A method for decomposing degraded photovoltaic modules using an additive-assisted hydrothermal method
By using an additive-assisted hydrothermal method to decompose degraded photovoltaic modules, the problems of low recovery rate, high energy consumption, and serious pollution in existing technologies have been solved, achieving efficient and environmentally friendly separation and recycling of photovoltaic module materials.
Patent Information
- Application Number
- CN202611600702.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for recycling decommissioned photovoltaic modules suffer from low recovery rates with physical methods, high energy consumption and severe pollution with pyrolysis methods, and low efficiency and the use of toxic solvents with chemical methods, making it difficult to achieve efficient and environmentally friendly material separation and recycling.
The auxiliary hydrothermal method is adopted to decompose retired photovoltaic modules under mild conditions through two hydrothermal reactions. The first reaction removes the backsheet, and the second reaction uses additives such as hydrogen peroxide, sodium bicarbonate, ozone or hypochlorous acid to oxidize and degrade the EVA film in an aqueous environment, thereby achieving the separation of glass and solar cells.
It achieves efficient and environmentally friendly separation of photovoltaic module materials, obtaining high-purity glass and silicon wafers, reducing energy consumption, avoiding the release of toxic gases, and simplifying the subsequent recycling process.
Smart Images

Figure CN123102724A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic module recycling technology, specifically relating to a method for decomposing retired photovoltaic modules using an additive-assisted hydrothermal method. Background Technology
[0002] Photovoltaic modules typically have a lifespan of 25 to 30 years. Retired photovoltaic modules possess both resource value and environmental risks. On one hand, they contain valuable materials such as high-purity silicon and silver; on the other hand, improper disposal can lead to environmental threats from the ethylene-vinyl acetate copolymer (EVA) film and the organic polymers in the backsheet. Therefore, developing efficient and clean recycling technologies for retired photovoltaic modules is of great significance.
[0003] Currently, recycling technologies for retired photovoltaic modules are mainly divided into three categories: physical methods, pyrolysis methods, and chemical methods, but all have significant shortcomings. Physical methods achieve material separation through mechanical crushing and screening. While they can recover over 85% of the glass, the recovery rate for high-value materials such as silicon and silver is less than 30%, and residual organic polymers can contaminate subsequent purification processes, severely restricting the high-value recovery of resources. Pyrolysis decomposes EVA in an inert atmosphere at 400℃~500℃ to recover silicon wafers, but faces three major challenges: high energy consumption, secondary pollution, and material damage. Processing one ton of modules requires 800kWh~1000kWh of electricity; pyrolysis of fluorinated backsheets releases toxic HF gas; and the high-temperature environment causes a microcrack rate of over 15% in silicon wafers, reducing their reuse value. Chemical methods, while achieving a 90% silicon recovery rate by dissolving EVA in organic solvents at 80℃, suffer from the carcinogenicity of trichloroethylene, high wastewater treatment costs, and inefficient reaction times exceeding 24 hours. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a method for the hydrothermal decomposition of retired photovoltaic modules using additives. This invention proposes a method for the hydrothermal decomposition of retired photovoltaic modules using additives, employing water as the reaction medium to achieve the stepwise decomposition of the backsheet and EVA film under mild conditions, ultimately obtaining high-purity glass and silicon wafers—valuable materials—to achieve the green and efficient recycling of retired photovoltaic modules.
[0005] A method for decomposing degraded photovoltaic modules using an additive-assisted hydrothermal method includes the following steps: After removing the frames and junction boxes from the retired photovoltaic modules, the photovoltaic panel laminate is obtained; The photovoltaic panel laminate is subjected to a first hydrothermal reaction, which is carried out in an aqueous environment at 180℃~300℃ for 1h~5h to hydrolyze and separate the backsheet, resulting in solid-liquid separation and obtaining the photovoltaic panel. The photovoltaic panel undergoes a second hydrothermal reaction at 180°C–300°C for 1–5 hours in an aqueous environment containing additives. This causes the EVA film to oxidize and degrade, separating the glass from the solar cells, yielding glass and solar cells. The additive concentration in the aqueous environment is 8%–10% by mass. Under the influence of the additives, the EVA film undergoes oxidative degradation, its molecular chains break, and the adhesion between the EVA film and the glass and solar cells disappears. After the reaction, solid-liquid separation is performed to obtain the separated glass, solar cells, and decomposition products. The glass can be directly recycled or used as a glass raw material. The solar cells can be further used to extract high-value materials such as silicon and silver. Since the backsheet contains sulfur (F), to avoid the influence of F on the solar cells during the reaction, a two-stage hydrothermal reaction is chosen. The first hydrothermal reaction is only used to remove the backsheet. During this process, the EVA film protects the solar cells, allowing them to be reused for recycling. In this invention, the first hydrothermal reaction occurs only in an aqueous environment, causing hydrothermal decomposition of the backsheet, breaking the organic polymer molecular chains, and the decomposition products dissolving in water or forming small solid particles. After the reaction is complete, solid-liquid separation is performed. The separated solid is the photovoltaic panel with the backsheet removed, i.e., the glass-EVA-cell-EVA stack. The filtrate contains backsheet decomposition products, which can be further recycled.
[0006] The additive is at least one of hydrogen peroxide, sodium bicarbonate, ozone, and hypochlorous acid. Sodium bicarbonate is an alkaline substance, and alkaline substances have a positive effect on the separation of photovoltaic panels.
[0007] The additives must possess oxidizing capabilities and be able to promote the breakage of EVA molecular chains under hydrothermal conditions of 180℃~300℃ without damaging the solar cells. Hydrogen peroxide, ozone, and hypochlorous acid are all oxidizing substances that can generate reactive oxygen species under hydrothermal reaction conditions, attacking the weak bonds in the EVA molecular chains and accelerating its degradation. Although sodium bicarbonate is not a strong oxidant, the alkaline environment it provides can promote the deacetylation reaction of EVA, altering the degradation pathway of EVA, weakening the intermolecular forces, and thus assisting in the degradation and separation of EVA.
[0008] The backsheet material is TPT / TPE; TPT is a three-layer composite structure of polyvinyl fluoride-polyester-polyvinyl fluoride; wherein, polyvinyl fluoride is abbreviated as PVF, polyester as PET, and polyvinyl fluoride as PVF. TPE is a two-layer structure of polyester-polyolefin / thermoplastic elastomer; polyolefin / thermoplastic elastomer is abbreviated as TPE.
[0009] In another preferred embodiment, the additive is hydrogen peroxide. If the additive is not chosen appropriately, such as a strong acid, strong alkali, or a corrosive oxidant, it may corrode the solar cell under hydrothermal high-temperature conditions, reducing its recycling value. Furthermore, solid-liquid separation is required after the reaction, and the residue of the additive should not burden subsequent separation and purification. The decomposition products of hydrogen peroxide are only water and oxygen, providing an ideal chemical environment for the oxidative chain scission of EVA. There is sufficient oxygen to participate in the reaction, and highly reactive free radicals initiate chain degradation. This allows hydrogen peroxide to effectively degrade the EVA film at a concentration of 8% to 10% by mass, balancing economy and processing efficiency, and without introducing additional impurity ions or corrosive substances into the system, making it the gentlest for the solar cell. In addition, hydrogen peroxide decomposes into water and oxygen, sodium bicarbonate decomposes into sodium carbonate and water, and ozone and hypochlorous acid also mainly decompose into harmless substances. These additives do not form difficult-to-clean residue layers on the surface of solid products such as glass and solar cells after the reaction.
[0010] In another preferred embodiment, the pressure of the hydrothermal reaction is 1 MPa to 8 MPa.
[0011] In another preferred embodiment, in the first hydrothermal reaction, the amount of water used is sufficient to immerse the photovoltaic panel.
[0012] In another preferred embodiment, after solid-liquid separation in the first hydrothermal reaction, the filtrate is concentrated and recovered for use as a chemical raw material or for resource utilization.
[0013] In another preferred embodiment, the photovoltaic panel laminate consists of glass, EVA film, solar cell, EVA film and backsheet from top to bottom.
[0014] In another preferred embodiment, the temperatures of the first hydrothermal reaction and the second hydrothermal reaction are both 230°C to 260°C.
[0015] In another preferred embodiment, the temperatures of both the first and second hydrothermal reactions are 240°C.
[0016] Compared with the prior art, the present invention has the following beneficial effects: This invention employs a two-stage hydrothermal reaction at 180℃~300℃ to achieve the gentle decomposition of the backsheet and EVA film. Since the backsheet contains sulfur (F), to avoid the influence of F on the solar cells during the reaction, a two-stage hydrothermal reaction is chosen. The first hydrothermal reaction is used only to remove the backsheet; at this stage, the EVA film protects the solar cells, allowing them to be recycled. The second hydrothermal reaction is then carried out. The second hydrothermal reaction primarily uses water as the reaction medium, with an additive concentration of 8%~10% by mass. Under the action of the additive, the EVA film undergoes oxidative degradation, molecular chain breakage, and the adhesion between it and the glass and solar cells disappears. After the reaction, solid-liquid separation is performed to obtain the separated glass, solar cells, and decomposition products. The method of this invention does not generate toxic waste liquid throughout the process, the closed reaction does not release toxic HF gas, avoiding secondary pollution, and shortens the reaction time to 1~5 hours.
[0017] This invention removes the backsheet and EVA film sequentially through a step-by-step decomposition process. The separated glass and solar cell surfaces are free of organic residues, and the obtained silicon and silver high-value elements are relatively pure, making them easy to directly recycle and reuse. Attached Figure Description
[0018] Figure 1 Images of different samples: a is the backsheet, b is EVA, and c is the photovoltaic panel.
[0019] Figure 2 Images are from a hydrothermal decomposition experiment of the backplate. a is the backplate, b is the dissolved substance, and c is the undissolved substance.
[0020] Figure 3 The figure shows the effect of temperature on the decomposition of the backplate. a is 210℃, b is 220℃, c is 230℃, and d is 240℃.
[0021] Figure 4 The figure shows the effect of time on the decomposition of the backplate. a represents heating at 240℃ for 3 hours, and b represents heating at 240℃ for 4 hours.
[0022] Figure 5 The results of the effect of adding hydrogen peroxide on the decomposition of the backplate are shown in Figure a. a represents heating at 230℃ for 4 hours, and b represents heating at 230℃ for 4 hours.
[0023] Figure 6 The graph shows the backplate decomposition rate at temperatures ranging from 210℃ to 240℃.
[0024] Figure 7 The figure shows the effect of hydrogen peroxide concentration on EVA decomposition. a represents 0% hydrogen peroxide by mass, b represents 0.5% hydrogen peroxide by mass, c represents 1% hydrogen peroxide by mass, and d represents 1.5% hydrogen peroxide by mass.
[0025] Figure 8 The graph shows the effect of temperature on EVA decomposition, where a is 200℃, b is 210℃, c is 220℃, d is 230℃, and e is 240℃.
[0026] Figure 9 The graph shows the effect of time on EVA decomposition, where a represents 2 hours, b represents 3 hours, and c represents 4 hours.
[0027] Figure 10 The figure shows the effect of hydrogen peroxide concentration on the decomposition of photovoltaic panels. a represents hydrogen peroxide with a mass percentage concentration of 4%, b represents hydrogen peroxide with a mass percentage concentration of 6%, c represents hydrogen peroxide with a mass percentage concentration of 8%, and d represents hydrogen peroxide with a mass percentage concentration of 9%.
[0028] Figure 11 The graph shows the effect of temperature on the decomposition of photovoltaic panels. a is 240℃, b is 250℃, c is 260℃, and d is 270℃. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0030] Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0031] To address the issues of incomplete physical separation and low recovery rates of high-value materials, this invention achieves selective chemical decomposition of the backsheet and EVA film through hydrothermal reaction, rather than mechanical crushing, thereby obtaining high-purity glass and silicon wafers and improving the value of resource recycling.
[0032] To address the issues of high energy consumption, high temperature, and the release of toxic gases during the pyrolysis of fluorine-containing backsheets, this invention controls the reaction temperature at 180℃~300℃, significantly reducing energy consumption and avoiding thermal damage to silicon wafers. At the same time, the hydrothermal reaction is carried out in a closed liquid phase, which does not produce HF toxic gas and is environmentally friendly.
[0033] To address the problems of high cost and low efficiency in chemical methods that use toxic organic solvents such as trichloroethylene and waste liquid treatment, this invention uses water as the main reaction medium and adds only a small amount of green additives. The reaction time is greatly shortened, no toxic waste liquid is generated, and a highly efficient and environmentally friendly decomposition effect is achieved.
[0034] To address the problem that EVA films are difficult to decompose directly under pure hydrothermal conditions, this invention introduces hydrogen peroxide, sodium bicarbonate, ozone, and hypochlorous acid as green additives. Through the oxidation or catalytic effect of the additives, the EVA molecular chains are broken, thereby achieving efficient dissociation of the EVA film.
[0035] The following is a detailed explanation of a method for decomposing degraded photovoltaic modules using an additive-assisted hydrothermal method.
[0036] The experimental materials required in this embodiment are: a non-transparent double-sided composite backsheet, cut into rectangles and weighing 0.97 grams; a transparent EVA film, weighing 0.4 grams; and an unassembled single photovoltaic panel. Due to the limitations of the reactor size, the single photovoltaic panel was divided into three pieces using a glass cutter for ease of experimentation, as shown below. Figure 1 As shown.
[0037] The three samples were placed in a polytetrafluoroethylene (PTFE) liner, and the experiment was conducted in a high-temperature and high-pressure reactor. To ensure experimental safety and meet hydrothermal requirements, the maximum pressure of the reactor had to be no less than 22 MPa and no more than 30 MPa. 100 ml of water was injected into the liner to stabilize the water filling rate at 50%. The filling rate was defined as the proportion of solvent to the internal volume of the reactor. This filling rate was the most conducive to maintaining this requirement. A stable filling rate is beneficial for the analysis and comparison of experimental data and meets the requirements of industrialization.
[0038] Then, place the inner liner into the stainless steel reactor, tighten the reactor, and place it in the electric heating drying oven. Set the temperature and time, and the drying oven will follow the prescribed reaction procedure. After reaching the set temperature, stabilize at that temperature. After the set time is reached, open the oven to cool down. After the temperature has cooled to room temperature, use a vacuum filter to separate and filter the reaction solution, and observe the phenomenon.
[0039] To illustrate the impact of different raw materials and processing parameters, this embodiment designed four variables. Based on different experimental materials, the temperature and time of the hydrothermal reaction were set to explore the degree of dissolution and decomposition of the photovoltaic module under different variables, and to find the optimal temperature and time for decomposition. Specific parameter designs are shown in Table 1.
[0040] Table 1 Parameter Settings project Experimental variables unit Experimental materials Backsheet, EVA film, photovoltaic panel — reaction temperature 200、210、220、230、240、250、260、270 ℃ reaction time 1、2、3、4 h hydrogen peroxide mass percentage concentration 0、0.5、1、1.5 % Note: — indicates that this item is not included.
[0041] Qualitative analysis of the separation and recycling situation was conducted through comparative observation. The separation of various components of the solar panel and the integrity of crystalline silicon were compared and observed under different reaction conditions. The experimental effects were evaluated, and the most suitable reaction temperature and reaction time for separating waste photovoltaic modules in the hydrothermal system were selected.
[0042] 1. Backplate hydrothermal decomposition.
[0043] 1) Effect of temperature on backplate decomposition: Results Figure 2 As shown and Figure 3 As shown, four temperatures were selected: 210℃, 220℃, 230℃, and 240℃. Based on the weight of the filtered material after the reaction and the analysis of undissolved matter deposited at the bottom of the reactor, the weight of the filtered material after 210℃ was 0.44g, after 220℃ it was 0.18g, after 230℃ it was 0.15g, and after 240℃ it was 0.06g. It can be seen that the degree of decomposition of the backplate is better as the heating temperature increases, with 240℃ being the optimal temperature.
[0044] 2) The effect of time on backplate disintegration: such as Figure 4 As shown, at 240℃, there are many undissolved substances at the bottom of the reactor after 3 hours, and fewer undissolved substances remain after 4 hours. As time increases, the reaction on the back plate becomes more intense.
[0045] 3) The effect of hydrogen peroxide on backplate decomposition: such as Figure 5 As shown, after adding hydrogen peroxide, the backplate adheres to the bottom of the reactor after the reaction. In contrast, the backplate without hydrogen peroxide dissolves better.
[0046] The above experiments show that when the hydrothermal temperature is set between 210℃ and 240℃, the main experimental phenomenon is that solid powder is suspended in the reactor, and undissolved solid matter generally adheres to the bottom. At 240℃, the longer the reaction time, the higher the decomposition rate of the backplate. The experimental time was determined to be 4 hours, and four temperatures (210℃, 220℃, 230℃, and 240℃) were selected. Analysis of the weight of the filtered material after the reaction and the undissolved matter deposited at the bottom of the reactor was performed. Figure 6 As shown, the decomposition rate of the backplate increases significantly from 210℃ to 220℃, reaching its maximum at 240℃. This indicates that the reaction is most effective at 240℃. Furthermore, when 1% hydrogen peroxide was added, the decomposition rate was found to be comparable to that without hydrogen peroxide in the hydrothermal decomposition experiment.
[0047] 2. Hydrothermal decomposition of EVA film.
[0048] 1) The effect of hydrogen peroxide concentration on EVA decomposition like Figure 7 As shown, without the addition of hydrogen peroxide, EVA changes from transparent to yellow, expands but does not decompose. As the concentration of hydrogen peroxide increases, the degree of EVA decomposition deepens. Based on the observation, the effect of 1% hydrogen peroxide by mass percentage is similar to that of 1.5% hydrogen peroxide by mass percentage.
[0049] 2) The effect of temperature on EVA decomposition.
[0050] like Figure 8As shown, EVA does not completely decompose at temperatures below 210℃, but completely decomposes at temperatures of 210℃ and above, resulting in the filtration of a dark brown substance from the reaction solution.
[0051] 3) The effect of time on EVA decomposition.
[0052] like Figure 9 As shown, when heated for 2 hours, EVA decomposes into small pieces, but remains white. After 3 hours, it does not dissolve and turns yellow. After 4 hours, it dissolves completely.
[0053] The experimental results show that when the time is set to 4 hours, the hydrogen peroxide concentration remains constant at 1%, and the heating temperature is 200℃, the reactor contains a significant amount of pale yellow undissolved matter, which is viscous, and the filtered material is yellowish-white. At 210℃, the reaction solution is dark brown, the filtered material is black, and there is no undissolved matter. At 220℃, the filtered material is black. At 230℃, the reaction solution contains a small amount of clearly visible yellow undissolved matter, and the filtered material is dark brown. At 240℃, brown slag-like matter is present in the solution. Based on these observations, the hydrothermal treatment effect of the EVA membrane is best at 4 hours, a hydrogen peroxide concentration of 1%, and temperatures of 210℃ and 220℃.
[0054] The optimal temperature was set at 220℃, and the hydrogen peroxide concentration was 1% by mass. The experimental phenomena were observed at 2h, 3h, and 4h. The color of the reaction solution gradually deepened with time. At 2h, the filtered material was yellowish-white, at 3h it was yellowish-brown, and at 4h it turned dark brown.
[0055] The temperature was 220℃, and the reaction time was 4 hours. The mass percentage concentration of hydrogen peroxide was changed to 0%, 0.5%, 1%, and 1.5%. When the mass percentage concentration of hydrogen peroxide was less than 1%, undissolved solids were present after the reaction. When the mass percentage concentration of hydrogen peroxide was 1.5%, there were no flaky undissolved substances in the solution, but small pieces of gelatinous matter were present in the filtrate. In summary, when there is only EVA film in the reactor and no other substances, a hydrogen peroxide mass percentage concentration of 1% is optimal.
[0056] 3. Hydrothermal decomposition of photovoltaic panels.
[0057] Based on the hydrothermal treatment experimental results of the backsheet and EVA in sections 1 and 2 above, a hydrothermal treatment experiment of the complete photovoltaic panel was conducted.
[0058] The most critical aspect of hydrothermal treatment of photovoltaic panels is the softening and dissolution of EVA, reducing its adhesive properties. Two layers of EVA in the photovoltaic panel require reaction: one layer between the solar cell and the glass (hereinafter referred to as the upper EVA layer); and another layer between the backsheet and the solar cell (hereinafter referred to as the lower EVA layer). Using 100 ml of water, the experiment involved varying the temperature, time, and amount of hydrogen peroxide. Based on analysis, the approximate optimal separation parameter range was determined. The results of reacting at 240℃ for 4 hours under different hydrogen peroxide concentrations are shown below. Figure 10 As shown. From Figure 10 As can be seen from 'a', using hydrogen peroxide with a mass percentage concentration of 4%, the glass detached, the backing plate and lower layer of EVA remained undissolved, while most of the upper layer of EVA dissolved; from Figure 10 As can be seen from b, using hydrogen peroxide with a mass percentage concentration of 6%, the backing plate and lower layer of EVA dissolved, while most of the upper layer of EVA remained undissolved; from Figure 10 As can be seen from 'c', using 8% hydrogen peroxide, the upper EVA layer basically dissolved, while the backing and lower EVA layers remained undissolved; from Figure 10 As shown in 'd', using hydrogen peroxide with a mass percentage concentration of 9%, the EVA and backsheet are basically dissolved, and the crystalline silicon crumbles. From the above analysis, it can be seen that the hydrogen peroxide concentration plays a crucial role in the separation of photovoltaic panels. When the hydrogen peroxide concentration is insufficient, EVA is difficult to decompose; when the mass percentage concentration of hydrogen peroxide reaches 8% or higher, most of the EVA decomposes, and the exposed crystalline silicon can be seen. Therefore, when processing photovoltaic panels, the hydrogen peroxide mass percentage concentration should be above 8%.
[0059] The results of the reaction at different hydrothermal temperatures for 4 hours, and with the addition of hydrogen peroxide at a mass percentage concentration of 10%, are shown in Figure 11. Figure 11 As shown in Figure 'a', at 240℃, the backsheet and lower EVA layer are basically dissolved, while the upper EVA layer is partially dissolved; at 250℃, the glass does not detach, the upper EVA layer does not dissolve, and the backsheet and lower EVA layer partially dissolve; at 260℃, the glass detaches, the upper EVA layer partially dissolves, and the backsheet and lower EVA layer are basically dissolved; at 270℃, the glass detaches, the upper EVA layer does not dissolve, and the backsheet and lower EVA layer are mostly dissolved. From the above analysis, it can be concluded that the photovoltaic panel exhibits the best separation effect at 260℃, with the backsheet and lower EVA layer completely decomposing, the edges of the upper EVA layer completely dissolving, and bubbles appearing inside.
[0060] It should be noted that when numerical ranges are involved in this invention, it should be understood that the two endpoints of each numerical range, as well as any value between the two endpoints, can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described in this invention to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments, and all such changes and modifications fall within the scope of this invention.
[0061] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. If these modifications and variations fall within the scope of equivalents of this invention, then this invention also intends to include these modifications and variations.
Claims
1. A method for decomposing degraded photovoltaic modules using an additive-assisted hydrothermal method, characterized in that, Includes the following steps: After removing the frames and junction boxes from the retired photovoltaic modules, the photovoltaic panel laminate is obtained; The photovoltaic panel laminate is subjected to a first hydrothermal reaction, which is carried out in an aqueous environment at 180℃~300℃ for 1h~5h to hydrolyze and separate the backsheet, resulting in solid-liquid separation and obtaining the photovoltaic panel. The photovoltaic panel undergoes a second hydrothermal reaction at 180℃~300℃ for 1h~5h in an aqueous environment containing additives, causing oxidative degradation of the EVA film and separation of the glass and solar cell, yielding glass and solar cell. The mass percentage concentration of the additives in the aqueous environment is 8%~10%. The additive is hydrogen peroxide; The back panel is made of TPT / TPE; TPT is a three-layer composite structure of polyvinyl fluoride-polyester-polyvinyl fluoride; TPE is a two-layer structure of polyester-polyolefin / thermoplastic elastomer.
2. The method for decomposing decommissioned photovoltaic modules using an additive-assisted hydrothermal method according to claim 1, characterized in that, The pressure of the hydrothermal reaction is 1 MPa to 8 MPa.
3. The method for decomposing decommissioned photovoltaic modules using an additive-assisted hydrothermal method according to claim 1, characterized in that, In the first hydrothermal reaction, the amount of water used is enough to submerge the photovoltaic panel.
4. The method for decomposing decommissioned photovoltaic modules using an additive-assisted hydrothermal method according to claim 1, characterized in that, In the first hydrothermal reaction, after solid-liquid separation, the filtrate is concentrated and recovered.
5. The method for decomposing decommissioned photovoltaic modules using an additive-assisted hydrothermal method according to claim 1, characterized in that, The photovoltaic panel laminate consists of glass, EVA film, solar cell, EVA film and backsheet from top to bottom.
6. The method for decomposing decommissioned photovoltaic modules using an additive-assisted hydrothermal method according to claim 1, characterized in that, The temperatures of the first and second hydrothermal reactions are both 230℃~260℃.
7. The method for decomposing decommissioned photovoltaic modules using an additive-assisted hydrothermal method according to claim 6, characterized in that, The temperatures of both the first and second hydrothermal reactions are 240°C.