (5 kPa), without further evacuation to 20 Pa. Due to the high residual oxygen content in the system, some magnesium vapor was oxidized to MgO, which not only reduced the effective magnesium vapor concentration but also led to a significant increase in the MgO content in the product. Simultaneously, the residual oxygen reacted with silicon to form SiO2, reducing the silicon yield. The reduction rate dropped to approximately 65%, and XRD showed a significant enhancement of the MgO diffraction peak in the crude product. Example 2 achieved a reduction rate of 99.3% under high vacuum (20 Pa). This demonstrates that high vacuum is crucial for preventing magnesium vapor oxidation and improving reduction efficiency.
[0119] Comparative Example 4 Similar to the steps in Example 1, the only difference is that instead of using an evaporation container 120, micron-sized magnesium powder (particle size ≤ 50 μm) is directly mixed with acid-washed montmorillonite and then added to the reaction container 110. The mass ratio of magnesium powder to acid-washed montmorillonite is the same as in Example 1. Because the magnesium powder is in direct contact with SiO2, the reduction reaction is violently exothermic, resulting in excessively high local temperatures and the formation of a large number of byproducts. The two-dimensional platy morphology of montmorillonite is severely damaged, and particle agglomeration is obvious (particle size > 500 nm). The reduction rate of montmorillonite is only about 68%. In contrast, Example 2 uses an evaporation container 120 to allow magnesium to react with the material in vapor form, resulting in a mild and uniform reaction with a reduction rate of 99.3% and complete preservation of the morphology. This demonstrates that the tandem gas-solid reaction of the present invention avoids local overheating and morphology damage.
[0120] Comparative Example 5 Similar to the steps in Example 1, the only difference is that the heating temperature of evaporation zone 123 is set to 800°C (lower than the 1150~1700°C required for carbothermal reduction). Due to the insufficient temperature, the carbothermal reduction reaction (MgO + C → Mg + CO) is incomplete, resulting in extremely low magnesium vapor production and a reduction rate of only about 30% for acid-washed montmorillonite. This indicates that the temperature of evaporation zone 123 must reach a corresponding threshold based on the type of magnesium source to effectively produce magnesium.
[0121] Comparative Example 6 Similar to the steps in Example 1, the only difference is that the reaction vessel 110 does not have a tilting plate 1144 inside; the material is tumbled solely by the rotation of the container. Due to the lack of the tilting plate 1144's lifting effect, the material accumulates inside the container, and the magnesium vapor can only contact the surface material. The reduction of the internal material is insufficient, and the reduction rate drops from 99.3% in Example 2 to approximately 65%. This demonstrates that the tilting plate 1144 is a crucial structure for achieving sufficient contact between the material and the magnesium vapor.
[0122] Comparative Example 7 Similar to the steps in Example 1, the only difference is that the carbothermic reduction feedstock (magnesium oxide, coke, and calcium fluoride) is not compressed into blocks, but is directly loaded into the evaporation zone 123 in powder form. The powder is prone to dust generation at high temperatures, and this dust enters the reaction vessel 110 with the magnesium vapor, contaminating the product. Simultaneously, the powder has poor permeability, resulting in an unstable magnesium vapor generation rate. Significant carbon impurities appear in the product, and the silicon content decreases from 94.0% to 78%. This indicates that compressing the carbothermic reduction feedstock into blocks is beneficial for stable magnesium production and reduced dust.
[0123] Application Examples The carbon-containing elemental silicon obtained in Example 1 was used as the negative electrode material for lithium-ion batteries, and coin cells were assembled according to the following method: Preparation of the working electrode: The active material (carbon-containing elemental silicon), Super P, and PAA-Li were mixed uniformly at a mass ratio of 8:1:1, coated onto copper foil, vacuum dried, and cut into discs with a diameter of 12 mm. Both the counter electrode and the reference electrode were lithium metal sheets. The electrolyte was a mixed solution of ethylene carbonate and dimethyl carbonate containing 1 mol / L LiPF6 (volume ratio 1:1), with 10 wt.% fluoroethylene carbonate added. Battery assembly was carried out in an argon atmosphere glove box, with water and oxygen concentrations both below 0.1 ppm.
[0124] The electrode sheet prepared from carbon-containing elemental silicon obtained in Example 1 was subjected to cycle performance testing at a current density of 1.0 A / g, with the first three cycles activated at a low current density of 0.1 A / g. The results are as follows... Figure 7As shown, the material has an initial coulombic efficiency of 71%, a specific capacity of up to 2162 mAh / g at a current density of 1.0 A / g, and a specific capacity of 1839 mAh / g after 50 cycles, demonstrating good cycle stability and promising application prospects in the field of lithium-ion batteries.
[0125] In summary, this invention provides a metal vapor reduction furnace and a method for preparing silicon-based nanomaterials. The metal vapor reduction furnace couples the evaporation container 120 and the reaction container 110 in series, enabling independent temperature control of the evaporation zone 123 and the reaction container 110, as well as material replacement without cooling. Combined with automatic feeding and discharging, furnace body 114 rotation and tilting, vacuum and atmosphere control, and porous condensation recovery, long-cycle production can be achieved without disrupting the vacuum or cooling. The material production process uses appropriate methods to generate metal vapor depending on the type of metal vapor. Magnesium vapor can be obtained through carbothermal reduction, the Pidgeon process, or direct heating and evaporation of magnesium ingots / magnesium alloys. Calcium vapor is obtained by heating and evaporating elemental calcium or calcium-containing alloys. Sodium or potassium vapor is obtained by heating and evaporating elemental sodium, elemental potassium, or sodium-potassium alloys. The resulting metal vapor is used to efficiently reduce silicon-containing precursors, key metal minerals, industrial solid waste, or nano-alloy precursors under vacuum. Following acid washing, water washing, and drying, target products such as nano-silicon / silicon-carbon composites, nano-metals, nano-alloys, or high-entropy alloys are obtained. The acid washing waste liquid can be used to replenish magnesium / aluminum sources and adjust the pH to prepare hydrotalcite. The condensable vapor recovered by condensation is converted into high-value-added powders. This invention significantly reduces energy consumption and cost, achieves high reduction rates, and accurately preserves the original microstructure of the reactants, showing broad industrial application prospects in lithium-ion battery anode materials, key metal extraction, solid waste resource utilization, and nano-alloy powder synthesis.
[0126] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A metal vapor reduction furnace, characterized in that, The metal vapor reduction furnace includes a reaction vessel, an evaporation vessel, an atmosphere control mechanism, and a condensation mechanism. The reaction vessel and the evaporation vessel are connected by a gas pipeline. The reaction vessel and the evaporation vessel are independently temperature controlled. The evaporation vessel is equipped with an evaporation temperature control mechanism, and the reaction vessel is equipped with a reaction temperature control mechanism. The atmosphere control mechanism is equipped with a suction pipe connected to the reaction vessel, and the condensation mechanism is located inside the suction pipe. The evaporation vessel is provided with a waiting area, an evaporation area, and a cooling area in sequence along the horizontal direction. The gas pipeline is connected to the evaporation area. A heat-insulating transition area is provided between the gas pipeline and the reaction vessel, and heat-insulating baffles are stacked in the transition area along the airflow direction.
2. The metal vapor reduction furnace according to claim 1, characterized in that, A first heat-insulating partition layer that can be raised and lowered is provided between the reserve zone and the evaporation zone, and a second heat-insulating partition layer that can be raised and lowered is provided between the evaporation zone and the cooling zone; the evaporation temperature control mechanism is located in the evaporation zone.
3. The metal vapor reduction furnace according to claim 1, characterized in that, The reaction vessel includes a furnace body, which is provided with a feed inlet, a discharge outlet, a discharge plate, a tilting plate, and a heat insulation layer. The discharge plate is located on the outlet side of the furnace body, and the tilting plates are located inside the furnace body and are evenly spaced. The reaction temperature control mechanism is located on the outer wall of the furnace body, and the heat insulation layer covers the outer surface of the reaction temperature control mechanism.
4. The metal vapor reduction furnace according to claim 3, characterized in that, The metal vapor reduction furnace also includes a feeding hopper and a feeder, wherein the feeder is a screw feeder and is connected to the feed inlet of the furnace body, and the feeding hopper is connected to the feeder; And / or, the metal vapor reduction furnace further includes a mixing mechanism, which is either a stirrer extending into the furnace body to stir the material or a rotating mechanism for driving the furnace body to rotate; when the mixing mechanism is a rotating mechanism, transition zones are provided on both sides of the furnace body, the gas pipe is inserted into the furnace body through the transition zones, the gas pipe is provided with a movable rotating interface, the feed inlet and the exhaust pipe are arranged side by side and are both inserted into the furnace body through the transition zones, and movable rotating interfaces are also provided on the outer sides of the feeder and the exhaust pipe, the movable rotating interfaces are used to maintain the stability of the gas pipe, the feeder and the exhaust pipe when the furnace body rotates; And / or, the metal vapor reduction furnace further includes a tilting mechanism for tilting the furnace body. The tilting mechanism includes a support body, a support platform, a bearing, and a push rod. The support body is disposed on the support platform, and the furnace body is rotatably disposed on the surface of the support body. One side of the furnace body is connected to the bearing, and the other side is connected to the push rod. The push rod pushes the furnace body to tilt.
5. The metal vapor reduction furnace according to claim 3, characterized in that, The gas pipeline, feeder, extraction pipe, and discharge hopper are arranged as follows: the feed hopper and feeder are fixed on the support at the end of the furnace body and tilt synchronously with the furnace body; the gas pipeline is rigidly fixed to the furnace body and moves with it, and is connected to an external fixed pipeline through a movable rotating interface; the extraction pipe is embedded in the gas pipeline and moves with it, and is also connected to the external system through a movable rotating interface, and then connected to the vacuum system through a flexible hose; the discharge port of the furnace body is connected to the discharge hopper through a rigid guide, and the two are sealed together by a sealing sleeve to ensure vacuum sealing and maintain material passage when the push rod tilts the furnace body.
6. The metal vapor reduction furnace according to claim 1, characterized in that, The atmosphere control mechanism includes a vacuum pump. One end of the extraction pipe extends into the reaction vessel and is connected to the reaction vessel, while the other end is connected to the vacuum pump. A filter is provided at one end of the extraction pipe inside the reaction vessel. A filter chamber is provided inside the extraction pipe on the side closer to the vacuum pump. A filter plate is also provided inside the extraction pipe. A vacuum gauge and a vacuum meter are provided on the extraction pipe. And / or, the condensation mechanism includes a porous condenser disposed on the suction pipe and located between the filter chamber and the vacuum pump, the porous condenser being filled with porous metal or ceramic packing for condensing and recovering unreacted metal vapor; And / or, the heat insulation baffle is a stainless steel sheet stacked in concentric circles or spirals, and the heat insulation baffle is also used to prevent dust in the reaction vessel from flowing back into the evaporation vessel and to support the gas pipe so that it is centered.
7. A method for preparing silicon-based nanomaterials, characterized in that, It is carried out using a metal vapor reduction furnace as described in any one of claims 1-6, the method comprising: S1. The reactants are placed in the reaction vessel, and the metal raw material is placed in the evaporation zone of the evaporation vessel. The atmosphere control mechanism evacuates the reaction vessel and the evaporation vessel. The reactants include at least one of the following: clay minerals with natural nanostructures or their modified products, silicon-containing precursors, metal-containing minerals, industrial solid waste, or synthetic nanomaterial precursors. S2. After evacuating to <800 Pa, the evaporation temperature control mechanism and the reaction temperature control mechanism are activated respectively to raise the temperature of the evaporation container to 600~1700℃ to generate metal vapor. The metal vapor enters the reaction container through the gas pipeline. The reaction container is then raised to 600~900℃ to allow the metal vapor to undergo a gas-solid reduction reaction with the reactants, yielding a crude reduced product containing byproduct metal oxides. S3. The crude reduced product is post-processed by acid washing, water washing and drying to remove the by-product metal oxides, and a silicon-based material product is obtained. The gas after the reaction is recovered by the condensation mechanism.
8. The method for preparing silicon-based nanomaterials according to claim 7, characterized in that, The clay minerals include any one or more of montmorillonite, kaolinite, halloysite, palygorskite, talc, black talc, muscovite, soapstone, biotite, lepidolite, illite, chlorite, sepiolite, and pyrophyllite; the modified product is obtained by at least one of heat treatment, acid treatment, mechanical treatment, organic modification, or inorganic modification. And / or, the silicon-containing precursor includes at least one of silica materials, industrial by-products, and silicon-carbon precursors; the silica materials include any one or more of fumed silica, precipitated silica, silica sol, mesoporous silica, quartz, silica, and quartz sand; the industrial by-products include any one or more of waste solar panels, silica ash, rice husk ash, and fly ash; the silicon-carbon precursors include any one or more of rice husks, straw, bamboo leaves, reeds, bagasse, silicon-containing plastics, silicon-containing rubber, and waste clay.
9. The method for preparing silicon-based nanomaterials according to claim 7, characterized in that, The metal raw material is a mixture containing metal minerals and reducing agents. The evaporation temperature control mechanism can heat the evaporation zone to 1100~1700℃, so that the mixture undergoes carbothermic reduction or metalothermic reduction reaction to generate metal vapor in situ. Alternatively, the metal raw material may be magnesium ingot, magnesium alloy, elemental calcium, calcium alloy, elemental sodium, elemental potassium, or sodium-potassium alloy, and the evaporation temperature control mechanism may heat the evaporation zone to 600~1300℃, causing the metal raw material to evaporate and generate metal vapor.
10. The method for preparing silicon-based nanomaterials according to claim 7, characterized in that, The molar ratio of the metal raw material to the reactants is 0.3~2.5:1; And / or, the reactants are premixed with inorganic salts at a mass ratio of 0.1 to 5:1, wherein the inorganic salts include at least one selected from NaCl, LiCl, KCl, CaCl2 and MgCl2; And / or, before evacuation, an inert gas is introduced into the evaporation vessel and the reaction vessel.