A highly efficient supported catalyst and its preparation method
By using amino and thiol-functionalized mesoporous silica supports, stepwise immobilization of organotin and organobismuth active components is achieved, solving the problems of difficult catalyst separation and recovery and insufficient fixation of active components in existing technologies, thereby improving the stability and catalytic efficiency of the catalyst.
Patent Information
- Application Number
- CN202611512735.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing organometallic catalysts suffer from problems such as difficulty in separating and recovering homogeneous catalysts, insufficient ability to immobilize active metal components, and difficulty in simultaneously and stably immobilizing tin and bismuth bimetallic catalytic components.
Mesoporous silica carriers were modified with amino and thiol groups. After removing the template agent by solvent extraction, they were immobilized stepwise with organotin and organobismuth active components. The immobilization was achieved by coordination or chemical interaction between amino and thiol groups and the metal center.
It improves the stability of organotin and organobismuth active components and the cycle stability of the catalyst, reduces the residual metal components in the product, and is suitable for heterogeneous catalytic reactions.
Smart Images

Figure CN123102418A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chemical catalysis technology, specifically relating to a highly efficient supported catalyst and its preparation method, and particularly to a method for obtaining a heterogeneous supported catalyst with high stability of active components by modifying a mesoporous silica support with amino and mercapto bifunctionalization and loading organotin and organobismuth active components in a stepwise immobilization manner. Background Technology
[0002] Organotin compounds (such as dibutyltin dilaurate) and organobismuth compounds (such as bismuth octanoate and bismuth isononanoate) are both commonly used Lewis acid catalysts, exhibiting good catalytic activity in reactions such as polyurethane synthesis, esterification, and transesterification. Organotin catalysts are characterized by high catalytic efficiency and wide applicability; however, because they typically exist in a homogeneous form in the reaction system, catalyst separation after the reaction is difficult, and controlling residual metal elements remains is a challenge. Organobismuth catalysts, due to their relatively low toxicity, are considered an important supplement to organotin catalytic systems.
[0003] To improve catalyst recyclability and reduce the risk of active metal components entering the product system, researchers have recently explored loading organometallic catalysts onto solid supports to form heterogeneous catalysts. Commonly used supports include polymer supports, metal oxide supports, and mesoporous silica materials. Among these, mesoporous silica materials, due to their high specific surface area, regular pore structure, and abundant surface silanol groups, can be modified with silane coupling agents to introduce different functional groups, thus showing great application potential in catalyst immobilization.
[0004] In existing technologies, coupling agents such as aminosilanes and mercaptosilanes are typically used to functionalize mesoporous silica, and then the active components are immobilized through coordination or chemical interactions between the functional groups and the metal centers. However, existing methods still have the following problems:
[0005] (1) The single functional site has limited ability to fix metal components. During the liquid phase reaction, the active components may desorb or migrate, affecting the long-term stability of the catalyst.
[0006] (2) When two different metal catalytic components are simultaneously loaded on the same support, traditional impregnation or blending methods are difficult to control the fixed order and spatial distribution of the two active components, which may lead to mutual influence of active sites and reduce catalytic performance.
[0007] (3) Some existing studies mainly focus on the preparation of powder catalysts, while there is still a lack of research on supported catalysts that simultaneously meet the requirements of stable fixation of active components and particulate application.
[0008] Therefore, developing a method for preparing a supported catalyst that can utilize multifunctional anchoring points to achieve stepwise fixation of organotin and organobismuth active components, while taking into account catalytic activity, stability, and the requirements for particulate applications, has practical application value. Summary of the Invention
[0009] The purpose of this invention is to provide a highly efficient supported catalyst and its preparation method. This invention aims to solve the problems of existing organometallic catalysts: the difficulty in separating and recovering homogeneous catalysts, and the potential presence of metal residues in the products; the insufficient ability to immobilize active metal components when a single functional site is loaded; and the difficulty in separately positioning and immobilizing different active components when tin and bismuth bimetallic catalytic components are loaded simultaneously.
[0010] To achieve the above objectives, the present invention adopts the following technical solution:
[0011] This invention provides a method for preparing a highly efficient supported catalyst, comprising the following steps:
[0012] Step (1) Remove the template agent from the mesoporous silica by solvent extraction, and pre-hydrolyze the aminosilane and mercaptosilane in an aqueous organic solvent. Then react with the mesoporous silica to make the silanol group formed by pre-hydrolysis condense with the silanol group on the surface of the support, thereby obtaining a bifunctional mesoporous silica support with amino and mercapto functional sites on the surface.
[0013] In the above process, solvent extraction to remove the template agent is to obtain open channels and exposed surface silanol groups in preparation for subsequent silane grafting. The pre-hydrolyzed aminosilane can undergo a condensation reaction with the silanol groups on the support surface, thereby introducing amino functional groups into the support surface.
[0014] Step (2) The organotin catalyst is added to the bifunctionalized mesoporous silica support and fixed in an anhydrous organic solvent. The molar amount of tin in the organotin is controlled to be 40%-60% of the molar amount of mercapto in the support. The organotin components are fixed on the support surface through coordination or chemical interaction between amino groups, mercapto groups and tin centers, while retaining some mercapto sites to obtain the intermediate Cat-Sn.
[0015] In this process, the tin center in the organotin compound is fixed to the amino and thiol groups on the surface of the support through coordination or chemical interaction, resulting in the intermediate Cat-Sn, which is a support for organotin active components.
[0016] Step (3) The Cat-Sn is dispersed in an organic solvent, and an organic bismuth precursor and a condensing agent are added to react, so that the organic bismuth component is fixed on the surface of the support through coordination with the thiol group on the support surface or other chemical interactions. After the reaction is completed, the support is washed to obtain a support simultaneously loaded with organic tin component and organic bismuth component.
[0017] In the above process, the addition of the condensing agent helps to promote a more stable binding state between the organobismuth precursor and the functional sites on the support surface, so that the organobismuth component is stably fixed on the support and spatially adjacent to the already immobilized organotin component; however, this invention is not limited to a specific mechanism. The role of the condensing agent is to promote the activation of the carboxylic acid ligand in the organobismuth carboxylate and increase the contact probability between the bismuth center and the sulfur-containing electron donor sites on the support surface, thereby enhancing the stable binding of the organobismuth component on the support surface.
[0018] Step (4) The support simultaneously loaded with organotin and organobismuth components is dried, shaped and sieved to obtain a highly efficient supported catalyst.
[0019] Preferably, in step (1), the mesoporous silica is SBA-15.
[0020] Preferably, in step (1), the solvent extraction conditions are: reflux and stirring at 70-80°C for 12-24 hours in an ethanol-concentrated hydrochloric acid mixture, and repeated extraction 1-2 times; the ethanol-concentrated hydrochloric acid mixture is obtained by mixing 1g of carrier with 100mL of ethanol and 5mL of 37% concentrated hydrochloric acid.
[0021] Preferably, in step (1), the aminosilane is 3-aminopropyltrimethoxysilane or 3-aminopropyltriethoxysilane; the mercaptosilane is selected from one or more of 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane or 3-mercaptopropylmethyldimethoxysilane.
[0022] Preferably, in step (1), the pre-hydrolysis conditions of aminosilane and mercaptosilane are as follows: aminosilane, mercaptosilane, water and organic solvent are mixed and stirred at 20-40°C for 0.5-2 hours, wherein the molar ratio of water to the total molar amount of aminosilane and mercaptosilane is 1:1-3:1; the reaction temperature of the mesoporous silica support with the pre-hydrolyzed silane component is 80-100°C and the reaction time is 2-3 hours; the fixed reaction temperature of the amino and mercapto bifunctionalized mesoporous silica support with the organotin catalyst is 60-80°C and the fixed reaction time is 4-5 hours.
[0023] Preferably, in step (2), the organotin catalyst is dibutyltin dilaurate; and the solvent for the organotin fixation reaction is limonene.
[0024] Preferably, in step (3), the organic bismuth precursor is selected from one or more of bismuth octoate, bismuth isononanoate, bismuth neodecanoate, bismuth naphthenate, and bismuth 2-ethylhexanoate.
[0025] Preferably, in step (3), the condensing agent is N,N'-dicyclohexylcarbodiimide (DCC), the stirring reaction is carried out at room temperature for 24 hours, and the washing is performed 3-5 times.
[0026] Preferably, in step (4), the vacuum drying conditions are: vacuum drying temperature of 55-65℃, vacuum drying time of 10-14h, and sieve mesh of 20-40 mesh.
[0027] Preferably, the amino density of the amination support is 0.2-2.0 mmol / g; the Sn loading in the support catalyst is 0.1-10 wt%; the thiol density of the thiol support is 0.5-3.0 mmol / g; the Bi loading is 0.05-5 wt%; and the Sn:Bi molar ratio is 10:1-1:2.
[0028] It should be noted that the fixation of the organobismuth component in this invention does not solely rely on physical adsorption. Due to the presence of electron-donating sulfur atoms on the surface of the mercaptosilane-modified support, their lone pairs of electrons can coordinate with the Bi centers. Simultaneously, the carboxylate group in the organobismuth carboxylate can participate in regulating the coordination environment of the metal center, enabling the bismuth component to form a stable bonded state on the support surface. The stability of bismuth during recycling can be evaluated using ICP leaching experiments.
[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. This invention uses aminosilane and mercaptosilane to bifunctionalize mesoporous silica, constructing multiple types of metal binding sites on the carrier surface, providing different modes of action for the subsequent fixation of tin and bismuth active components, and improving the fixation stability of active components.
[0031] 2. This invention employs a stepwise immobilization method, first tin and then bismuth, to fix different active metal components in a predetermined order. This helps reduce the competitive adsorption effects generated during the simultaneous loading of the two metal components. Compared to simultaneous impregnation loading, this invention controls the tin component to preferentially occupy some thiol binding sites, and then utilizes the remaining functional sites to fix the bismuth component, thus providing relatively independent immobilization environments for different active metal centers.
[0032] 3. By controlling the amount of organotin added, this invention enables some thiol groups to participate in the fixation of tin components, while retaining some functional sites for the binding of bismuth components, which is beneficial to improving the stable loading effect of different active components in the tin-bismuth composite catalyst.
[0033] 4. The catalyst obtained by this invention is dried, shaped and sieved to form particulate material, which facilitates its subsequent application in fixed bed or other heterogeneous catalytic devices.
[0034] 5. Catalytic performance testing and metal content detection can further evaluate the catalyst activity and stability, indicating that the catalyst has the potential to reduce the migration of metal components during the catalytic process. Attached Figure Description
[0035] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0036] Figure 1 This is the infrared spectrum of the unmodified porous material SBA-15 of the present invention;
[0037] Figure 2 This is the infrared spectrum of the supported catalyst obtained in Example 1 of the present invention. Detailed Implementation
[0038] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0039] Unless otherwise specified, all reagents used in the embodiments of this invention are commercially available products.
[0040] The Sn and Bi loadings in the catalyst were measured using inductively coupled plasma optical emission spectrometry (ICP-OES); the elemental chemical state of the catalyst surface was analyzed using X-ray photoelectron spectroscopy (XPS); and the catalyst structure was characterized using Fourier transform infrared spectroscopy (FTIR).
[0041] Example 1
[0042] This embodiment discloses a method for preparing a supported catalyst, including the following steps:
[0043] Step (1) Take 10g of mesoporous silica SBA-15 and add it to the ethanol-concentrated hydrochloric acid mixture for template extraction. The following steps were performed: Ethanol dosage: 100 mL / g carrier; Concentrated hydrochloric acid: 5 mL (37 wt%); The mixture was refluxed and stirred at 70-80℃ for 12-24 h, and the extraction was repeated 1-2 times; Subsequently, 3 mL of 3-aminopropyltriethoxysilane (APTES) and 4.8 mL of 3-mercaptopropyltrimethoxysilane (MPTMS) were added to a mixed solvent consisting of 120 mL of limonene and 30 mL of ethanol, followed by the addition of deionized water to achieve a 1:1 molar ratio of water to APTES and MPTMS. The mixture was stirred at room temperature for 0.5 h to allow partial hydrolysis of the silanes. Then, the extracted SBA-15 was added, and the mixture was refluxed at 100℃ for 3 h under nitrogen protection to allow the silanol groups formed by pre-hydrolysis to condense with the silanol groups on the surface of SBA-15; After the reaction, the mixture was washed three times with limonene and ethanol, and then vacuum dried at 80℃ for 6 h to obtain an amino and mercapto bifunctionalized mesoporous silica carrier.
[0044] Step (2) The above bifunctionalized mesoporous silica support was added to 80 mL of limonene, and then 0.8 g of dibutyltin dilaurate (DBTDL) was added. The mixture was stirred at 80 °C for 4 h. After the reaction was completed, the mixture was filtered and washed 4 times with alternating limonene and ethanol to obtain the intermediate Cat-Sn of the supported organotin component.
[0045] Step (3) Co-immobilization of organobismuth components: 3g Cat-Sn was dispersed in 50mL dichloromethane, and 0.3g bismuth octanoate and 0.5g N,N'-dicyclohexylcarbodiimide (DCC) were added sequentially. The mixture was continuously magnetically stirred at room temperature for 24h. After the reaction was completed, the solid was collected by filtration and washed 5 times with dichloromethane to obtain a support simultaneously loaded with organotin and organobismuth components.
[0046] Step (4) Post-processing and molding: The support simultaneously loaded with organotin and organobismuth components is transferred to a vacuum drying oven and dried at 60°C for 12 hours. The dried catalyst powder is pressed into tablets under a pressure of 10 MPa, then crushed and sieved to collect 20-mesh particles, thus obtaining the target support catalyst, denoted as Cat-SnBi-1.
[0047] Catalytic performance evaluation: 10g of Cat-SnBi-1 catalyst particles were packed into a tubular supported reactor. Diphenylmethane diisocyanate (MDI) and polyether polyol with a number average molecular weight of 2000 Mn were mixed uniformly at 45±2℃ in an equimolar ratio. Cat-SnBi-1 containing 0.1% of the mass of the polyether polyol with supported organotin and organobismuth was added. The NCO value of the outlet material was measured periodically and the conversion rate was calculated. At the same time, product samples were collected for Sn and Bi content detection. After the reaction was completed, the supported catalyst was recovered by filtration and reused for the catalytic synthesis of polyurethane.
[0048] Figure 1 The infrared spectrum of the unmodified SBA-15 is shown. Figure 2 The infrared spectrum of the supported catalyst obtained in Example 1 is shown. Figure 2 and Figure 1 In comparison, at 2927cm -1 and 2857cm -1 A distinct -CH2- stretching vibration absorption peak appeared nearby, along with a peak at 1572 cm⁻¹. -1 Absorption peaks attributable to the NH bending vibration were observed nearby, indicating that the aminosilane had been successfully modified onto the support surface. Specifically, Figure 1 It has no SH characteristic absorption. Figure 2 At 2550cm -1 No obvious free thiol (SH) stretching vibration peaks were observed nearby. Combined with subsequent ICP test results, it can be inferred that some thiol sites participated in the metal component immobilization process. The ICP test results and cycle stability experiments indicate that the organotin and organobismuth components are stably immobilized on the support surface through coordination or chemical interactions. At 1709 cm⁻¹... -1 The absorption peak observed at 1599 cm⁻¹ may be related to organic carboxylic acid groups, indicating that the organobismuth carboxylate precursor participated in the loading process. -1 and 1410cm -1 The absorption peaks appearing nearby are attributed to carboxylate (COO) groups. - The asymmetric and symmetric stretching vibrations of the instrument have a wavenumber difference (Δν) of approximately 189 cm. -1 The results indicate that the carboxylate group may participate in coordination with the metal center. Combined with the above infrared spectral characteristics, this suggests that there may be coordination interactions or other chemical interactions between the organotin and organobismuth components and the support, which is beneficial to improving the immobilization stability of the active components on the support surface.
[0049] Example 2
[0050] The difference between this embodiment and Example 1 is the organotin fixation temperature. Specifically, the DBTDL fixation reaction temperature was adjusted to 60°C, while the other conditions remained the same as in Example 1. The resulting catalyst was Cat-SnBi-2.
[0051] Example 3
[0052] The difference between this embodiment and Embodiment 1 is that stannous octoate is used instead of DBTDL.
[0053] Specifically: Add 0.8 g of stannous octoate and react in limonene at 80 °C for 4 h, following the same steps. The resulting catalyst is Cat-SnBi-3.
[0054] Example 4
[0055] The difference between this embodiment and Embodiment 1 is that the organic bismuth precursor is different.
[0056] Bismuth isononanoate 0.35g was used instead of bismuth octanoate, with the remaining steps remaining the same. The resulting catalyst was Cat-SnBi-4.
[0057] Comparative Example 1
[0058] Compared with Example 1, Comparative Example 1 only supported an organotin catalyst.
[0059] Preparation process: Cat-Sn was prepared according to steps (1) and (2) of Example 1. The organic bismuth loading step was not performed.
[0060] Comparative Example 2
[0061] Compared with Example 1, Comparative Example 2 only supported an organic bismuth catalyst.
[0062] The bifunctionalized carrier from Example 1 was used. Bismuth octanoate 0.3 g and DCC 0.5 g were added directly, without Sn immobilization. This yielded Cat-Bi.
[0063] Comparative Example 3
[0064] Simulates the traditional homogeneous catalyst usage method. DBTDL and bismuth octoate are directly added to the MDI / polyether system. Concentrations: DBTDL: 500 ppm; Bismuth octoate: 300 ppm.
[0065] Comparative Example 4
[0066] Compared with Example 1, Comparative Example 4 did not add a condensing agent during the fixation treatment of the organobismuth precursor after the preparation of Cat-Sn: Cat-Sn was dispersed in dichloromethane, and the same amount of organobismuth precursor as in Example 1 was added but DCC was not added. The remaining operating conditions (stirring time, number of washings, drying and molding) were the same as in Example 1, and the catalyst Cat-SnBi-C4 was obtained; the catalytic evaluation was carried out according to the method of Example 1.
[0067] Comparative Example 5
[0068] Compared with Example 1, Comparative Example 5 only underwent amino-modification of the carrier and then loaded with organotin and organobismuth. Specifically, step (1) carrier pretreatment and functionalization modification: 10g of mesoporous silica SBA-15 was added to an ethanol-concentrated hydrochloric acid mixture (1g of carrier was mixed with 100mL of ethanol + 5mL of 37% concentrated hydrochloric acid), and refluxed and stirred at 70-80℃ for 12-24 hours. The extraction was repeated 1-2 times. 5mL of 3-aminopropyltriethoxysilane was added to a mixed solvent consisting of 120mL of limonene and 30mL of ethanol, and then deionized water was added to make the molar ratio of water to 3-aminopropyltriethoxysilane 5:1. The mixture was stirred at room temperature for 0.5h for pre-hydrolysis. Subsequently, the extracted SBA-15 was added, and under nitrogen protection, the mixture was refluxed and stirred at 100℃ for 3h to allow the silanol groups formed by pre-hydrolysis to undergo a condensation reaction with the silanol groups on the surface of SBA-15. After the reaction was completed, the product was cooled to room temperature and washed three times with limonene and ethanol by centrifugation. It was then dried under vacuum at 80°C for 6 hours to obtain an aminated mesoporous silica support. The organotin fixation, organobismuth fixation, post-treatment and molding were the same as in Example 1 to obtain the catalyst Cat-SnBi-C5. The catalytic performance evaluation was exactly the same as in Example 1.
[0069] Comparative Example 6
[0070] Compared with Example 1, Comparative Example 6 only underwent mercapto modification of the carrier before loading organotin and organobismuth. Specifically, step (1) carrier pretreatment and functionalization modification: 10g of mesoporous silica SBA-15 was added to an ethanol-concentrated hydrochloric acid mixture (1g of carrier was mixed with 100 mL of ethanol and 5 mL of 37% concentrated hydrochloric acid), and refluxed and stirred at 70-80℃ for 12-24 hours. The extraction was repeated 1-2 times. 8mL of 3-mercaptopropyltrimethoxysilane was added to a mixed solvent consisting of 120mL of limonene and 30mL of ethanol, and then deionized water was added to make the molar ratio of water to 3-mercaptopropyltrimethoxysilane 5:1. The mixture was stirred at room temperature for 0.5h for pre-hydrolysis. Subsequently, the extracted SBA-15 was added, and under nitrogen protection, the mixture was refluxed and stirred at 100℃ for 3h to allow the silanol groups formed by pre-hydrolysis to undergo a condensation reaction with the silanol groups on the surface of SBA-15. After the reaction was completed, the product was cooled to room temperature and washed three times with limonene and ethanol by centrifugation. It was then dried under vacuum at 80°C for 6 hours to obtain a thiolized mesoporous silica support. The organotin fixation, organobismuth fixation, post-treatment and molding were the same as in Example 1 to obtain the catalyst Cat-SnBi-C6. The catalytic performance evaluation was exactly the same as in Example 1.
[0071] To evaluate the compositional characteristics, stability of active components, and catalytic performance of the supported catalyst obtained in this invention, metal loading analysis, metal leaching tests, and catalytic reaction performance tests were performed on the prepared catalysts. Specifically, the metal loading test was used to evaluate the actual loading of Sn and Bi active components in the catalysts obtained in different embodiments; the metal leaching test was used to evaluate the migration behavior of active components during the liquid-phase reaction; and the catalytic performance test was used to evaluate the catalytic efficiency and recycling stability of the catalyst for the polyurethane synthesis reaction. The Sn and Bi loading in the catalyst was measured using inductively coupled plasma optical emission spectrometry (ICP-OES); the amount of metal elements dissolved during catalyst recycling was detected using ICP-OES; and the NCO conversion rate during the polyurethane reaction was determined using di-n-butylamine titration.
[0072] Table 1 Catalyst composition and metal loading
[0073]
[0074] Test method: The prepared catalyst sample was subjected to acid digestion treatment, and the Sn and Bi element contents were detected by ICP-OES. The metal loading was calculated based on the catalyst mass.
[0075] Table 2 Metal leaching test during liquid phase reaction process
[0076]
[0077] Test conditions: MDI / polyether polyol = 1:1, catalyst dosage 0.1wt%, premix at 45±2°C, filter and separate the catalyst after 2 hours of reaction, and conduct ICP-OES detection on the reaction product.
[0078] Table 3 Comparison of catalytic performance of typical catalysts
[0079] Table 3 is mainly used to evaluate the short-period recycling performance of the catalyst, and Table 4 further evaluates the catalytic activity retention and metal residue during the long-period recycling process.
[0080]
[0081] Test method: The di-n-butylamine titration method is used to determine the content of residual isocyanate groups in the reaction system, and the NCO conversion rate is calculated. During the cycle test, the catalyst is recovered after each reaction, washed and dried, and then reused for the catalytic reaction.
[0082] Detection and characterization methods and performance evaluation: The catalysts or reaction systems obtained in the above examples and comparative examples are systematically evaluated, with the methods as follows.
[0083] (1) Polyurethane conversion rate: The di-n-butylamine titration method is used to determine the NCO value, and the isocyanate conversion rate is calculated accordingly.
[0084] (2) Product formation rate and molecular weight distribution: The product formation rate (g / h) is counted after 50 cycles of use; the product molecular weight distribution Mw / Mn is determined by gel permeation chromatography (GPC). The sample is dissolved with tetrahydrofuran (THF) or dimethylformamide (DMF) as the solvent, filtered and then injected. The conditions such as mobile phase and column temperature are set conventionally in the art, and calibration is performed using polystyrene standards.
[0085] (3) Metal residue and leaching: The polyurethane product or the carrier after 50 cycles of use is pretreated by microwave digestion, and then the Sn and Bi contents are determined by ICP-MS; the active component retention rate is calculated as the ratio of the mass of the metal element in the carrier after recycling to the mass of the corresponding metal element in the initial carrier; the limit of detection (LOD) and limit of quantitation (LOQ) are determined according to laboratory methodological validation; when the measured value is lower than LOD, it is recorded as <LOD. In this experiment: LOD(Sn)=0.01ppm, LOD(Bi)=0.01ppm.
[0086] It should be noted that Table 2 is used to evaluate the liquid-phase metal leaching behavior during the use of the catalyst, and Table 4 is used to evaluate the metal residue in the product after long-term recycling, and the two have different test objects and evaluation purposes.
[0087] The test results are shown in Tables 4 to 5:
[0088] Table 4. Test results of catalytic performance and metal residue in products after long-term cyclic use.
[0089]
[0090] Table 5 Comparison of Cyclic Stability and Product Molecular Weight Distribution of Different Catalytic Systems
[0091]
[0092] As shown in Tables 4 and 5, the bimetallic supported catalysts obtained in Examples 1-4 of this invention all exhibited high catalytic activity in the polyurethane synthesis reaction. Even after multiple cycles, the catalysts maintained high catalytic activity, while the residual amounts of tin and bismuth in the products were significantly reduced. Compared with homogeneous catalysts, the catalysts of this invention can reduce the residual Sn and Bi in the reaction products and improve the cycling stability of the active components.
[0093] As shown in Comparative Examples 1-3, when only a single metal component is loaded or a homogeneous catalytic approach is used, the catalytic performance, metal residue, and cycle stability cannot simultaneously meet the requirements. This invention employs a synergistic Sn and Bi bimetallic approach and a bifunctionalized support immobilization strategy to enable the catalyst to possess both catalytic activity and stability. While the homogeneous catalytic system can maintain a certain level of catalytic activity and product molecular weight distribution, the lack of immobilization of the active component leads to difficulties in catalyst separation and metal residue issues.
[0094] As can be seen from Comparative Examples 5-6, compared with single-amino or thiolized carriers, bifunctionalized carriers can provide two different types of action sites, amino and thiol, giving tin and bismuth components a more stable fixation environment, which is beneficial to improving the stable loading effect of organotin and organobismuth active components.
[0095] Therefore, the supported catalyst and its preparation method provided by the present invention, by constructing a mesoporous silica support with amino and thiol bifunctionalization and adopting a stepwise immobilization strategy of tin first and then bismuth, achieves the synergistic immobilization of organotin and organobismuth active components based on different functional sites, effectively improving the problems of insufficient stability of traditional single-site loading and mutual influence when multiple metal components are loaded at the same time, and improving the cycle stability of the catalyst.
[0096] The above description is merely a preferred embodiment of the present invention and does not limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention, which is defined by the claims.
Claims
1. A method for preparing a highly efficient supported catalyst, characterized in that, Includes the following steps: Step (1) Remove the template agent from the mesoporous silica using solvent extraction, pre-hydrolyze the aminosilane and mercaptosilane in an aqueous organic solvent, and then reflux them with the mesoporous silica to allow the silanol groups formed by the pre-hydrolysis to condense with the silanol groups on the surface of the mesoporous silica, thereby obtaining an amino and mercapto bifunctional mesoporous silica carrier. Step (2) The organotin catalyst is added to the bifunctionalized mesoporous silica support and fixed in an anhydrous organic solvent. The molar amount of tin in the organotin is controlled to be 40%-60% of the molar amount of mercapto in the support. The organotin components are fixed on the support surface through coordination or chemical interaction between amino groups, mercapto groups and tin centers, while retaining some mercapto sites to obtain the intermediate Cat-Sn. Step (3) The Cat-Sn is dispersed in an organic solvent, and an organic bismuth precursor and a condensing agent are added to react, so that the organic bismuth component is fixed on the surface of the support through coordination with the thiol group on the support surface or other chemical interactions. After the reaction is completed, the support is washed to obtain a support simultaneously loaded with organic tin component and organic bismuth component. Step (4) The support simultaneously loaded with organotin and organobismuth components is dried, shaped and sieved to obtain a highly efficient supported catalyst.
2. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (1), the mesoporous silica is SBA-15.
3. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (1), the solvent extraction conditions are as follows: in the ethanol-concentrated hydrochloric acid mixture, reflux and stir at 70-80℃ for 12-24 hours, and repeat the extraction 1-2 times; the ethanol-concentrated hydrochloric acid mixture is obtained by mixing 1g of carrier with 100mL of ethanol and 5mL of 37% concentrated hydrochloric acid.
4. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (1), the aminosilane is 3-aminopropyltrimethoxysilane or 3-aminopropyltriethoxysilane; the mercaptosilane is selected from one or more of 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane or 3-mercaptopropylmethyldimethoxysilane.
5. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (1), the pre-hydrolysis conditions of the aminosilane and mercaptosilane are as follows: the aminosilane, mercaptosilane, water and organic solvent are mixed and stirred at 20-40℃ for 0.5-2h, wherein the molar ratio of water to the total molar amount of aminosilane and mercaptosilane is 1:1-3:1; the reaction temperature of the mesoporous silica support and the pre-hydrolyzed silane component is 80-100℃ and the reaction time is 2-3h.
6. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (2), the organotin catalyst is dibutyltin dilaurate; the solvent for the organotin fixation reaction is limonene; the fixation reaction temperature of the amino and mercapto bifunctionalized mesoporous silica support and the organotin catalyst is 60-80℃, and the fixation reaction time is 4-5h.
7. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (3), the organic solvent is dichloromethane; the organic bismuth precursor is selected from one or more of bismuth octoate, bismuth isononanoate, bismuth neodecanoate, bismuth naphthenate, and bismuth 2-ethylhexanoate.
8. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, The condensing agent mentioned in step (3) is N,N'-dicyclohexylcarbodiimide (DCC). The stirring reaction is carried out at room temperature for 24 hours, and the washing is performed 3-5 times.
9. The method for preparing the highly efficient supported catalyst according to claim 1, characterized in that, In step (4), the vacuum drying conditions are: vacuum drying temperature of 55-65℃, vacuum drying time of 10-14h, and sieve mesh of 20-40 mesh.
10. A highly efficient supported catalyst, characterized in that, The catalyst comprises: a bifunctionalized mesoporous silica support having amino and mercapto groups introduced by aminosilane and mercaptosilane on its surface; an organotin component immobilized on the support, the organotin component being fixed through coordination or chemical interaction between amino groups, mercapto groups and tin centers; and an organobismuth component immobilized on the support, the organobismuth component being fixed through coordination or chemical interaction between mercapto sites and bismuth centers; wherein: the Sn loading in the catalyst is 0.1-10 wt%, the Bi loading is 0.05-5 wt%, and the Sn to Bi molar ratio is 10:1-1:2.