A Fe-N4 and CaS-containing iron-sulfur-doped cyanobacterial carbon material and its combination with nano-zero-valent iron for the remediation of chlorinated hydrocarbons through reduction and dechlorination.

By preparing iron-sulfur-doped cyanobacterial carbon materials containing Fe-N4 and CaS and using them in combination with nano-zero-valent iron, the problems of low electron utilization efficiency and difficulty in reducing high-energy-barrier chlorinated hydrocarbons in the existing technology were solved, and a highly efficient dechlorination effect of chlorinated hydrocarbons was achieved.

CN123102302APending Publication Date: 2026-11-17JIANGNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611525379.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to prepare simple and cost-effective material systems that can both improve electron utilization efficiency and effectively reduce high-barrier chlorinated hydrocarbons, such as 1,2DCA.

Method used

Iron-sulfur-doped cyanobacterial carbon material containing Fe-N4 and CaS was prepared by mixing cyanobacterial mud with ferrous sulfate heptahydrate and pyrolyzing it under an inert atmosphere. This material was then used in conjunction with nano-zero-valent iron to form a remediation composition.

Benefits of technology

It significantly improves the dechlorination capability for high-energy-barrier chlorinated hydrocarbons, increases electronic efficiency, completely removes TCE within 24 hours, and achieves a dechlorination rate of 23.8% and an electronic efficiency of 80.5% for 1,2DCA within 50 days.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102302A_ABST
    Figure CN123102302A_ABST
Patent Text Reader

Abstract

This invention discloses an iron-sulfur-doped cyanobacterial carbon material containing Fe-N4 and CaS, and its method for remediation of chlorinated hydrocarbons by combining it with nano-zero-valent iron, belonging to the field of groundwater pollution remediation technology. The invention involves mixing cyanobacterial mud and ferrous sulfate heptahydrate at a mass ratio of 10:1, drying and grinding to obtain a precursor powder. The precursor powder is then pyrolyzed under an inert atmosphere to obtain an iron-sulfur-doped cyanobacterial carbon material containing both FeN4 coordination structure and calcium sulfide (CaS). This iron-sulfur-doped cyanobacterial carbon material is then compounded with nano-zero-valent iron to form a remediation composition, which is subsequently used for the remediation of chlorinated hydrocarbons by reduction, achieving excellent dechlorination rates. This invention uses cyanobacterial mud as a resource, has a simple preparation process, and controllable costs. It can improve the electron utilization efficiency of the zero-valent iron system and enhance the dechlorination capacity for recalcitrant chlorinated hydrocarbons, making it suitable for groundwater remediation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of groundwater pollution remediation technology, and in particular to an iron-sulfur-doped cyanobacterial carbon material containing Fe-N4 and CaS, and a remediation method for its combination with nano-zero-valent iron for the reduction and dechlorination of chlorinated hydrocarbons. Background Technology

[0002] Chlorinated hydrocarbons are widely used in industrial processes such as equipment cleaning and chemical production. Due to their high chemical stability, high mobility, and high toxicity, they easily form long-term pollutants in soil and groundwater. Trichloroethylene (TCE) is a typical chlorinated olefin pollutant and is frequently detected in contaminated sites. 1,2 Dichloroethane (1,2) DCA is a typical chlorinated alkane pollutant. Its reduction dechlorination reaction has a high activation energy barrier, making it difficult to achieve effective conversion through conventional remediation systems.

[0003] Nano-zero-valent iron (nZVI) is a commonly used reducing agent for the reductive dechlorination of chlorinated hydrocarbons, offering advantages such as low cost and strong reducing power. However, the electrons released by ZVI in the aqueous phase are easily consumed by side reactions such as hydrogen evolution reaction, resulting in low electron utilization efficiency; simultaneously, for 1,2... For high-energy-barrier pollutants such as DCA, conventional ZVI systems typically struggle to achieve effective dechlorination.

[0004] The remediation of cyanobacterial blooms generates large amounts of cyanobacterial sludge, which is rich in nitrogenous organic components and inorganic elements such as calcium. Utilizing this cyanobacterial sludge as a resource to prepare environmental remediation materials can help reduce material costs and improve resource utilization efficiency. However, current technologies still lack a material system that is simple to prepare, cost-effective, and can simultaneously improve electronic efficiency and the dechlorination capacity of high-energy-barrier chlorinated hydrocarbons. Summary of the Invention

[0005] [Technical Issues] This invention provides a material system that is easy to prepare, cost-controllable, and can simultaneously improve electronic efficiency and the dechlorination capability of high-barrier chlorinated hydrocarbons.

[0006] [Technical Solution] This invention aims to provide an Fe-containing A method for preparing cyanobacterial-derived char material with N4 coordination structure and calcium sulfide (CaS), and a method for combining this material with nZVI for use with chlorinated hydrocarbons (such as TCE and 1,2-dichlorocarbons). A remediation composition and method for DCA-based reduction dechlorination to improve the electron utilization efficiency of ZVI systems and enhance their resistance to high-energy-barrier chlorinated hydrocarbons (1,2). Dechlorination capability of DCA.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an iron-sulfur-doped cyanobacterial carbon material, wherein the carbon material is prepared by pyrolysis of a mixture of cyanobacterial mud and ferrous sulfate heptahydrate under an inert atmosphere; the iron-sulfur-doped cyanobacterial carbon material also contains Fe. N4 coordination structure and calcium sulfide (CaS).

[0008] Secondly, the present invention provides a method for preparing the above-mentioned iron-sulfur-doped cyanobacterial carbon material, comprising the following steps: S1: Mix blue-green algae mud with ferrous sulfate heptahydrate until well mixed to obtain a mixture; S2: Dry and grind the mixture to obtain precursor powder; S3: Place the precursor powder under an inert atmosphere At After pyrolysis for a period of time and cooling, iron-sulfur-doped blue-green algae carbon material is obtained.

[0009] In one embodiment of the present invention, in S1, the solid content of the blue-green algae mud is 5%.

[0010] In one embodiment of the present invention, in S1, the mass ratio of cyanobacterial mud to ferrous sulfate heptahydrate is 2-10:1. More preferably, it is 5-10:1.

[0011] In one embodiment of the present invention, in step S2, the drying temperature is 30-60°C. o C, the timeframe is 1-5 days. Specific options include 35. o Dry at C for 3 days.

[0012] In one embodiment of the present invention, in step S3, the pyrolysis temperature is 800-900 °C. o C; Time is 1-5 hours. Specific options include 800. o Pyrolysis at C for 2 hours.

[0013] In one embodiment of the present invention, in S3, the inert atmosphere may specifically be a nitrogen atmosphere.

[0014] Thirdly, the present invention provides a remediation composition for the reductive dechlorination of chlorinated hydrocarbons, comprising the iron-sulfur-doped cyanobacterial carbon material and nZVI.

[0015] In one embodiment of the present invention, the mass ratio of the iron-sulfur-doped cyanobacterial carbon material to nZVI is 1:1.

[0016] In one embodiment of the present invention, the preparation method of nZVI includes: dissolving ferrous sulfate heptahydrate in deoxygenated deionized water under an inert atmosphere to form a ferrous salt solution; adding sodium borohydride solution dropwise under continuous N2 introduction and stirring to carry out a reduction reaction to generate zero-valent iron nanoparticles; after the reaction is completed, the reaction solution is separated into solid and liquid, the solid is collected, washed, and nZVI is obtained.

[0017] In one embodiment of the present invention, CaS in the iron-sulfur-doped cyanobacterial carbon material releases sulfides in the aqueous phase, causing iron sulfide FeS to form on the surface of the nZVI. x layer.

[0018] Fourthly, the present invention provides a method for remediating chlorinated hydrocarbon pollutants in water or groundwater, wherein the remediation composition is added to the water to be treated to cause the chlorinated hydrocarbons to undergo reduction and dechlorination.

[0019] In one embodiment of the present invention, the chlorinated hydrocarbon includes chlorinated C1-4 alkanes and chlorinated C1-4 alkenes. Specifically, it is selected from: trichloroethylene (TCE) and / or 1,2 Dichloroethane (1,2) DCA).

[0020] In one embodiment of the present invention, the repair conditions are: the amount of repair composition added is 1 g / L.

[0021] In one embodiment of the present invention, the reaction temperature for reduction dechlorination is 20-30°C. o C.

[0022] In one embodiment of the present invention, the initial concentration of chlorinated hydrocarbons in the water to be treated is 10 mg / L, and the pH is >6.

[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) At a dosage of 1 g / L, an initial TCE concentration of 10 mg / L, a pH > 6, and a pH of approximately 25 o Under C conditions, TCE can be completely removed within 24 hours, with a dechlorination rate of 84.3%. 96.7% of the dechlorination products are acetylene, and the electron efficiency is 80.5%.

[0024] (2) Under the same system conditions, 1,2 DCA achieved a dechlorination rate of 23.8% within 50 days, thus improving its ability to dechlorinate high-energy-barrier chlorinated hydrocarbons.

[0025] (3) Comparative experiments show that nZVI alone cannot achieve TCE and 1,2 within 24 h. DCA dechlorination; iron-sulfur doped cyanobacterial carbon material alone achieved only 8.15% TCE dechlorination within 24 hours and could not achieve 1,2 DCA dechlorination; the carbon material of this invention, when compounded with nZVI, affects TCE and 1,2 DCA exhibited a significantly enhanced dechlorination capability. Attached Figure Description

[0026] Figure 1 The XRD pattern of the iron-sulfur-doped cyanobacterial carbon material.

[0027] Figure 2 XPS spectrum of iron-sulfur doped cyanobacterial carbon material.

[0028] Figure 3 The Mössbauer spectrum is for iron-sulfur-doped cyanobacterial carbon materials.

[0029] Figure 4 TEM and EDS surface scan images of the sample after iron-sulfur-doped cyanobacterial carbon material was combined with nZVI.

[0030] Figure 5 This invention relates to the dechlorination results of the composition for TCE.

[0031] Figure 6 This invention aims to improve the dechlorination results of the composition for 1,2-DCA. Detailed Implementation

[0032] The present invention will be further described below with reference to the embodiments, but the scope of protection of the present invention is not limited to the following embodiments.

[0033] In this invention, "removal rate" refers to the proportion by which the concentration of the target pollutant in the reaction system decreases; "dechlorination rate" refers to the proportion by which the target pollutant undergoes reduction and dechlorination transformation; and "electron efficiency" refers to the proportion of electrons released by zero-valent iron used for the dechlorination reaction. The electron efficiency is calculated based on the electron equivalents consumed by the dechlorination reaction and the electron equivalents consumed by the hydrogen evolution reaction.

[0034] Example 1: Preparation of iron-sulfur-doped cyanobacterial carbon materials Take cyanobacterial mud with a solids content of 5% and mix it thoroughly with ferrous sulfate heptahydrate at a mass ratio of 10:1 (cyanobacterial mud: ferrous sulfate heptahydrate) to obtain a mixture. Place the mixture at 35°C. o The product was dried at temperature C for 3 days to obtain a dry solid. The dry solid was then ground to obtain a precursor powder.

[0035] The obtained precursor powder was placed in a tube furnace and heated to 800°C under nitrogen protection. o The material was heated to C and kept at that temperature for 2 hours. After cooling to room temperature, it was removed to obtain iron-sulfur-doped blue-green algae carbon material.

[0036] Example 2: Material Structure Characterization XRD tests were performed on the iron-sulfur-doped cyanobacterial carbon material obtained in Example 1, and the results are as follows: Figure 1 As shown. Figure 1 The XRD diffraction pattern of iron-sulfur-doped cyanobacterial carbon shows characteristic peaks of CaS, indicating the presence of the CaS crystalline phase in the material.

[0037] XPS testing was performed on the material obtained in Example 1, and the results are as follows: Figure 2 As shown. Figure 2 The display shows that Fe-N appears in the characteristic spectrum of N 1s. x The characteristic peaks of the coordination structure indicate the presence of Fe-N in the material. x The relevant coordination characteristic signals have been obtained, but the type of coordination structure still needs to be further determined.

[0038] The material obtained in Example 1 was subjected to Mössbauer spectroscopy, and the results are as follows: Figure 3 As shown. Figure 3 Display: In 57 The presence of characteristic peaks for Fe-N4 in the Mössbauer spectrum reveals the presence of Fe in the material. N x The coordination structure is Fe-N4.

[0039] The material obtained in Example 1 was compounded with nZVI and subjected to TEM and EDS surface scan tests. The results are as follows: Figure 4 As shown. Figure 4 The results show that nZVI is anchored to the surface of the carbon material, and co-localization signals of Fe and S appear on the outer layer of nZVI, indicating that iron sulfide (FeS) is formed on the surface of nZVI during the compounding process. x )layer.

[0040] Example 3: Preparation of nZVI Under an inert atmosphere, 5 g of ferrous sulfate heptahydrate was dissolved in 450 mL of deoxygenated deionized water to form a ferrous salt solution. A reduction reaction was carried out by continuously introducing N2 at a rate of 2 L / min and stirring, and 30 g / L sodium borohydride solution was added dropwise to generate zero-valent iron nanoparticles. The reduction process lasted for 20 minutes. The resulting solid was separated and washed with deoxygenated deionized water to obtain nZVI, which was stored under an inert atmosphere for later use.

[0041] Example 4: Preparation of the repair composition The iron-sulfur-doped cyanobacterial carbon material obtained in Example 1 was mixed with the nZVI obtained in Example 3 at a mass ratio of 1:1 to obtain a remediation composition for the reductive dechlorination of chlorinated hydrocarbons.

[0042] Example 5: TCE Dechlorination Experiment and Results Prepare a TCE-contaminated water sample to achieve an initial TCE concentration of 10 mg / L; add the remediation composition obtained in Example 4 to the reaction system at a dosage of 1 g / L; control the pH of the system to be greater than 6 (the experimental conditions were anoxic deionized water, pH=8.3), and the reaction temperature to 25°C. o The reaction was carried out under closed oscillation for 24 hours at approximately °C.

[0043] The concentration of TCE and the distribution of dechlorination products were detected by gas chromatography, and the dechlorination rate and electronic efficiency were calculated.

[0044] The formula for calculating the removal rate is: Removal rate = TCE concentration at the end of the reaction / TCE concentration at the beginning of the reaction.

[0045] The dechlorination rate is calculated as follows: Dechlorination rate = Dechlorination product concentration / TCE concentration at the initial moment of the reaction.

[0046] The formula for calculating electronic efficiency is: Electronic efficiency = Electrons consumed in the generation of dechlorination products from TCE / (Electrons consumed in the generation of dechlorination products from TCE + Electrons consumed in the production of hydrogen from nZVI).

[0047] Experimental results show that the removal rate of TCE within 24 h is 100%, the dechlorination rate is 84.3%, and some TCE is adsorbed by carbon materials; 96.7% of the dechlorination products are acetylene; the electronic efficiency is 80.5%.

[0048] Example 6: 1,2 DCA Dechlorination Experiment and Results Prepare 1,2 DCA contaminated water samples, causing 1,2 The initial concentration of DCA was 10 mg / L; the remediation composition described in Example 4 was added to the reaction system at a dosage of 1 g / L; the pH of the system was controlled to be greater than 6, and the reaction temperature was 25°C. o Around 50 days of closed-loop reaction at around 30°C.

[0049] 1,2 Detected by gas chromatography The concentration of DCA and the dechlorination products were determined, and the dechlorination rate was calculated.

[0050] Experimental results show that: 1,2 DCA achieved a dechlorination rate of 23.8% within 50 days; 92.4% of the dechlorination products were ethylene.

[0051] Comparative Example 1: Only nZVI was added Under the same conditions as in Example 5, only nZVI (dosage 1 g / L, initial TCE concentration 10 mg / L, pH > 6, 25) was added. oAround C (closed reaction for 24 h), the test results showed that there were no dechlorination products within 24 h, meaning that TCE dechlorination could not be achieved.

[0052] Under the same conditions as in Example 6, only nZVI (dosage 1 g / L, 1,2) was added. DCA initial concentration 10 mg / L, pH>6, 25 o Around C (closed reaction for 24 hours), the test results showed that no dechlorination products were produced within 50 days, meaning that 1,2 DCA dechlorination.

[0053] Comparative Example 2: Only iron-sulfur-doped blue-green algae char was added Under the same conditions as in Example 5, only the carbon material obtained in Example 1 was added (addition amount 1 g / L, initial TCE concentration 10 mg / L, pH>6, 25). o The reaction was carried out in a closed system at around 24°C for 24 hours. The test results showed that the TCE dechlorination rate was 8.15% within 24 hours.

[0054] Under the same conditions as in Example 6, only the carbon material obtained in Example 1 was added (addition amount 1 g / L, 1, 2). DCA initial concentration 10 mg / L, pH>6, 25 o Around C (closed reaction for 24 hours), test results showed that 1,2 could not be achieved within 50 days. DCA dechlorination.

[0055] As demonstrated by the examples and comparative examples, the remediation composition formed by combining the iron-sulfur-doped cyanobacterial carbon material of the present invention with nZVI exhibits significantly better performance than either nZVI alone or carbon material alone in terms of TCE removal, dechlorination rate, product selectivity, and electronic efficiency. Furthermore, it achieves remediation of 1,2... The dechlorination capacity of high-barrier chlorinated hydrocarbons such as DCA is improved; at the same time, the dechlorination effect of the remediation composition formed by the iron-sulfur-doped cyanobacterial carbon material and nZVI is also better than the sum of the effects of nZVI alone and carbon material alone, indicating that the two types of materials (iron-sulfur-doped cyanobacterial carbon material and nZVI) in the composition have a synergistic effect.

[0056] Comparative Example 3: Fe-free N4 iron-sulfur-doped cyanobacterial carbon materials and their combination with nano-zero-valent iron for the reductive dechlorination of chlorinated hydrocarbons Preparation of cyanobacterial charcoal material: Cyanobacterial mud with a solid content of 5% was placed in a 35°C container. o The product was dried at C for 3 days to obtain a dry solid. The dried solid was ground to obtain a precursor powder; subsequently, the precursor powder was placed in a tube furnace and heated to 800°C under nitrogen protection. o The material was heated to temperature C for 2 hours, cooled to room temperature, and then removed to obtain cyanobacterial carbon material.

[0057] Preparation of CaS sulfided nZVI: The nZVI obtained in Example 3 was mixed with CaS at a mass ratio of 13:2 to obtain CaS sulfided nZVI.

[0058] Referring to Example 4, the obtained cyanobacterial carbon material was mixed with the nZVI obtained in Example 3 at a mass ratio of 1:1 to obtain the repair composition C1.

[0059] Referring to Example 4, the obtained cyanobacterial carbon material and the obtained CaS sulfide nZVI were mixed at a mass ratio of 1:1 to obtain the remediation composition C2.

[0060] Under the same conditions as in Example 5, the above-mentioned remediation composition C1 or remediation composition C2 was added to conduct a TCE degradation experiment (addition amount 1 g / L, initial TCE concentration 10 mg / L, pH>6, 25). o The reaction was carried out under sealed conditions for 24 hours. The test results showed that within 24 hours, the coupling of cyanobacterial carbon with nZVI (remediation composition C1) could only achieve 25.2% TCE dechlorination (i.e., dechlorination rate), while the coupling of cyanobacterial carbon with CaS sulfurized nZVI (remediation composition C2) could only achieve 49.7% TCE dechlorination.

[0061] As can be seen from the examples and comparative examples, the Fe-N4 structure of the iron-sulfur doped cyanobacterial carbon material of the present invention can significantly improve the dechlorination performance of nZVI-based materials.

[0062] Comparative Example 4: Comparison of dechlorination performance of remediation materials obtained under different iron-sulfur doping conditions Referring to Example 1, the mass ratio of cyanobacterial mud to ferrous sulfate heptahydrate was adjusted, while other parameters remained unchanged, to obtain the corresponding iron-sulfur-doped cyanobacterial carbon material. Referring to Example 4, the corresponding remediation composition was obtained.

[0063] Under the same conditions as in Example 5, TCE degradation experiments were conducted by adding each remediation composition (dosage 1 g / L, initial TCE concentration 10 mg / L, pH > 6, 25). o The reaction was carried out at approximately 100°C in a sealed environment for 24 hours. The test results are shown in Table 1.

[0064] Table 1. Dechlorination results of remediation materials obtained under different iron-sulfur doping conditions

[0065] Comparative analysis of results: The results show that when the mass ratio of cyanobacterial mud to ferrous sulfate heptahydrate is 10:1, the prepared cyanobacterial carbon material can achieve the highest dechlorination rate after being mixed with nano-zero valent iron. Therefore, 10:1 is the optimal mass ratio parameter of cyanobacterial mud / ferrous sulfate heptahydrate for this process.

[0066] The above description is merely an embodiment of the present invention. Any equivalent changes or substitutions made based on the concept of the present invention should fall within the protection scope of the present invention.

Claims

1. An iron-sulfur-doped cyanobacteria-carbon material, characterized in that, The carbon material is prepared by pyrolysis of a mixture of cyanobacterial mud and ferrous sulfate heptahydrate under an inert atmosphere; the iron-sulfur-doped cyanobacterial carbon material also contains Fe. N4 coordination structure and calcium sulfide (CaS).

2. A method for preparing the iron-sulfur-doped cyanobacterial carbon material according to claim 1, characterized in that, Includes the following steps: S1: Mix blue-green algae mud with ferrous sulfate heptahydrate until well mixed to obtain a mixture; S2: Dry and grind the mixture to obtain precursor powder; S3: Place the precursor powder under an inert atmosphere At After pyrolysis for a period of time and cooling, iron-sulfur-doped blue-green algae carbon material is obtained.

3. The preparation method according to claim 2, characterized in that, In S1, the mass ratio of blue-green algae mud to ferrous sulfate heptahydrate is 10:

1.

4. The preparation method according to claim 2, characterized in that, In S2, the drying temperature is 30-60°C. o C, the time is 1-5 days.

5. The preparation method according to claim 2, characterized in that, In S3, the pyrolysis temperature is 800-900℃. o C; Time is 1-5 hours.

6. The preparation method according to any one of claims 2-5, characterized in that, The inert atmosphere can specifically be nitrogen atmosphere.

7. A remediation composition for the reductive dechlorination of chlorinated hydrocarbons, characterized in that, This includes the iron-sulfur-doped cyanobacterial carbon material and nano-zero-valent iron as described in claim 1.

8. The repair composition according to claim 7, characterized in that, The mass ratio of the iron-sulfur-doped cyanobacterial carbon material to nano-zero-valent iron is 1:

1.

9. A method for remediating chlorinated hydrocarbon pollutants in water or groundwater, characterized in that, The remediation composition of claim 7 or 8 is added to the water body to be treated, causing the chlorinated hydrocarbons to undergo reductive dechlorination.

10. The method according to claim 9, characterized in that, The chlorinated hydrocarbons include chlorinated C1-4 alkanes and chlorinated C1-4 alkenes; the dosage of the remediation composition relative to the water to be treated is 1 g / L; the reaction temperature for reduction and dechlorination is 20-30°C. o C.