A Fe 0 FeMoS composite materials, their preparation methods, and applications
By preparing Fe0FeMoS composite material, the problem of the difficulty in achieving efficient photocatalytic reduction and degradation of perfluorinated and polyfluorinated alkyl compounds under mild conditions in the existing technology was solved. The efficient and stable photocatalytic reduction and defluorination effect was achieved, especially the degradation rate and defluorination rate of PFOS were significantly improved, and the material still maintains high efficiency after multiple cycles of use.
Patent Information
- Application Number
- CN202611197808.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to efficiently photocatalytically reduce and degrade perfluorinated and polyfluorinated alkyl compounds (such as PFOA and PFOS) under mild conditions, especially in releasing F- via the reductive dehalogenation pathway. Furthermore, existing iron-molybdenum-sulfur-based catalytic materials cannot achieve efficient and stable photocatalytic reduction and defluorination.
A Fe0FeMoS composite material was prepared, comprising a sheet-like nanoflower-like FeMoS framework and nano-zero-valent iron Fe0 particles supported thereon. The Fe0FeMoS composite material was formed by titrating the reduction of the precursor FeMoS with a mixed solution of Na2S2O4 and NaBH4 under inert gas protection. This composite material was used for photocatalytic reduction and degradation of perfluorinated and polyfluorinated alkyl compounds in water.
It achieves efficient photocatalytic reduction and degradation of PFAS under mild conditions of pH 5-8, with a PFOS degradation rate of 91.3% and a defluorination rate of 55.1%. Moreover, after 5 cycles, it still maintains a degradation rate of over 85% and a defluorination rate of over 44%, demonstrating excellent cycle stability.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalytic materials, and more specifically, to a Fe... 0 FeMoS composite materials, their preparation methods, and applications. Background Technology
[0002] The CF bond energy in perfluorinated and polyfluorinated alkyl compounds (PFAS) molecules is extremely high, and their chemical structure is extremely stable. Conventional oxidation technologies are difficult to achieve effective degradation and defluorination, which has become a major problem in the field of water environment management.
[0003] To achieve the defluorination of highly stable PFASs, various redox technologies have been studied, including photocatalysis, sonochemical oxidation, electrocatalysis, ozone oxidation, hydrated electrons, ultraviolet / sulfite oxidation, and plasma. However, most methods require harsh conditions such as far-ultraviolet light for activation, resulting in poor practicality. For long-chain perfluorinated compounds containing two or more carbon atoms (such as PFOA and PFOS), achieving efficient defluorination under mild conditions remains extremely challenging, with very few successful reports, especially regarding the release of F via the reductive dehalogenation pathway. - This remains a key challenge that has yet to be overcome in this field.
[0004] Most existing iron-molybdenum-sulfur-based catalytic materials can only achieve advanced oxidation processes by activating persulfate. For example, the g-C3N4 modified FeMoS4 material disclosed in patent CN115041213A is only suitable for the oxidative removal of easily degradable organic pollutants such as dyes, and cannot achieve photocatalytic reduction defluorination of PFAS.
[0005] Nano-zero valent iron (Fe) 0 Although it possesses strong reducing ability, it is prone to aggregation and oxidation in aqueous phase, exhibits low electron utilization, and poor stability. The nano-zero-valent iron / graphite carbon nitride photocatalytic material disclosed in patent CN121695911A is only used in the field of algae suppression; the core-shell type iron sulfide / zero-valent iron composite material disclosed in patent CN111097449A is only used for the reduction and photocatalytic degradation of conventional pollutants such as Cr(VI), nitrophenol, and methyl orange, neither of which can provide an efficient and stable photocatalytic reduction defluorination pathway for PFAS. Summary of the Invention
[0006] To overcome the shortcomings of the prior art in achieving efficient photocatalytic reduction and defluorination of long-chain PFAS under mild conditions, this invention provides a Fe... 0 FeMoS composite material; Another object of the present invention is to provide a Fe 0 Preparation method of FeMoS composite material; Another object of the present invention is to provide a Fe 0Applications of FeMoS composite materials.
[0007] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows: A Fe 0 The FeMoS composite material comprises a sheet-like nanoflower-like FeMoS framework and nano-zero-valent iron Fe supported thereon. 0 Particles; the FeMoS framework is composed of symbiotic MoS2 and FeS2 crystal phases, and the nano-zero-valent iron Fe... 0 The particles fill the interlayer space of the sheet-like nanoflower-like FeMoS framework.
[0008] Preferably, the Fe 0 The X-ray diffraction pattern of the FeMoS composite material has characteristic diffraction peaks at 2θ of 14°±1°, 33°±1° and 45°±1°.
[0009] A Fe 0 The preparation method of FeMoS composite material includes the following steps: Under inert gas protection, the precursor FeMoS was dispersed in water and reduced by titration with a mixed solution of Na2S2O4 and NaBH4. After complete reaction, Fe was obtained. 0 FeMoS composite material; wherein the ratio of the precursor FeMoS to water is 0.1~0.5 g: 100~250 mL.
[0010] Furthermore, the volume ratio of the Na2S2O4 solution, NaBH4 solution, and water dispersing FeMoS is 80~120:80~120:150~250; Furthermore, the concentration of the Na2S2O4 solution is 0.1~1.5 mol / L, and the concentration of the NaBH4 solution is 0.1~1.0 mol / L.
[0011] Preferably, the concentration of the Na2S2O4 solution is 1 mol / L, and the concentration of the NaBH4 solution is 0.5 mol / L.
[0012] Preferably, titration is performed at a rate of 5-8 mL / min, and stirring is carried out at a speed of 550-650 r / min; Preferably, the magnetic stirring is performed for 15-20 minutes; Preferably, the above products are washed by centrifugation with water and ethanol, respectively; Preferably, the drying process is carried out in a vacuum oven at a temperature of 60-80°C for 6 hours, and then stored in a nitrogen atmosphere for later use.
[0013] Furthermore, the precursor FeMoS is prepared by the following method: Na2MoO4·2H2O, thiourea, and FeCl3·6H2O are mixed evenly and then subjected to a hydrothermal reaction to obtain the precursor FeMoS.
[0014] Preferably, Na2MoO4·2H2O, thiourea, and FeCl3·6H2O are mixed in water, stirred evenly at room temperature, and then subjected to a hydrothermal reaction. After the hydrothermal reaction product cools naturally, it is washed by alternating centrifugation with water and ethanol, and then dried to obtain the precursor FeMoS.
[0015] Furthermore, the mass ratio of Na2MoO4·2H2O, thiourea, and FeCl3·6H2O is 2~4:2~4:3~5.
[0016] Preferably, the molar ratio of Na2MoO4·2H2O, thiourea, and FeCl3·6H2O is 1:3:1.
[0017] Furthermore, the ratio of the total mass of Na2MoO4·2H2O, thiourea, and FeCl3·6H2O to water is 10~12 g: 50~70 mL.
[0018] Preferably, the stirring time is 15-20 min.
[0019] Furthermore, the hydrothermal reaction temperature is 160~200℃; preferably, the hydrothermal reaction time is 20~24 h.
[0020] Preferably, after being stirred evenly, the mixture is transferred to a stainless steel high-pressure reactor lined with polytetrafluoroethylene for reaction.
[0021] Preferably, the mixture is washed by centrifugation with water for 30-40 minutes, then washed by centrifugation with ethanol for 1-2 hours, followed by centrifugation with ethanol for 12-16 hours.
[0022] Preferably, the drying temperature is 60~80℃, the drying time is 6 h, and then the product is stored in a nitrogen atmosphere for later use.
[0023] A Fe 0 FeMoS composite material, composed of Fe 0 FeMoS was prepared using a specific method.
[0024] A Fe 0 FeMoS composite materials are used as catalysts with photocatalytic reduction capabilities.
[0025] Furthermore, it can be used for photocatalytic reduction and degradation of perfluorinated and polyfluoroalkyl compounds in water.
[0026] Preferably, catalytic degradation is carried out at pH 5-8.
[0027] Preferably, Fe 0 The dosage of FeMoS composite material in water is 100~500 mg / L.
[0028] The perfluorinated and polyfluoroalkyl compounds include perfluorooctane sulfonic acid (PFOS) and perfluorooctanoic acid (PFOA).
[0029] During the degradation process, Fe 0 Upon light excitation, FeMoS first generates photogenerated carriers from the active sites of molybdenum disulfide. These photogenerated carriers, due to their high conductivity, rapidly separate, with electrons combining with hydrogen ions to produce high-energy hydrogen radicals. However, due to the presence of the FeS2 structure, the direct combination of high-energy hydrogen atoms to form hydrogen is inhibited. The hydrogen radicals then attack perfluorooctane sulfonic acid suspended in the solution, thus efficiently and energy-savingly obtaining high-energy hydrogen atoms for a clean hydrogen-fluorine atom substitution reaction, achieving a high-speed and efficient degradation process and stability of perfluorinated compounds. Furthermore, nano-zero-valent iron provides electrons to the system, which combine with oxygen in the solution to form superoxide radicals, further catalyzing the perfluorooctane sulfonic acid reaction and promoting the efficient defluorination of perfluorooctane sulfonic acid. Simultaneously, photogenerated electrons also participate in the reduction and oxidation of nano-zero-valent iron, maintaining the stability of the material throughout the system and repairing damaged nanoparticles. Perfluorooctane sulfonic acid not only undergoes surface reduction upon contact with a catalyst, but also a mineralization process. The perfluorooctane sulfonic acid reduced to octane sulfonic acid is eventually mineralized into CO2 and H2O by superoxide radicals, thus achieving harmlessness.
[0030] Compared with the prior art, the beneficial effects of the technical solution of the present invention are: The Fe prepared by this invention 0 The FeMoS composite material exhibits excellent photocatalytic reduction degradation and defluorination performance of PFAS. The degradation rate of PFAS can reach 91.3%, and the defluorination rate can reach 55.1%. After five cycles, the degradation rate remains above 85%, and the defluorination rate remains above 44%, demonstrating excellent cycle stability. It maintains high catalytic efficiency under mild conditions of pH 5–8, making it widely applicable and enabling efficient, stable, and deep reduction defluorination of PFAS in water. Attached Figure Description
[0031] Figure 1 SEM images of different materials are shown: (a) MoS2; (b) FeS2; (c) FeMoS; (d) Fe prepared in Example 1. 0 FeMoS; Figure 2Fe in Example 1 0 EDS images of FeMoS: (a) is the overall SEM morphology; (b) is the elemental mapping overview; (c) is the C elemental distribution map; (d) is the Fe elemental distribution map; (e) is the Mo elemental distribution map; (f) is the S elemental distribution map. Figure 3 Fe, as described in Example 1 of this invention 0 XRD patterns of FeMoS before and after PFOS degradation; Figure 4 Fe in Example 1 0 Degradation rate (a) and defluorination rate (b) of FeMoS in photocatalytic degradation of PFAS in water. Figure 5 Fe in Example 1 0 The degradation rate (a) and defluorination rate (b) of PFAS in water during the 1st to 5th cycles of FeMoS recycling. Figure 6 For Fe 0 Degradation rate (a) and defluorination rate (b) of FeMoS and FeMoS at different catalytic pH for 6 h of photocatalytic degradation of PFOS. Detailed Implementation
[0032] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.
[0033] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.
[0034] Example 1 A Fe 0 The preparation method of FeMoS composite material is as follows: (1) Preparation of FeMoS 3.63 g (0.015 mol) Na₂MoO₄·2H₂O, 3.42 g (0.045 mol) thiourea, and 4.0545 g (0.015 mol) FeCl₃·6H₂O were dissolved in 60 mL of deionized water and magnetically stirred for 15 min to accelerate dissolution. The solution was then transferred to a 100 mL polytetrafluoroethylene-lined high-pressure reactor and heated at 180 °C for 24 h in a constant-temperature electric heating drying oven. After the reaction was complete, the mixture was washed three times each with deionized water and ethanol, dried under vacuum at 60 °C for 6 h, and then stored under a nitrogen atmosphere for later use.
[0035] (2) Fe 0 Preparation of FeMoS Add 0.2 g of the previously synthesized FeMoS to a three-necked flask, and add deionized water to a final volume of 200 mL. Under a nitrogen atmosphere, titrate a mixture of 100 mL Na₂S₂O₄ solution (1 mol / L) and 100 mL NaBH₄ solution (0.5 mol / L) to the three-necked flask at a rate of 7 mL / min, while simultaneously stirring the solution in the three-necked flask at 600 r / min. After titration, continue magnetic stirring for 15 min to ensure complete reaction, yielding a black solid. Wash the solid three times with deionized water (after ultrasonic de-airing) and three times with ethanol. Quickly transfer the black solid to a vacuum drying oven and dry it under vacuum at 60 °C for 6 h. Remove the solid and store it under a nitrogen atmosphere for later use.
[0036] (3) Fe 0 Application of FeMoS in photocatalytic degradation of PFAS in water Accurately weigh 50 mg of Fe 0 FeMoS powder was placed in a quartz reactor, and 100 mL of freshly prepared PFOS solution with pH 6.5 and an initial concentration of 10 mg / L was added. The system was then stirred in the dark for 30 min to reach adsorption equilibrium (with FeMoS as a control).
[0037] Example 2 Same as in Example 1, in step (2), the amount of FeMoS is 0.1 g; the amount of Na2S2O4 is 80 mL; the amount of NaBH4 is 80 mL; the amount of deionized water is 150 mL; and other conditions remain unchanged.
[0038] Example 3 Same as in Example 1, in step (2), the amount of FeMoS is 0.3 g; the amount of Na2S2O4 is 120 mL; the amount of NaBH4 is 120 mL; the amount of deionized water is 250 mL; and other conditions remain unchanged.
[0039] Example 4 Same as in Example 1, in step (3), Fe 0 The FeMoS dosage was changed to 10, 15, 25, and 30 mg, respectively.
[0040] Example 5 Similar to Example 1, in step (3), PFOS solutions with pH values of 5 and 8 were used respectively, with FeMoS as a control.
[0041] Comparative Example 1 Same as in Example 1, in step (1), the amount of Na2MoO4·2H2O is 1 g; the amount of thiourea is 1 g; the amount of FeCl3·6H2O is 1.5 g; and the amount of deionized water is 50 mL, while other conditions remain unchanged.
[0042] Comparative Example 2 Same as in Example 1, in step (1), the amount of Na2MoO4·2H2O is 4 g; the amount of thiourea is 4 g; the amount of FeCl3·6H2O is 5.5 g; and the amount of deionized water is 70 mL, while other conditions remain unchanged.
[0043] Test methods 1. Degradation rate and defluorination rate Accurately weigh 50 mg of Fe 0 FeMoS powder was placed in a quartz reactor, and 100 mL of freshly prepared PFOS solution with pH=6.5 and an initial concentration of 10 mg / L was added. The reactor was then placed in the dark and magnetically stirred for 30 min to allow the catalyst and pollutants to reach adsorption-desorption equilibrium. After adsorption equilibrium was reached, a 300 W xenon lamp (equipped with an AM 1.5G filter to simulate sunlight) was turned on, and samples were taken at 0, 1, 2, 3, 4, 5, and 6 h of illumination. The samples were filtered through a 0.22 μm PES filter and stored in the dark for the determination of PFOS degradation rate and defluorination rate. PFOS concentration was determined by high-performance liquid chromatography (HPLC) using a Phenomenex Luna C18(2)100A column (4.6 mm × 150 mm, 5 μm), a column temperature of 40℃, mobile phase A being 10 mM ammonium acetate aqueous solution and mobile phase B being methanol, with a flow rate of 0.5 mL / min and gradient elution. F⁻ concentration was determined by ion chromatography using an IC-SA2(G) column, with a 3.2 mM Na₂CO₃ and 1.0 mM NaHCO₃ mixed solution as eluent, a flow rate of 0.8 mL / min, a column temperature of 25℃, and an injection volume of 20 μL. The defluorination rate was expressed as the percentage of released F⁻ moles relative to the total fluorine moles in the PFOS molecules.
[0044] 2. Effects of reaction conditions on the test (1) Effect of catalyst dosage: The initial concentration of PFOS was controlled at 10 mg / L, pH=6.5, reaction volume at 100 mL, and light exposure at 6 h. The catalyst dosage was set at 10, 15, 25, 30, and 50 mg, and the tests were conducted according to the steps described in "Degradation rate and defluorination rate".
[0045] (2) Effect of initial pH: The catalyst dosage was controlled at 50 mg, the initial PFOS concentration was 10 mg / L, the reaction volume was 100 mL, and the light exposure was 6 h. The pH was adjusted to 5, 6.5, and 8, and the tests were carried out according to the steps described in "Degradation rate and defluorination rate"; a pure FeMoS control was set up simultaneously.
[0046] 3. Cyclic Use Performance Test Fe will complete the photocatalytic reaction 0 The FeMoS catalyst was collected, washed and dried sequentially with deionized water, and then reused in the next round of PFOS degradation experiments. Each experiment was conducted according to the steps described in "Degradation Rate and Defluorination Rate" above, and the catalyst was recycled 5 times to evaluate its cyclic stability. The retention rate of PFOS degradation rate and defluorination rate was used as the evaluation index in the cyclic experiments.
[0047] Analysis and Explanation 1. Structural and compositional characterization Figure 1 (a) It can be seen that MoS2 has a typical sheet-like nanoflower skeleton structure, which is assembled from a large number of thin sheet layers and has a large specific surface area. Figure 1 (b) FeS2 exhibits an irregular sheet-like granular structure with obvious stacking between particles; Figure 1 (c) It can be seen that FeMoS retains a similar sheet-like nanoflower skeleton structure to MoS2, but due to the introduction of Fe, the specific surface area is reduced and the number of exposed active sites is reduced. Figure 1 (d) It can be observed that FeMoS retains its lamellar framework structure after treatment with a strong reducing agent, while a large amount of zero-valent iron (Fe2+) is formed between the lamellar layers. 0 Spherical particles are coated with nanoflower-like FeMoS crystals, forming a core-shell-like coating structure—the outer layer of sheet-like nanoflower structure isolates Fe... 0 Passivation caused by contact with air significantly improves the stability of the material.
[0048] Figure 2 For Fe 0 Elemental distribution map of FeMoS (EDS mapping). Wherein: Figure 2 (a) is Fe 0 A comprehensive SEM image of FeMoS, serving as a reference for elemental distribution; Figure 2 (b) is an overview of the element mapping (including elements such as C, Au, Mo, Fe, O, and S); Figure 2 (c)~(f) correspond to the mapping diagrams of each element, respectively. It can be observed that Fe, Mo, and S are uniformly distributed in the material, without any local enrichment or deficiency of any element, indicating that Fe... 0 FeMoS is not Fe 0It's not a simple physical mixture of FeS2 and MoS2, but rather the structures of FeS2 and MoS2 have fused together to form a new crystal during hydrothermal synthesis. In subsequent reduction treatment, Fe is converted into Fe... 0 The form precipitates in situ from the FeMoS framework, while maintaining the uniformity of the overall elemental distribution.
[0049] Depend on Figure 3 It can be seen that Fe before and after the reaction 0 The characteristic peak positions of FeMoS are basically consistent, mainly MoS2 (near 14° (100) crystal plane), FeS2 (near 33° (002) crystal plane) and Fe 0 Characteristic peaks (around 45°); after the reaction, each characteristic peak remains clearly distinguishable, crystallinity decreases only slightly, and Fe... 0 The characteristic peaks remained stable after the reaction without significant attenuation, indicating that Fe 0 The crystal structure of FeMoS remained intact during the photocatalytic reaction. 0 The particles are stably present on the FeMoS framework surface, verifying that the material has excellent structural stability under reaction conditions.
[0050] 2. Effects of process conditions on catalytic performance As can be seen from Table 1, the Fe obtained in Example 1 0 FeMoS exhibited a PFOS degradation rate of 91.3% and a defluorination rate of 55.1%; while pure FeMoS without Na2S2O4 / NaBH4 reduction treatment had a degradation rate of only 27.3% and a defluorination rate of only 15.9% under the same test conditions. The former's degradation rate was approximately 3.34 times that of the latter, and its defluorination rate was approximately 3.46 times that of the latter, fully demonstrating that the strong reducing agent reduction step plays a decisive role in improving the performance of FeMoS.
[0051] In Comparative Example 1, the amount of each solid raw material was significantly reduced compared to Example 1 (approximately 1 / 3.5 to 1 / 4 of that in Example 1), resulting in a lower precursor concentration. Its PFOS degradation rate was only 26.2%, and its defluorination rate was only 15.8%. In Comparative Example 2, the amount of each raw material was higher than that in Example 1 (approximately 1.1 to 1.4 times that in Example 1), resulting in a higher precursor concentration. Its PFOS degradation rate was only 28.1%, and its defluorination rate was only 16.1%. Comparative Examples 1 and 2 showed comparable performance to unreduced pure FeMoS, indicating that, under similar molar ratios, simply adjusting the precursor ratio has limited effect on improving the intrinsic activity of FeMoS. The 60 mL water volume used in Example 1 was well-matched with the high-pressure reactor volume (100 mL). In Comparative Example 1, insufficient water limited the solubility of the reactants, while in Comparative Example 2, excessive water resulted in overfilling and pressure conditions deviating from the optimal range. Based on this, Na2S2O4 / NaBH4 reduction treatment is a method for preparing highly active FeMoS. 0A key step in FeMoS formation—only through this step can nano-Fe be precipitated in situ within the FeMoS framework. 0 And form FeMoS sheets to coat Fe 0 Only after the core-shell structure of the particles is established does the material exhibit a significantly enhanced photocatalytic reduction degradation and defluorination capability for PFOS.
[0052] Table 1. PFOS degradation and defluorination effects of Example 1 and the comparative example. Degradation rate (%) Defluorination rate (%) Example 1 91.3 55.1 FeMoS 27.3 15.9 Example 2 84.2 43.8 Example 3 85.7 49.8 Comparative Example 1 26.2 15.8 Comparative Example 2 28.1 16.1 As shown in Table 2, Fe 0 The FeMoS structure is stable, and even after five reaction cycles, its catalytic activity remains above 85%, maintaining its high efficiency and stability. In Example 1, the degradation rate remained at 85.2% after five cycles (a decrease of only about 6.1 percentage points), down from 91.3% in the first cycle; the defluorination rate remained at 44.9% after five cycles, down from 55.1% in the first cycle. The defluorination rate decreased more rapidly in the first three cycles (a decrease of about 9.2 percentage points), and tended to stabilize in the fourth and fifth cycles. This stability mechanism is mainly attributed to the high structural stability of the FeMoS framework itself. Figure 3 (No significant changes were observed in the XRD patterns before and after the reaction); in-situ precipitated nano-Fe 0 The particles are coated with nano-flower-like FeMoS sheets. Figure 1 d) Forming a core-shell-like structure, effectively isolating Fe 0 Passivation caused by contact with O2 in the air; Fe during cycling 0 It mainly acts as a medium for transferring electrons, without changing its own valence state. Figure 3 Fe 0 The characteristic peaks remain stable after the reaction.
[0053] Table 2 Fe in Example 1 0 Degradation and defluorination effects of FeMoS after 1-5 cycles 1 time 2 times 3 times 4 times 5 times Degradation rate (%) 91.3 89.5 87.9 87.3 85.2 Defluorination rate (%) 55.1 47.8 45.9 44.6 44.9 3. Effect of photocatalytic degradation reaction conditions on the results When the sampling time in this group of experiments was extended to 72-80 hours, Figure 4 (a) It can be seen that the PFOS degradation process mainly occurs in the first 40 hours of the reaction, and basically reaches equilibrium after about 40 hours. The maximum degradation rate is greater than 95%, and the residual concentration of PFOS in the solution is less than 2 μM at equilibrium. Figure 4 (b) The defluorination process exhibits a significant lag compared to the degradation process, reaching equilibrium after approximately 56 hours, with a maximum defluorination rate of about 55%. This indicates that PFOS was not completely mineralized after a short-term experiment of 6 hours, and fluorine-containing intermediates still existed, thus the defluorination rate continued to increase over a longer timescale; Fe 0FeMoS exhibits long-term, sustained, and highly efficient photocatalytic reduction capabilities, enabling deep defluorination of PFOS.
[0054] Table 3. Example 4: Different Fe 0 Degradation results of FeMoS catalyst input 10 mg 15 mg 25 mg 30 mg 50 mg Degradation rate (%) 81.5 84.4 89.5 93.4 91.3 Defluorination rate (%) 41.5 45.5 48.6 51.2 55.1 As shown in Table 3, when the catalyst dosage was increased to 50 mg, the degradation rate actually decreased slightly to 91.3%—this is because the excess catalyst particles agglomerated and the light scattering effect occurred in the reaction system, causing some Fe to be degraded. 0 FeMoS particles are shielded, reducing their effective light utilization; the defluorination rate increases continuously with increasing dosage in the range of 10-50 mg, because the defluorination rate is dominated by the number of electrons directly donated by Fe0. 0 FeMoS2 Fe 0 The enrichment of photogenerated electrons on the particle surface increases continuously with the dosage, thereby enhancing the ability to reduce and break CF bonds in PFOS.
[0055] Depend on Figure 6 It is evident that the degradation rate of Fe0FeMoS remained at a high level (>80%) within the pH range of 5–8. The degradation rate decreased slightly when the pH changed from weakly acidic to weakly alkaline, but the overall fluctuation was not significant, demonstrating a wide pH adaptability. In contrast, the degradation rate of unreduced FeMoS only remained in the 20%–30% range within the same pH range. 0 The defluorination rate of FeMoS remains relatively stable (approximately 50%–55%) within the pH range of 5–8, exhibiting significantly lower pH sensitivity than its degradation rate. The MoS2 component within the FeMoS framework possesses the ability to construct a slightly acidic surface environment, which can, to some extent, resist the influence of external alkaline pH on catalytic activity; under alkaline conditions, Fe… 0 The FeMoS surface is neutralized by the constructed slightly acidic environment, under acidic conditions H + Higher concentrations and more high-energy hydrogen atoms generated by photogenerated electron reduction can more efficiently attack the CF bonds in PFOS—the synergistic effect of these two factors enables Fe... 0 FeMoS maintains highly efficient and stable degradation and defluorination performance within the pH range of 5 to 8.
[0056] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A Fe 0 FeMoS composite material, characterized in that, The composite material comprises a sheet-like, nanoflower-like FeMoS framework and nano-zero-valent iron Fe supported thereon. 0 Particles; the FeMoS framework is composed of symbiotic MoS2 and FeS2 crystal phases, and the nano-zero-valent iron Fe... 0 The particles fill the interlayer space of the sheet-like nanoflower-like FeMoS framework.
2. The Fe according to claim 1 0 The method for preparing FeMoS composite material is characterized by, Includes the following steps: Under inert gas protection, the precursor FeMoS was dispersed in water and reduced by titration with a mixed solution of Na2S2O4 and NaBH4. After complete reaction, Fe was obtained. 0 FeMoS composite material; wherein the ratio of the precursor FeMoS to water is 0.1~0.5 g: 100~250 mL.
3. The Fe according to claim 2 0 The method for preparing FeMoS composite material is characterized by, The volume ratio of the Na2S2O4 solution, NaBH4 solution and water dispersing FeMoS is 80~120:80~120:150~250.
4. The Fe according to claim 2 0 The method for preparing FeMoS composite material is characterized by, The concentration of the Na2S2O4 solution is 0.1~1.5 mol / L, and the concentration of the NaBH4 solution is 0.1~1.0 mol / L.
5. The Fe according to claim 2 0 The method for preparing FeMoS composite material is characterized by, The precursor FeMoS was prepared by the following method: Na2MoO4·2H2O, thiourea, and FeCl3·6H2O were mixed evenly and then subjected to a hydrothermal reaction to obtain the precursor FeMoS.
6. The Fe according to claim 5 0 The method for preparing FeMoS composite material is characterized by, The mass ratio of Na2MoO4·2H2O, thiourea, and FeCl3·6H2O is 2~4:2~4:3~5.
7. The Fe according to claim 5 0 The method for preparing FeMoS composite material is characterized by, The ratio of the total mass of Na2MoO4·2H2O, thiourea, and FeCl3·6H2O to water is 10~12 g: 50~70 mL.
8. The Fe according to claim 5 0 The method for preparing FeMoS composite material is characterized by, The hydrothermal reaction temperature is 160~200℃, and the hydrothermal reaction time is 20~24 h.
9. A Fe 0 The application of FeMoS composite materials is characterized by... Used as a catalyst with photocatalytic reduction capabilities.
10. The Fe according to claim 9 0 The application of FeMoS composite materials is characterized by... It is used for photocatalytic reduction and degradation of perfluorinated and polyfluorinated alkyl compounds in water.
Citation Information
Patent Citations
Nano zero-valent iron composite material with superstrong reducibility and photocatalytic performance
CN111097449A
Nanometer zero-valent iron / graphite carbon nitride photocatalytic material as well as preparation method and application thereof