A method for preparing 5-series aluminum alloy extruded tubing for GIL casing

By developing a method for preparing 5-series aluminum alloy extruded tubing, the weld defects of the rotary welding process and the comprehensive performance issues of the extrusion process in the production of GIL casings have been resolved, resulting in a highly reliable and high-performance integrated extruded tubing suitable for high-voltage power transmission equipment.

CN123102776APending Publication Date: 2026-11-17LIAONING ZHONGWANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611512267.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing spin welding process in GIL shell production has problems such as frequent weld defects, performance degradation in the heat-affected zone, and lengthy production process. The extrusion process has problems such as excessive extrusion pressure, significant pressure build-up, difficulty in controlling dimensional accuracy and surface quality, and difficulty in achieving comprehensive performance.

Method used

The method for preparing 5-series aluminum alloy extruded tubes includes precise control of alloy composition, optimization of homogenization process, matching of extrusion process window, and coordinated design of low-temperature annealing process. By replacing the traditional aluminum plate spin welding process with extrusion molding, weak links in the weld are eliminated, and airtightness and structural reliability are improved.

Benefits of technology

Stable extrusion molding of large-diameter, thin-walled, long 5-series aluminum alloy tubes has been achieved, eliminating weak points in the weld seams, improving the airtightness and structural reliability of the tubes, and taking into account both mechanical and electrical properties to meet the comprehensive application requirements of high-voltage power transmission equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102776A_ABST
    Figure CN123102776A_ABST
Patent Text Reader

Abstract

This invention proposes a method for preparing 5-series aluminum alloy extruded tubing for GIL (Gas Inlet and Outlet) casings, including steps such as batching, melting and casting, ingot homogenization, extrusion, quenching, online drawing, length cutting, and finished product annealing, to obtain tubing for GIL casings. This invention achieves stable extrusion forming of large-diameter, thin-walled, long-length 5-series aluminum alloy tubing through precise control of alloy composition, optimization of homogenization processes, matching of extrusion process windows, and synergistic design of low-temperature annealing processes. It replaces the traditional aluminum plate welding process with integrated extrusion forming, eliminating weak points in the weld seam at the source and significantly improving the airtightness and structural reliability of the tubing. Simultaneously, it solves the technical problems of excessive extrusion pressure, unstable forming, poor dimensional accuracy, numerous surface defects, and difficulty in simultaneously achieving mechanical and electrical properties in existing extrusion processes, providing highly reliable and high-performance integrated extruded tubing products for high-voltage power transmission equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy processing technology, and specifically discloses a method for preparing 5-series aluminum alloy extruded tubing for GIL casing. Background Technology

[0002] As my country's ultra-high-voltage (UHV) transmission network extends into complex areas such as deep canyons, high altitudes, and strong earthquake zones, gas-insulated transmission lines (GILs) have become essential equipment for high-voltage power transmission in high-risk terrains due to their technological advantages, including a fully enclosed tubular structure, all-weather stable operation, and a reduction in transmission corridor occupancy by more than 50%. The GIL protective enclosure is the core component responsible for bearing the insulating gas seal and ensuring structural mechanical strength; its manufacturing precision and service reliability directly determine the operational safety of the transmission system.

[0003] Due to its combination of moderate strength, excellent corrosion resistance, and formability, 5-series aluminum alloys have become the preferred material for lightweight upgrades of GIL (Gas Infrared) casings. Currently, the industry commonly uses a manufacturing process of aluminum sheet spinning followed by spinning and welding for GIL aluminum alloy casings. However, extrusion molding technology, with its integrated molding, continuous structure, and high production efficiency, is gradually becoming the technological development direction to replace the traditional spinning and welding process. However, for large-diameter, thin-walled, and long-length 5-series high-magnesium alloy power tubing, the industry has not yet formed a mature and stable extrusion preparation system, which cannot meet the dual requirements of material performance and manufacturing processes for GIL equipment upgrades.

[0004] The mainstream manufacturing method for GIL aluminum alloy shells currently involves aluminum plate spin welding: aluminum alloy plates are spun into cylindrical structures through multiple passes, the cylinders are closed by longitudinal seam welding, and then long-length sections of tubing are spliced ​​together by circumferential seam welding. Post-weld processes include defect detection and surface finishing to obtain the finished product. Traditional spin welding suffers from reliability issues. The aluminum alloy welding process is prone to defects such as porosity, cracks, and inclusions. The heat-affected zone exhibits coarse grains and significantly reduced mechanical properties, resulting in weaknesses in the shell's airtightness and structural strength, making it unsuitable for extremely complex service scenarios. Furthermore, spin welding involves multiple weld seam processing, post-weld cleaning, and seam-by-seam flaw detection, leading to a long production chain, high labor costs, and low yield, hindering the large-scale deployment of GIL equipment. Existing extrusion processes cannot meet the requirements of power tubing. These processes suffer from technical problems such as excessive extrusion pressure, unstable forming, poor dimensional accuracy, significant pressure build-up, difficulty in controlling dimensional accuracy and surface quality, numerous surface defects, and the inability to simultaneously achieve both mechanical and electrical properties.

[0005] To address the aforementioned problems, it is essential to research and design a novel method for preparing 5-series aluminum alloy extruded tubing for GIL casings, thereby overcoming the existing issues in GIL casing production. Summary of the Invention

[0006] To address the technical problems in existing GIL shell production, such as frequent weld defects, performance degradation in the heat-affected zone, and lengthy production process in the spin welding process, as well as the problems in the extrusion process, such as excessively high breakthrough pressure, significant pressure stagnation, difficulty in controlling dimensional accuracy and surface quality, and difficulty in achieving comprehensive performance, this invention proposes a method for preparing 5-series aluminum alloy extruded tubing for GIL shells.

[0007] This invention provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casings, comprising the following steps:

[0008] S1. Batching: Prepare aluminum alloy raw materials according to the following weight ratios: Si: ≤0.10%, Fe: ≤0.30%, Cu: ≤0.06%, Mn: ≤0.06%, Mg: 2.25%~2.35%, Cr: 0.20%~0.30%, Zn: ≤0.06%, Single impurity: ≤0.05%, Total impurities: ≤0.15%, Balance: Al;

[0009] S2. Melting and casting: The aluminum alloy raw material prepared in step S1 is placed into a melting furnace for melting and casting to obtain a casting rod;

[0010] S3. Homogenization of casting rod: The casting rod obtained in step S2 is homogenized to obtain an ingot. The homogenization temperature is 470±3℃ and the homogenization time is 11~12h.

[0011] S4. Extrusion: The ingot obtained in step S3 is placed into an extrusion device for extrusion molding to obtain a pipe. The temperature of the extrusion die is set to 480-500℃, the temperature of the ingot is set to 510-530℃, the extrusion speed of the extrusion device is set to 0.8-1.0m / min, and the extrusion ratio is 15-16.

[0012] S5. Quenching, online drawing and length cutting: The tube obtained in step S5 is quenched, and the quenched tube is stretched and straightened before being cut into the specified length.

[0013] S6. Finished product annealing: The cut tubing obtained in step S5 is annealed at (350±3)℃ for 1 hour and slowly cooled to room temperature to obtain GIL shell tubing.

[0014] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is provided. In step S1, the ingredients are: Si: ≤0.08%, Fe: ≤0.20%, Cu: ≤0.05%, Mn: ≤0.05%, Mg: 2.25%~2.30%, Cr: 0.24%~0.30%, Zn: ≤0.05%, single impurity: ≤0.05%, total impurities: ≤0.15%, and the balance is Al.

[0015] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is provided. In step S1, the ingredients are: Si: ≤0.05%, Fe: ≤0.15%, Cu: ≤0.03%, Mn: ≤0.03%, Mg: 2.25%~2.28%, Cr: 0.25%~0.28%, Zn: ≤0.03%, single impurity: ≤0.05%, total impurities: ≤0.15%, and the balance is Al.

[0016] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is described, wherein in step S3, the homogenization temperature is 470°C and the homogenization time is 12 hours.

[0017] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is described. In step S4, before extruding the ingot, a 6-series alloy ingot is used for die preparation. After the extrusion is stabilized, the process is switched to the ingot obtained in step S2.

[0018] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is provided, wherein the 6-series alloy ingot is a 6063 ingot.

[0019] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is described, wherein in step S4, the tube is extruded using a 90MN extrusion press.

[0020] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing is described, wherein in step S4, the extrusion ratio is 15.7.

[0021] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing, wherein in step S6, the annealing process is 350°C × 1 h.

[0022] According to some embodiments of this application, a method for preparing a 5-series aluminum alloy extruded tube for a GIL shell is provided. In step S6, the wall thickness tolerance of the tube for the GIL shell is ±0.3 mm, and the electrical conductivity is 30 MS / m.

[0023] This invention proposes a method for preparing 5-series aluminum alloy extruded tubing for GIL (Gas Insulation Line) casings. Through precise control of alloy composition, optimization of homogenization processes, matching of extrusion process windows, and coordinated design of low-temperature annealing processes, it achieves stable extrusion forming of large-diameter, thin-walled, long-length 5-series aluminum alloy tubing. This method replaces the traditional aluminum plate welding process with integrated extrusion forming, eliminating weak points in the weld seam at the source and significantly improving the tubing's airtightness and structural reliability. Simultaneously, it solves the technical problems of excessive extrusion pressure, unstable forming, poor dimensional accuracy, numerous surface defects, and difficulty in simultaneously achieving mechanical and electrical properties in existing extrusion processes. This provides high-reliability, high-performance integrated extruded tubing products for high-voltage power transmission equipment. This invention improves the alloy's hot deformation behavior, reduces extrusion breakthrough pressure, and enhances the stability of the forming process; eliminates elemental segregation in the ingot, ensuring uniformity of the tubing's microstructure and properties; effectively controls the dimensional accuracy and surface quality of the tubing, reducing forming defects, and balancing the tubing's mechanical strength and ductility to meet the comprehensive usage requirements of high-voltage power transmission equipment casings; at the same time, the tubing possesses good electrical conductivity, reducing induced current loss and temperature rise in the casing. This invention relies on the synergistic innovation of internal control of casting composition, homogenization to eliminate segregation, extrusion and heat treatment processes to replace the spin welding process for GIL shell tubing. The tubing has excellent dimensional accuracy, wall thickness tolerance meets ±0.3mm, no secondary processing is required, the product conductivity reaches 30MS / m, and the exfoliation corrosion reaches PB level or above. It has excellent comprehensive performance and meets the GIL shell industry standard. Attached Figure Description

[0024] Figure 1 This is a schematic flowchart of a method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to the present invention. Detailed Implementation

[0025] The embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and should not be construed as limiting the scope of the invention.

[0026] Example 1: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casings, such as... Figure 1 As shown, it includes the following steps:

[0027] S1. Batching: Prepare aluminum alloy raw materials according to the following weight ratios: Si: ≤0.10%, Fe: ≤0.30%, Cu: ≤0.06%, Mn: ≤0.06%, Mg: 2.25%~2.35%, Cr: 0.20%~0.30%, Zn: ≤0.06%, Single impurity: ≤0.05%, Total impurities: ≤0.15%, Balance: Al;

[0028] As a core solid solution strengthening element in 5-series alloys, Mg's content exhibits a dual constraint on extrusion behavior. From the perspective of solid solution strengthening, the relationship between the yield strength increment of Al-Mg solid solutions and Mg atomic concentration approximately follows... The theoretical basis for setting the lower limit of Mg content is based on a target elongation strength ≥70MPa (annealed state), combined with the yield strength of pure aluminum matrix of approximately 30MPa, requiring a solid solution strengthening contribution ≥40MPa. From the perspective of hot deformation behavior, the influence of Mg content on the extrusion process is more complex: when the Mg content is below 2.25%, the solid solution strengthening effect is insufficient, the high-temperature rheological stress of the alloy decreases significantly, and the low matrix strength during extrusion leads to metal flow instability, manifested as abnormally high extrusion pressure and frequent pressure build-up; while when the Mg content is above 2.35%, although the solid solution strengthening effect is enhanced, the alloy plasticity decreases sharply, the hot working window narrows, and the tendency for hot cracking increases significantly. Therefore, precisely locking the Mg content in the narrow range of 2.25-2.35% is essentially the optimal balance point between ensuring the strength base and the stability of extrusion molding.

[0029] In this embodiment, Cr and Mg elements work synergistically to form dispersed Al in the alloy. 18 Cr2Mg3 type intermetallic compounds. On the one hand, this type of dispersed phase can pin dislocations and grain boundaries, inhibit grain growth during extrusion and annealing, refine the microstructure, and help improve the matrix strength, compensating for the shortcomings of single Mg solid solution strengthening. On the other hand, the uniform precipitation of the dispersed phase can optimize the grain boundary state and improve the pipe's resistance to exfoliation corrosion. In this embodiment, the Cr content is controlled at 0.20-0.30%, which is precisely matched with the Mg content of 2.25-2.35%. If the Cr content is too low, the dispersed phase precipitation will be insufficient, and the effect of microstructure refinement and corrosion performance improvement will be limited. If the Cr content is too high, it is easy to form coarse needle-like Cr phases, which will cut the matrix and reduce plasticity and surface quality. At the same time, the stability of Mg content is a prerequisite for the uniform precipitation of Cr phase. Mg segregation will lead to local Cr phase agglomeration and growth, losing the dispersion strengthening effect. Therefore, the two need to be controlled and matched simultaneously.

[0030] Furthermore, this embodiment strictly limits the content of impurity elements such as Si and Fe. Si readily combines with Mg to form the Mg2Si phase, consuming dissolved Mg atoms and weakening the solid solution strengthening effect. Simultaneously, Si and Fe together form a needle-like β-AlFeSi hard and brittle phase, which distributes along the metal flow lines during extrusion, disrupting the matrix continuity and leading to defects such as streaks, peeling, and microcracks on the pipe surface, reducing surface finish and dimensional accuracy. Impurity atoms such as Fe and Si, and the resulting second phase, are the core sources of electron scattering, significantly increasing the probability of lattice electron scattering, reducing alloy conductivity, and increasing eddy current losses and temperature rise during GIL shell operation. Using Si ≤ 0.10% and Fe ≤ 0.30% as control thresholds can significantly reduce the formation of the hard and brittle second phase, ensuring the quality of the extruded surface, while simultaneously reducing electron scattering effects, stabilizing the pipe's electrical conductivity, and indirectly ensuring the effective solid solution concentration of Mg.

[0031] Preferably, the ingredients can be: Si: ≤0.08%, Fe: ≤0.20%, Cu: ≤0.05%, Mn: ≤0.05%, Mg: 2.25%~2.30%, Cr: 0.24%~0.30%, Zn: ≤0.05%, single impurity: ≤0.05%, total impurities: ≤0.15%, and the balance is Al.

[0032] More preferably, the ingredients can be: Si: ≤0.05%, Fe: ≤0.15%, Cu: ≤0.03%, Mn: ≤0.03%, Mg: 2.25%~2.28%, Cr: 0.25%~0.28%, Zn: ≤0.03%, single impurity: ≤0.05%, total impurities: ≤0.15%, and the balance is Al.

[0033] S2. Melting and casting: The aluminum alloy raw materials prepared in step S1 are placed into a melting furnace for melting and casting to obtain a casting rod.

[0034] S3. Homogenization of the casting rod: The casting rod obtained in step S2 is homogenized to obtain the ingot. The homogenization temperature is 470±3℃ and the homogenization time is 11~12h. More preferably, the homogenization temperature is 470℃ and the homogenization time is 12h. Homogenization can eliminate segregation inside the ingot, especially the core segregation of Mg element. Conventional casting is prone to low Mg content in the core. Homogenization can make Mg and Cr elements evenly distributed, ensuring that the overall deformation resistance of the ingot is consistent, reducing the extrusion breakthrough pressure, and providing a uniform microstructure for subsequent extrusion processes.

[0035] S4. Extrusion: The ingot obtained in step S3 is placed into an extrusion apparatus for extrusion molding to obtain a tube. The temperature of the extrusion die is set to 480–500°C, the temperature of the ingot is set to 510–530°C, the extrusion speed of the extrusion apparatus is set to 0.8–1.0 m / min, and the extrusion ratio is 15–16, more preferably 15.7. In this embodiment, a specific extrusion process window is designed for the characteristics of large diameter and thin wall of GIL tubes: a relatively high ingot temperature of 510–530°C and a die temperature of 480–500°C are set to ensure that the alloy is in the optimal plastic processing temperature range and reduce deformation resistance. A relatively low product speed is used, and by controlling the extrusion speed to 0.8–1.0 m / min, overheating due to deformation heat is prevented, avoiding surface carbonization and black spot defects.

[0036] In one embodiment, a 6-series alloy ingot, such as a 6063 ingot, is used for initial die preparation. After the extrusion stabilizes, the process switches to a 5052 ingot to reduce the initial breakthrough pressure. Utilizing the high rigidity of the 90MN large-tonnage extruder, combined with an extrusion ratio of 15.7, the metal flow lines are continuously distributed along the pipe's axial direction, thus eliminating the weak point of the weld seam from a mechanistic perspective.

[0037] S5. Quenching, online drawing and length cutting: Quench the tube obtained in step S5, and then cut the quenched tube into the specified length after stretching and straightening.

[0038] S6. Finished Product Annealing: The cut tubing obtained in step S5 is annealed at (350±3)℃ for 1 hour, more preferably at 350℃ for 1 hour, and then slowly cooled to room temperature to obtain GIL shell tubing. This embodiment uses a low-temperature annealing process of 350℃ for 1 hour instead of the traditional full annealing. This eliminates residual stress generated during extrusion while retaining some work hardening effect. Simultaneously, aging allows the Mg-Cr phase to precipitate diffusely, ensuring the material has excellent ductility and high conductivity, meeting the dual requirements of the power industry for conductivity and mechanical strength.

[0039] In this application, the entire process is coupled: the four processes of component design, homogenization treatment, extrusion molding, and low-temperature annealing do not act independently, but are an organic whole that mutually restricts and synergistically enhances each other, jointly achieving a balance between the stability and overall performance of the pipe forming. Any deviation in the parameters of any process will disrupt the overall performance balance and prevent the desired effect from being achieved. Specifically:

[0040] In composition design, the Mg content (2.25-2.35%) determines the alloy's solid solution strengthening potential and hot deformation behavior, the Cr content (0.20-0.30%) sets the upper limit for dispersion strengthening, and the levels of impurities such as Si and Fe define the ceiling for electrical conductivity. Once the composition deviates from the design window, subsequent process adjustments cannot compensate for the loss of the performance baseline. In the homogenization process, the 470℃×12h homogenization regime aims to eliminate Mg dendritic segregation in the ingot, allowing Mg atoms to diffuse from grain boundary enrichment areas into the grain interior, achieving compositional homogenization. This step is indispensable because Mg segregation in the as-cast state directly leads to two consequences: first, areas with excessively high Mg concentrations are prone to low-melting-point eutectic melting during subsequent extrusion heating; second, areas with excessively low Mg concentrations suffer from insufficient solid solution strengthening and uneven extrusion stress distribution. Only after sufficient homogenization, with Mg uniformly distributed in the matrix, can stable and controllable rheological stress and a uniform microstructure be obtained during subsequent extrusion. If the homogenization temperature is too low or the time is insufficient, residual Mg segregation will significantly increase the extrusion breakthrough pressure and cause the pipe wall thickness tolerance to become uncontrollable. If the homogenization temperature is too high, such as exceeding 575℃, overheating may occur, leading to ingot scrap. During extrusion molding, the extrusion process transforms the homogenized ingot into a pipe with a continuous axial streamline structure. The selection of extrusion temperature must consider two constraints simultaneously: if the temperature is too low, the deformation resistance will be too high, and the breakthrough pressure will increase; if the temperature is too high, the deformation heat will accumulate, leading to local overheating and surface black spot defects. The extrusion speed also has upper and lower limits; if the speed is too fast, it will aggravate the deformation heat effect, while if the speed is too slow, the production efficiency will not meet the needs of industrialization. More importantly, during the extrusion process, the solid solution state of solute atoms such as Mg and Cr is "frozen" in the matrix, providing initial conditions for the precipitation behavior during subsequent annealing—the extrusion exit temperature directly affects the nucleation density and distribution uniformity of the precipitated phases during annealing. During finished product annealing, the low-temperature annealing at 350℃ for 1 hour is neither traditional full annealing nor simple stress-relief annealing, but a precise heat treatment that combines all three. Its multiple functions include: eliminating residual extrusion stress, inducing partial recrystallization to restore plasticity, and promoting the dispersed precipitation of the Mg-Cr phase through low-temperature aging. The choice of annealing temperature is directly constrained by the preceding processes. If the extrusion exit temperature is too high, resulting in grain coarsening, low-temperature annealing cannot refine the grains; if homogenization is insufficient, leading to residual Mg segregation, the β phase will preferentially precipitate along the segregation band during annealing, impairing corrosion resistance. Therefore, the 350℃ for 1 hour annealing regime is the "optimal solution" only established under the premise that the aforementioned composition design, homogenization regime, and extrusion process have all been precisely executed. Deviation from any preceding parameter will render this annealing regime ineffective.

[0041] The GIL casing tubing produced using this embodiment has a wall thickness tolerance of ±0.3mm, requires no secondary processing, has an electrical conductivity of 30MS / m, exhibits a peel corrosion rating of PB or higher, and demonstrates excellent overall performance, meeting the GIL casing industry standards.

[0042] Example 2: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, including the following steps: S1. Batching: Prepare aluminum alloy raw materials according to the weight ratios in Table 1:

[0043] Table 1 Aluminum Alloy Raw Material Proportions

[0044]

[0045] S2. Melting and casting: The aluminum alloy raw material prepared in step S1 is placed into a melting furnace for melting and casting to obtain a casting rod;

[0046] S3. Homogenization of casting rod: The casting rod obtained in step S2 is homogenized to obtain an ingot. The homogenization temperature is 470℃ and the homogenization time is 12h.

[0047] S4. Extrusion: A 9000T horizontal extrusion press is used to produce GIL shell profiles with an outer dimension of Φ402mm and a wall thickness of 11mm. For 6063 ingot casting, a 700mm long casting rod is used, with a casting rod heating temperature of T520 / W511℃, a die heating temperature of 495℃, an extrusion barrel temperature of 448℃, and an extrusion speed of 1.2m / min. For 5-series ingot casting, a 960mm long casting rod is used, with a casting rod heating temperature of T519 / W510℃ and an extrusion speed of 0.9m / min.

[0048] S5. Quenching, online drawing and length cutting: The tube obtained in step S5 is quenched, and the quenched tube is stretched and straightened before being cut into the specified length.

[0049] S6. Finished product annealing: The cut tubing obtained in step S5 is annealed at 350℃ for 1 hour and then slowly cooled to room temperature to obtain GIL shell tubing.

[0050] Mechanical properties were tested on the GIL casing tubing produced in this embodiment. Testing equipment: AG-X 100KN electronic universal testing machine. Testing method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 2.

[0051] Table 2 Mechanical property results

[0052]

[0053] High-magnification microstructure testing was performed on the GIL casing tubing produced in this embodiment: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products microstructure inspection methods—Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 3:

[0054] Table 3 Metallographic high-magnification results

[0055]

[0056] The conductivity of the GIL casing tubing produced in this embodiment was tested: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 4:

[0057] Table 4 Conductivity Test Results

[0058]

[0059] Intergranular corrosion testing was performed on the GIL casing tubing produced in this embodiment. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 5.

[0060] Table 5 Results of intergranular corrosion test

[0061]

[0062] Example 3: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, including the following steps: S1. Batching: Prepare aluminum alloy raw materials according to the weight ratios in Table 6:

[0063] Table 6 Aluminum Alloy Raw Material Proportions

[0064]

[0065] S2. Melting and casting: The aluminum alloy raw material prepared in step S1 is placed into a melting furnace for melting and casting to obtain a casting rod;

[0066] S3. Homogenization of casting rod: The casting rod obtained in step S2 is homogenized to obtain an ingot. The homogenization temperature is 470℃ and the homogenization time is 12h.

[0067] S4. Extrusion: A 9000T horizontal extrusion press is used to produce GIL shell profiles with an outer dimension of Φ402mm and a wall thickness of 11mm. For 6063 ingot casting, a 700mm long casting rod is used, with a casting rod heating temperature of T523 / W510℃, a die heating temperature of 485℃, an extrusion barrel temperature of 442℃, and an extrusion speed of 1.0m / min. For 5-series ingot casting, a 960mm long casting rod is used, with a casting rod heating temperature of T522 / W511℃ and an extrusion speed of 0.9m / min.

[0068] S5. Quenching, online drawing and length cutting: The tube obtained in step S5 is quenched, and the quenched tube is stretched and straightened before being cut into the specified length.

[0069] S6. Finished product annealing: The cut tubing obtained in step S5 is annealed at 350℃ for 1 hour and then slowly cooled to room temperature to obtain GIL shell tubing.

[0070] Mechanical properties were tested on the GIL casing tubing produced in this embodiment. Testing equipment: AG-X 100KN electronic universal testing machine. Testing method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 7.

[0071] Table 7 Mechanical property results

[0072]

[0073] High-magnification microstructure testing was performed on the GIL casing tubing produced in this embodiment: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products microstructure inspection methods—Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 8:

[0074] Table 8 Metallographic High Magnification Results

[0075]

[0076] The conductivity of the GIL casing tubing produced in this embodiment was tested: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 9:

[0077] Table 9 Conductivity Test Results

[0078]

[0079] Intergranular corrosion testing was performed on the GIL casing tubing produced in this embodiment. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 10.

[0080] Table 10 Intergranular corrosion test results

[0081]

[0082] Example 4: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the Cr content in this example is 0.24%.

[0083] Mechanical properties were tested on the GIL casing tubing produced in this embodiment. Testing equipment: AG-X 100KN electronic universal testing machine. Testing method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 11.

[0084] Table 11 Mechanical property results

[0085]

[0086] High-magnification microstructure testing was performed on the GIL casing tubing produced in this embodiment: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products microstructure inspection methods—Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 12:

[0087] Table 12 Metallographic High Magnification Results

[0088]

[0089] The conductivity of the GIL casing tubing produced in this embodiment was tested: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 13.

[0090] Table 13 Conductivity Test Results

[0091]

[0092] Intergranular corrosion testing was performed on the GIL casing tubing produced in this embodiment. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 14.

[0093] Table 14 Intergranular corrosion test results

[0094]

[0095] Example 5: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing. The method described in Example 2 is used, except that in Example 2, Cr is 0.30% and Fe is 0.20%.

[0096] Mechanical properties were tested on the GIL casing tubing produced in this embodiment. Testing equipment: AG-X 100KN electronic universal testing machine. Testing method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 15.

[0097] Table 15 Mechanical property results

[0098]

[0099] High-magnification microstructure testing was performed on the GIL casing tubing produced in this embodiment: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products microstructure inspection methods—Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 16:

[0100] Table 16 Metallographic High Magnification Results

[0101]

[0102] The conductivity of the GIL casing tubing produced in this embodiment was tested: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 17.

[0103] Table 17 Conductivity Test Results

[0104]

[0105] Intergranular corrosion testing was performed on the GIL casing tubing produced in this embodiment. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 18.

[0106] Table 18 Intergranular corrosion test results

[0107]

[0108] Example 6: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the Cr content in this example is 0.25%.

[0109] Mechanical properties were tested on the GIL casing tubing produced in this embodiment. Testing equipment: AG-X 100KN electronic universal testing machine. Testing method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 19.

[0110] Table 19 Mechanical property results

[0111]

[0112] High-magnification microstructure testing was performed on the GIL casing tubing produced in this embodiment: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products microstructure inspection methods—Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 20:

[0113] Table 20 Metallographic High Magnification Results

[0114]

[0115] The conductivity of the GIL casing tubing produced in this embodiment was tested: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 21:

[0116] Table 21 Conductivity Test Results

[0117]

[0118] Intergranular corrosion testing was performed on the GIL casing tubing produced in this embodiment. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 22.

[0119] Table 22 Intergranular corrosion test results

[0120]

[0121] Example 7: This example provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing. The method described in Example 2 is used, except that the Cr content in this example is 0.28% and the Fe content is 0.15%.

[0122] Mechanical properties were tested on the GIL casing tubing produced in this embodiment. Testing equipment: AG-X 100KN electronic universal testing machine. Testing method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 23.

[0123] Table 23 Mechanical property results

[0124]

[0125] High-magnification microstructure testing was performed on the GIL casing tubing produced in this embodiment: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products microstructure inspection methods—Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 24:

[0126] Table 24 Metallographic High Magnification Results

[0127]

[0128] The conductivity of the GIL casing tubing produced in this embodiment was tested: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 25.

[0129] Table 25 Conductivity Test Results

[0130]

[0131] Intergranular corrosion testing was performed on the GIL casing tubing produced in this embodiment. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 26.

[0132] Table 26 Intergranular corrosion test results

[0133]

[0134] Comparative Example 1 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the Mg content in this comparative example is 2.10%.

[0135] Mechanical properties were tested on the GIL casing tubing produced in this comparative example. Testing equipment: AG-X 100KN electronic universal testing machine. Test method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 27.

[0136] Table 27 Mechanical Performance Results

[0137]

[0138] High-magnification microstructure testing was performed on the GIL casing tubing produced in this comparative example. Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products – Microstructure inspection methods – Part 1: Microstructure inspection methods. The high-magnification metallographic microstructure results are shown in Table 28.

[0139] Table 28 Metallographic High Magnification Results

[0140]

[0141] Conductivity tests were performed on the GIL casing tubing produced in this comparative example: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 29.

[0142] Table 29 Conductivity Test Results

[0143]

[0144] Intergranular corrosion testing was conducted on the GIL casing tubing produced in this comparative example. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 30.

[0145] Table 30 Intergranular corrosion test results

[0146]

[0147] When the Mg content is less than 2.25%, the solid solution strengthening effect is insufficient, the high-temperature rheological stress of the alloy decreases significantly, the low matrix strength leads to metal flow instability, the yield strength (Rp0.2) is far below the target value ≥70MPa, and the extrusion pressure is abnormal during the extrusion process.

[0148] Comparative Example 2 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the Mg content in this comparative example is 2.50%.

[0149] Mechanical properties were tested on the GIL casing tubing produced in this comparative example. Testing equipment: AG-X 100KN electronic universal testing machine. Test method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 31.

[0150] Table 31 Mechanical property results

[0151]

[0152] High-magnification microstructure testing was performed on the GIL casing tubing produced in this comparative example: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products - Microstructure inspection methods - Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 32:

[0153] Table 32 Metallographic High Magnification Results

[0154]

[0155] Conductivity tests were performed on the GIL casing tubing produced in this comparative example: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 33.

[0156] Table 33 Conductivity Test Results

[0157]

[0158] Intergranular corrosion testing was conducted on the GIL casing tubing produced in this comparative example. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 34.

[0159] Table 34 Intergranular corrosion test results

[0160]

[0161] When the Mg content exceeds 2.35%, the alloy's plasticity decreases sharply, the hot working window narrows, and the tendency for hot cracking increases significantly. The elongation after fracture is far below the requirement of ≥10%, and the intergranular corrosion grade drops to PC level.

[0162] Comparative Example 3 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the Cr content in this comparative example is 0.12%.

[0163] Mechanical properties were tested on the GIL casing tubing produced in this comparative example. Testing equipment: AG-X 100KN electronic universal testing machine. Test method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 35.

[0164] Table 35 Mechanical property results

[0165]

[0166] High-magnification microstructure testing was performed on the GIL casing tubing produced in this comparative example: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products - Microstructure inspection methods - Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 36:

[0167] Table 36 Metallographic High-Magnification Structure Results

[0168]

[0169] Conductivity tests were performed on the GIL casing tubing produced in this comparative example: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 37.

[0170] Table 37 Conductivity Test Results

[0171]

[0172] Intergranular corrosion testing was conducted on the GIL casing tubing produced in this comparative example. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 38.

[0173] Table 38 Intergranular corrosion test results

[0174]

[0175] When the Cr content is less than 0.20%, the dispersed phase precipitation is insufficient, which cannot effectively pin dislocations and grain boundaries. Grain growth is severe during extrusion and annealing, and the elongation strength is only 62~66MPa, which is lower than the target value of ≥70MPa.

[0176] Comparative Example 4 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the homogenization temperature in this comparative example is 540°C and the homogenization time is 16 hours.

[0177] Mechanical properties were tested on the GIL casing tubing produced in this comparative example. Testing equipment: AG-X 100KN electronic universal testing machine. Test method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 39.

[0178] Table 39 Mechanical property results

[0179]

[0180] High-magnification microstructure testing was performed on the GIL casing tubing produced in this comparative example: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products - Microstructure inspection methods - Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 40:

[0181] Table 40 Metallographic High Magnification Results

[0182]

[0183] Conductivity tests were performed on the GIL casing tubing produced in this comparative example: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 41.

[0184] Table 41 Conductivity Test Results

[0185]

[0186] Intergranular corrosion tests were conducted on the GIL casing tubing produced in this comparative example. Test equipment: digital display constant temperature water bath. Test method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 42.

[0187] Table 42 Intergranular corrosion test results

[0188]

[0189] The homogenization temperature of 540℃ severely damages the mechanical properties and corrosion resistance of the alloy, with a yield strength of only 64~68MPa, which does not meet the requirement of ≥70MPa, and the intergranular corrosion level drops to PC level.

[0190] Comparative Example 5 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the extrusion speed in this comparative example is 2.0 m / min.

[0191] Excessive extrusion speed leads to rapid accumulation of deformation, severely increasing extrusion pressure and causing stagnation, making it impossible to extrude the finished GIL shell.

[0192] Comparative Example 6 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the extrusion speed in this comparative example is 0.3 m / min.

[0193] Excessive extrusion speed results in the metal remaining in the extrusion cylinder for too long, causing a significant drop in temperature, increased deformation resistance, and higher extrusion pressure. At the same time, the metal flow becomes discontinuous, making it difficult to extrude the pipe.

[0194] Comparative Example 7 provides a method for preparing 5-series aluminum alloy extruded tubing for GIL casing, using the method described in Example 2. The difference from Example 2 is that the annealing process in this comparative example is the conventional full annealing process at 410°C for 2 hours.

[0195] Mechanical properties were tested on the GIL casing tubing produced in this comparative example. Testing equipment: AG-X 100KN electronic universal testing machine. Test method: GB / T16865-2013 "Tension Test Specimens and Methods for Processed Articles of Wrought Aluminum, Magnesium and Their Alloys". The mechanical test results are shown in Table 43.

[0196] Table 43 Mechanical property results

[0197]

[0198] High-magnification microstructure testing was performed on the GIL casing tubing produced in this comparative example: Testing equipment: AXIO universal research-grade inverted materials microscope. Testing standard: GB / T6892-2015 General industrial aluminum and aluminum alloy extruded profiles. Testing method: GB / T3246.1-2012 Deformed aluminum and aluminum alloy products - Microstructure inspection methods - Part 1: Microstructure inspection methods. The metallographic high-magnification microstructure results are shown in Table 44:

[0199] Table 44 Metallographic High Magnification Results

[0200]

[0201] Conductivity tests were performed on the GIL casing tubing produced in this comparative example: Testing equipment: SMP-10 eddy current conductivity meter. Testing method: GB / T / 12966-2022 "Eddy current test method for conductivity of aluminum and aluminum alloys". The conductivity test results are shown in Table 45.

[0202] Table 45 Conductivity Test Results

[0203]

[0204] Intergranular corrosion testing was conducted on the GIL casing tubing produced in this comparative example. Testing equipment: digital display constant temperature water bath. Testing method: GB / T22639-2022 "Peel Corrosion Test Method for Aluminum Alloy Products". The intergranular corrosion test results are shown in Table 46.

[0205] Table 46 Intergranular corrosion test results

[0206]

[0207] Traditional full annealing at 410℃ for 2 hours resulted in complete recrystallization of the alloy, leading to abnormally coarse grains and a sharp drop in yield strength to 54-58 MPa, far below the target value of ≥70 MPa. Simultaneously, the electrical conductivity decreased to approximately 28.50 MS / m, and the intergranular corrosion level dropped to PC grade.

[0208] The embodiments of the present invention are given for illustrative and descriptive purposes only, and are not intended to be exhaustive or to limit the invention to the forms disclosed. Many modifications and variations will be apparent to those skilled in the art. The embodiments were chosen and described in order to better illustrate the principles and practical application of the invention, and to enable those skilled in the art to understand the invention and to design various embodiments with various modifications suitable for a particular purpose.

Claims

1. A method for preparing a 5-series aluminum alloy extruded tube for a GIL casing, characterized in that, Includes the following steps: S1. Batching: Prepare aluminum alloy raw materials according to the following weight ratios: Si: ≤0.10%, Fe: ≤0.30%, Cu: ≤0.06%, Mn: ≤0.06%, Mg: 2.25%~2.35%, Cr: 0.20%~0.30%, Zn: ≤0.06%, Single impurity: ≤0.05%, Total impurities: ≤0.15%, Balance: Al; S2. Melting and casting: The aluminum alloy raw material prepared in step S1 is placed into a melting furnace for melting and casting to obtain a casting rod; S3. Homogenization of casting rod: The casting rod obtained in step S2 is homogenized to obtain an ingot. The homogenization temperature is 470±3℃ and the homogenization time is 11~12h. S4. Extrusion: The ingot obtained in step S3 is placed into an extrusion device for extrusion molding to obtain a pipe. The temperature of the extrusion die is set to 480-500℃, the temperature of the ingot is set to 510-530℃, the extrusion speed of the extrusion device is set to 0.8-1.0m / min, and the extrusion ratio is 15-16. S5. Quenching, online drawing and length cutting: The tube obtained in step S5 is quenched, and the quenched tube is stretched and straightened before being cut into the specified length. S6. Finished product annealing: The cut tubing obtained in step S5 is annealed at (350±3)℃ for 1 hour and slowly cooled to room temperature to obtain GIL shell tubing.

2. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S1, the ingredients are: Si: ≤0.08%, Fe: ≤0.20%, Cu: ≤0.05%, Mn: ≤0.05%, Mg: 2.25%~2.30%, Cr: 0.24%~0.30%, Zn: ≤0.05%, single impurity: ≤0.05%, total impurities: ≤0.15%, and the balance is Al.

3. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S1, the ingredients are: Si: ≤0.05%, Fe: ≤0.15%, Cu: ≤0.03%, Mn: ≤0.03%, Mg: 2.25%~2.28%, Cr: 0.25%~0.28%, Zn: ≤0.03%, single impurity: ≤0.05%, total impurities: ≤0.15%, and the balance is Al.

4. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S3, the homogenization temperature is 470℃ and the homogenization time is 12h.

5. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S4, before extruding the ingot, a 6-series alloy ingot is used for die forming. After the extrusion is stable, the process is switched to the ingot obtained in step S2.

6. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 5, characterized in that, The 6-series alloy ingot is a 6063 ingot.

7. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S4, extrusion is performed using a 90MN extruder.

8. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S4, the extrusion ratio is 15.

7.

9. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S6, the annealing process is 350℃ for 1 hour.

10. The method for preparing a 5-series aluminum alloy extruded tube for a GIL casing according to claim 1, characterized in that, In step S6, the wall thickness tolerance of the tubing used for the GIL casing is ±0.3 mm, and the electrical conductivity is 30 MS / m.