An ultra-thin-walled aluminum alloy bent pipe, its processing method and application
By employing low-temperature pretreatment, multi-pass progressive bending, and low-temperature stabilization treatment, the quality and consistency issues in the processing of ultra-thin-walled aluminum alloy bent tubes have been resolved, enabling the production of high-precision and high-strength aluminum alloy bent tubes suitable for high-end equipment applications.
Patent Information
- Application Number
- CN202611284185.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing processes for processing ultra-thin-walled aluminum alloy bent tubes suffer from problems such as easy wrinkling, easy cracking, large springback, large residual stress, poor consistency in batch production, and low production efficiency, which cannot meet the precision assembly requirements of high-end fields such as new energy vehicles and 3C electronics.
The processing method combines low-temperature pretreatment, multi-pass progressive bending, low-temperature stabilization treatment and springback compensation. The pretreatment eliminates residual stress during forming, the multi-pass progressive bending evenly distributes the deformation, springback compensation is performed after bending, and finally low-temperature stabilization treatment is performed to maintain the strength of the aluminum alloy and eliminate residual stress.
It significantly improves the finished product qualification rate and dimensional accuracy of ultra-thin-walled aluminum alloy bent tubes, maintains good mechanical properties, and has good long-term stability. It is suitable for high-end equipment such as battery cooling pipes for new energy vehicles, precision structural components for 3C electronics, lightweight photovoltaic brackets, and rail transit cable trays.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of aluminum alloy pipe processing, and in particular to an ultra-thin-walled aluminum alloy bent pipe, its processing method, and its application. Background Technology
[0002] 6XXX series aluminum alloys (represented by 6063) have become core materials for lightweighting in high-end equipment such as new energy vehicle battery cooling pipes, precision structural components for 3C electronics, lightweight photovoltaic brackets, and rail transit cable trays due to their advantages such as low density, high strength, and good corrosion resistance. Among them, ultra-thin-walled aluminum alloy bent tubes with a wall thickness of ≤1.5mm can maximize weight reduction, and the market demand is growing at an average annual rate of over 20%.
[0003] Currently, the mainstream manufacturing process for aluminum alloy bent tubes in the industry is the single-stage high-pressure bending process: the tube is clamped between a fixed mold and a movable mold, and the movable mold is driven by a hydraulic cylinder to complete the bending deformation in one go. After bending, it cools naturally to obtain the finished product. After years of development, this process has been successfully applied in the manufacturing of thick-walled aluminum alloy bent tubes with a wall thickness of ≥2.0mm, and can meet the basic needs of the low-to-mid-end market.
[0004] Regarding springback control, traditional processes primarily employ an offline, experience-based pre-compensation method: This involves statistically analyzing the average springback amount under specific material, wall thickness, and bending radius through small-batch trial production. A compensation value greater than the target angle is then pre-set in the bending process, relying on experience to offset the springback deformation. For residual stress control, some companies use high-temperature aging treatments above 150℃. However, this process leads to a decrease in the strength of the aluminum alloy and cannot completely eliminate the residual stress generated during bending.
[0005] However, existing processes have significant limitations for ultra-thin-walled aluminum alloy pipes with a wall thickness of ≤1.5mm. These limitations are mainly manifested in the following ways: Traditional single-bending high-pressure bending processes result in concentrated deformation, failing to resolve the inherent problems of wrinkling, cracking, and high springback in ultra-thin-walled aluminum alloy pipes. This leads to a finished product pass rate of only 70%-85%, and dimensional accuracy is difficult to consistently reach IT8 level, failing to meet the precision assembly requirements of high-end fields such as new energy vehicles and 3C electronics. During a single bend, local deformation of the pipe exceeds its plastic limit, causing internal metal buildup that easily leads to wrinkles (10%-20% scrap rate due to wrinkles), while excessive tensile stress on the external side easily causes cracking. Uneven deformation results in large fluctuations in springback, which traditional offline pre-compensation cannot accurately control, with finished product springback generally ≥±1.0°. Several other minor issues also exist. 1. High residual stress and poor long-term dimensional stability: After bending, there is a residual stress of up to 70-90MPa inside the pipe, which will be slowly released during use, causing the product dimensions to gradually deform and affecting the long-term reliability of the equipment. 2. Poor consistency in batch production: Process parameters are extremely sensitive to fluctuations in material properties and changes in ambient temperature. The springback and cross-sectional accuracy of different batches of products vary greatly, which cannot meet the quality requirements of large-scale production. 3. Disconnected process links: Bending, inspection and stabilization processes are independent of each other, requiring manual transfer and parameter setting, resulting in low production efficiency and easy introduction of human error and secondary damage; 4. Existing stabilization processes have significant side effects: High-temperature aging treatment at temperatures above 150℃ can reduce the tensile strength of aluminum alloys by 15%-20%, thus reducing the mechanical properties of the products.
[0006] Therefore, improvements to the existing processes are still necessary. Summary of the Invention
[0007] The main objective of this application is to provide a processing method for ultra-thin-walled aluminum alloy bent pipes, which aims to solve the technical problem of poor quality of ultra-thin-walled aluminum alloy bent pipes obtained by existing methods.
[0008] To achieve the above objectives, the technical solution provided by the present invention is as follows: In a first aspect, the present invention provides a method for processing an ultra-thin-walled aluminum alloy bent tube, wherein the wall thickness of the ultra-thin-walled aluminum alloy bent tube is 0.8-1.5 mm, comprising the following steps: Pretreatment: The pipe blank is pretreated to obtain the pipe to be bent. The pretreatment includes annealing the pipe blank at 80-120℃ after extrusion. Bending: The pipe to be bent is bent multiple times through a mold, and then springback compensation is performed to obtain the bent pipe. Stabilization treatment: The bent pipe is kept at 90-110℃ for stabilization treatment to obtain the aluminum alloy bent pipe.
[0009] The processing method of this invention first employs low-temperature treatment in the pretreatment process to ensure the strength of the aluminum alloy and eliminate residual stress from forming. Simultaneously, it combines multiple progressive bending passes to distribute the total deformation to each pass, resulting in no obvious wrinkles on the inner side and no cracking on the outer side. After bending, springback compensation is performed, and the amount of springback is strictly controlled. Finally, it undergoes low-temperature stabilization treatment and natural cooling to room temperature to ensure the strength of the aluminum alloy and eliminate residual stress from forming. The resulting tube has low springback, high dimensional accuracy, and long-term stability, while maintaining its mechanical properties. It is particularly suitable for processing ultra-thin-walled aluminum alloy bent tubes.
[0010] Preferably, the tube blank is a 6XXX series aluminum alloy tube blank; more preferably, the 6XXX series aluminum alloy is 6061 or 6063.
[0011] Preferably, the outer diameter of the pipe blank is 10-50mm, such as 10mm, 20mm, 30mm, 40mm, 50mm, etc.
[0012] Preferably, the tensile strength of the pipe to be bent is ≥160MPa.
[0013] Preferably, the elongation after fracture of the pipe to be bent is ≥14%.
[0014] Preferably, the residual stress of the pipe to be bent is ≤15MPa.
[0015] Preferably, the straightness of the pipe to be bent is ≤0.8mm / m.
[0016] Preferably, the extrusion temperature is 450-550℃.
[0017] Preferably, the extrusion speed is 15-25 m / min.
[0018] Preferably, the annealing treatment at 80-120℃ takes 50-70 minutes.
[0019] Preferably, the stabilization treatment time is 45-75 minutes. The holding time can be shortened when the temperature is higher and extended when the temperature is lower; it can also be adjusted according to the batch size of the pipes. For larger batches, the holding time can be appropriately extended to ensure uniform temperature. Preferably, the temperature difference during stabilization treatment is ≤5℃.
[0020] Preferably, the pretreatment further includes adjusting the Si and Mg content in the tube billet before extrusion. In 6XXX series alloys, Mg and Si elements can form the Mg2Si strengthening phase. The content and ratio of these two elements directly determine the plasticity, strength, and residual stress of the tube, significantly affecting the bending springback, cross-sectional deformation, and finished product yield of the aluminum tube. A reasonable Mg and Si ratio results in uniform Mg2Si precipitation, uniform grain size after extrusion of the cast rod, and excellent performance indicators of the extruded tube. Preferably, the Si content is adjusted to 0.43-0.48 wt% and the Mg content to 0.62-0.68 wt%.
[0021] Preferably, the number of bending passes is 2-4, such as 2, 3, 4, etc., to distribute the total deformation amount to each pass.
[0022] Preferably, the bending angle of each pass is 1 / 4 to 1 / 2 of the total target angle; preferably, the bending angle of each pass is evenly distributed, such as a total bend of 90° divided into 3 passes of 30°.
[0023] Preferably, the bending and pressure holding time for each pass is 1-2 seconds.
[0024] Preferably, the bending speed is 8-12 mm / s.
[0025] Preferably, the bending thrust is 80-120N.
[0026] Preferably, the mold used for the multi-pass bending includes a mandrel, an anti-wrinkle mold, a fixed mold, a bending mold, and a guide mold. The mandrel is placed inside the cavity of the pipe to be bent to support the inner wall and prevent collapse. The anti-wrinkle mold surface matches the outer curvature of the pipe to be bent and is installed between the bending mold and the guide mold, closely adhering to the outer side of the pipe to suppress wrinkles during bending. The guide mold is located behind the anti-wrinkle mold and moves synchronously with the pipe feed direction via a guide rail or slider mechanism, serving as a guide and positioning function. The fixed mold is fixed to the inlet side of the bending mold and serves as a reference point for adjusting the mandrel extension amount (i.e., the distance the front end of the mandrel extends beyond the center of the fixed mold). This extension amount adjusts the fit between the anti-wrinkle mold and the pipe, ensuring that each module adapts to different bending angles and pipe diameters. The bending mold rotates and pulls the pipe to be bent, and the fixed mold rotates synchronously with the bending mold.
[0027] Preferably, the mandrel is a variable diameter combined mandrel with a multi-segment flexible hinge structure. The length of each segment is 0.7-0.9 times the outer diameter of the pipe to be bent, and the diameter of the mandrel is 0.1-0.2 mm smaller than the inner diameter of the pipe to be bent.
[0028] Preferably, the gap between the anti-wrinkle mold and the pipe is ≤0.05mm.
[0029] Preferably, the mandrel extension is 0.8-1.2 mm.
[0030] In this application, springback compensation is performed after the mold undergoes multiple bending processes.
[0031] Preferably, the rebound compensation rebound amount is controlled within ±0.5°.
[0032] Springback compensation can be based on a springback compensation prediction model. This model takes parameters such as pipe material, wall thickness, outer diameter, bending radius, and bending speed as input, automatically outputs the predicted springback amount, and combines this with actual detection data to provide an initial springback compensation angle. The model is continuously updated based on real-time detection results. The springback compensation prediction model can be established using regression analysis or based on neural network training. Preferably, a neural network model is used, as it can be trained based on more dimensional process data, improving prediction accuracy.
[0033] In some specific embodiments of this application, a CNC online springback compensation system is used to detect and correct springback errors in real time. The online springback compensation system includes a springback detection device and a springback compensation model. By inputting parameters such as pipe material, wall thickness, outer diameter, bending radius, and bending speed, the springback prediction model can provide a predicted springback amount. The detection device then detects the springback amount in real time and calculates the difference between the actual springback amount and the predicted springback amount. If the difference is greater than a set value, the springback prediction model parameters are automatically updated, and the initial compensation angle of the next workpiece is adjusted. If the actual springback amount is outside the ±0.5° range, it is determined to be a defective product, automatically marked, and diverted.
[0034] Preferably, the rebound amount is detected by a contact encoder or a laser angle. More preferably, a contact encoder is used for detection, which is less expensive and suitable for scenarios with slightly lower accuracy requirements.
[0035] In a second aspect, the present invention also provides an ultra-thin-walled aluminum alloy bent pipe processed by the above-described processing method.
[0036] Preferably, the tensile strength of the ultra-thin-walled aluminum alloy bend is ≥170MPa.
[0037] Preferably, the residual stress of the ultra-thin-walled aluminum alloy bend is ≤8.0MPa.
[0038] Preferably, after 1000 temperature cycles from -40℃ to 85℃, the dimensional change of the ultra-thin-walled aluminum alloy bend is ≤0.05mm.
[0039] Preferably, the roundness of the cross-section of the ultra-thin-walled aluminum alloy bend is ≤3%.
[0040] In a third aspect, the present invention also provides the application of the above-mentioned ultra-thin-walled aluminum alloy bent tube in new energy vehicle battery cooling pipes, 3C electronic precision structural components, photovoltaic lightweight brackets, and rail transit cable trays.
[0041] Compared with the prior art, the advantages of the present invention are as follows: 1) The processing method of this invention, through low-temperature pretreatment before bending combined with low-temperature stabilization treatment after bending, does not lead to a decrease in the strength of aluminum alloy. The resulting aluminum alloy bent tube has good mechanical strength retention, and the tensile strength of the finished product after bending remains above 170MPa. At the same time, the low-temperature stabilization treatment fully eliminates residual stress (92.7% of residual stress can be eliminated), and the residual stress can be reduced to 7.2MPa. The aluminum alloy bent tube has good long-term dimensional stability. After 1000 temperature cycle tests from -40℃ to 85℃, the dimensional change is ≤0.05mm, and there is no deformation after long-term use.
[0042] 2) The processing method of the present invention adopts multi-pass progressive bending to evenly disperse deformation stress, with no obvious wrinkles on the inner side and no cracks on the outer side. The resulting aluminum alloy bent tube has fewer forming defects, and the overall production qualification rate is increased from the traditional 70%-85% to ≥98%, which greatly reduces production costs.
[0043] 3) The processing method of the present invention adopts a springback compensation model to achieve adaptive optimization of parameters, effectively offsetting the influence of material performance fluctuations and environmental changes. The resulting aluminum alloy bent tubes have high consistency in batch production. When 1000 products are produced continuously, the springback fluctuation range is ≤0.1° and the cross-sectional roundness fluctuation range is ≤0.3%.
[0044] 4) The aluminum alloy bent pipes obtained by the processing method of this invention have excellent core precision indicators: the average springback of the finished product is 0.32°, which is stably controlled within the range of ≤±0.5°; the average roundness of the pipe section is 2.13%, which meets the design requirement of ≤3%; the dimensional accuracy stably reaches IT8 level, which meets the precision assembly requirements of high-end equipment.
[0045] In summary, it can be seen that the ultra-thin-walled aluminum alloy bent tubes obtained by the processing method of the present invention have good mechanical properties, high dimensional accuracy, and long-term stability. They can be used as core materials for lightweighting of high-end equipment such as battery cooling pipes for new energy vehicles, precision structural components for 3C electronics, lightweight photovoltaic brackets, and rail transit cable trays. Detailed Implementation
[0046] The following description, in conjunction with specific embodiments, illustrates the points. It should be noted that the following embodiments do not constitute a limitation on the scope of protection claimed by the present invention.
[0047] Unless otherwise specified, the raw materials, reagents or devices used in the following examples are available from conventional commercial sources or can be obtained by existing known methods.
[0048] Example 1: 90° bend of φ20mm×t1.2mm 6063 aluminum alloy tube 1) Preprocessing Prepare 6063 aluminum alloy tubing with an outer diameter of 20mm and a wall thickness of 1.2mm as tubing blank; The Si and Mg composition in the 6063 aluminum alloy tube blank was finely adjusted to Si: 0.45wt% and Mg: 0.65wt%. Then, the tube was extruded at 500℃ and 20m / min. After extrusion, it was subjected to low-temperature stress-relief annealing at 100℃ for 60min to obtain the tube to be bent. Its tensile strength was 162MPa, elongation after fracture was 16.2%, residual stress was 9.8MPa, and straightness was 0.68mm / m.
[0049] 2) Bending and springback compensation The bending die used includes a mandrel, an anti-wrinkle die, a fixed die, a bending die, and a guide die. The mandrel is placed inside the cavity of the pipe to be bent to support the inner wall and prevent collapse. The anti-wrinkle die surface matches the outer curvature of the pipe to be bent and is installed between the bending die and the guide die, closely adhering to the outer side of the pipe to suppress wrinkles during bending. The guide die is located behind the anti-wrinkle die and moves synchronously with the pipe feed direction via a guide rail or slider mechanism, serving as a guide and positioning function. The fixed die is fixed to the inlet side of the bending die and serves as a reference point for adjusting the mandrel extension amount (i.e., the distance the front end of the mandrel extends beyond the center of the fixed die). This extension amount adjusts the fit between the anti-wrinkle die and the pipe, ensuring that each module adapts to different bending angles and pipe diameters. The bending die rotates and pulls the pipe to be bent, forming the shape, while the fixed die rotates synchronously with the bending die.
[0050] After the pipe is fed in, the guide mold first presses and straightens the pipe, then the mandrel extends into the bending area to support and prevent collapse. The fixing mold closes and clamps the pipe end with the bending mold. Then the bending mold rotates and pulls the pipe to wind and form. During the bending process, the anti-wrinkle mold is close to the outside of the pipe to suppress wrinkles during bending. The guide mold continues to feed material.
[0051] The mandrel is a variable diameter combined mandrel with a 3-segment flexible hinge structure. The length of each segment is 0.8 times the outer diameter of the pipe to be bent, and the diameter of the mandrel is 0.1 mm smaller than the inner diameter of the pipe to be bent. The mandrel protrusion is 1.0 mm. The gap between the anti-wrinkle mold and the pipe is ≤0.05 mm.
[0052] During the bending process, a CNC online springback compensation system detects and corrects springback errors in real time, controlling the springback amount within ±0.5°. The online springback compensation system includes a springback detection device and a springback compensation model. The springback detection device is a laser sensor. The springback compensation model is a springback prediction model established using regression analysis based on over 1000 sets of test data from ultra-thin-walled aluminum alloy pipes with different materials, wall thicknesses, and bending radii. Input parameters include pipe material, wall thickness, outer diameter, bending radius, and bending speed, and the model can output the initial compensation angle. The detection device detects the springback amount in real time, calculates the difference between the actual and predicted springback amounts. If the difference is >0.1°, the springback prediction model parameters are automatically updated, and the initial compensation angle for the next workpiece is adjusted. If the actual springback amount is outside the ±0.5° range, the workpiece is judged as defective, automatically marked, and diverted.
[0053] First, the pipe to be bent obtained in step 1) is bent in 3 passes through the mold. The bending speed is 10mm / s and the pushing force is 100N. The first pass: bend to 30° and hold pressure for 1s; the second pass: bend to 60° and hold pressure for 1s; the third pass: initial compensation angle is 90.5° and hold pressure for 2s.
[0054] After the pressure holding period ended, the laser sensor detected that the actual springback angle was 90.18°, and the actual springback amount was calculated to be 0.32°. The difference between this and the predicted value of 0.5° was 0.18°. The system automatically updated the model parameters, and the initial compensation amount for the next workpiece was adjusted to 0.48°.
[0055] 3) Stabilization treatment: Qualified pipes are placed in a low-temperature oven and kept at 100℃ for 60 minutes. They are then naturally cooled to room temperature to obtain aluminum alloy bent pipes.
[0056] Test results: Tensile strength: 172MPa; Bending springback: 0.32°; Cross-sectional roundness: 2.08%; Residual stress: 7.2MPa; Dimensional accuracy: IT8 grade; 100% pass rate in continuous production of 100 pieces.
[0057] Example 2: 120° bend of φ15mm×t1.0mm 6063 aluminum alloy tube 1) Preprocessing Prepare 6063 aluminum alloy tubing with an outer diameter of 15mm and a wall thickness of 1.0mm as tubing blank; The Si / Mg composition of the 6063 aluminum alloy tube blank was finely adjusted to Si: 0.45% and Mg: 0.65%. An extrusion temperature of 500℃ and an extrusion speed of 20m / min were used. After extrusion, a low-temperature stress-relief annealing process was performed at 100℃ for 60min to obtain the tube to be bent. Its tensile strength was 164MPa, elongation after fracture was 16.2%, residual stress was 9.8MPa, and straightness was 0.68mm / m. 2) Bending and springback compensation The bending die and CNC online springback compensation system used are the same as in Example 1. The difference is that the mandrel extension of the bending die is 0.9 mm.
[0058] During the bending process, the rebound error is detected and corrected in real time by the CNC online springback compensation system, and the springback amount is controlled within ±0.5°.
[0059] First, the pipe to be bent obtained in step 1) is bent in 4 passes through the mold, each pass bending 30°, bending speed 9mm / s, and push force 90N. Pass 1: bend to 30° and hold pressure for 1s; Pass 2: bend to 60° and hold pressure for 1s; Pass 3: bend to 90° and hold pressure for 1s; Pass 4: initial compensation angle 120.6° and hold pressure for 2s.
[0060] After the pressure holding period ended, the laser sensor detected that the actual angle after the rebound was 120.19° and the actual rebound amount was 0.41°. The system automatically updated the model parameters.
[0061] 3) Stabilization treatment: Qualified pipes are placed in a low-temperature oven and kept at 100℃ for 55 minutes. They are then naturally cooled to room temperature to obtain aluminum alloy bent pipes.
[0062] Test results: tensile strength 172MPa, bending springback: 0.41°; cross-sectional roundness: 2.25%; residual stress: 7.8MPa; dimensional accuracy: IT8 grade; 100 pieces were produced continuously, with a pass rate of 99%.
[0063] Comparative Example 1: Traditional Single-Bending Process Using the same blank and mold as in Example 1, a single 90° bend was performed with an initial compensation angle of 91° and a bending speed of 10 mm / s. No low-temperature stabilization treatment was performed.
[0064] Finished product inspection results: bending springback 1.2°, cross-sectional roundness 5.6%, residual stress 82MPa, overall pass rate 78%.
[0065] Comparative Example 2: 90° bending test of 6063 aluminum tube without substrate optimization treatment Comparative Example 2-1 The difference from Example 1 is that step 1) does not include a low-temperature stress-relief annealing step; specifically: 1) Preprocessing Prepare 6063 aluminum alloy tubing with an outer diameter of 20mm and a wall thickness of 1.2mm as tubing blank; The Si and Mg composition in the 6063 aluminum alloy tube blank was finely adjusted to Si: 0.45wt% and Mg: 0.65wt%. The tube to be bent was extruded at an extrusion temperature of 500℃ and an extrusion speed of 20m / min. The tube had a tensile strength of 158MPa, an elongation after fracture of 11.5%, a residual stress of 42.6MPa, and a straightness of 2.12mm / m.
[0066] The remaining steps are the same.
[0067] Finished product test results: Tensile strength: 161MPa; bending springback: 0.76°; cross-sectional roundness: 3.92%; residual stress: 30.5MPa; dimensional accuracy: IT9; continuous production of 100 pieces with a pass rate of 86%.
[0068] Comparative Example 2-2 The difference from Example 1 is that the content of Si and Mg is not adjusted in step 1). Specifically: 1) Preprocessing Prepare 6063 aluminum alloy tubing with an outer diameter of 20mm and a wall thickness of 1.2mm as tubing blank; The extrusion temperature was 500℃ and the extrusion speed was 20m / min. The pipe to be bent was obtained by extrusion with a tensile strength of 160MPa, an elongation after fracture of 9.7%, a residual stress of 48.3MPa, and a straightness of 2.45mm / m.
[0069] The remaining steps are the same.
[0070] Finished product test results: Tensile strength: 164 MPa; bending springback: 0.93°; cross-sectional roundness: 4.65%; residual stress: 37.2 MPa; dimensional accuracy: IT10; continuous production of 100 pieces with a pass rate of 79%.
[0071] Comparative Example 3: Changing the stabilization treatment temperature Based on Example 1, the temperature of the stabilization process in step 3) is changed, and the remaining steps are the same as in Example 1.
[0072] Comparative Example 3-1: No stabilization treatment After bending in step 2), place the bent parts to cool naturally without putting them in an oven for insulation.
[0073] Pipe to be bent: tensile strength 160MPa, elongation after fracture 16.2%, residual stress 9.8MPa, straightness 0.68mm / m; Finished product inspection results: tensile strength 160MPa, springback 1.12°, cross-sectional roundness 3.15%, residual stress 36.8MPa, dimensional accuracy IT10; 83% pass rate out of 100 pieces produced continuously. Comparative Example 3-2: Lowering the stabilization treatment temperature 3) Stabilization treatment: Qualified pipes are placed in a low-temperature oven and kept at 60℃ for 60 minutes. They are then naturally cooled to room temperature to obtain aluminum alloy bent pipes.
[0074] Pipe to be bent: tensile strength 161MPa, elongation after fracture 16.2%, residual stress 9.8MPa, straightness 0.68mm / m; Finished product inspection results: tensile strength 164MPa, springback 0.71°, cross-sectional roundness 2.63%, residual stress 19.4MPa, dimensional accuracy IT10; 100 pieces were produced continuously, with a pass rate of 91%.
[0075] Comparative Example 3-3: High-temperature aging as a substitute for low-temperature stabilization (160℃ for 60 min) 3) Stabilization treatment: Qualified pipes are placed in a low-temperature oven and kept at 160℃ for 60 minutes. They are then naturally cooled to room temperature to obtain aluminum alloy bent pipes.
[0076] Pipe to be bent: tensile strength 162MPa, elongation after fracture 16.2%, residual stress 9.8MPa, straightness 0.68mm / m; Finished product inspection results: tensile strength 193MPa, springback 0.29°, but the pipe has slight age hardening; cross-sectional roundness 2.12%, residual stress 6.9MPa; the pipe surface has slight oxidation and graying, and micro-intergranular cracks appear in the bending area; dimensional accuracy IT10; 100 pipes were produced continuously, with a pass rate of 89%.
[0077] The main process conditions and performance statistics of each embodiment and comparative example are shown in Table 1.
[0078] The performance testing methods involved in Table 1 are explained below: Tensile strength and elongation after fracture: In accordance with GB / T 16865-2023 "Tension Test Specimens and Methods for Processed Products of Wrought Aluminum, Magnesium and Their Alloys", tensile specimens of profiles with a gauge length of 50 mm were prepared. Tensile tests were conducted at room temperature on a universal testing machine in accordance with GB / T 228.1-2021 "Metallic Materials - Tensile Testing - Part 1: Room Temperature Test Method" to determine the tensile strength and elongation after fracture.
[0079] Residual stress: Refer to YS / T 1634-2023 "Evaluation Method for Residual Stress of Aluminum and Aluminum Alloy Products" and measure residual stress according to the layer-by-layer method.
[0080] Straightness, cross-sectional roundness, and dimensional accuracy: Refer to GB / T 14846-2014 "Dimensional Deviations of Aluminum and Aluminum Alloy Extruded Profiles" and measure using micrometers, angle gauges, platforms, feeler gauges, roundness testers, etc.
[0081] Unless otherwise specified, all performance test results mentioned above are based on test results under room temperature conditions.
[0082] Table 1. Process conditions and performance statistics for the examples and comparative examples
[0083] A comparison of Example 1 and Comparative Example 1 shows that, compared to traditional single-bending without pre-bending low-temperature pretreatment and post-bending low-temperature stabilization treatment, the processing method of the present invention largely preserves the mechanical properties of ultra-thin-walled aluminum alloy bent pipes, reduces residual stress, and achieves good pipe processing accuracy and a high pass rate. A comparison of Example 1 and Comparative Examples 2-1 and 2-2 shows that adjusting the Si and Mg content and implementing low-temperature treatment during the pre-bending stage can greatly ensure pipe strength and reduce residual stress, thereby guaranteeing accuracy and dimensional stability during the bending process. Both are indispensable; the Si / Mg content affects the formation of the Mg2Si strengthening phase, and the low-temperature treatment affects the crystal form of the strengthening phase and residual stress, etc. The comparison between Example 1 and Comparative Examples 3-1, 3-2 and 3-3 shows that after bending, stabilization treatment at a suitable temperature can greatly improve residual stress, affecting tensile strength and bending performance. The temperature should not be too high or too low. If it is below 90℃, residual stress cannot be effectively eliminated. If it is above 110℃, aging will occur, the pipe surface will oxidize and turn gray, and cracks will appear.
[0084] This application's solution systematically addresses the cracking, springback fluctuations, and cross-sectional collapse issues of ultra-thin-walled aluminum tubes during bending by employing a combination of composition control, low-temperature stress-relief annealing, multi-pass bending, and springback compensation. The interrelationships of the various technical methods are as follows: (1) Si / Mg composition regulation and low temperature stress relief annealing: By rationally matching Si / Mg elements, the substrate can obtain the optimal match between strength and plasticity, reduce the residual stress of the base material, and provide a stable blank for bending; both are indispensable, and it is difficult to meet the requirements of high strength and large deformation capacity at the same time by single composition regulation or single annealing treatment.
[0085] (2) Optimize the substrate and multiple bending: By optimizing the substrate composition and annealing process, the plasticity of the substrate is improved. Combined with step-by-step multi-bending, the stress of a single deformation is reduced, and stress concentration cracking of the pipe wall is avoided.
[0086] (3) Multi-pass bending die coordination: During the bending process, the mandrel and anti-wrinkle die of the die form physical support for the inner and outer walls of the pipe, continuously suppressing the wrinkling of the pipe wall and the loss of roundness of the cross section during the gradual deformation process, ensuring the roundness and accuracy of the bending part.
[0087] (4) Strong plasticized substrate and stable bending process and online springback compensation closed loop: The low residual stress strong plasticized substrate combined with the multi-pass bending process greatly narrows the springback fluctuation. On this basis, the compensation angle is dynamically corrected by real-time iterative prediction model such as laser detection, and the springback is controlled within ±0.5°. Defective products are eliminated to form a closed loop control.
[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for processing ultra-thin-walled aluminum alloy bent pipes, characterized in that, The ultra-thin-walled aluminum alloy bend has a wall thickness of 0.8-1.5mm and includes the following steps: Pretreatment: The pipe blank is pretreated to obtain the pipe to be bent. The pretreatment includes annealing the pipe blank at 80-120℃ after extrusion. Bending: The pipe to be bent is bent multiple times through a mold, and then springback compensation is performed to obtain the bent pipe. Stabilization treatment: The bent pipe is kept at 90-110℃ for stabilization treatment to obtain the aluminum alloy bent pipe.
2. The processing method according to claim 1, characterized in that, The tube blank is a 6XXX series aluminum alloy tube blank; And / or, the outer diameter of the pipe blank is 10-50 mm; And / or, the pipe to be bent shall at least meet one of the following characteristics: a) tensile strength ≥ 160 MPa, b) elongation after fracture ≥ 14%, c) residual stress ≤ 15 MPa, d) straightness ≤ 0.8 mm / m.
3. The processing method according to claim 1, characterized in that, The extrusion temperature is 450-550℃. And / or, the extrusion speed is 15-25 m / min; And / or, the annealing treatment at 80-120℃ takes 50-70 minutes; And / or, the stabilization treatment time is 45-75 min.
4. The processing method according to claim 1, characterized in that, The pretreatment also includes adjusting the Si and Mg content in the tube blank before extrusion.
5. The processing method according to claim 1, characterized in that, The number of multiple bends is 2-4; And / or, the curvature angle for each pass is 1 / 4 to 1 / 2 of the total target angle; And / or, the bending pressure holding time for each pass is 1-2 seconds; And / or, the bending speed is 8-12 mm / s; And / or, the bending thrust is 80-120N.
6. The processing method according to claim 1, characterized in that, The dies used in the multi-pass bending include a mandrel, an anti-wrinkle die, a fixing die, a guide die, and a bending die; The mandrel is placed inside the cavity of the pipe to be bent. The anti-wrinkle model surface matches the outer curvature of the pipe to be bent, and is installed between the bending mold and the guide mold, closely adhering to the outer side of the pipe to be bent; The guide mold is located behind the anti-wrinkle mold and moves synchronously with the tube feeding direction via a guide rail or slider mechanism, serving as a guide and positioning mechanism; The fixed mold is fixed to the inlet side of the bending mold and serves as a reference point for adjusting the distance by which the front end of the mandrel extends beyond the center of the fixed mold, i.e., the mandrel extension amount. The fit between the anti-wrinkle mold and the outer side of the pipe to be bent is adjusted by the mandrel extension amount. The bending die rotates and pulls the pipe to be bent into shape, and the fixing die follows the bending die to rotate synchronously.
7. The processing method according to claim 6, characterized in that, The mandrel is a variable diameter composite mandrel with a multi-segment flexible hinge structure. The length of each segment is 0.7-0.9 times the outer diameter of the pipe to be bent, and the diameter of the mandrel is 0.1-0.2 mm smaller than the inner diameter of the pipe to be bent. And / or, the mandrel extension is 0.8-1.2 mm; And / or, the gap between the anti-wrinkle mold and the pipe is ≤0.05mm.
8. The processing method according to claim 1, characterized in that, The rebound compensation rebound amount is controlled within ±0.5°. And / or, the springback compensation is based on a springback prediction model, the input parameters of which include at least one of pipe material, wall thickness, outer diameter, bending radius, and bending speed, and the output parameter of the model is the initial compensation angle.
9. The ultra-thin-walled aluminum alloy bent tube obtained by the processing method according to any one of claims 1-8, wherein the aluminum alloy bent tube satisfies at least one of the following characteristics: A) Tensile strength at room temperature ≥170MPa; B) Residual stress ≤ 8.0 MPa; C) After 1000 cycles of temperature cycling from -40℃ to 85℃, the dimensional change is ≤0.05mm; D) Cross-sectional roundness ≤ 3%.
10. The application of the ultra-thin-walled aluminum alloy bent tube as described in claim 9 in new energy vehicle battery cooling pipes, 3C electronic precision structural components, photovoltaic lightweight brackets, and rail transit cable trays.