A continuous cold rolling production process and system for special steel strips for engineering structures
By mechanically marking the dwell time of the strip segment in the storage looper and adjusting the curvature compensation in stages, combined with the absorption tension of the looper rolls and the gas injection control in the annealing furnace, the problem of uneven strip shape and mechanical properties in the continuous cold rolling production line was solved, and the uniformity of the strip length direction and the quality stability of the strip were achieved.
Patent Information
- Application Number
- CN202611439254.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
When producing special strip steel for engineering structures in existing continuous cold rolling production lines, the strip steel in the storage loop undergoes plastic bending deformation and tension fluctuations due to uneven residence time, resulting in uneven strip shape and mechanical properties along the length direction of the finished strip steel.
By mechanically marking the dwell time of the strip segment in the storage looper, adjusting the roll gap reduction of the multi-roll straightener in stages for curvature compensation, setting up liftable looper rolls between each rolling mill stand to absorb tension fluctuations, controlling the gas injection temperature in the annealing furnace, and setting up electric field shielding and non-contact distance measurement winding during oiling, the uniformity of strip shape and mechanical properties can be achieved.
It eliminates residual curvature defects in the storage loop, stabilizes the strip shape, suppresses tension fluctuations throughout the process, and achieves uniform performance and quality stability in the length direction of the strip.
Smart Images

Figure CN123102739A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal pressure processing technology, and in particular to a continuous cold rolling process and system for producing steel strips for engineering structures. Background Technology
[0002] Specialized steel strips for engineering structures are key load-bearing materials in bridges, buildings, and construction machinery. Their shape quality, uniformity of mechanical properties, and surface quality directly affect the load-bearing reliability and service life of downstream components. With the continuous improvement of the quality requirements for steel strips in high-end equipment manufacturing, traditional intermittent cold rolling production methods can no longer meet the demands in terms of production efficiency and quality stability. Continuous cold rolling production lines have become the mainstream method for producing specialized steel strips for engineering structures due to their high production efficiency and stable product quality.
[0003] Existing continuous cold rolling production lines typically employ a process flow of feeding coiled strip steel blanks, uncoiling, descaling, multi-stand continuous rolling, online annealing, oiling, and recoiling. To achieve continuous production without shutting down the machine, a storage loop is set up between the uncoiling section and the rolling section. During the coil change, the strip steel stored in the storage loop is used to maintain continuous downstream production.
[0004] The above methods can basically meet the quality requirements in the production of conventional specification strip steel, but they have the following disadvantages in the continuous production of special strip steel for engineering structures:
[0005] First, when thick strip steel for engineering projects is stored in the existing storage loop in a catenary state, it is prone to plastic bending deformation under the combined effect of its own gravity and the curvature of the loop. Moreover, the residence time of the strip steel in the storage loop varies with the frequency of coil changing and the production rhythm. The strip segment with a longer residence time has a greater degree of plastic bending deformation, while the strip segment with a shorter residence time has a smaller degree of plastic bending deformation. This results in a periodic defect of uneven curvature residue along the length of the strip steel. Subsequent rolling processes cannot completely eliminate this curvature residue, and the final finished strip steel exhibits periodic fluctuations in plate shape along the length.
[0006] Secondly, in a continuous cold rolling production line, tension exists in multiple sections, including the uncoiling section, the storage looper outlet, the curvature compensation section, the descaling section, the sections between rolling mill stands, the annealing furnace inlet and inside the furnace, the oiling section, and the coiling section. The tension in each section fluctuates due to factors such as equipment transmission errors, changes in strip cross-section, and rolling force fluctuations. Tension fluctuations in the upstream section are transmitted to the downstream section through the strip and accumulate segment by segment, causing the actual reduction of the strip in each pass during the rolling process to fluctuate periodically along the length direction. This leads to uneven work hardening and recrystallization, and ultimately, periodic differences in the yield strength and tensile strength of the finished strip along the length direction.
[0007] Based on this, a continuous cold rolling process and system for special strip steel for engineering structures is designed to suppress the accumulation of tension fluctuations throughout the entire process. This has important engineering significance for improving the shape quality and mechanical property uniformity of special strip steel for engineering structures. Summary of the Invention
[0008] To solve one of the above-mentioned technical problems, the present invention adopts the following technical solution: a continuous cold rolling production process for special steel strips for engineering structures, comprising the following steps:
[0009] S1. Steel strip blank feeding and waste material separation treatment;
[0010] S2. Mechanical tracking and marking of storage and belt segment dwell time in storage loop: The steel belt after the material head is cut off is pulled into the downstream storage loop and stored in the form of a catenary. At the same time, the steel belt entering the storage loop is mechanically marked segment by segment along the length direction, and the dwell time of each marked segment in the storage loop is tracked.
[0011] S3. Segment-by-segment reverse bending curvature compensation based on residence time classification: When the marked belt segment leaves the storage loop, the roll gap reduction of the multi-roll straightener unit on the exit side is adjusted according to the residence time of the belt segment in the storage loop, and a larger reverse bending amount is applied to the belt segment with a longer residence time.
[0012] S4. Variable incident angle descaling and surface transverse roughness uniformity: The steel strip after curvature compensation is sent into the descaling process to remove the surface oxide scale. During the descaling process, the incident angle of the descaling medium relative to each point in the width direction of the steel strip is kept equal.
[0013] S5. Multi-pass calendering and thinning, and tension fluctuation absorption between the stand and the machine frame are achieved through looper control;
[0014] S6. Heat treatment and uniform temperature control inside the furnace;
[0015] S7. Edge electric field shielding oil coating and surface film homogenization;
[0016] S8. True outer diameter tracking winding and interlayer pressure control: The oiled steel strip is pulled to the winding machine for non-stop winding. During the winding process, the true outer diameter of the steel coil is directly measured by non-contact distance measurement, and the winding tension is reduced synchronously according to the true outer diameter.
[0017] Preferably, the segmented mechanical marking in S2 is achieved by stamping semi-circular indentations on the side edge of the steel strip. The spacing between adjacent indentations is fixed. Photoelectric sensors installed at the inlet and outlet of the storage loop record the time when the indentation enters and leaves the storage loop, respectively. The difference between the two times is the dwell time of the strip segment corresponding to the indentation in the storage loop.
[0018] Preferably, the curvature compensation is performed according to the following steps:
[0019] The first step is that when the photoelectric sensor at the outlet of the storage looper detects the marked indentation, it compares the dwell time of the belt segment corresponding to the indentation with the three preset dwell time intervals to determine the curvature compensation level to which the belt segment belongs.
[0020] The second step is that when the head of the belt segment reaches the first roller of the multi-roller straightener unit, each pressing drive mechanism corresponding to the gear position presses down synchronously according to the preset roller gap value, and the upper roller and the lower roller form a reverse bending curvature corresponding to the gear position.
[0021] The third step involves the steel strip winding alternately around nine rollers, undergoing alternating reverse bending.
[0022] Fourth step: When the tail of the belt segment leaves the last roller of the multi-roller straightener unit, the drive mechanism is pressed down to return to the initial waiting position, waiting for the next marked belt segment to arrive;
[0023] The fifth step involves installing a contact curvature detection plate at the outlet of the multi-roll straightener unit. The lower surface of the steel strip passes against the curvature detection plate, and the residual curvature of the steel strip is determined by the uniformity of the pressure distribution on the pressure sensors arranged along the running direction of the steel strip on the curvature detection plate. The more uniform the pressure distribution, the smaller the residual curvature. When the pressure distribution difference exceeds the set threshold, it is determined that the residual curvature of the strip segment exceeds the set range. The position of the strip segment with residual curvature exceeding the set range is recorded in the control system, and this position record is synchronously tracked to the downstream process along with the progress of the steel strip.
[0024] Preferably, the three dwell time intervals in S3 correspond to the roll gap reduction of each gear. The first gear corresponds to the shortest dwell time interval, with the smallest roll gap reduction; the second gear corresponds to the middle dwell time interval, with the roll gap reduction being 1.5 to 1.8 times that of the first gear; and the third gear corresponds to the longest dwell time interval, with the roll gap reduction being 2.2 to 2.6 times that of the first gear.
[0025] Preferably, the variable incident angle descaling is performed according to the following steps:
[0026] The first step is to measure the actual width of the steel strip before it enters the descaling process using a width measuring instrument, and then transmit the width signal to the control system of the adjustable spray beam.
[0027] The second step is to control the position of each nozzle in the width direction and adjust the swing angle synchronously so that the high-pressure water jets of all nozzles within the width range of the steel strip have the same incident angle relative to the surface of the steel strip directly below them, and the nozzles outside the width range of the steel strip stop spraying.
[0028] The third step involves high-pressure water being ejected from the nozzle and impacting the surface of the steel strip. Under the mechanical impact of the high-pressure water, the oxide scale is peeled off from the steel strip substrate, and the peeled oxide scale falls into the water collection tank below and is discharged.
[0029] The fourth step is to remove residual moisture from the surface of the descaled steel strip, and then set up a surface roughness tester at the rear to collect surface roughness values at five measuring points at equal intervals along the width of the steel strip.
[0030] The fifth step involves sending the steel strip to the downstream cold rolling mill after surface roughness testing.
[0031] Preferably, the loose roller type tension fluctuation absorption is performed according to the following steps:
[0032] The first step is that after the steel strip comes out of the upstream mill, it hangs down and falls on the looper roll. The end continues to enter the downstream mill. Under the action of the constant pressure cylinder, the looper roll lifts up the steel strip to form the lifting looper section.
[0033] The second step is that when the steel strip tension transmitted from the upstream mill increases, the increased steel strip tension increases the downward pressure generated by the tension compensation looper roll, which overcomes the lifting force of the constant pressure cylinder and presses the looper roll vertically downward, increasing the length of the steel strip supporting the looper section.
[0034] The third step is that when the steel strip tension transmitted from the upstream mill decreases, the downward pressure generated by the steel strip tension on the looper roll decreases, and the lifting force of the constant pressure cylinder pushes the tension looper roll vertically upward, reducing the length of the steel strip in the lifting looper section and releasing the stored steel strip length.
[0035] The fourth step is to monitor the vertical displacement of the looper roll in real time by the displacement sensor. When the displacement exceeds the set upper and lower limits, the speed regulation system of the upstream mill will finely adjust the rolling speed of the upstream mill to return the looper roll to the set position.
[0036] The fifth step is to set the air supply pressure of the cylinder for each tension compensation looper roller according to the set tension value between the frames.
[0037] Preferably, the cold rolling mill in S5 is a five-stand continuous rolling mill, with loop rolls configured between each pair of adjacent stands. The cylinder air supply pressure of the five loop rolls increases progressively from the first stand to the fifth stand, and the air supply pressure difference between two adjacent loop rolls is equal.
[0038] Preferably, the electric field shielding in S7 is achieved by setting a grounded metal shielding plate on each side of the steel strip during operation, controlling the shielding plate surface to be parallel to the side of the steel strip, the distance between the edge of the shielding plate near the edge of the steel strip and the edge of the steel strip is 5 to 15 mm, and the length of the shielding plate along the running direction of the steel strip is greater than the effective width of the electrostatic oiling electrode along the running direction of the steel strip.
[0039] Preferably, the S6 bell-type annealing furnace includes a heating section, a heat preservation section and a cooling section. The protective gas injection operation is carried out between each pair of adjacent furnace rollers (or furnace plates) in the heating section, heat preservation section and cooling section. Each group consists of a spray beam that spans the width of the furnace. The upper surface of the spray beam has two rows of spray holes with valves.
[0040] The furnace gas injection-type temperature uniformity control in the width direction is performed according to the following steps:
[0041] The first step is to heat the annealing furnace to the working temperature. The furnace circulation fan draws the protective gas from the furnace and sends it to the spray beams of the heating section and the heat preservation section through the gas supply pipeline. After the gas is pressurized inside each gas supply chamber of the spray beam, it is sprayed upward from the spray holes with valves on the upper surface. The sprayed protective gas impacts the lower surface of the steel strip and then diffuses along the width and length of the steel strip, causing the protective gas in the furnace to form a convection circulation.
[0042] The second step is that when the steel strip is running in the heating section, the protective gas sprayed by the spray beam forms an impact jet on the lower surface of the steel strip. The impact jet destroys the gas boundary layer on the lower surface of the steel strip, increases the convective heat transfer coefficient between the lower surface of the steel strip and the furnace gas, and accelerates the heat exchange between the lower surface of the steel strip and the furnace gas.
[0043] Third, when the steel strip is running in the insulation section, the insulation section spray beam continuously supplies circulating protective gas into the furnace to maintain the convection circulation in the furnace. The gas supply pressure of the insulation section spray beam is lower than that of the heating section spray beam.
[0044] The fourth step is to supply air to each air supply chamber independently and adjust the air supply pressure separately. The air supply pressure of the air supply chambers in the cooling section is adjusted according to the temperature distribution in the width direction of the steel strip.
[0045] Fifth, protective gas, cooled by the furnace cooler, is introduced into the spray beam in the cooling section. The temperature of the sprayed protective gas is lower than that of the steel strip. When the protective gas impacts the lower surface of the steel strip, it dissipates the heat of the steel strip through forced convection. The diameter of the nozzle with valve at the edge of the air supply chamber of the spray beam in the cooling section is smaller than that of the nozzle with valve at the middle, so that the gas flow rate at the edge is lower than that at the middle.
[0046] Preferably, in step S6, the heating section heats the steel strip to above the recrystallization temperature, the heat preservation section keeps the steel strip within this temperature range until recrystallization is complete, and the cooling section cools the steel strip to the set discharge temperature. Temperature measuring points are set at the edge and middle of the steel strip along the width direction at the outlet of the cooling section. When the temperature difference between the edge and the middle exceeds the set threshold, the opening of the proportional valve on the nozzle of the air supply chamber at the edge is adjusted according to the direction of the temperature difference to change the air supply flow rate at the edge: when the edge temperature is lower than the middle temperature, the air supply flow rate at the edge is reduced, and when the edge temperature is higher than the middle temperature, the air supply flow rate at the edge is increased.
[0047] The present invention also provides a continuous cold rolling production system for steel strips for engineering structures, the system being used to implement the process method described above.
[0048] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0049] 1. By mechanically tracking and marking the dwell time of each strip segment in the storage loop of the existing production line, and adjusting the roll gap reduction of the curvature compensation unit according to the dwell time, a larger reverse bending amount is applied to the strip segment with a longer dwell time, thus eliminating the time-varying curvature residual defects of thick strip steel caused by uneven dwell time in the storage loop, and the finished strip steel has a uniform and stable shape along the length direction.
[0050] 2. By setting up adjustable tension compensation loop rolls between each rolling mill stand, the vertical displacement of the loop rolls passively absorbs the tension fluctuations transmitted from the upstream stand, suppressing the gradual accumulation of tension fluctuations in multiple sections throughout the entire process. The actual reduction of the strip in each rolling pass is stable, the degree of work hardening and recrystallization are uniform, and the mechanical properties of the finished strip have no periodic differences along the length direction.
[0051] 3. By injecting protective gas between the furnace rollers (or furnace plates) in the annealing furnace and directing it downwards onto the strip, the heating and holding sections promote gas convection circulation within the furnace, while the cooling section utilizes low-temperature protective gas for forced convection cooling. By adjusting the gas flow rate in different areas along the width, uniform temperature control along the width of the strip is achieved, avoiding uneven microstructure and properties caused by temperature differences between the edges and the center.
[0052] 4. By setting ground electric field shielding on both sides of the strip during oiling, the edge effect of electrostatic oiling is suppressed, and the oil film thickness on the strip surface is uniform along the width direction, avoiding subsequent use problems caused by oil richness at the edges.
[0053] 5. By directly measuring the true outer diameter of the steel coil through non-contact distance measurement, and synchronously reducing the winding tension according to the true outer diameter, constant control of interlayer pressure is achieved during the winding process, avoiding strip adhesion caused by excessive interlayer pressure in the inner ring and loosening caused by insufficient interlayer pressure in the outer ring. Attached Figure Description
[0054] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. In all the drawings, similar elements or components are generally identified by similar reference numerals. In the drawings, the elements or components are not necessarily drawn to scale.
[0055] Figure 1 This is a schematic diagram of the force applied by the looper roll to the steel strip between two adjacent rolling mills according to the present invention.
[0056] Figure 2 This is a schematic diagram of the added structure inside an existing annealing furnace according to the present invention.
[0057] Figure 3 This is a partial structural schematic diagram of the arrangement of the nozzles in this invention.
[0058] Figure 4 This is a schematic diagram of the force application state structure of the auxiliary looper roller steel strip of the present invention.
[0059] In the diagram, 1. Upstream mill; 2. Downstream mill; 3. Loop roll; 4. Constant pressure cylinder; 5. Steel strip; 6. Heating section; 7. Insulation section; 8. Cooling section; 9. Furnace roll (or furnace plate); 10. Spray beam; 11. Spray hole; 12. Air supply chamber; 13. Frame; 14. Loop roll. Detailed Implementation
[0060] The embodiments of the technical solution of the present invention will now be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore merely examples and should not be used to limit the scope of protection of the present invention. The specific structure of the present invention is as follows: Figures 1-4 As shown in the image.
[0061] A continuous cold rolling production process for special steel strip for engineering structures includes the following steps: S1. Steel strip blank feeding and waste material diversion treatment: The coiled steel strip blank is hoisted to the uncoiler for uncoiling, and the head of the steel strip is pulled through the shearing station to cut off the irregular waste material. The cut waste material is introduced into a waste material collection line independent of the main line, and the main line steel strip continues to be conveyed downstream.
[0062] S2. Mechanical tracking and marking of storage and belt segment dwell time in storage loop: The steel belt after the material head is cut off is pulled into the downstream storage loop and stored in the form of a catenary. At the same time, the steel belt entering the storage loop is mechanically marked segment by segment along the length direction, and the dwell time of each marked segment in the storage loop is tracked.
[0063] S3. Segment-by-segment reverse bending curvature compensation based on residence time classification: When the marked belt segment leaves the storage loop, the roll gap reduction of the multi-roll straightener unit on the exit side is adjusted according to the residence time of the belt segment in the storage loop, and a larger reverse bending amount is applied to the belt segment with a longer residence time.
[0064] S4. Variable incident angle descaling and surface transverse roughness uniformity: The steel strip after curvature compensation is sent into the descaling process to remove the surface oxide scale. During the descaling process, the incident angle of the descaling medium relative to each point in the width direction of the steel strip is kept equal.
[0065] S5. Multi-pass rolling and thinning and tension fluctuation absorption through looper control between stands: The descaled steel strip is fed into the cold rolling mill for multi-pass rolling and thinning. Looper control is achieved by setting up liftable looper rolls between each stand. The tension fluctuation transmitted from the upstream stand is absorbed by using the tension compensation of the vertical displacement of the existing looper rolls.
[0066] S6. Heat treatment and uniform temperature control in the furnace: The rolled steel strip is sent into the annealing furnace for overall heat treatment. After being heated to the set temperature range and held at that temperature, the cooling is controlled. Protective gas is introduced into the lower surface of the steel strip in the furnace. The protective gas sprayed from the heating and holding sections impacts the lower surface of the steel strip and then diffuses along the furnace, promoting the convection circulation of the protective gas in the furnace. The cooling section uses protective gas with a temperature lower than that of the steel strip to perform forced convection cooling on the lower surface of the steel strip and adjusts the gas flow rate in different areas of the steel strip width direction.
[0067] S7. Edge electric field shielding oiling and surface film homogenization: The annealed steel strip is sent to the oiling process to form an anti-rust oil film on the surface of the steel strip. During the oiling process, electric field shielding is set on both sides of the steel strip.
[0068] S8. True outer diameter tracking winding and interlayer pressure control: The oiled steel strip is pulled to the winding machine for non-stop winding. During the winding process, the true outer diameter of the steel coil is directly measured by non-contact distance measurement, and the winding tension is reduced synchronously according to the true outer diameter.
[0069] Specifically, the starting point of the continuous cold rolling process for engineering structural steel strips in this solution is to solve the problems of time-varying curvature residual defects caused by uneven residence time of thick steel strips in the storage looper in existing continuous cold rolling production lines, as well as the problem of uneven mechanical properties caused by the cumulative tension fluctuations in multiple sections throughout the process. This solution performs traceable curvature compensation based on the residence time of the strip segment at the exit of the storage looper. Between each rolling stand, the existing looper roll structure, which is purely mechanical, passively absorbs tension fluctuations. In the annealing furnace, gas injection is used to achieve temperature uniformity in the width direction. In the oiling stage, the edge electric field shielding is used to suppress the edge effect of the oil film. In the winding stage, the interlayer pressure is kept constant by directly measuring the actual outer diameter. This forms a quality control chain from curvature compensation, tension control, temperature uniformity, oiling uniformity to constant winding pressure.
[0070] Building upon this foundation, the material storage function of the looper is further integrated with the traceability marking function for curvature residue. Marking detection is installed at the looper's inlet and outlet, and the dwell time of each strip segment is used as a direct input parameter for curvature compensation. This allows the looper to simultaneously possess the function of traceability marking for strip dwell time, providing accurate input data for curvature compensation. Simultaneously, a purely mechanical passive tension fluctuation absorption method replaces traditional speed-regulated tension control. In existing technologies, tension fluctuations between stands are typically suppressed by adjusting the rolling speed of the upstream mill. However, speed regulation response is lagging and can cause transient fluctuations in rolling force and thickness. This solution utilizes the vertically adjustable displacement of the existing looper rolls to passively absorb tension fluctuations. The response speed is determined by the mechanical inertia of the looper rolls, which is much faster than electrical speed regulation. Furthermore, the absorption process does not affect the stability of the rolling speed, fundamentally avoiding mutual interference between tension control and thickness control. It should be noted that the looper rolls are existing mature products and, in this application, are driven by existing constant-pressure cylinders for lifting and lowering.
[0071] Preferably, the segmented mechanical marking in S2 is achieved by stamping semi-circular indentations on the side edge of the steel strip. The spacing between adjacent indentations is fixed. Photoelectric sensors installed at the inlet and outlet of the storage loop record the time when the indentation enters and leaves the storage loop, respectively. The difference between the two times is the dwell time of the strip segment corresponding to the indentation in the storage loop.
[0072] Specifically, the mechanical tracking mark for the dwell time of the strip segment in this solution provides accurate and traceable input parameters for the subsequent curvature compensation process. It transforms the dwell time of the strip segment from a passive process parameter into an active control input. In terms of marking method, a semi-circular indentation is stamped on the side edge of the steel strip. The indentation is stamped on the side end face of the steel strip on both sides in the width direction. This part is usually removed as trimming allowance during subsequent shearing of the finished product. Even if the trimming is not done, the small indentation on the side edge does not affect the performance of the steel strip as an engineering structural material. In terms of detection method, a photoelectric sensor is used to align the path of the indentation with the side of the steel strip. When the indentation passes through the detection optical path of the photoelectric sensor, the contour of the side edge of the steel strip changes instantaneously. The photocurrent output by the photoelectric sensor generates a corresponding pulse. The moment of this pulse is recorded as the moment when the indentation passes through the detection point. Specifically, the photoelectric sensor at the inlet of the storage loop records the moment when the concave point enters the storage loop, and the photoelectric sensor at the outlet records the moment when the same concave point leaves the storage loop. The difference between the two moments is the dwell time of the strip corresponding to the concave point in the storage loop. Since the spacing between the concave points is fixed, each concave point corresponds to a steel strip of a certain length, and the correspondence between the dwell time and the strip is clear and unambiguous.
[0073] Building upon this, a method of marking strip segments by stamping indentations on the side edge of the steel strip has been further implemented, which does not affect the subsequent processing quality of the upper and lower surfaces of the steel strip. At the same time, non-contact time recording can be achieved by utilizing the changes in light signals when the indentations pass through the photoelectric sensor, avoiding scratches on the steel strip surface and wear on the detection wheel caused by contact marking detection.
[0074] Preferably, the multi-roller straightener unit in S3 adopts an existing nine-roller straightener, and the curvature compensation is performed according to the following steps:
[0075] The first step is that when the photoelectric sensor at the outlet of the storage looper detects the marked indentation, it compares the dwell time of the belt segment corresponding to the indentation with the three preset dwell time intervals to determine the curvature compensation level to which the belt segment belongs.
[0076] The second step is that when the head of the belt segment reaches the first roller of the multi-roller straightener unit, each pressing drive mechanism corresponding to the gear position presses down synchronously according to the preset roller gap value, and the upper roller and the lower roller form a reverse bending curvature corresponding to the gear position.
[0077] The third step involves the steel strip winding alternately around nine rollers, undergoing alternating reverse bending.
[0078] Fourth step: When the tail of the belt segment leaves the last roller of the multi-roller straightener unit, the drive mechanism is pressed down to return to the initial waiting position, waiting for the next marked belt segment to arrive;
[0079] The fifth step involves installing a contact curvature detection plate at the outlet of the multi-roll straightener unit. The lower surface of the steel strip passes against the curvature detection plate, and the residual curvature of the steel strip is determined by the uniformity of the pressure distribution on the pressure sensors arranged along the running direction of the steel strip on the curvature detection plate. The more uniform the pressure distribution, the smaller the residual curvature. When the pressure distribution difference exceeds the set threshold, it is determined that the residual curvature of the strip segment exceeds the set range. The position of the strip segment with residual curvature exceeding the set range is recorded in the control system, and this position record is synchronously tracked to the downstream process along with the progress of the steel strip.
[0080] Specifically, this solution is used to eliminate time-varying curvature residue caused by differences in residence time when thick steel strips are stored in a catenary configuration within a storage loop. When thick steel strips are stored in a storage loop, the weight of the strip itself causes bending stress in the catenary segment. When this bending stress exceeds the yield strength of the steel strip, plastic bending deformation occurs, and the degree of plastic deformation increases with the residence time. This process is similar to the creep behavior of metallic materials under constant stress; segments with longer residence times exhibit greater plastic bending deformation and larger residual curvature, while segments with shorter residence times exhibit less plastic bending deformation and smaller residual curvature.
[0081] This solution features a dedicated multi-roll straightening unit between the storage looper outlet and the descaling process. The roll gap reduction is adjusted in stages based on the belt segment dwell time, applying a larger reverse bending amount to segments with longer dwell times. The plastic deformation generated by the reverse bending offsets the residual curvature in the same direction within the storage looper. The alternating arrangement of the multi-rollers causes the steel strip to undergo multiple alternating reverse bending processes within the unit, with each bend having the opposite curvature direction, ultimately resulting in a uniform and near-zero residual curvature along the length of the steel strip. Furthermore, the dwell time of the belt segment within the storage looper is used as a direct input parameter for curvature compensation, enabling source-based compensation based on the cause of residual curvature. This solution uses dwell time as a direct cause of residual curvature for feedforward compensation. When the belt segment reaches the multi-roll straightening unit, the corresponding compensation amount is applied based on its dwell time. The timing of compensation precisely corresponds to the location of the defect, resulting in compensation accuracy far exceeding that of post-feedback correction.
[0082] Meanwhile, multi-level graded reduction can be used to replace continuous stepless adjustment, reducing the response speed requirements and control complexity of the reduction drive action. Curvature compensation of thick steel strips requires a large reduction amount and force. Continuous stepless adjustment requires the reduction drive action to continuously change the reduction amount in real time during the operation of the steel strip, which places extremely high demands on the response speed and control accuracy of the hydraulic system, resulting in high equipment investment and maintenance costs. This solution divides the residence time into three intervals, corresponding to three fixed reduction amounts. The reduction drive action only needs to switch between three fixed positions, which reduces the response speed requirement, simplifies control, and the three intervals cover the main distribution range of residence time in industrial production. The compensation effect meets the engineering requirements.
[0083] More importantly, the contact curvature detection step at the outlet of the multi-roller straightener unit monitors the compensation effect in real time, records the position of belt segments with residual curvature exceeding the set range, and tracks them downstream. This forms a dual guarantee with feedforward compensation as the main method and feedback detection as the auxiliary method, ensuring that the curvature compensation effect is stable and reliable.
[0084] Preferably, the three dwell time intervals in S3 correspond to the roll gap reduction of each gear. The first gear corresponds to the shortest dwell time interval, with the smallest roll gap reduction; the second gear corresponds to the middle dwell time interval, with the roll gap reduction being 1.5 to 1.8 times that of the first gear; and the third gear corresponds to the longest dwell time interval, with the roll gap reduction being 2.2 to 2.6 times that of the first gear.
[0085] Specifically, when thick steel strips are stored in a catenary state within the storage loop (a catenary state specifically refers to the curved shape formed by a chain or rope fixed at both ends, of uniform texture and flexible, naturally drooping under its own weight; in this storage loop, the steel strip enters from the loop entrance, droops naturally inside the loop, and is then pulled out from the loop exit. The suspended section of the steel strip within the loop is only subject to its own weight and tension at both ends, and its naturally drooping shape is a catenary state (or approximately a catenary)), it undergoes plastic deformation under constant bending stress. The degree of plastic deformation increases with the duration of residence, and the rate of increase is not linear, but rather exhibits a creep characteristic of being fast at first and then slowing down: in the initial stage of residence time, the plastic deformation increases rapidly with time, and when the residence time reaches a certain level, the rate of increase in plastic deformation gradually slows down and tends to stabilize. When the dwell time moves from the short interval to the middle interval, the increase in curvature residue is greater than the increase from 0 to the upper limit of the short interval. However, when moving from the middle interval to the long interval, the increase in curvature residue slows down. Therefore, the increasing ratio of curvature compensation reduction should match the nonlinear growth characteristics of curvature residue, rather than simply increasing proportionally to the dwell time interval.
[0086] This scheme sets the second-level reduction amount to 1.5 to 1.8 times that of the first level, and the third-level reduction amount to 2.2 to 2.6 times that of the first level. The increasing ratio of the reduction amount is greater than the increasing ratio of the residence time interval, and the increase from the second level to the third level is slightly greater than the increase from the first level to the second level. This ratio is determined based on the creep deformation characteristics of thick steel strips in commonly used steel grades in engineering structures (such as Q345, Q420, etc.) under the conditions of room temperature to 100℃ and catenary curvature radius of 5 to 15m.
[0087] Based on this, an unconventional design was further implemented, in which the incremental ratio of the reduction amount is greater than the incremental ratio of the residence time interval, matching the nonlinear growth characteristics of the creep curvature residue of thick steel strips. In the existing technology, the compensation for the plate shape usually assumes that the plate shape defect and the influencing factors are linearly related and adopts a linear compensation method. This scheme considers the nonlinear characteristics of the creep deformation of thick steel strips in the storage loop and adopts a graded compensation with a larger incremental ratio, resulting in higher matching accuracy between the compensation amount and the actual curvature residue. Meanwhile, the three reduction increments have engineering margins to accommodate the differences in residual curvature characteristics of steel strips under different materials, thicknesses, and looper curvature radii. The reduction can be adjusted and controlled as needed. Engineering structural steel strips cover a variety of materials and specifications. Different materials have different yield strengths and creep characteristics. Steel strips of different thicknesses have different bending stresses under the same catenary curvature. Different storage looper curvature radii also have different values. These factors will lead to differences in residual curvature characteristics. The proportional relationship of the three reduction increments in this solution adopts a range rather than a fixed value. When using it, the appropriate end value can be selected within the range according to the specific material and specifications, which has a wide range of applicability.
[0088] More importantly, the ratio of the three reduction amounts is matched with the structure of alternating bending of multiple rollers. The total compensation amount is several times that of a single bending compensation amount due to the multiple alternating reverse bending. Even if the absolute value of the single reduction amount is not large, the total compensation amount after multiple alternating bending is sufficient to offset the curvature residue of the thick steel strip, avoiding the steel strip surface indentation and roller wear caused by excessive reduction amount of a single roller.
[0089] Further explanation is needed: the aforementioned catenary state refers to the curved state formed by the steel strip being supported at both ends by the inlet and outlet rollers within the storage loop, with the middle section suspended, and naturally drooping under its own gravity. The middle section of the steel strip does not contact any idler rollers, and its curve shape is determined by the mechanical balance of the steel strip tension, the weight per unit length of the steel strip, and the loop span.
[0090] Preferably, the variable incident angle descaling is performed according to the following steps:
[0091] The first step is to measure the actual width of the steel strip before it enters the descaling process using a width measuring instrument, and then transmit the width signal to the control system of the adjustable spray beam.
[0092] The second step is to control the position of each nozzle in the width direction and adjust the swing angle synchronously so that the high-pressure water jets of all nozzles within the width range of the steel strip have the same incident angle relative to the surface of the steel strip directly below them, and the nozzles outside the width range of the steel strip stop spraying.
[0093] The third step involves high-pressure water being ejected from the nozzle and impacting the surface of the steel strip. Under the mechanical impact of the high-pressure water, the oxide scale is peeled off from the steel strip substrate, and the peeled oxide scale falls into the water collection tank below and is discharged.
[0094] The fourth step is to remove residual moisture from the surface of the descaled steel strip, and then set up a surface roughness detector at the rear to collect the surface roughness values of five measuring points at equal intervals along the width of the steel strip. When the roughness difference between adjacent measuring points exceeds the set threshold, it is fed back to the control system of the adjustable spray beam to correct the oscillation angle of the nozzle.
[0095] The fifth step involves sending the steel strip to the downstream cold rolling mill after surface roughness testing.
[0096] The descaling process described in S4 uses high-pressure water nozzles, each equipped with a separate switch, to spray along the width of the steel strip to achieve high-pressure water descaling. The descaling medium is high-pressure water.
[0097] Specifically, this solution uses spherical nozzles. The swing angle of each nozzle is adjusted (mechanically or manually) according to its position in the width direction, ensuring that the actual incident angle of the high-pressure water jet from all nozzles within the width of the steel strip is equal relative to the surface of the steel strip directly below. This solution achieves geometrically uniform control of the incident angle, enabling uniform descaling under the same pressure and flow rate. The equipment is simple and the effect is stable. Simultaneously, nozzles exceeding the width of the steel strip stop spraying, preventing direct impact of high-pressure water on the equipment frame and pit, thus avoiding equipment wear and energy waste. This solution controls the nozzles exceeding the bandwidth to stop spraying based on the steel strip width signal detected by the width measuring instrument, protecting the equipment and reducing energy consumption. A surface roughness detector at the descaling process exit monitors the descaling effect in real time. When the roughness difference between adjacent measuring points exceeds a set threshold, feedback is used to correct the swing angle of the corresponding nozzle, forming a feedforward adjustment of the incident angle and roughness feedback correction. This ensures that the descaling effect remains uniform and stable under conditions such as changes in steel strip width, nozzle wear, and water pressure fluctuations.
[0098] Preferably, the loose roller type tension fluctuation absorption is performed according to the following steps:
[0099] The first step is that after the steel strip comes out of the upstream mill, it hangs down and falls on the looper roll. The end continues to enter the downstream mill. Under the action of the constant pressure cylinder, the looper roll lifts up the steel strip to form the lifting looper section.
[0100] The second step is that when the steel strip tension transmitted from the upstream mill increases, the increased steel strip tension increases the downward pressure generated by the tension compensation looper roll, which overcomes the lifting force of the constant pressure cylinder and presses the looper roll vertically downward, increasing the length of the steel strip supporting the looper section.
[0101] The third step is that when the steel strip tension transmitted from the upstream mill decreases, the downward pressure generated by the steel strip tension on the looper roll decreases, and the lifting force of the constant pressure cylinder pushes the tension looper roll vertically upward, reducing the length of the steel strip in the lifting looper section and releasing the stored steel strip length.
[0102] The fourth step is to monitor the vertical displacement of the looper roll in real time by the displacement sensor. When the displacement exceeds the set upper and lower limits, the speed regulation system of the upstream mill will finely adjust the rolling speed of the upstream mill to return the looper roll to the set position.
[0103] The fifth step involves setting the cylinder air supply pressure for each tension compensation looper roll according to the set tension value between its stands, with the cylinder air supply pressure for each tension compensation looper roll increasing sequentially along the rolling line direction.
[0104] The looper rolls described in S5 are arranged between every two adjacent cold rolling mills, and the looper rolls are driven by existing constant pressure cylinders.
[0105] Specifically, the tension fluctuation absorption of the inter-stand tension compensation looper roll in this solution aims to suppress tension fluctuations between stands during cold rolling, and prevent tension fluctuations from the upstream stand from being transmitted to the downstream stand and accumulating segment by segment.
[0106] In continuous cold rolling production, the strip tension between stands is a key parameter for ensuring the stability of the rolling process. Excessive tension can easily lead to strip narrowing or even breakage, while insufficient tension can cause the strip to deviate and wrinkle. This solution involves installing adjustable tension-compensating looper rolls between every two adjacent stands. After exiting the upstream stand, the strip passes downwards over the looper rolls and then upwards into the downstream stand. The looper rolls lift the strip from below, forming a support looper section, passively absorbing tension fluctuations through the vertical displacement of the looper rolls.
[0107] The lifting and lowering of the looper roll is entirely determined by the mechanical balance between the steel strip tension and the cylinder lifting force. The response speed is determined by the mechanical inertia of the looper roll and the steel strip, which is much faster than electrical speed regulation. Moreover, the absorption process does not change the rolling speed of any mill, thus avoiding mutual interference between tension control and thickness control.
[0108] Based on this, the vertical displacement of the looper roll passively absorbs tension fluctuations, replacing the traditional mill speed-regulated tension control. This avoids mutual interference between tension control and speed control. This solution provides purely mechanical passive absorption, with fast response and no impact on thickness control. Simultaneously, a constant-pressure cylinder provides a constant lifting force, ensuring that the strip tension provided by the looper roll remains essentially constant throughout its lifting stroke. This avoids tension fluctuations caused by changes in the looper roll's position. In this solution, the constant-pressure cylinder-driven looper roll's thrust is determined by the air supply pressure, remaining constant throughout the entire stroke. The strip tension provided by the looper roll is independent of its position, resulting in higher tension stability.
[0109] Preferably, the cold rolling mill in S5 is a five-stand continuous rolling mill, with loop rolls configured between each pair of adjacent stands. The cylinder air supply pressure of the five loop rolls increases progressively from the first stand to the fifth stand, and the air supply pressure difference between two adjacent loop rolls is equal.
[0110] Specifically, in this scheme, the inter-stand tension compensation looper roll pressure of the five-stand continuous rolling mill increases progressively, so that the set tension between each stand matches the work hardening characteristics of the steel strip after each pass of cold rolling. During the cold rolling process, the steel strip's grains are elongated and broken up with each pass, the dislocation density increases, work hardening occurs, and the yield strength increases.
[0111] The degree of work hardening accumulates with each pass, and the yield strength of the strip increases progressively from the first stand to the fifth stand. To maintain a stable rolling process, the strip tension between stands should be in appropriate proportion to the strip's yield strength: if the tension is too low, the strip is prone to deviation between stands, leading to instability in the rolling line; if the tension is too high, the strip will undergo additional plastic elongation under tension, resulting in narrowing of width and thickness fluctuations, or even strip breakage.
[0112] In this design, the air supply pressure of the five tension-compensating looper rolls increases progressively from the first stand to the fifth stand. The air supply pressure determines the strip tension provided by the looper rolls; the progressive increase in supply pressure corresponds to a progressive increase in strip tension, matching the increase in yield strength caused by work hardening. The equal pressure difference between adjacent looper rolls ensures a linear increase in tension along the rolling line with a uniform rate of increase, avoiding transient fluctuations in strip thickness caused by sudden tension changes between adjacent stands.
[0113] Based on this, the air supply pressure of the looper roller cylinder increases progressively from frame to frame, so that the tension set between frames increases synchronously with the yield strength of the steel strip after work hardening. The tension setting is more scientific, which avoids deviation caused by insufficient tension in the later frame and avoids narrowing caused by excessive tension in the earlier frame.
[0114] Meanwhile, when the tension between adjacent frames changes abruptly, the steel strip will experience instantaneous elastic elongation changes in the abrupt change area, which will be transformed into transient fluctuations in thickness. These fluctuations cannot be completely eliminated in subsequent frames and will eventually remain on the finished steel strip. In this solution, the tension increases linearly without abrupt change points, ensuring the stability of the steel strip thickness.
[0115] More importantly, multiple looper rollers independently absorb the tension fluctuations at the outlet of their respective frames, forming a multi-stage tension fluctuation absorption chain. Once the tension fluctuations of the upstream frames are absorbed by the corresponding looper rollers, they are no longer transmitted to the downstream, thus suppressing the gradual accumulation of tension fluctuations.
[0116] Preferably, the electric field shielding in S7 is achieved by setting a grounded metal shielding plate on each side of the steel strip during operation, controlling the shielding plate surface to be parallel to the side of the steel strip, the distance between the edge of the shielding plate near the edge of the steel strip and the edge of the steel strip is 5 to 15 mm, and the length of the shielding plate along the running direction of the steel strip is greater than the effective width of the electrostatic oiling electrode along the running direction of the steel strip.
[0117] Specifically, the core advantages of electrostatic oiling are precise and controllable oil application and uniform oil film. However, in actual production, the oil film thickness at the edges of the steel strip is significantly greater than that in the middle, a phenomenon known as edge-rich oil. The mechanism of edge-rich oil lies in the edge effect of the electrostatic field: the steel strip acts as a grounding electrode, and its surface electric field distribution is distorted at the edges. The electric field lines originate from the oiling electrode and bend outwards at the edges of the steel strip, resulting in a higher electric field strength at the edges than in the middle. Charged oil mist particles experience a greater electric field force at the edges, leading to greater deposition and ultimately a thicker oil film at the edges than in the middle. After the steel strip is wound up, the oil film in the edge-rich area is squeezed out under interlayer pressure, contaminating the end face of the steel coil and packaging materials. When the steel strip is unwound, oil drips from the edge-rich area, contaminating downstream equipment and the environment. Edge-rich oil also affects the quality of subsequent coating and welding on the steel strip surface. This solution involves simply placing a grounded metal shielding plate on each side of the steel strip. The shielding plate is kept at an appropriate distance from the edge of the steel strip. The presence of the grounded shielding plate changes the electric field distribution at the edge of the steel strip, causing the electric field lines that were originally bending outward to be attracted by the shielding plate and terminated on the shielding plate. The electric field intensity on the surface of the edge of the steel strip is reduced to be comparable to that in the middle, thereby suppressing oil enrichment at the edge.
[0118] Preferably, the annealing furnace in S6 can be a bell-type annealing furnace (but not limited to bell-type annealing furnaces) including a heating section, a holding section, and a cooling section. The protective gas injection operation is performed between each pair of adjacent furnace rollers (or furnace plates) in the heating section, holding section, and cooling section. Each group consists of a spray beam that spans the width of the furnace. The upper surface of the spray beam has two rows of spray holes with valves. The uniform temperature control of the gas injection in the width direction in the furnace is performed according to the following steps:
[0119] The first step is to heat the annealing furnace to the working temperature. The furnace circulation fan draws the protective gas from the furnace and sends it to the spray beams of the heating section and the heat preservation section through the gas supply pipeline. After the gas is pressurized inside each gas supply chamber of the spray beam, it is sprayed upward from the spray holes with valves on the upper surface. The sprayed protective gas impacts the lower surface of the steel strip and then diffuses along the width and length of the steel strip, causing the protective gas in the furnace to form a convection circulation.
[0120] The second step is that when the steel strip is running in the heating section, the protective gas sprayed by the spray beam forms an impact jet on the lower surface of the steel strip. The impact jet destroys the gas boundary layer on the lower surface of the steel strip, increases the convective heat transfer coefficient between the lower surface of the steel strip and the furnace gas, and accelerates the heat exchange between the lower surface of the steel strip and the furnace gas.
[0121] Third, when the steel strip is running in the insulation section, the insulation section spray beam continuously supplies circulating protective gas into the furnace to maintain the convection circulation in the furnace. The gas supply pressure of the insulation section spray beam is lower than that of the heating section spray beam.
[0122] The fourth step is to supply air to each air supply chamber independently and adjust the air supply pressure separately. The air supply pressure of the air supply chambers in the cooling section is adjusted according to the temperature distribution in the width direction of the steel strip.
[0123] Fifth, protective gas, cooled by the furnace cooler, is introduced into the spray beam in the cooling section. The temperature of the sprayed protective gas is lower than that of the steel strip. When the protective gas impacts the lower surface of the steel strip, it dissipates the heat of the steel strip through forced convection. The diameter of the nozzle with valve at the edge of the air supply chamber of the spray beam in the cooling section is smaller than that of the nozzle with valve at the middle, so that the gas flow rate at the edge is lower than that at the middle.
[0124] Specifically, this solution aims to eliminate temperature differences along the width of the steel strip within the annealing furnace, reducing the microstructure and property differences caused by uneven temperature distribution between the edges and the center. The steel strip undergoes heating, holding, and cooling processes within the annealing furnace, completing microstructural evolution such as recrystallization, grain growth, and phase transformation, ultimately achieving the desired mechanical properties. This scheme involves installing zoned gas supply spray beams between each furnace roller (or furnace plate) inside the furnace. Protective gas is sprayed onto the underside of the (whole coil of steel strip) to control the temperature distribution in the width direction: In the heating and holding sections, furnace-circulating protective gas with the same furnace temperature is introduced. The gas impacts the lower surface of the steel strip, forming an impact jet that disrupts the gas boundary layer, increases the convective heat transfer coefficient, promotes gas convection circulation within the furnace, and makes the temperature in the width direction of the steel strip more uniform. In the cooling section, protective gas cooled by an external furnace cooler is introduced. The low-temperature gas impacts the lower surface of the steel strip for forced convective cooling. Simultaneously, the design of the nozzles with valves at the edges, with smaller orifice diameters than those in the middle, ensures that the gas flow rate at the edges is lower than in the middle, resulting in lower cooling intensity at the edges and compensating for the lower temperature caused by faster heat dissipation at the edges.
[0125] The heating and heat preservation sections achieve convective heat equalization, while the cooling section achieves uniform cooling. Different functions are achieved in different furnace sections by changing the gas supply. At the same time, the nozzle diameter with valves on the edge of the cooling section spray beam is smaller than that in the middle, so the gas flow rate and cooling intensity on the edge are lower than those in the middle. This compensates for the lower temperature caused by the rapid heat dissipation at the edge of the steel strip. The cooling intensity distribution between the edge and the middle is directly adjusted by the difference in nozzle diameter with valves. The smaller nozzle diameter on the edge results in a lower flow rate and weaker cooling, and the temperature on the edge naturally rises to be comparable to that in the middle. This design does not require additional edge heating equipment; uniform temperature in the width direction can be achieved solely through the difference in the spray beam structure.
[0126] Preferably, in step S6, the heating section heats the steel strip to above the recrystallization temperature, the heat preservation section keeps the steel strip within this temperature range until recrystallization is complete, and the cooling section cools the steel strip to the set discharge temperature. Temperature measuring points are set at the edge and middle of the steel strip along the width direction at the outlet of the cooling section. When the temperature difference between the edge and the middle exceeds the set threshold, the opening of the proportional valve on the nozzle of the air supply chamber at the edge is adjusted according to the direction of the temperature difference to change the air supply flow rate at the edge: when the edge temperature is lower than the middle temperature, the air supply flow rate at the edge is reduced, and when the edge temperature is higher than the middle temperature, the air supply flow rate at the edge is increased.
[0127] Specifically, for steel strips used in engineering structures, the uniformity of the cooling rate along the width of the cooling section directly determines the uniformity of the mechanical properties of the finished steel strip along its width. If the cooling rate at the edges is greater than that at the center, the phase transformation structure at the edges is finer and the strength is higher, while the phase transformation structure at the center is coarser and the strength is lower. Ultimately, the finished steel strip exhibits differences in mechanical properties along its width, affecting downstream applications. The main reason for the difference in cooling rate along the width of the cooling section is that the heat dissipation area at the edges of the steel strip is larger than that at the center. Under the same gas jet cooling conditions, the total heat dissipation rate at the edges (gas convection heat transfer + side end face radiation heat dissipation) is greater than that at the center, resulting in a higher cooling rate at the edges than at the center.
[0128] This design utilizes the structural difference in the cooling section's spray beam design—where the nozzle diameter with valves on the edges is smaller than that in the middle—to ensure a lower gas flow rate at the edges, thus providing a basic level of uniform cooling rate. However, since this structural difference is fixed, this design sets temperature measurement points at both the edges and the middle of the steel strip along the width of the cooling section outlet. These points monitor the actual temperatures at the edges and middle of the steel strip in real time. When the temperature difference exceeds a set threshold, the opening of the proportional valve in the edge air supply chamber is dynamically adjusted based on the direction of the temperature difference: if the edge temperature is lower than the middle temperature, it indicates that the edge cooling rate is too high; therefore, the edge air supply flow rate is reduced to weaken the edge cooling intensity, causing the edge temperature to rise again. If the edge temperature is higher than the middle temperature, it indicates that the edge cooling rate is insufficient; therefore, the edge air supply flow rate is increased to enhance the edge cooling intensity, causing the edge temperature to decrease.
[0129] The flow rate at the perimeter is dynamically adjusted via a proportional valve, allowing for real-time correction based on the actual temperature difference. This provides strong adaptability and maintains uniform temperature under various specifications and operating conditions. Simultaneously, temperature feedback adjustment only affects the perimeter gas supply chambers, without impacting the central gas supply flow rate, thus preventing central temperature fluctuations. Existing technologies typically adjust the overall gas supply pressure or furnace temperature setting, which can cause synchronous fluctuations in the central temperature, the primary control target for the cooling section. This solution allows for independent zone adjustment; perimeter flow rate adjustment has minimal impact on the central gas supply, resulting in a relatively stable central temperature with only minor adjustments to the perimeter temperature.
[0130] Preferably, the non-contact ranging in S8 is laser ranging, with the measuring beam of the laser rangefinder pointing horizontally towards the outer circumference of the steel coil. The actual outer diameter tracking and winding is performed according to the following steps:
[0131] The first step is to measure the distance from the outer surface of the winding machine spindle to the laser rangefinder before the winding begins, using this distance as a reference distance.
[0132] The second step is during the winding process. The laser rangefinder measures the real-time distance from the outer surface of the steel coil to the rangefinder at a fixed sampling frequency. The radial wall thickness of the steel coil is obtained by subtracting the real-time distance from the reference distance. Twice the radial wall thickness is added to the mandrel diameter to obtain the true outer diameter of the steel coil.
[0133] The third step is to embed pressure sensors at different radial positions between the steel strip layers of the first coil during calibration winding to measure the pressure per unit area between the layers. Based on the measured results, the decrease in winding tension as the actual outer diameter increases is determined and the tension decrease curve is calibrated. When the finished steel coil is wound in subsequent cycles, the control system calls the winding tension value corresponding to the calibration curve based on the actual outer diameter of the steel coil.
[0134] The fourth step involves converting the retrieved winding tension value into a torque setpoint for the winding machine motor, which then drives the winding machine mandrel to rotate and complete the steel strip winding.
[0135] Fifth step: When the actual outer diameter of the steel coil reaches the set outer diameter of the finished coil, the winding machine slows down and stops, the steel strip is cut off by the shearing station, the tail end is finished by the winding machine, and the laser rangefinder is reset to the reference distance measurement state to wait for the next coil to be wound.
[0136] Specifically, during the winding process, the steel strip is wound layer by layer onto the mandrel under winding tension, forming a steel coil with a certain radial pressure. Interlayer pressure refers to the radial contact pressure between two adjacent layers of steel strip. Excessive interlayer pressure can easily lead to surface indentations, oil film extrusion, and steel strip adhesion. Insufficient interlayer pressure results in a loose steel coil, prone to pyramiding and collapse. This solution uses a laser rangefinder to directly measure the actual outer diameter of the steel coil, eliminating the cumulative error in outer diameter calculation. The first coil calibration method is used to measure the interlayer pressure and calibrate the tension reduction curve, ensuring precise matching between the tension reduction curve and actual working conditions.
[0137] Laser ranging is used to directly measure the true outer diameter of the steel coil, replacing the traditional method of calculating the outer diameter based on winding speed and steel strip thickness. This eliminates the cumulative error in outer diameter calculation. Laser ranging directly measures the distance from the outer surface of the steel coil to the rangefinder, and the true outer diameter is obtained through geometric conversion. The measured value is independent of the number of winding turns and has no cumulative error. The accuracy of the outer diameter measurement is determined by the resolution of the laser rangefinder, which can meet the accuracy requirements of tension reduction control.
[0138] Meanwhile, during the first roll calibration, pressure sensors are embedded at different radial positions between the steel strip layers as needed to directly measure the interlayer unit area pressure at different outer diameters. Based on the measured results, the tension reduction curve is derived, so that the tension reduction curve is accurately matched with the actual working conditions, resulting in high accuracy in interlayer pressure control.
[0139] Preferably, the synergistic process of curvature compensation and tension absorption is performed according to the following steps:
[0140] In the first step, after the steel strip is alternately bent in the opposite direction by the multiple rolls of the multi-roll straightening unit, the residual curvature is controlled within the set threshold. The steel strip enters the inlet tension roll between the outlet of the multi-roll straightening unit and the first cold rolling mill in a straight state.
[0141] The second step is to apply a stable pre-tension to the steel strip by the inlet tension roller, so that the steel strip establishes a uniform initial tension field before entering the first cold rolling mill. The initial tension field is evenly distributed along the width direction of the steel strip.
[0142] The third step involves the steel strip being rolled by the first cold rolling mill. The work hardening generated during the first rolling pass increases the yield strength of the steel strip.
[0143] Fourth step: When the multi-roll straightener applies a large reverse bending amount to a certain marked belt segment, the running resistance of the belt segment in the multi-roll straightener increases, causing instantaneous tension fluctuation at the inlet tension roller. The instantaneous tension fluctuation is absorbed by the existing auxiliary looper rollers configured as needed behind the inlet tension roller through vertical displacement.
[0144] Fifth step: After the tension fluctuations are absorbed, the tension of the steel strip entering the second cold rolling mill returns to a stable level. If subsequent instantaneous tension fluctuations occur, the absorption process should be completed using the method described above.
[0145] Specifically, when the multi-roll straightener switches between different speeds, the operating resistance changes abruptly. This change in resistance translates into instantaneous fluctuations in strip tension. This solution addresses this by establishing a process connection chain connecting curvature compensation, the inlet tension roll, the auxiliary looper roll, and the first cold rolling mill. This chain uses vertical displacement to absorb the instantaneous tension fluctuations caused by the multi-roll straightener's speed switching. When the multi-roll straightener applies a large reverse bending amount to a marked strip segment, the operating resistance of that segment increases, the tension at the inlet tension roll increases instantaneously, and the auxiliary looper roll descends under the increased tension, causing the strip to bend deeper and absorbing the elastic elongation of the strip caused by the increased tension. When the speed switches back to a smaller reduction, the operating resistance decreases, the tension decreases instantaneously, the auxiliary looper roll rises, releasing the strip length. After being absorbed by the auxiliary looper roll, the strip tension entering the first cold rolling mill returns to a stable level, and the tension fluctuations caused by curvature compensation are not transmitted to the rolling section.
[0146] Meanwhile, the auxiliary looper roll and the tension compensation looper roll between the stands have the same structure, forming a multi-stage tension fluctuation absorption chain from the curvature compensation section to the rolling section, suppressing tension fluctuations step by step. In this scheme, the auxiliary looper is set at the exit of the curvature compensation section, so that the tension fluctuations are absorbed before entering the rolling mill, resulting in more stable rolling quality.
[0147] Preferably, after the looper roll at the exit of the last cold rolling mill in S5 stabilizes the tension of the steel strip, the steel strip undergoes the existing surface degreasing and cleaning process to remove residual rolling oil, and then undergoes squeezing and hot air drying to remove surface moisture. After exiting the buffer, it enters the S6 annealing furnace. After the steel strip is annealed in S6 and exits the furnace, it undergoes the S7 oiling process to apply surface oil.
[0148] Specifically, it is essential to ensure that the cold-rolled steel strip enters the annealing furnace with a clean surface, stable tension, and a matching speed, and maintains a tension within the annealing furnace that does not exceed the safe range of high-temperature yield strength to prevent plastic deformation of the steel strip at high temperatures.
[0149] After degreasing and cleaning, the steel strip surface still retains cleaning fluid and moisture. If it enters the annealing furnace directly, the moisture will rapidly vaporize at high temperatures, causing fluctuations in the steel strip temperature and furnace atmosphere. Furthermore, impurities in the moisture will remain on the steel strip surface. Therefore, after degreasing and cleaning, most of the surface moisture needs to be removed by squeezing rollers, followed by a hot air drying device to completely remove any remaining moisture.
[0150] The output torque of the furnace rollers (or furnace plates) is set according to the high-temperature yield strength of the steel strip inside the furnace, ensuring that the tension of the steel strip in each section of the furnace is less than one-third of the yield strength of the steel strip at that temperature, leaving sufficient safety margin and avoiding plastic deformation of the steel strip at high temperatures. Furthermore, a torque control mode is implemented for each furnace roller (or furnace plate) in the annealing furnace, with the output torque of the furnace rollers (or furnace plates) set according to the high-temperature yield strength of the steel strip, ensuring that the tension inside the furnace is less than one-third of the yield strength at that temperature, thus preventing plastic deformation of the steel strip due to excessive tension at high temperatures.
[0151] Meanwhile, degreasing and cleaning, squeezing and drying, looper and inlet tension roller are set between cold rolling and annealing to ensure that the steel strip entering the annealing furnace is clean, has stable tension and matching speed; the steel strip is oiled after annealing and exiting the furnace. The oiling process is clearly defined after annealing to avoid the problems of rolling oil carbonization and surface carbon residue caused by oil-on annealing.
[0152] Preferably, the operating speeds of processes S1 to S8 are synchronously matched with the rolling speed of the S5 cold rolling mill. The storage capacity of the storage looper is determined based on the time required for coil changing and the rolling speed. During coil changing, the running speed of the steel strip at the outlet of the storage looper remains unchanged, and feeding is suspended at the inlet side. The steel strip stored in the storage looper maintains continuous downstream production. The running speed of the steel strip in the S6 annealing furnace is connected to the rolling speed through the outlet looper set between the cold rolling mill and the annealing furnace. The heat treatment time is determined by the furnace length and the running speed of the steel strip. The running speed of the steel strip in the S7 oiling process is equal to the outlet speed of the annealing furnace. The winding speed of the S8 coiler is equal to the outlet speed of the steel strip in the oiling process. The rotation speed of the coiler decreases synchronously as the actual outer diameter of the steel coil increases.
[0153] Specifically, this scheme uses the rolling speed as the speed benchmark for the entire process, and the speeds of other processes are synchronously matched with the rolling speed: the operating speeds of the uncoiler, the material storage looper outlet, the multi-roll straightener unit, and the descaling process are equal to the rolling speed, ensuring that the speeds of each process upstream of the rolling section are consistent with the rolling speed; the strip running speed of the annealing furnace is connected to the rolling speed through the outlet looper, which buffers the speed difference between cold rolling and annealing, and the annealing furnace speed is automatically adjusted according to the material storage amount of the outlet looper to keep the material storage amount of the outlet looper at a median level; the oiling process speed is equal to the annealing furnace outlet speed, ensuring that the oiling speed matches the strip running speed and the oiling amount is uniform; the winding line speed is equal to the oiling outlet speed, and the winding machine speed decreases synchronously as the actual outer diameter of the steel coil increases, maintaining a constant winding line speed.
[0154] The amount of material stored in the storage looper is determined based on the time required for coil changing and the rolling speed. During coil changing, the exit speed of the storage looper remains unchanged, and the feeding on the inlet side is suspended. The steel strip stored in the storage looper maintains continuous downstream production, thus achieving uninterrupted production during coil changing.
[0155] The winding speed decreases synchronously as the actual outer diameter of the steel coil increases, maintaining a constant winding linear speed and avoiding fluctuations in winding tension and scratches on the steel strip surface caused by fluctuations in linear speed.
[0156] The present invention also provides a continuous cold rolling production system for steel strips for engineering structures, the system being used to implement the process method described above.
[0157] The present invention will be further described in detail below with reference to specific embodiments: This embodiment is implemented based on an existing continuous cold rolling production line. The steel strip blank material processed in this embodiment is Q345B, the blank thickness is 3.0mm, the width is 1250mm, and the finished product thickness is 1.2mm.
[0158] The rolling speed of the cold rolling mill is 120 m / min. The three roll gap reduction of the multi-roll straightener are as follows: the first level corresponds to the shortest dwell time range, with an upper roll reduction of 0.5 mm; the second level corresponds to the middle dwell time range, with an upper roll reduction of 0.8 mm (1.6 times that of the first level); and the third level corresponds to the longest dwell time range, with an upper roll reduction of 1.2 mm (2.4 times that of the first level).
[0159] The operation steps of the example are as follows:
[0160] S1. The coiled steel strip blank is hoisted to the uncoiler for uncoiling. The head of the traction steel strip is pulled through the shearing station to cut off irregular material heads. The cut-off waste material is introduced into a waste collection line independent of the main line, and the main line steel strip continues to be conveyed downstream.
[0161] S2. The steel strip, after the material head has been removed, is pulled into the storage loop and stored in a catenary configuration. Before the steel strip enters the storage loop, a semi-circular indentation is punched on the side edge of the steel strip using a stamping device, with an interval of 500mm between adjacent indentations. The inlet photoelectric sensor of the storage loop records the entry time of the indentation, and the outlet photoelectric sensor records the exit time of the indentation. The difference between the two times is the residence time of the strip segment corresponding to that indentation in the storage loop.
[0162] S3. When the marked indentation reaches the photoelectric sensor at the outlet of the storage looper, the dwell time of the belt segment is compared with three preset dwell time intervals (0-60s, 60-120s, and over 120s) to determine the curvature compensation level. When the head of the belt segment reaches the first roller of the multi-roller straightener unit, the pressing drive mechanism of the corresponding level synchronously presses down to the preset roller gap value, and the steel strip alternately winds around the nine rollers, undergoing seven reverse bends. When the tail of the belt segment leaves the last roller, the pressing drive mechanism rises back to the waiting position. The contact-type curvature detection plate at the outlet of the multi-roller straightener unit detects the residual curvature of the steel strip, records the position of belt segments that exceed the set range, and tracks them downstream.
[0163] S4. Before the steel strip enters the high-pressure water descaling process, the width gauge detects the actual width of the steel strip as 1250mm, and the width signal is transmitted to the adjustable spray beam control system. Each nozzle on the adjustable spray beam synchronously adjusts its swing angle according to its position in the width direction, ensuring that the high-pressure water jet injection angle of all nozzles within the width range is 20 degrees. Nozzles exceeding the width limit stop spraying. High-pressure water impacts the steel strip surface to remove oxide scale, and the peeled oxide scale is discharged into the water collection tank with the water flow. After descaling, the steel strip passes through a squeeze roller to remove surface moisture. A surface roughness detector collects roughness values at five measuring points along the width direction. When the difference between adjacent measuring points exceeds a set threshold, feedback is provided to correct the swing angle of the corresponding nozzle.
[0164] S5. The descaled steel strip is fed into a five-stand cold rolling mill for five passes of rolling and thinning, with a total reduction rate of 60%. The tension compensation looper rolls between each pair of adjacent stands lift the steel strip under the action of a constant pressure cylinder to form a protruding looper section.
[0165] When the strip tension from the upstream stand increases, the downward pressure of the strip on the looper roll increases, overcoming the cylinder lifting force and causing the looper roll to descend vertically. This increases the length of the strip in the top looper section, absorbing the elastic elongation of the strip caused by the increased tension. When the tension decreases, the cylinder lifting force causes the looper roll to rise, the U-shape to become shallower, and the strip length to be released. Displacement sensors monitor the looper roll displacement in real time, and when it exceeds the upper or lower limits, the upstream mill speed is finely adjusted to return the looper roll to the center position. The air supply pressure of the five looper roll cylinders increases progressively from stand to stand.
[0166] S6. After rolling, the steel strip is degreased, cleaned, squeezed dry, and buffered at the outlet looper before being sent to the annealing furnace. In the heating section, the furnace's circulating fan draws protective gas from the furnace and sends it to the spray beam. After being pressurized in three chambers, the gas is ejected upwards from the valved nozzles on the upper surface, impacting the lower surface of the steel strip and then diffusing, promoting gas convection circulation within the furnace. The steel strip is heated to 820℃ in the heating section. In the heat preservation section, the spray beam continuously supplies circulating gas to maintain convection, with a supply pressure lower than that in the heating section. In the cooling section, the spray beam supplies protective gas cooled by an external cooler. The low-temperature gas impacts the lower surface of the steel strip, forcing convection cooling. The valved nozzles at the edges of the cooling section spray beam have a smaller diameter than those in the center, resulting in a lower flow rate at the edges compared to the center.
[0167] Temperature measurement points at the outlet of the cooling section monitor the temperature at the edges and center. When the edge temperature is lower than the center temperature, the air supply flow rate at the edge is reduced; when the edge temperature is higher than the center temperature, the air supply flow rate at the edge is increased. The steel strip is cooled to 120°C in the cooling section before exiting the furnace.
[0168] S7. After annealing, the steel strip is fed into an electrostatic oiling machine to form a 1.2g / m² anti-rust oil film on its surface. During oiling, a grounded metal shielding plate is placed on each side of the steel strip, with the plate surface parallel to the side of the steel strip and a distance of 10mm between the shielding plate and the edge of the steel strip. The length of the shielding plate along the running direction of the steel strip is greater than the effective width of the oiling electrode. A linear guide mechanism drives the two shielding plates to move synchronously according to the steel strip width signal, maintaining a constant distance between them.
[0169] The grounding shield plate changes the electric field distribution at the edge of the steel strip, suppresses the edge effect of electrostatic oiling, and makes the oil film thickness uniform along the width direction.
[0170] S8. After oiling, the steel strip is pulled to the winding machine for non-stop winding. Before winding begins, a laser rangefinder measures the distance from the outer surface of the mandrel to the rangefinder as the reference distance. During winding, the laser rangefinder measures the real-time distance from the outer surface of the steel coil to the rangefinder at a fixed sampling frequency. The radial wall thickness is obtained by subtracting the real-time distance from the reference distance. The true outer diameter of the steel coil is obtained by adding twice the radial wall thickness to the mandrel diameter.
[0171] During the initial coil calibration and winding, pressure sensors are embedded at different radial positions between the steel strip layers to measure the interlayer pressure. Based on the measurement results, a decrease curve of winding tension as a function of the actual outer diameter is calibrated. Subsequent finished coil windings use the tension value corresponding to the calibration curve based on the actual outer diameter. This tension value is converted into a torque setpoint for the winding machine motor, decreasing the winding tension from 50kN at the inner diameter to 25kN at the outer diameter, maintaining constant interlayer pressure. When the actual outer diameter of the steel coil reaches the set outer diameter for the finished product, the winding machine decelerates and stops, the steel strip is cut, the tail end is wound, and the laser rangefinder resets to await the next coil.
[0172] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention. For those skilled in the art, any alternative improvements or transformations made to the implementation of the present invention fall within the protection scope of the present invention.
[0173] Any aspects of this invention not described in detail are well-known to those skilled in the art.
Claims
1. A continuous cold rolling production process for special steel strips for engineering structures, characterized in that, Includes the following steps: S1. Steel strip blank feeding and waste material separation treatment; S2. Mechanical tracking and marking of storage and belt segment dwell time in storage loop: The steel belt after the material head is cut off is pulled into the downstream storage loop and stored in the form of a catenary. At the same time, the steel belt entering the storage loop is mechanically marked segment by segment along the length direction, and the dwell time of each marked segment in the storage loop is tracked. S3. Segment-by-segment reverse bending curvature compensation based on residence time classification: When the marked belt segment leaves the storage loop, the roll gap reduction of the multi-roll straightener unit on the exit side is adjusted according to the residence time of the belt segment in the storage loop, and a larger reverse bending amount is applied to the belt segment with a longer residence time. S4. Variable incident angle descaling and surface transverse roughness uniformity: The steel strip after curvature compensation is sent into the descaling process to remove the surface oxide scale. During the descaling process, the incident angle of the descaling medium relative to each point in the width direction of the steel strip is kept equal. S5. Multi-pass calendering and thinning, and tension fluctuation absorption between the stand and the machine frame are achieved through looper control; S6. Heat treatment and uniform temperature control inside the furnace; S7. Edge electric field shielding oil coating and surface film homogenization; S8. True outer diameter tracking winding and interlayer pressure control: The oiled steel strip is pulled to the winding machine for non-stop winding. During the winding process, the true outer diameter of the steel coil is directly measured by non-contact distance measurement, and the winding tension is reduced synchronously according to the true outer diameter.
2. The process method according to claim 1, characterized in that, The segmented mechanical marking described in S2 is achieved by stamping semi-circular indentations on the side edge of the steel strip. The spacing between adjacent indentations is fixed. Photoelectric sensors installed at the inlet and outlet of the storage loop record the time when the indentation enters and leaves the storage loop, respectively. The difference between the two times is the dwell time of the strip segment corresponding to the indentation in the storage loop.
3. The process method according to claim 2, characterized in that, The curvature compensation is performed according to the following steps: The first step is that when the photoelectric sensor at the outlet of the storage looper detects the marked indentation, it compares the dwell time of the belt segment corresponding to the indentation with the three preset dwell time intervals to determine the curvature compensation level to which the belt segment belongs. The second step is that when the head of the belt segment reaches the first roller of the multi-roller straightener unit, each pressing drive mechanism corresponding to the gear position presses down synchronously according to the preset roller gap value, and the upper roller and the lower roller form a reverse bending curvature corresponding to the gear position. The third step involves the steel strip winding alternately around nine rollers, undergoing alternating reverse bending. Fourth step: When the tail of the belt segment leaves the last roller of the multi-roller straightener unit, the drive mechanism is pressed down to return to the initial waiting position, waiting for the next marked belt segment to arrive; The fifth step involves installing a contact curvature detection plate at the outlet of the multi-roll straightener unit. The lower surface of the steel strip passes against the curvature detection plate, and the residual curvature of the steel strip is determined by the uniformity of the pressure distribution on the pressure sensors arranged along the running direction of the steel strip on the curvature detection plate. The more uniform the pressure distribution, the smaller the residual curvature. When the pressure distribution difference exceeds the set threshold, it is determined that the residual curvature of the strip segment exceeds the set range. The position of the strip segment with residual curvature exceeding the set range is recorded in the control system, and this position record is synchronously tracked to the downstream process along with the progress of the steel strip.
4. The process method according to claim 3, characterized in that, The three dwell time intervals mentioned in S3 correspond to the roll gap reduction of each gear. The first gear corresponds to the shortest dwell time interval, with the smallest roll gap reduction; the second gear corresponds to the middle dwell time interval, with the roll gap reduction being 1.5 to 1.8 times that of the first gear; and the third gear corresponds to the longest dwell time interval, with the roll gap reduction being 2.2 to 2.6 times that of the first gear.
5. The process method according to claim 1, characterized in that: The variable incident angle descaling is performed according to the following steps: The first step is to measure the actual width of the steel strip before it enters the descaling process using a width measuring instrument, and then transmit the width signal to the control system of the adjustable spray beam. The second step is to control the position of each nozzle in the width direction and adjust the swing angle synchronously so that the high-pressure water jets of all nozzles within the width range of the steel strip have the same incident angle relative to the surface of the steel strip directly below them, and the nozzles outside the width range of the steel strip stop spraying. The third step involves high-pressure water being ejected from the nozzle and impacting the surface of the steel strip. Under the mechanical impact of the high-pressure water, the oxide scale is peeled off from the steel strip substrate, and the peeled oxide scale falls into the water collection tank below and is discharged. The fourth step is to remove residual moisture from the surface of the descaled steel strip, and then set up a surface roughness tester at the rear to collect surface roughness values at five measuring points at equal intervals along the width of the steel strip. The fifth step involves sending the steel strip to the downstream cold rolling mill after surface roughness testing.
6. The process method according to claim 1, characterized in that, The looper roller type tension fluctuation absorption is performed according to the following steps: The first step is that after the steel strip comes out of the upstream mill, it hangs down and falls on the looper roll. The end continues to enter the downstream mill. Under the action of the constant pressure cylinder, the looper roll lifts up the steel strip to form the lifting looper section. The second step is that when the steel strip tension transmitted from the upstream mill increases, the increased steel strip tension increases the downward pressure generated by the tension compensation looper roll, which overcomes the lifting force of the constant pressure cylinder and presses the looper roll vertically downward, increasing the length of the steel strip supporting the looper section. The third step is that when the steel strip tension transmitted from the upstream mill decreases, the downward pressure generated by the steel strip tension on the looper roll decreases, and the lifting force of the constant pressure cylinder pushes the tension looper roll vertically upward, reducing the length of the steel strip in the lifting looper section and releasing the stored steel strip length. The fourth step is to monitor the vertical displacement of the looper roll in real time by the displacement sensor. When the displacement exceeds the set upper and lower limits, the speed regulation system of the upstream mill will finely adjust the rolling speed of the upstream mill to return the looper roll to the set position. The fifth step is to set the air supply pressure of the cylinder for each tension compensation looper roller according to the set tension value between the frames.
7. The process method according to claim 6, characterized in that, The cold rolling mill described in S5 is a five-stand continuous rolling mill. Loose rolls are configured between each pair of adjacent stands. The air supply pressure of the cylinders of the five loose rolls increases progressively from the first stand to the fifth stand, and the air supply pressure difference between two adjacent loose rolls is equal.
8. The process method according to claim 1, characterized in that, The electric field shielding described in S7 involves setting a grounded metal shielding plate on each side of the steel strip during operation, controlling the shielding plate surface to be parallel to the side of the steel strip, and the distance between the edge of the shielding plate near the edge of the steel strip and the edge of the steel strip is 5 to 15 mm. The length of the shielding plate along the running direction of the steel strip is greater than the effective width of the electrostatic oiling electrode along the running direction of the steel strip.
9. The process method according to claim 1, characterized in that, The S6 annealing furnace includes a heating section, a holding section, and a cooling section. The protective gas injection operation is carried out between each pair of adjacent furnace plates in the heating section, the holding section, and the cooling section. Each group consists of a spray beam that spans the width of the furnace. The upper surface of the spray beam has two rows of spray holes with valves. The furnace gas injection-type temperature uniformity control in the width direction is performed according to the following steps: The first step is to heat the annealing furnace to the working temperature. The furnace circulation fan draws the protective gas from the furnace and sends it to the spray beams of the heating section and the heat preservation section through the gas supply pipeline. After the gas is pressurized inside each gas supply chamber of the spray beam, it is sprayed upward from the spray holes with valves on the upper surface. The sprayed protective gas impacts the lower surface of the steel strip and then diffuses along the width and length of the steel strip, causing the protective gas in the furnace to form a convection circulation. The second step is that when the steel strip is running in the heating section, the protective gas sprayed by the spray beam forms an impact jet on the lower surface of the steel strip. The impact jet destroys the gas boundary layer on the lower surface of the steel strip, increases the convective heat transfer coefficient between the lower surface of the steel strip and the furnace gas, and accelerates the heat exchange between the lower surface of the steel strip and the furnace gas. Third, when the steel strip is running in the insulation section, the insulation section spray beam continuously supplies circulating protective gas into the furnace to maintain the convection circulation in the furnace. The gas supply pressure of the insulation section spray beam is lower than that of the heating section spray beam. The fourth step is to supply air to each air supply chamber independently and adjust the air supply pressure separately. The air supply pressure of the air supply chambers in the cooling section is adjusted according to the temperature distribution in the width direction of the steel strip. Fifth, protective gas, cooled by the furnace cooler, is introduced into the spray beam in the cooling section. The temperature of the sprayed protective gas is lower than that of the steel strip. When the protective gas impacts the lower surface of the steel strip, it dissipates the heat of the steel strip through forced convection. The diameter of the nozzle with valve at the edge of the air supply chamber of the spray beam in the cooling section is smaller than that of the nozzle with valve at the middle, so that the gas flow rate at the edge is lower than that at the middle.
10. A continuous cold rolling production system for special steel strips for engineering structures, characterized in that: The system is used to implement the process method as described in any one of claims 1-9.