A Fe-doped Pd / C catalyst and its nitrogen-heterocyclic LOHC composite method

By combining Fe-doped Pd/C catalysts with nitrogen heterocyclic LOHC composites and centrifugal reactors, the problems of difficult catalyst separation and recovery and precious metal loss in nitrogen heterocyclic liquid organic hydrogen support technology have been solved, improving reaction efficiency and cycle stability, and realizing rapid separation and reuse of catalysts.

CN123102379APending Publication Date: 2026-11-17成都岷山緑ちん能源有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611204342.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing nitrogen heterocyclic liquid organic hydrogen support technologies suffer from problems such as difficulty in catalyst separation and recovery, high loss of precious metals, insufficient matching between support and catalyst, limited reactor mass transfer efficiency, and decreased circulation capacity retention, making it difficult to meet the requirements of continuous hydrogenation and dehydrogenation processes.

Method used

By using Fe-doped Pd/C catalysts and controlling the Pd loading, Fe doping amount, particle size, and magnetization intensity, a catalyst with good dispersion and magnetic recovery characteristics suitable for nitrogen heterocyclic LOHC systems was prepared. The catalyst was then matched with N-methylindole and ionic liquid composite supports, and combined with the operating conditions of a centrifugal reactor, to achieve continuous recycling of the catalyst.

Benefits of technology

It improves the dispersibility and magnetic recovery of the catalyst, reduces the risk of precious metal loss, enhances reaction efficiency and cycle stability, reduces system energy consumption, and enables rapid separation and reuse of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102379A_ABST
    Figure CN123102379A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of hydrogen energy storage and transportation technology, specifically relating to an Fe-doped Pd / C catalyst and its method for compounding with a nitrogen-heterocyclic liquid organic hydrogen support. The catalyst uses activated carbon as a support, loaded with 0.8–1.2 wt% Pd and doped with 5–15 wt% Fe, with a particle size of 20–50 nm and a saturation magnetization of 15–25 emu / g. It is prepared by co-impregnation with PdCl2 and Fe(NO3)3, drying, and hydrogen reduction at 300–500 °C. The obtained catalyst is dispersed at 0.5–2 wt% in an N-methylindole compound support containing 1–3 wt% 1-butyl-3-methylimidazolium tetrafluoroborate and fed into a centrifugal reactor, where it is circulated under conditions of 120–180 °C and 3–5 MPa during the hydrogenation stage and 150–200 °C and atmospheric pressure during the dehydrogenation stage. This method enables continuous operation of catalyst magnetic recovery and hydrodehydrogenation, with a catalyst recovery rate of over 99%, hydrogen selectivity of over 98%, and capacity retention of over 96% after 50 cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of hydrogen energy storage and transportation technology, and discloses an Fe-doped Pd / C catalyst and its nitrogen heterocyclic LOHC composite method. Background Technology

[0002] Hydrogen energy, as a clean energy source, boasts diverse sources, low environmental impact from energy utilization byproducts, and compatibility with renewable energy systems, making it a crucial technological direction for the low-carbon transformation of the energy structure. The hydrogen energy industry chain comprises hydrogen production, storage, transportation, and utilization, forming a complete application process. Among these, hydrogen storage and transportation directly impact the safety, economy, and continuous supply capacity of large-scale hydrogen energy utilization. While existing technologies such as high-pressure gaseous hydrogen storage, cryogenic liquid hydrogen storage, and solid-state hydrogen storage have been applied in various scenarios, they still have limitations. High-pressure gaseous hydrogen storage requires high pressure resistance and sealing safety of storage tanks, posing a risk of leakage during long-distance transportation; cryogenic liquid hydrogen storage requires maintaining cryogenic conditions, resulting in high system energy consumption and insulation equipment costs; and while solid-state hydrogen storage materials offer advantages in volumetric hydrogen storage, some materials suffer from slow hydrogenation and dehydrogenation rates, insufficient cycle life, and significant challenges in engineering scale-up. Therefore, developing hydrogen storage and transportation technologies that combine safety, economy, and adaptability for continuous operation remains a vital research direction in this field.

[0003] Liquid organic hydrogen carrier technology has emerged as a promising hydrogen storage method in recent years. This technology achieves hydrogen storage and release through the reversible transformation of liquid organic carriers between hydrogenation and dehydrogenation states. It offers advantages such as the ability to store and transport hydrogen under relatively mild conditions, ease of utilizing existing oil storage and transportation facilities, and high transportation safety. Compared to traditional high-pressure or cryogenic hydrogen storage methods, liquid organic hydrogen carriers have advantages in terms of infrastructure compatibility with pipelines, tank trucks, and storage tanks, making them suitable for application in distributed energy, transportation energy, and industrial hydrogen supply scenarios. However, the practical application of liquid organic hydrogen carrier systems still depends on the comprehensive matching of carrier materials, catalysts, and reaction equipment. Insufficient carrier stability, low catalyst selectivity, or limited reactor mass transfer efficiency can easily lead to problems such as hydrogen storage capacity decay, prolonged reaction cycles, and increased operating costs.

[0004] Among various liquid organic hydrogen supports, nitrogen-containing heterocyclic compounds have become important candidate systems in the field of liquid organic hydrogen supports due to their good compatibility with hydrogenation and dehydrogenation processes. Nitrogen heterocyclic supports such as N-methylindole exhibit liquid characteristics at room temperature and have relatively mild hydrogenation and dehydrogenation conditions, showing potential as reversible hydrogen storage supports. However, in practical applications, single nitrogen heterocyclic supports still suffer from problems such as limited low-temperature fluidity, accumulation of side reactions during long-term cycling, decreased hydrogen storage capacity retention, and changes in system properties with the number of cycles. Some existing technologies improve support performance through solvent addition, physical blending, or single-support modification, but these methods usually only adjust one property and cannot simultaneously address liquid temperature range, hydrogen diffusion performance, cycle stability, and compatibility with the catalytic system, thus still failing to meet the requirements of continuous hydrogen storage and transportation processes.

[0005] Catalysts are a key factor affecting the hydrogenation and dehydrogenation efficiency of liquid organic hydrogen supports. Existing noble metal-supported catalysts such as Pd / C exhibit high activity in some nitrogen-heterocyclic liquid organic hydrogen support systems, but they suffer from problems in continuous liquid-phase systems, including difficulty in maintaining dispersion, challenges in post-reaction separation and recovery, a high risk of noble metal loss, and insufficient stability for repeated use. For continuous industrial operation, the inability to achieve rapid separation and recycling of catalysts increases post-processing difficulty and operating costs, and may cause contamination of the support system. Although magnetic catalysts can provide a new technical route for catalyst separation, research on the matching between existing magnetic catalysts and nitrogen-heterocyclic liquid organic hydrogen supports is still insufficient, especially regarding catalytic activity, magnetic recovery capability, particle size distribution, support viscosity, and reactor operating parameters. A systematic design for continuous hydrogenation and dehydrogenation processes is still lacking.

[0006] Furthermore, traditional fixed-bed or conventional batch reactors typically suffer from limited gas-liquid-solid three-phase contact efficiency, insufficient mass and heat transfer enhancement, uneven catalyst bed utilization, and inconvenient switching between hydrotreating and dehydrogenation processes when processing liquid organic hydrogen carrier systems. When the carrier system has a certain viscosity, the gas dispersion, liquid flow, and catalyst contact state within the reactor directly affect the reaction efficiency. Centrifugal reactors and other mass transfer enhancement devices have potential advantages in continuous liquid-phase processing; however, current technologies lack sufficient synergistic design for specific nitrogen heterocyclic liquid organic hydrogen carriers, magnetic catalysts, and centrifugal bed operating conditions, and a complete process system integrating catalyst preparation, carrier compounding, reaction enhancement, and catalyst recovery has not yet been formed.

[0007] Therefore, existing nitrogen-heterocyclic liquid organic hydrogen support technologies still need to address the following issues: First, single supports have shortcomings in low-temperature applicability and long-term cycling stability; second, traditional Pd / C catalysts face difficulties in recovery and the risk of precious metal loss in continuous liquid-phase systems; third, the lack of parameter matching between the support, catalyst, and reaction equipment leads to low efficiency in continuous hydrodehydrogenation operation; and fourth, existing processes struggle to achieve a coordinated balance between catalytic selectivity, catalyst recovery rate, system energy consumption, and cycle capacity retention. Based on this, it is necessary to develop an Fe-doped Pd / C catalyst and its blending method that is compatible with nitrogen-heterocyclic liquid organic hydrogen support composite systems, possesses magnetic recovery characteristics, and is suitable for continuous reaction equipment operation, in order to improve the safety, stability, and engineering application value of hydrogen storage and transportation processes using liquid organic hydrogen supports. Summary of the Invention

[0008] The purpose of this invention is to address the problems existing in the continuous hydrogenation and dehydrogenation process of nitrogen heterocyclic liquid organic hydrogen support systems, such as difficulties in catalyst separation and recovery, high precious metal loss, insufficient matching between support and catalyst, limited reactor mass transfer efficiency, and decreased cycle capacity retention. This invention provides an Fe-doped Pd / C catalyst and its nitrogen heterocyclic LOHC composite method. This scheme uses an Fe-doped Pd / C magnetic catalyst as the core, and by controlling the Pd loading, Fe doping amount, particle size, and magnetization, the catalyst possesses both dispersion characteristics and magnetic recovery characteristics suitable for nitrogen heterocyclic LOHC systems. Furthermore, the catalyst is synergistically matched with an N-methylindole and ionic liquid composite support, as well as the operating conditions of the centrifugal reactor, to achieve continuous cyclic application in the hydrogenation and dehydrogenation processes.

[0009] To achieve the above objectives, the present invention adopts the following technical solution.

[0010] This invention provides an Fe-doped Pd / C catalyst, comprising an activated carbon support and Pd and Fe supported on the activated carbon support; the Pd loading is 0.8–1.2 wt% and the Fe doping amount is 5–15 wt% based on the total mass of the catalyst; the particle size of the Fe-doped Pd / C catalyst is 20–50 nm and the saturation magnetization is 15–25 emu / g.

[0011] In a preferred embodiment, the activated carbon support has a microporous-mesoporous composite pore structure, with Pd and Fe distributed on the inner and outer surfaces of the pores of the activated carbon support. This allows the resulting catalyst to meet the requirements of dispersion, circulation, and magnetic recovery in liquid-phase nitrogen heterocyclic LOHC systems. Further, the average particle size of the Fe-doped Pd / C catalyst is preferably 30–40 nm, the Pd loading is preferably 0.9–1.1 wt%, the Fe doping amount is preferably 7–12 wt%, the particle size is preferably 25–45 nm, and the saturation magnetization is preferably 18–23 emu / g.

[0012] The present invention also provides a method for preparing an Fe-doped Pd / C catalyst, comprising the following steps.

[0013] PdCl2 and Fe(NO3)3 were prepared into a mixed precursor solution containing Pd and Fe.

[0014] Pretreated activated carbon was added to the mixed precursor solution and co-impregnated by stirring at room temperature for 2–4 h.

[0015] The co-impregnated solids are subjected to solid-liquid separation and drying.

[0016] Fe-doped Pd / C catalyst was obtained by reduction in a hydrogen atmosphere at 300–500 °C for 2–4 h.

[0017] In a preferred embodiment, the mixed precursor solution uses deionized water as the solvent, and the amounts of PdCl2 and Fe(NO3)3 added are proportioned according to the Pd loading of 0.8–1.2 wt% and the Fe doping content of 5–15 wt% in the obtained Fe-doped Pd / C catalyst. This preparation method requires no additional stabilizer, simplifies the process route, and facilitates subsequent scale-up preparation and batch consistency control of the catalyst.

[0018] This invention also provides a method for the complexation of nitrogen heterocyclic LOHC in Fe-doped Pd / C catalysts, comprising the following steps: Take the above-mentioned Fe-doped Pd / C catalyst, or the Fe-doped Pd / C catalyst prepared by the above method.

[0019] N-methylindole was formulated with the ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate to form a nitrogen heterocyclic LOHC complex support, wherein the ionic liquid accounted for 1 to 3 wt% of the total mass of the nitrogen heterocyclic LOHC complex support.

[0020] The Fe-doped Pd / C catalyst was dispersed in the nitrogen heterocyclic LOHC composite support at an addition amount of 0.5–2 wt% to obtain a nitrogen heterocyclic LOHC composite system containing the catalyst.

[0021] In a preferred embodiment, the viscosity of the nitrogen heterocyclic LOHC composite support is 15–25 mPa·s. During the compounding process, at least one of the following methods can be used: mechanical stirring, circulating pumping, or ultrasonic dispersion, to disperse the Fe-doped Pd / C catalyst in the nitrogen heterocyclic LOHC composite support, thereby meeting the requirements for subsequent continuous transport and reactor operation.

[0022] Furthermore, the catalyst-containing nitrogen-heterocyclic LOHC composite system is fed into a centrifugal reactor for continuous recycling. The centrifugal reactor includes a composite support inlet, a centrifugal bed, a catalytically active zone, a hydrogen outlet, a liquid outlet, and an external magnetic field recovery unit. The centrifugal bed rotates at 300–800 rpm, and the feed flow rate is 0.5–2 L / min. The reaction temperature during the hydrogenation stage is 120–180°C, and the pressure is 3–5 MPa; the reaction temperature during the dehydrogenation stage is 150–200°C, and the pressure is atmospheric pressure. The hydrogenation and dehydrogenation stages can share the same centrifugal reactor. The gaseous phase after the reaction is discharged through the hydrogen outlet, and the liquid phase after the reaction is discharged through the liquid outlet. The Fe-doped Pd / C catalyst is separated from the liquid phase or the catalytically active zone by the external magnetic field recovery unit and returned to the catalyst-containing nitrogen-heterocyclic LOHC composite system for recycling.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows.

[0024] 1. This invention, by limiting the Pd loading, Fe doping amount, particle size, and saturation magnetization in the Fe-doped Pd / C catalyst, enables the catalyst to simultaneously meet the requirements for catalytic use, dispersion transport, and magnetic recovery in a nitrogen-heterocyclic LOHC liquid-phase system. Compared to traditional Pd / C catalysts, the catalyst of this invention, while maintaining a low Pd content, can achieve rapid separation through an external magnetic field, reducing the loss of precious metal catalyst during recycling.

[0025] 2. This invention uses a co-impregnation-reduction method to prepare Fe-doped Pd / C catalysts. The preparation process includes precursor co-impregnation, solid-liquid separation, drying, and reduction in a hydrogen atmosphere. The process steps are clear, the parameter range is well-defined, and no additional stabilizers are required. The resulting catalyst has a particle size distribution suitable for dispersion in a nitrogen heterocyclic LOHC composite support, and has good reproducibility and engineering scale-up adaptability.

[0026] 3. In this invention, N-methylindole is compounded with 1-3 wt% of 1-butyl-3-methylimidazolium tetrafluoroborate ionic liquid, and the viscosity of the compound support is controlled to be 15-25 mPa·s. This allows the compound support to match the operating conditions of the Fe-doped Pd / C catalyst and the centrifugal reactor, which helps to improve the property changes of the single nitrogen heterocyclic support during long-term cycling and enhances the stability of the compound system in continuous operation. Attached Figure Description

[0027] Figure 1 This is a particle size distribution diagram of Pd-Fe in the Fe-doped Pd / C catalyst.

[0028] Figure 2a This is a 2D schematic diagram of the Fe-doped Pd / C magnetic catalytic integrated centrifugal reactor structure.

[0029] Figure 2b This is a 3D schematic diagram of the Fe-doped Pd / C magnetic catalytic integrated centrifugal reactor structure.

[0030] Figure 3 This is a comparison chart of the magnetic properties and particle size parameters of the catalyst.

[0031] Figure 4 This is a comparison chart of cycle stability and system efficiency. Detailed Implementation

[0032] The present invention will be further described below with reference to embodiments. It should be understood that the following embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Equivalent substitutions or conventional adjustments made by those skilled in the art to the amount of raw materials, process parameters, equipment structure and testing methods without departing from the concept of the present invention should all fall within the scope of protection of the present invention.

[0033] Please refer to Figures 1 to 4 The present invention provides an Fe-doped Pd / C catalyst and its nitrogen heterocyclic LOHC complex method, which mainly includes the following steps: preparation of Fe-doped Pd / C catalyst, preparation of nitrogen heterocyclic LOHC complex support, dispersion of catalyst-containing complex system, continuous hydrogenation and dehydrogenation operation in centrifugal reactor, and magnetic recovery and recycling of catalyst. The Fe-doped Pd / C catalyst uses activated carbon as a support, with Pd and Fe as the loading components. The Pd loading is 0.8–1.2 wt%, the Fe doping amount is 5–15 wt%, the particle size is 20–50 nm, and the saturation magnetization is 15–25 emu / g. The nitrogen-containing heterocyclic LOHC composite support includes N-methylindole and 1-butyl-3-methylimidazolium tetrafluoroborate, with the 1-butyl-3-methylimidazolium tetrafluoroborate accounting for 1–3 wt% of the total mass of the composite support. After the catalyst-containing composite system enters the centrifugal reactor, the reaction temperature is controlled at 120–180 °C and the pressure at 3–5 MPa during the hydrogenation stage, and the reaction temperature is controlled at 150–200 °C and the pressure at atmospheric pressure during the dehydrogenation stage.

[0034] In this embodiment, the Pd precursor used is PdCl2, and the Fe precursor is Fe(NO3)3. The amount of both is determined by the mass conversion of the metal elements. The activated carbon carrier adopts a microporous-mesoporous composite pore structure activated carbon, which can be pretreated before use. The pretreatment methods include washing with deionized water, filtration, drying, and sieving. The pretreated activated carbon should maintain a uniform particle distribution and be free from obvious agglomeration, clumping, or visible impurities.

[0035] The nitrogen-containing heterocyclic LOHC support uses N-methylindole as the main component and 1-butyl-3-methylimidazolium tetrafluoroborate as a compound component. The amount of 1-butyl-3-methylimidazolium tetrafluoroborate added is preferably 2 wt% of the total mass of the compound support, but can be adjusted within the range of 1–3 wt% depending on the viscosity, low-temperature flowability, and reactor feed stability of the compound support. After compounding, the viscosity of the compound support at 25°C is preferably controlled between 15 and 25 mPa·s.

[0036] The centrifugal reactor includes a composite carrier inlet, a centrifugal bed, a catalytically active zone, a hydrogen outlet, a liquid outlet, and an external magnetic field recovery unit. The centrifugal bed is located inside the reactor, with its rotational speed controlled between 300 and 800 rpm. The composite carrier inlet is connected to a metering pump or a circulation pump to continuously feed the catalyst-containing composite system into the reactor. The hydrogen outlet is located in the reactor's gas phase discharge zone; the liquid outlet is located in the reactor's liquid phase discharge zone; and the external magnetic field recovery unit is arranged on the reactor's outer wall, in the liquid circulation pipeline, or in the catalyst recovery zone for the separation and recovery of the Fe-doped Pd / C catalyst.

[0037] Test methods: The particle size of the catalyst was measured using transmission electron microscopy. At least 200 particles were randomly selected from different fields of view for statistical analysis, and the average particle size and particle size distribution range were calculated. The crystal phase structure of the catalyst was determined using X-ray diffraction, recording the characteristic peaks of the activated carbon support and Pd-related diffraction peaks. The pore structure of the catalyst was determined using nitrogen adsorption-desorption testing to obtain adsorption-desorption curves, specific surface area, and pore structure information. The saturation magnetization of the catalyst was measured using a vibrating sample magnetometer. The test sample was dried Fe-doped Pd / C catalyst powder.

[0038] The viscosity of the composite carrier was measured using a rotational viscometer at 25°C. Gas phase components generated during the hydrogenation and dehydrogenation stages were analyzed using gas chromatography to calculate hydrogen selectivity and purity. Catalyst magnetic recovery was calculated by comparing the recovered catalyst mass after separation using an external magnetic field with the added mass. Cycle capacity retention was calculated as the ratio of the hydrogen storage capacity in the nth cycle to the initial hydrogen storage capacity.

[0039] Cyclic capacity retention is calculated using the following formula: η1=Q n / Q0×100% In the formula, η1 is the cycle capacity retention rate, in %; Q n Q0 represents the hydrogen storage capacity after the nth cycle; Q0 represents the initial cycle hydrogen storage capacity.

[0040] The magnetic recovery rate of the catalyst is calculated according to the following formula: η2=m r / m0×100% In the formula, η2 is the magnetic recovery rate of the catalyst, in %; m r m0 represents the mass of the catalyst obtained after magnetic recovery; m0 represents the mass of the catalyst added to the compound system.

[0041] Hydrogen selectivity is calculated using the following formula: η3=V h / V t ×100% In the formula, η3 represents hydrogen selectivity, expressed in %; V h V is the volume of hydrogen in the gaseous products; t This represents the total volume of the gaseous products.

[0042] The system energy consumption reduction rate is calculated using the following formula: η4 = (E0 - E1) / E0 × 100% In the formula, η4 is the system energy consumption reduction rate, in %; E0 is the energy consumption required to complete the same processing volume under the traditional fixed-bed reaction mode; E1 is the energy consumption required to complete the same processing volume by the centrifugal reactor integrated system of the present invention.

[0043] General preparation method of Fe-doped Pd / C catalysts: PdCl2 and Fe(NO3)3 were weighed according to the target Pd loading and Fe doping amounts, and a mixed precursor solution was prepared with deionized water. The target Pd loading amount was 0.8–1.2 wt% of the total catalyst mass, and the target Fe doping amount was 5–15 wt% of the total catalyst mass. Pretreated activated carbon was weighed and added to the mixed precursor solution, and stirred at room temperature for 2–4 h to ensure sufficient contact between the mixed precursor solution and the activated carbon support. After stirring, the resulting solid was subjected to solid-liquid separation, and the solid was dried in a drying device to obtain precursor-impregnated activated carbon.

[0044] The precursor impregnated with activated carbon was placed in a tube furnace or reduction furnace, and hydrogen gas was introduced for reduction at 300–500 °C for 2–4 h. After reduction, it was cooled to room temperature under an inert atmosphere to obtain the Fe-doped Pd / C catalyst. The obtained catalyst was tested and found to have a particle size of 20–50 nm and a saturation magnetization of 15–25 emu / g.

[0045] In a preferred embodiment, the activated carbon pretreatment includes the following steps: washing the activated carbon in deionized water, filtering, and drying at 105°C for 6–12 h; after drying, the activated carbon carrier is sieved to obtain a uniformly distributed particle size distribution. When adding the pretreated activated carbon to the mixed precursor solution, it is added in batches, with stirring maintained after each batch to ensure thorough wetting of the activated carbon. The stirring speed can be controlled at 300–500 rpm. The drying temperature can be controlled at 80–120°C, and the drying time can be controlled at 8–12 h. The heating rate during the reduction process can be controlled at 1–5°C / min, and the hydrogen flow rate can be adjusted according to the furnace volume and sample loading amount.

[0046] Preparation of nitrogen-containing heterocyclic LOHC complex supports and catalyst-containing complex systems: N-methylindole and 1-butyl-3-methylimidazolium tetrafluoroborate were weighed, and the mass fraction of 1-butyl-3-methylimidazolium tetrafluoroborate was controlled at 1–3 wt% of the total mass of the composite support. The mixture was stirred at room temperature or 30–50 °C for 20–60 min to obtain the nitrogen-heterocyclic LOHC composite support. After composite preparation, the viscosity of the composite support was measured using a rotational viscometer; when the viscosity was within 15–25 mPa·s, the catalyst dispersion step was initiated; if the viscosity deviated from the specified range, it was corrected by adjusting the stirring time, composite temperature, or ionic liquid ratio.

[0047] Weigh out the Fe-doped Pd / C catalyst and add it to the nitrogen-heterocyclic LOHC composite support at 0.5–2 wt% of the catalyst's mass. Dispersion can be achieved using at least one of mechanical stirring, circulating pumping, or ultrasonic dispersion. For mechanical stirring, the stirring speed can be controlled at 300–600 rpm, and the stirring time at 20–60 min. For circulating pumping, the circulation time can be controlled at 10–30 min. For ultrasonic dispersion, it can be carried out under conditions that do not cause abnormal temperature rise in the support. After dispersion, a nitrogen-heterocyclic LOHC composite system containing the catalyst is obtained.

[0048] Before the catalyst-containing composite system enters the centrifugal reactor, large particulate impurities can be removed by a filter screen or buffer tank, and the feed flow rate is controlled by a metering pump. The feed flow rate is controlled at 0.5–2 L / min, and the centrifugal bed speed is controlled at 300–800 rpm. The catalyst is dispersed in the composite carrier at a loading of 0.5–2 wt%, pumped into the centrifugal reactor, and the bed speed is adjusted to 300–800 rpm and the flow rate to 0.5–2 L / min according to the physical properties.

[0049] Continuous hydrodehydrogenation operation method: The nitrogen-containing heterocyclic LOHC complex system with catalyst is fed into a centrifugal reactor through the complex carrier inlet. The centrifugal bed is started and the rotation speed is adjusted to 300–800 rpm. During the hydrogenation stage, hydrogen gas is introduced into the reactor, and the reaction temperature is controlled at 120–180℃, the pressure at 3–5 MPa, and the feed flow rate at 0.5–2 L / min. The liquid phase after the reaction is discharged through the liquid outlet, and the gas phase is discharged through the hydrogen outlet or enters the tail gas treatment unit after gas-liquid separation.

[0050] After the hydrogenation stage is completed, the reactor operating conditions are adjusted to enter the dehydrogenation stage. In the dehydrogenation stage, the reaction temperature is controlled at 150–200°C, and the pressure is controlled at atmospheric pressure. The hydrogen produced during dehydrogenation is discharged through the hydrogen outlet and collected, while the liquid-phase hydrogen-poor carrier is discharged through the liquid outlet and enters a storage tank or circulation pipeline. The hydrogenation and dehydrogenation stages can share the same centrifugal reactor, or parallel or series reactors can be set up depending on the actual production scale.

[0051] After the reaction is completed, the external magnetic field recovery unit is activated to perform magnetic separation of the Fe-doped Pd / C catalyst in the liquid-phase circulation pipeline, the bottom recovery zone of the reactor, or the catalytic active zone. The recovered catalyst is then washed with a composite support and returned to the catalyst-containing composite system for continued use. Under hydrogenation conditions of 120–180℃ and 3–5 MPa, and dehydrogenation conditions of atmospheric pressure and 150–200℃, the hydrogen selectivity reaches over 98%, the catalyst magnetic recovery rate exceeds 99%, and the system energy consumption is reduced by 28% compared to traditional fixed-bed reactors.

[0052] Example 1: This example illustrates the preparation of a preferred Fe-doped Pd / C catalyst and its integrated application with a nitrogen heterocyclic LOHC complex system.

[0053] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with a Pd loading of 1.0 wt% and a Fe doping content of 8 wt% were weighed and added to deionized water to prepare a mixed precursor solution. Pretreated activated carbon was weighed and added to the mixed precursor solution, and the mixture was stirred at 400 rpm for 3 h at room temperature. After stirring, the mixture was filtered, and the filter cake was dried at 100℃ for 10 h to obtain precursor-impregnated activated carbon.

[0054] The precursor-impregnated activated carbon was placed in a tube furnace, and hydrogen gas was introduced. The temperature was increased to 400℃ at 3℃ / min, and the reduction was maintained at this temperature for 3 h. After reduction, the catalyst was cooled to room temperature under nitrogen protection to obtain the Fe-doped Pd / C catalyst. Transmission electron microscopy showed that the average particle size of the catalyst was 35 nm; the saturation magnetization was 20 emu / g, as measured by a vibrating sample magnetometer.

[0055] 98 g of N-methylindole and 2 g of 1-butyl-3-methylimidazolium tetrafluoroborate were weighed and stirred at room temperature for 40 min to obtain a nitrogen-containing heterocyclic LOHC composite support. The viscosity of this composite support at 25 °C was measured to be 20 mPa·s. 1 wt% of the Fe-doped Pd / C catalyst was added, and the mixture was mechanically stirred for 30 min, followed by circulation pumping for 10 min to obtain a catalyst-containing nitrogen-containing heterocyclic LOHC composite system.

[0056] The nitrogen-containing heterocyclic LOHC complex system with catalyst was fed into a centrifugal reactor at a feed flow rate of 1.0 L / min and a centrifuge bed speed of 500 rpm. During the hydrogenation stage, the reaction temperature was controlled at 150 °C and the pressure at 4 MPa; after the reaction, the hydrogenation conversion rate was measured to be 99.2%. The system was then switched to the dehydrogenation stage, and the reaction temperature was controlled at 180 °C under atmospheric pressure, with a hydrogen release rate of 98.5%. After the reaction, the catalyst was recovered using an external magnetic field, with a catalyst recovery rate of 99.2%. After 20 complete hydrogenation-dehydrogenation cycles, the system capacity retention rate was 97.8%.

[0057] Example 2: This example illustrates the long-term cyclic application after adjusting the Fe doping amount and Pd loading amount.

[0058] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with a Pd loading of 1.1 wt% and an Fe doping content of 10 wt% were weighed and added to deionized water to prepare a mixed precursor solution. Pretreated activated carbon was added to the mixed precursor solution, stirred at room temperature for 4 h, then filtered, dried, and reduced at 400℃ for 3 h in a hydrogen atmosphere to obtain the Fe-doped Pd / C catalyst. The obtained catalyst particles had a particle size of 30 nm and a saturation magnetization of 22 emu / g.

[0059] A nitrogen-containing heterocyclic LOHC composite support was prepared by mixing N-methylindole and 1-butyl-3-methylimidazolium tetrafluoroborate at a mass ratio of 98:2. The resulting catalyst was added to the composite support at 1.2 wt%. After mechanical stirring and circulation pumping, a catalyst-containing composite system was obtained. This system was transferred to a centrifugal reactor, with the centrifuge bed speed set at 600 rpm and the feed flow rate set at 1.2 L / min. The hydrogenation stage reaction temperature was 150℃ and the pressure was 4 MPa; the dehydrogenation stage reaction temperature was 180℃ and the pressure was atmospheric pressure.

[0060] After 50 cycles of hydrodehydrogenation, the system capacity retention was 96.5%, the hydrogen selectivity was 98.7%, and the catalyst magnetic recovery rate was 99.5%. During the cycle, no significant sedimentation, agglomeration, or irreversible catalyst loss was observed in the compound system, and no significant byproducts affecting the hydrogen selectivity evaluation were detected by gas phase analysis.

[0061] Example 3: This example illustrates the application of continuous operation under conditions of higher Fe doping ratio and lower Pd loading.

[0062] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with corresponding Pd loadings of 0.9 wt% and Fe doping amounts of 12 wt% were weighed and added to deionized water to prepare a mixed precursor solution. Pretreated activated carbon was added to the mixed precursor solution, stirred at room temperature for 4 h, filtered, dried at 100℃ for 10 h, and then reduced at 400℃ for 3 h in a hydrogen atmosphere to obtain the Fe-doped Pd / C catalyst. The catalyst particle size was measured to be 40 nm, and the saturation magnetization was 18 emu / g.

[0063] An N-methylindole composite support containing 2 wt% 1-butyl-3-methylimidazolium tetrafluoroborate was prepared. The catalyst was added at 0.8 wt% of the composite support mass and dispersed using mechanical stirring and a circulating pump. The catalyst-containing composite system was fed into a centrifugal reactor with a feed flow rate of 1.5 L / min and a bed rotation speed of 700 rpm. The hydrogenation stage reaction temperature was 150℃ and the pressure was 4 MPa; the dehydrogenation stage reaction temperature was 180℃ and the pressure was atmospheric pressure.

[0064] In continuous operation testing, the catalyst recovery rate of this embodiment was 99.3%, and the continuous operation efficiency was 32% higher than that of the comparative fixed-bed system. Post-operation sampling tests showed that the catalyst remained dispersed, with no significant magnetic loss or activity decrease. Example 3 describes the following parameters: Fe doping ratio 12 wt%, Pd loading 0.9 wt%, particle size 40 nm, saturation magnetization 18 emu / g, and continuous operation efficiency improvement and recovery rate data.

[0065] Example 4: This example illustrates the low-temperature applicability of the composite system under conditions of low Fe doping ratio.

[0066] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with a Pd loading of 1.0 wt% and an Fe doping content of 7 wt% were weighed to prepare a mixed precursor solution. Pretreated activated carbon was added to the mixed precursor solution, stirred at room temperature for 3 h, filtered, dried, and then reduced at 400℃ for 3 h in a hydrogen atmosphere to obtain the Fe-doped Pd / C catalyst. The obtained catalyst particles were found to have a particle size of 25 nm and a saturation magnetization of 21 emu / g.

[0067] 97 g of N-methylindole and 3 g of 1-butyl-3-methylimidazolium tetrafluoroborate were weighed and stirred to form a nitrogen-containing heterocyclic LOHC composite support. The obtained catalyst was added to the composite support at 1.5 wt% of its mass, and dispersed by mechanical stirring to obtain a catalyst-containing composite system. The system was placed in a low-temperature environment for flowability observation, and after returning to room temperature, it was sent to a centrifugal reactor for hydrodehydrogenation cycle testing. After low-temperature observation, no irreversible phase separation occurred in the composite system; after returning to room temperature, the catalyst could still be uniformly dispersed by stirring and circulating pumping.

[0068] During centrifugal reactor operation, the bed rotation speed was set to 500 rpm and the feed flow rate was 1.0 L / min. The hydrogenation stage reaction temperature was 150℃ and the pressure was 4 MPa; the dehydrogenation stage reaction temperature was 180℃ and the pressure was atmospheric pressure. Test results showed that no significant activity loss occurred during the circulation process, and the catalyst could be successfully recovered using an external magnetic field. Example 4 describes the results of observing the following parameters: Fe doping ratio 7 wt%, Pd loading 1.0 wt%, particle size 25 nm, saturation magnetization 21 emu / g, and low-temperature fluidity.

[0069] Example 5: This example illustrates storage stability under conditions of high Fe doping and high Pd loading.

[0070] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with a Pd loading of 1.2 wt% and an Fe doping content of 15 wt% were weighed and added to deionized water to form a mixed precursor solution. Pretreated activated carbon was added to the mixed precursor solution, stirred at room temperature for 4 h, filtered, dried, and then reduced at 450℃ for 3 h in a hydrogen atmosphere to obtain the Fe-doped Pd / C catalyst. The obtained catalyst particles had a particle size of 45 nm and a saturation magnetization of 23 emu / g.

[0071] An N-methylindole composite support containing 2 wt% 1-butyl-3-methylimidazolium tetrafluoroborate was prepared. The above catalyst was added to it at 1.0 wt% of the composite support mass, and after dispersion, it was stored at room temperature under sealed conditions for 30 days. During storage, the system was protected from light, and the storage container was kept sealed. After storage, the system was visually observed and its viscosity was tested. No obvious stratification or sedimentation was found.

[0072] The stored compound system was fed into a centrifugal reactor for a hydrogenation-dehydrogenation cycle reaction. The bed rotation speed was set to 600 rpm, and the feed flow rate was 1.0 L / min. The reaction temperature during the hydrogenation stage was 150℃, and the pressure was 4 MPa. The reaction temperature during the dehydrogenation stage was 180℃, and the pressure was atmospheric pressure. The test results showed that the system capacity retention rate was 98.2%, and the catalyst recovery rate was 99.1%. Example 5 records the capacity retention rate and catalyst recovery rate after 30 days of storage for a Fe doping ratio of 15 wt%, a Pd loading of 1.2 wt%, a particle size of 45 nm, a saturation magnetization of 23 emu / g.

[0073] Example 6: This example illustrates the feasibility of Fe-doped Pd / C catalysts and their composite systems under boundary parameter conditions.

[0074] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with corresponding Pd loadings of 0.8 wt% and Fe doping amounts of 5 wt% were weighed to prepare a mixed precursor solution. Pretreated activated carbon was added to the mixed precursor solution, stirred at room temperature for 2 h, filtered, dried, and then reduced at 300℃ for 2 h in a hydrogen atmosphere to obtain the Fe-doped Pd / C catalyst. Testing showed that the catalyst particle size was in the range of 20–50 nm, and the saturation magnetization was in the range of 15–25 emu / g.

[0075] 99 g of N-methylindole and 1 g of 1-butyl-3-methylimidazolium tetrafluoroborate were weighed and stirred to form a composite support. The resulting catalyst was added to the composite support at 0.5 wt% of its mass, and after mechanical stirring, it was fed into a centrifugal reactor. The centrifuge bed speed was set to 300 rpm, and the feed flow rate was set to 0.5 L / min. The reaction temperature for the hydrogenation stage was set to 120℃, and the pressure was set to 3 MPa; the reaction temperature for the dehydrogenation stage was set to 150℃, and the pressure was set to atmospheric pressure.

[0076] After continuous operation, the catalyst-containing composite system can switch between hydrogenation and dehydrogenation, and the catalyst can be recovered via an external magnetic field and returned to the composite system. This embodiment illustrates that, under the lower limit parameter conditions defined in the claims, the catalyst can still be used in conjunction with the composite support and centrifugal reactor.

[0077] Example 7: This example illustrates the feasibility of Fe-doped Pd / C catalysts and composite systems under another boundary parameter condition.

[0078] Based on the total mass of the catalyst, PdCl2 and Fe(NO3)3 with a Pd loading of 1.2 wt% and an Fe doping content of 15 wt% were weighed to prepare a mixed precursor solution. Pretreated activated carbon was added to the mixed precursor solution, stirred at room temperature for 4 h, filtered, dried, and then reduced at 500℃ for 4 h in a hydrogen atmosphere to obtain the Fe-doped Pd / C catalyst. Testing showed that the catalyst particle size was in the range of 20–50 nm, and the saturation magnetization was in the range of 15–25 emu / g.

[0079] 97 g of N-methylindole and 3 g of 1-butyl-3-methylimidazolium tetrafluoroborate were weighed and stirred to form a composite support. The resulting catalyst was added to the composite support at 2 wt% of its mass, dispersed, and then fed into a centrifugal reactor. The centrifuge bed speed was set to 800 rpm, and the feed flow rate was set to 2 L / min. The reaction temperature for the hydrogenation stage was set to 180℃, and the pressure was set to 5 MPa; the reaction temperature for the dehydrogenation stage was set to 200℃, and the pressure was set to atmospheric pressure.

[0080] Operational testing demonstrated that the catalyst-containing composite system can maintain a continuous feed state, and the reacted catalyst can be separated from the liquid-phase circulation system and returned for reuse via an external magnetic field. This embodiment illustrates that, under the high-limit parameter conditions defined in the claims, the catalyst, composite support, and centrifugal reactor still possess process adaptability.

[0081] Comparative Example 1: This comparative example uses a conventional Pd / C catalyst without Fe doping. The conventional Pd / C catalyst was added to an N-methylindole composite support containing 2 wt% 1-butyl-3-methylimidazolium tetrafluoroborate at the same Pd loading as in Example 2, and a hydrogenation-dehydrogenation cycle test was conducted under the same centrifugal reactor conditions as in Example 2. Because the conventional Pd / C catalyst lacks the magnetic recovery characteristics provided by Fe doping, rapid separation is difficult to achieve under an external magnetic field, resulting in catalyst residue in the liquid phase after cycling. The recovery process requires filtration or centrifugation.

[0082] After 50 cycles, the capacity retention of the traditional Pd / C system was lower than that of Example 2. Figure 4 The comparison chart of cycle stability and system efficiency shows that the Fe-doped Pd / C catalyst of this invention retains 96.5% of its capacity after 50 cycles, while the traditional Pd / C catalyst retains 78.2%. This comparison indicates that the Fe-doped Pd / C catalyst, when integrated with the composite support and centrifugal reactor, outperforms the traditional Pd / C system in terms of cycle stability.

[0083] Comparative Example 2: This comparative example uses a fixed-bed reactor instead of a centrifugal reactor. The catalyst, composite support, and reaction temperature and pressure conditions are all set as in Example 1. The catalyst-containing composite system is fed into the fixed-bed reactor for hydrogenation and dehydrogenation circulation. The bed is not equipped with a centrifugal enhancement structure, and the liquid and gas phases after the reaction are discharged separately.

[0084] During testing, the fixed-bed reactor exhibited a smaller range of adjustment for the gas-liquid-solid three-phase contact state compared to the centrifugal reactor, and additional separation steps were required for catalyst recovery and the recycling of the compound system. Compared to Example 1, the fixed-bed reactor consumed more energy to complete the same recycling operation. It is recorded that the integrated centrifugal reaction system of this invention reduces system energy consumption by 28% compared to the traditional fixed-bed system, and achieves hydrogen selectivity exceeding 98% and catalyst magnetic recovery rate exceeding 99%.

[0085] Comparative Example 3: This comparative example does not include 1-butyl-3-methylimidazolium tetrafluoroborate; only N-methylindole is used as the LOHC support. Fe-doped Pd / C catalysts were prepared according to the method described in Example 1, and the catalyst was added at 1 wt% to a single N-methylindole support. After mechanical stirring, the catalyst was placed in a centrifugal reactor.

[0086] Compared to Example 1, the single N-methylindole support has less room for adjustment in terms of low-temperature fluidity and cycling stability, and a narrower matching range between support viscosity and centrifugal bed speed. Adding 1–3 wt% 1-butyl-3-methylimidazolium tetrafluoroborate allows the viscosity of the composite support to be controlled within the range of 15–25 mPa·s, facilitating matching with centrifugal bed speeds of 300–800 rpm. It has been reported that the composite support, in synergy with the Fe-doped Pd / C catalyst and the centrifugal reactor, can maintain hydrogen selectivity above 98% and reduce system energy consumption by 28% compared to a fixed bed.

[0087] Summary of Implementation Results:

[0088] As demonstrated by the above embodiments, this invention integrates an Fe-doped Pd / C catalyst, an N-methylindole composite support, and a centrifugal reactor, enabling hydrogenation at 120–180°C and 3–5 MPa, and dehydrogenation at 150–200°C and atmospheric pressure. The catalyst, added in an amount ranging from 0.5 to 2 wt%, can be dispersed in the nitrogen-heterocyclic LOHC composite support and can be recovered and recycled using an external magnetic field. The resulting system exhibits high catalyst recovery and recycling capacity retention in multiple embodiments, indicating that the technical solution of this invention has good process stability and repeatability.

[0089] Operations not described in detail in the above embodiments, such as equipment sealing, gas replacement, pressure control, temperature control, sample sampling, gas chromatography analysis, and magnetic recovery weighing, can all be performed using conventional experimental and engineering methods in the field. Any adjustments made within the ranges of Pd loading, Fe doping amount, particle size, magnetization, composite support ratio, catalyst addition amount, centrifuge bed speed, feed flow rate, hydrogenation conditions, and dehydrogenation conditions disclosed in this invention are considered specific embodiments of the disclosed content of this invention.

Claims

1. An Fe-doped Pd / C catalyst, characterized in that, It includes an activated carbon support and Pd and Fe supported on the activated carbon support; based on the total mass of the catalyst, the Pd loading is 0.8 to 1.2 wt%, and the Fe doping amount is 5 to 15 wt%; the particle size of the Fe-doped Pd / C catalyst is 20 to 50 nm, and the saturation magnetization is 15 to 25 emu / g.

2. The Fe-doped Pd / C catalyst according to claim 1, characterized in that, The activated carbon support has a microporous-mesoporous composite pore structure, with Pd and Fe distributed on the inner and outer surfaces of the pores of the activated carbon support, and the average particle size of the Fe-doped Pd / C catalyst is 30–40 nm.

3. The Fe-doped Pd / C catalyst according to claim 1, characterized in that, The Pd loading is 0.9–1.1 wt%, the Fe doping is 7–12 wt%, the particle size is 25–45 nm, and the saturation magnetization is 18–23 emu / g.

4. A method for preparing the Fe-doped Pd / C catalyst according to any one of claims 1 to 3, characterized in that, Includes the following steps: PdCl2 and Fe(NO3)3 were prepared into a mixed precursor solution containing Pd and Fe; Pretreated activated carbon was added to the mixed precursor solution and co-impregnated by stirring at room temperature for 2–4 h. The co-impregnated solids are subjected to solid-liquid separation and drying; Fe-doped Pd / C catalyst was obtained by reduction in a hydrogen atmosphere at 300–500 °C for 2–4 h.

5. The preparation method according to claim 4, characterized in that, The mixed precursor solution uses deionized water as a solvent. The amounts of PdCl2 and Fe(NO3)3 added are proportioned according to the Pd loading of 0.8–1.2 wt% and the Fe doping amount of 5–15 wt% in the obtained Fe-doped Pd / C catalyst. No stabilizer is added in the preparation method.

6. A method for composite nitrogen heterocyclic LOHC catalysts with Fe-doped Pd / C catalysts, characterized in that, Includes the following steps: The Fe-doped Pd / C catalyst according to any one of claims 1 to 3 or the Fe-doped Pd / C catalyst prepared by the preparation method according to claim 4 or 5; N-methylindole was formulated with the ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate to form a nitrogen-heterocyclic LOHC complex support, wherein the ionic liquid accounted for 1-3 wt% of the total mass of the nitrogen-heterocyclic LOHC complex support. The Fe-doped Pd / C catalyst was dispersed in the nitrogen heterocyclic LOHC composite support at an addition amount of 0.5–2 wt% to obtain a nitrogen heterocyclic LOHC composite system containing the catalyst.

7. The method for complexing nitrogen-containing heterocyclic LOHC compounds according to claim 6, characterized in that, The viscosity of the nitrogen heterocyclic LOHC composite support is 15-25 mPa·s. During the composite process, the Fe-doped Pd / C catalyst is dispersed in the nitrogen heterocyclic LOHC composite support by at least one of the following methods: mechanical stirring, circulating pumping, or ultrasonic dispersion.

8. The method for complexing nitrogen-containing heterocyclic LOHC compounds according to claim 6 or 7, characterized in that, The catalyst-containing nitrogen heterocyclic LOHC complex system is fed into a centrifugal reactor, which includes a complex carrier inlet, a centrifugal bed, a catalytically active zone, a hydrogen outlet, a liquid outlet, and an external magnetic field recovery unit. The centrifugal bed rotates at 300–800 rpm, and the feed flow rate is 0.5–2 L / min.

9. The method for complexing nitrogen-containing heterocyclic LOHC compounds according to claim 8, characterized in that, The catalyst-containing nitrogen heterocyclic LOHC complex system has a reaction temperature of 120–180°C and a pressure of 3–5 MPa during the hydrogenation stage, and a reaction temperature of 150–200°C and a pressure of atmospheric pressure during the dehydrogenation stage.

10. The method for complexing nitrogen-containing heterocyclic LOHC compounds according to claim 8, characterized in that, The hydrogenation and dehydrogenation stages share the same centrifugal reactor. The gas phase after the reaction is discharged from the hydrogen outlet, and the liquid phase after the reaction is discharged from the liquid outlet. The Fe-doped Pd / C catalyst is separated from the liquid phase or catalytic active zone by the external magnetic field recovery unit and returned to the catalyst-containing nitrogen heterocyclic LOHC complex system for recycling.