Hydraulic integrated multi-way valve casting process for excavator
By using 3D modeling design and layered core shooting molding, combined with exhaust column, overflow column and bottom pouring technology, the casting problem of hydraulic integral multi-way valve for excavators was solved, realizing high-precision, sand-free casting production and improving the reliability and durability of the valve body.
Patent Information
- Application Number
- CN202611480258.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for casting hydraulic integral multi-way valves for excavators face challenges such as difficulty in sand core forming, easy core breakage, porosity, shrinkage cavities, difficulty in cleaning sand from oil passages, and high dimensional accuracy requirements, resulting in insufficient valve body reliability and durability.
The sand core and gating system are designed using 3D modeling, layered core shooting molding, combined with venting columns and overflow columns, bottom pouring and chilling, and alloy element addition for efficient filling and solidification control. Finally, the oil passages are cleaned by high-frequency vibration and shot peening.
It achieves high precision and dense structure of sand cores, meets the hardness standard in thick-walled areas, and ensures clean internal oil passages free of residual sand, thereby improving the reliability and fatigue resistance of castings and meeting the operating requirements of hydraulic multi-way valves.
Smart Images

Figure CN123102937A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of casting technology, and specifically relates to a casting process for an integral hydraulic multi-way valve for excavators. Background Technology
[0002] As a core hydraulic control component of large-tonnage hydraulic excavators, the integrated multi-way valve is subject to the harsh working conditions of long-term continuous operation of hydraulic excavators, and its valve body has extremely high requirements for reliability and durability. At present, integrating multiple independent plate valve body castings into an integrated multi-way valve body casting has become the mainstream trend of industry technology development. However, the high integration of the valve body structure significantly increases the difficulty of casting process implementation. The hydraulic integrated multi-way valve casting for excavators is a typical representative of this type of highly integrated casting.
[0003] The casting production of this type of casting faces multiple technical bottlenecks: First, the internal oil channels of the casting are distributed in a three-dimensional space, which not only greatly increases the difficulty of sand core shooting, but also makes the sand core prone to core breakage defects due to erosion by molten iron during the pouring process, and the large volume of the internal sand core is prone to porosity defects; Second, the wall thickness increases significantly after the valve body is integrated, and shrinkage cavities and porosity defects are prone to occur inside the casting, which seriously weakens the pressure bearing performance of the valve body; Third, the high thermal modulus and slow solidification rate in some thick-walled areas can easily lead to low hardness of the casting matrix material, which cannot meet the service performance requirements; Fourth, the curved structure of the oil channels in the valve body and the small local aperture make it difficult to clean the sand in the inner cavity of the casting after pouring, making it difficult to ensure the cleanliness of the oil channels; Fifth, the oil groove formed by casting needs to be precisely matched with the oil groove of the valve core after subsequent machining, which requires high dimensional accuracy of the casting. Summary of the Invention
[0004] The purpose of this invention is to provide a casting process for an integral hydraulic multi-way valve for excavators, which can produce qualified castings of integral multi-way valves for excavators in batches with high sand core precision and strength, stable filling, dense structure, qualified hardness in thick-walled areas, and clean internal oil passages free of residual sand.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is a casting process for an integral hydraulic multi-way valve for excavators, comprising the following steps:
[0006] Step 1: Based on the internal oil passage structure of the valve body, construct a three-dimensional model of the sand core and a three-dimensional model of the valve body's external sand mold in three-dimensional modeling software, and design the casting system;
[0007] Step 2: Decompose the sand core 3D model into an upper main sand core 3D model and a lower main sand core 3D model, and further decompose the local structures in the upper main sand core 3D model and the lower main sand core 3D model that cannot be formed by core shooting in one time to obtain several independent local sand core 3D models.
[0008] Local structures that cannot be formed in one shot include: structures that interfere with each other after being integrally shot with adjacent structures and cannot be demolded; local structures with undercut and concave features; and structures with multi-directional intersecting oil channels at corners.
[0009] Step 3: Based on the three-dimensional model of the upper main sand core, the three-dimensional model of the lower main sand core, and the three-dimensional model of the local sand core, manufacture the core box mold; based on the three-dimensional model of the valve body outer sand mold, manufacture the mold plate mold; set the exhaust column and overflow column on the mold plate mold.
[0010] Step 4: Using the core shooting process, the upper main sand core, the lower main sand core, and various local sand cores are manufactured separately using a core box mold;
[0011] Step 5: Place each local sand core at the corresponding fixed position of the core box mold corresponding to the upper main sand core or the corresponding fixed position reserved in the core box mold corresponding to the lower main sand core, and then perform secondary core shooting to obtain the upper secondary core shooting sand core and the lower secondary core shooting sand core. Local sand cores that do not meet the conditions for secondary core shooting will not participate in secondary core shooting.
[0012] The reasons why some sand cores do not meet the conditions for secondary core shooting include: interference with the demolding path after secondary core shooting of the main sand core, resulting in the inability to demold; insufficient placement space; inability to design reliable positioning in the upper or lower main sand core; and insufficient bonding surface with the upper or lower main sand core or lack of geometric overlap transition.
[0013] Step 6: Combine the upper secondary core shooting sand core, the lower secondary core shooting sand core, and the local sand cores that do not meet the secondary core shooting conditions into a whole sand core and open the vent holes. Apply water-based casting coating to the surface of the whole sand core.
[0014] Step 7: After the water layer of water-based casting coating on the surface of the integral sand core has evaporated, apply casting coating a second time and place the integral sand core in a drying oven to dry.
[0015] Step 8: Based on the mold plate, manufacture the upper and lower sand molds to simultaneously form the sand mold venting holes, overflow holes and gating system, and simultaneously place the heating riser sleeve on the upper sand mold and the chill on the lower sand mold;
[0016] Step 9: Apply a casting alcohol-based coating to the contact surfaces of the upper and lower sand molds with the molten iron, and then ignite the casting alcohol-based coating to dry it.
[0017] Step 10: Place the integral sand core in the lower sand mold, and place the upper sand mold on top of the lower sand mold using positioning pins to form a complete casting cavity;
[0018] Step 11: Melt the molten iron;
[0019] Step 12: Pour the molten iron and simultaneously sprinkle in an inoculant. After the molten iron cools in the casting cavity, remove the sand to obtain the valve body casting.
[0020] Step 13: Remove the gating system and any remaining hot riser sleeves that are connected to the valve body casting;
[0021] Step 14: Perform shot blasting on the outer surface of the valve body casting;
[0022] Step 15: Perform a core vibration operation on the valve body casting;
[0023] Step 16: Shot peening the oil passages of the valve body casting and inspecting them with an endoscope. For areas where residual sand is still present, shot peening is performed again until the residual sand on the surface of the oil passages of the valve body casting is completely removed.
[0024] Step 17: Perform a quality inspection on the valve body casting.
[0025] In a further preferred embodiment, in step 3, the number of exhaust columns is 8 and their distribution positions correspond to the edge of the integral sand core. The cross-sectional area of the exhaust columns is larger than the cross-sectional area of the exhaust holes of the integral sand core. The number of overflow columns is 10 and they are distributed at the edge of the valve body casting forming area. The mold plate, exhaust columns and overflow columns are molded using furan resin sand.
[0026] In a further preferred embodiment, in step 4, the raw materials for the upper main sand core, the lower main sand core, and each local sand core are ceramsite sand coated with sand, and the heating temperature of the core box mold is 190-210℃.
[0027] In step 5, a secondary core shot is performed using ceramsite-coated sand.
[0028] In a further preferred embodiment, in step 8, the chill is placed below the casting forming area, the heating riser sleeve is located above the casting forming area, and the raw materials for the upper and lower sand molds are furan resin self-hardening sand.
[0029] In a further preferred embodiment, step 11 includes the following steps:
[0030] Step 11-1: Add pig iron, scrap steel, recycled materials, silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper to an induction furnace for melting. Based on the total mass of all materials entering the furnace, the mass fraction of pig iron is 48%, the mass fraction of scrap steel is 15%, the mass fraction of recycled materials is 36.8%, and the remaining components consist of silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper. Control the chemical composition of the molten iron in the induction furnace to the following mass percentages: C=3.7-3.75%, Si=1.5-1.55%, Mn=0.25-0.35%, P≤0.05%, S=0.006-0.015%, with the remainder being Fe and unavoidable impurities.
[0031] Step 11-2: Spheroidize the molten iron, then add 0.02% tin alloy and 0.6% primary inoculant by mass of the molten iron to the casting ladle, and then pour the spheroidized molten iron into the casting ladle.
[0032] In a further preferred embodiment, in step 11, the chemical composition of the molten iron in the ladle is controlled by mass percentage as follows: C=3.65-3.70%, Si=1.65-1.70%, Mn=0.35-0.40%, P≤0.05%, S=0.008-0.015%, Mg=0.035-0.045%, residual rare earth content≤0.003%, Cu=0.045-0.055%, Sn=0.020-0.025%, with the remainder being Fe and unavoidable impurities.
[0033] In a further preferred embodiment, in step 12, molten iron enters the mold cavity from the bottom of the valve body casting forming area, the pouring temperature is controlled at 1360-1400℃, and the amount of inoculant added is 0.02% of the total mass of the valve body casting.
[0034] In a further preferred embodiment, step 15 includes the following steps:
[0035] Step 15-1: Clamp the valve body casting on the vibratory core remover, vibrate for 20-25 minutes, and blow high-pressure air into the valve hole that communicates with the outside.
[0036] Step 15-2: After flipping the valve body casting, vibrate it again for 20-25 minutes and blow high-pressure air into the valve hole that communicates with the outside.
[0037] In a further preferred embodiment, in step 16, steel shot with a diameter of 0.3 mm is used for shot peening.
[0038] Compared with the prior art, the present invention has the following advantages:
[0039] (1) It can produce qualified castings of excavator integral multi-way valves in batches with high sand core precision and strength, stable filling, dense structure, hardness of thick wall position, and clean internal oil passage without residual sand.
[0040] (2) The local sand cores that are difficult to demold directly are fused together with the main sand core through secondary core shooting, and the bonding strength is higher than that of adhesive bonding; the internal cavity flash defects caused by core splicing are eliminated; the amount of manual core assembly work is reduced, the dimensional accuracy of sand cores is improved, and the dimensional accuracy of valve body castings is guaranteed.
[0041] (3) Bottom-pouring casting is adopted to achieve sequential filling from bottom to top; reduce turbulence and splashing of molten iron, reduce the risk of inclusion defects caused by oxidation of molten iron; reduce the scouring of sand core by molten iron, reduce the probability of core breakage defects, and improve the venting conditions of the cavity.
[0042] (4) The bottom chiller reduces the effective thermal modulus of the casting, accelerates the solidification of the valve body, and achieves efficient feeding by combining with the top heating riser, eliminating shrinkage cavities and porosity, ensuring that the internal structure of the valve body is dense and meets the requirements of pressure conditions.
[0043] (5) Add Mn, Cu and Sn alloying elements to the molten iron to improve the strength and hardness of the valve body matrix and meet the reliability and fatigue resistance of the hydraulic multi-way valve under repeated operation conditions. Attached Figure Description
[0044] Figure 1 This is a schematic diagram of the sand core decomposition scheme according to an embodiment of the present invention;
[0045] Figure 2 This is a schematic diagram of the casting scheme according to an embodiment of the present invention;
[0046] Figure 3 This is a schematic diagram of the secondary core firing of the upper main sand core according to an embodiment of the present invention;
[0047] Figure 4 This is a schematic diagram of the secondary core firing of the lower main sand core according to an embodiment of the present invention;
[0048] Figure 5 This is a schematic diagram of the overall sand core assembly according to an embodiment of the present invention;
[0049] Figure 6 This is a schematic diagram of the structure after the box is closed according to an embodiment of the present invention.
[0050] In the diagram: 1. Upper main sand core; 2. First partial sand core; 3. Second partial sand core; 4. Lower main sand core; 5. Third partial sand core; 6. Fourth partial sand core; 7. Fifth partial sand core; 8. Upper secondary core-shooting sand core; 9. Lower secondary core-shooting sand core; 10. Integral sand core; 11. Sand core vent hole; 12. Valve body casting; 13. Horizontal sprue; 14. Sand mold vent hole; 15. Heating riser sleeve; 16. Straight sprue; 17. Overflow hole; 18. Chill; 19. Ingate; 20. Upper sand core core box mold; 21. Lower sand core core box mold; 22. Upper box sand mold; 23. Lower box sand mold. Detailed Implementation
[0051] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0052] This invention discloses a casting process for an integral hydraulic multi-way valve for excavators, comprising the following steps:
[0053] Step 1: Based on the internal oil passage structure of the valve body, construct a three-dimensional model of the sand core and a three-dimensional model of the valve body's external sand mold in the three-dimensional modeling software, and design the casting system.
[0054] The gating system includes a sprue, a runner, and an ingate.
[0055] Step 2: Split the sand core 3D model into an upper main sand core 3D model and a lower main sand core 3D model. Further, separate the local structures in the upper and lower main sand core 3D models that cannot be formed by core shooting in one go, and obtain several independent local sand core 3D models.
[0056] Local structures that cannot be formed in one shot include: structures that interfere with each other after being integrally shot with adjacent structures and cannot be demolded; local structures with undercut and concave features; and structures with multi-directional intersecting oil channels at corners.
[0057] Specifically, if a structure that cannot be demolded due to interference after integral core injection molding with an adjacent structure uses the same core box for integral core injection molding with an adjacent structure, the sand cores will lock and jam with each other after molding. When pulling the core, the core box and the sand core will interfere with each other in space, and the core box cannot be pulled out along the core pulling direction, thus failing to meet the demolding conditions.
[0058] The local structure with its own inverted concave feature has an inverted concave shape opposite to the main core pulling direction, and there is no space to avoid the unidirectional core pulling; after core injection molding, the molded insert will be stuck by the sand core inverted, and the sand core is easily torn and damaged during demolding.
[0059] In structures with multiple intersecting oil channels at corners, the walls at the corners intersect and block each other, and there is no single direction for core extraction; after integral core injection molding, the molded inserts at the corners cannot be removed, and forced demolding will cause damage to the corner sand core, making it difficult to guarantee the accuracy of the oil channel contour.
[0060] Step 3: Based on the 3D model of the upper main sand core, the 3D model of the lower main sand core, and the 3D model of the local sand core, manufacture the core box mold. Based on the 3D model of the valve body shape sand mold, manufacture the mold plate mold. Set venting columns and overflow columns on the mold plate mold. The number of venting columns is 8 and their distribution positions correspond to the edge of the overall sand core. The cross-sectional area of the venting columns is larger than the cross-sectional area of the venting holes of the overall sand core. The number of overflow columns is 10 and they are distributed on the edge of the valve body casting forming area. The mold plate mold, venting columns, and overflow columns are molded using furan resin sand.
[0061] By setting multiple venting columns at the corresponding sand core edge positions on the mold plate, and ensuring that the cross-sectional area of the venting columns is larger than that of the sand core venting holes, sand mold venting holes can be formed simultaneously during the manufacture of the upper and lower sand molds. These sand mold venting holes effectively connect the internal venting channels of the sand core with the external environment, allowing the gas generated by the sand core during the molten iron pouring process to be quickly and fully discharged, preventing gas from stagnating in the mold cavity and forming porosity defects. Simultaneously, multiple overflow columns are arranged at the edge of the valve body forming area, enabling the simultaneous formation of overflow holes during the manufacture of the upper and lower sand molds. These overflow holes combine venting and overflow functions, promptly discharging low-temperature molten iron, inclusions, and residual gas from the mold cavity, optimizing the filling flow field, significantly improving the internal density of the valve body casting, effectively eliminating casting defects such as porosity and inclusions, and ensuring the structural integrity and pressure-bearing stability of the multi-way valve body under high-pressure conditions.
[0062] Step 4: The upper main sand core, lower main sand core and various local sand cores are manufactured separately using the core shooting process through the core box mold. The raw materials for the upper main sand core, lower main sand core and various local sand cores are ceramic sand coated sand. The heating temperature of the core box mold is 190-210℃.
[0063] Step 5: Place each local sand core at the corresponding fixed position of the core box mold corresponding to the upper main sand core or the corresponding fixed position reserved in the core box mold corresponding to the lower main sand core, and then use ceramsite sand coated sand to perform secondary core shooting to obtain the upper secondary core shooting sand core and the lower secondary core shooting sand core. Local sand cores that do not meet the conditions for secondary core shooting will not participate in secondary core shooting.
[0064] The reasons why some sand cores do not meet the conditions for secondary core shooting include: interference with the demolding path after secondary core shooting of the main sand core, resulting in the inability to demold; insufficient placement space; inability to design reliable positioning in the upper or lower main sand core; and insufficient joint surface with the upper or lower main sand core or lack of geometric overlap transition.
[0065] The secondary core-shooting process is used to connect the local sand cores with the upper and lower main sand cores. The bonding strength is higher than that of adhesive bonding. It can also eliminate gaps at the sand core connection, reduce the amount of manual assembly work, and avoid the occurrence of flash during core splicing, thereby improving the dimensional accuracy and strength of the sand cores.
[0066] Step 6: Combine the upper secondary core shot sand core, the lower secondary core shot sand core, and the local sand cores that do not meet the secondary core shot conditions into a whole sand core and open vent holes. Apply water-based casting coating to the surface of the whole sand core.
[0067] Step 7: After the water layer of water-based casting coating on the surface of the integral sand core has evaporated, apply casting coating a second time and place the integral sand core in a drying oven to dry.
[0068] Step 8: Based on the mold plate, manufacture the upper and lower sand molds to simultaneously form the sand mold venting holes, overflow holes, and gating system, and simultaneously place the heating riser sleeve and chill. The chill is placed below the casting forming area, and the heating riser sleeve is located above the casting forming area. The raw material for the upper and lower sand molds is furan resin self-hardening sand.
[0069] By setting chills at the bottom of the valve body, the solidification and heat dissipation of the valve body casting are accelerated, and the thermal modulus of the valve body casting is reduced. At the same time, a heating riser sleeve is used on the top surface of the valve body casting for top surface feeding. Through the cooling of the bottom chill and the upper and lower coupled temperature control feeding structure of the heating riser on the top surface, the valve body casting is rapidly and orderly solidified, ensuring continuous and effective feeding by the heating riser. This effectively suppresses shrinkage cavities and porosity defects inside the valve body casting, ensuring the high pressure bearing performance and internal density of the valve body casting. Furan resin sand is used for the upper and lower sand molds. Due to the high hardness of furan resin sand, it can resist the graphitization expansion of molten iron during the casting process, thereby achieving the effect of self-feeding in isolated areas, which is beneficial to improving the density of the internal matrix structure of the valve body casting.
[0070] Step 9: Apply a casting alcohol-based coating to the contact surfaces of the upper and lower sand molds with the molten iron, and then ignite the casting alcohol-based coating to dry it.
[0071] Step 10: Place the integral sand core in the lower sand mold, and place the upper sand mold on top of the lower sand mold using positioning pins to form a complete casting cavity.
[0072] Step 11-1: Add pig iron, scrap steel, recycled materials, silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper to an induction furnace for melting. Based on the total mass of all materials entering the furnace, the mass fraction of pig iron is 48%, the mass fraction of scrap steel is 15%, the mass fraction of recycled materials is 36.8%, and the remaining components consist of silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper. Control the chemical composition of the molten iron in the induction furnace to the following mass percentages: C=3.7-3.75%, Si=1.5-1.55%, Mn=0.25-0.35%, P≤0.05%, S=0.006-0.015%, with the remainder being Fe and unavoidable impurities.
[0073] Step 11-2: Spheroidize the molten iron, then add 0.02% tin alloy and 0.6% primary inoculant by mass of the molten iron to the casting ladle, and then pour the spheroidized molten iron into the casting ladle.
[0074] The chemical composition of the molten iron in the ladle, by mass percentage, is as follows: C=3.65-3.70%, Si=1.65-1.70%, Mn=0.35-0.40%, P≤0.05%, S=0.008-0.015%, Mg=0.035-0.045%, residual rare earth content≤0.003%, Cu=0.045-0.055%, Sn=0.020-0.025%, with the remainder being Fe and unavoidable impurities.
[0075] By adjusting the molten iron composition and adding manganese, copper, and tin elements during the molten iron smelting process, a hardness sample was cut from the 80mm thick wall in the center and tested with a Brinell hardness tester. The hardness increased from the original 165HBW to 210HBW, thus improving the hardness of the thick wall in the center of the valve body casting, thereby enhancing the material strength and rigidity of the central valve hole area of the valve body casting.
[0076] Step 12: Pour the molten iron and simultaneously add the inoculant. The molten iron enters the cavity from the bottom of the forming area of the valve body casting. The pouring temperature is controlled at 1360-1400℃. The amount of inoculant added is 0.02% of the total mass of the valve body casting. After the molten iron cools in the casting cavity, it is shaken off to obtain the valve body casting.
[0077] By employing a bottom-pouring method to smoothly fill the mold cavity with molten iron, and controlling the ratio of the cross-sectional areas of each component of the gating system to maximize the openness of the ingate, the molten iron reaches a laminar flow state. This ultimately achieves sequential filling from bottom to top, reducing molten iron splashing and turbulence, preventing molten iron oxidation, and reducing direct erosion of the sand core by molten iron, thus reducing the risk of sand core breakage.
[0078] Step 13: Remove the gating system and residual heat-generating riser sleeves that are connected to the valve body casting.
[0079] Step 14: Perform shot blasting on the outer surface of the valve body casting.
[0080] Step 15-1: Clamp the valve body casting on the vibratory core remover, vibrate for 20-25 minutes, and blow high-pressure air into the valve hole that communicates with the outside.
[0081] Step 15-2: After flipping the valve body casting, vibrate it again for 20-25 minutes and blow high-pressure air into the valve hole that communicates with the outside.
[0082] This invention uses high-frequency vibration to loosen and remove the sand core inside the valve body. At the same time, compressed air continuously blows through the valve hole cavity during the vibration process, which can efficiently shake off and remove most of the residual sand and loose core material inside the oil passage, thus achieving the initial sand removal of complex and tortuous oil passages.
[0083] Step 16: Shot peening the oil passages of the valve body casting with steel shot of 0.3mm diameter and inspecting with an endoscope. For areas where residual sand is still present, shot peening is performed again until the residual sand on the surface of the oil passages of the valve body casting is completely removed.
[0084] Through precise shot peening of the inner cavity, stubborn residual sand and oxide scale on the inner wall of the oil passage are impacted and removed, thoroughly eliminating various residues on the surface of the oil passage. This composite cleaning method is highly targeted and thorough, effectively solving the problems of irregularly shaped valve bodies, easy sand accumulation in intersecting oil passages, and incomplete sand removal in multi-way valves. It ensures that the inner wall of the oil passage is smooth and clean, avoiding problems such as hydraulic circuit blockage and valve core jamming caused by residual sand falling off, and significantly improving the internal forming quality of the valve body casting and the stability of hydraulic operation.
[0085] Step 17: Perform a quality inspection on the valve body casting.
[0086] The quality inspection adopts either full inspection or sampling inspection; wherein, full inspection involves visually inspecting the appearance of the valve body casting and using an endoscope to inspect the oil passage of the valve body casting; sampling inspection involves one or more of three-dimensional scanning detection and cross-section detection.
[0087] The three-dimensional scanning detection involves acquiring a scanning model of the casting using an industrial scanning camera, comparing the scanning model with the valve body design model, and determining the dimensional accuracy of the valve body casting.
[0088] The slice inspection involves sawing the valve body casting to obtain several slices and then inspecting the density of the cut surface and the metallographic structure. The cut surface density inspection is to detect the size and distribution of defects such as shrinkage porosity, shrinkage cavities, and inclusions inside the casting.
[0089] Specifically, when using 3D scanning inspection alone, a scanning model of the casting's appearance can be obtained, which can be used to inspect the forming dimensional accuracy of the outer part of the valve body casting;
[0090] When combining slicing inspection and 3D scanning inspection, the appearance scanning model of the valve body casting is first obtained by an industrial scanning camera in the complete state. Then, the valve body casting is cut to expose the internal oil passages to the external environment. The oil passage scanning model of the casting is then obtained by an industrial scanning camera. The appearance scanning model and the oil passage scanning model of the casting are then compared with the valve body design model to determine the dimensional accuracy of the full-size forming of the valve body casting.
[0091] The valve body castings prepared by this process have a matrix hardness greater than 200 HBW.
[0092] The casting process of the hydraulic integral multi-way valve for excavators of the present invention is further described below with reference to specific embodiments.
[0093] Example
[0094] like Figure 1-6 As shown, the specific parameters of the valve body casting 12 cast in this embodiment are as follows:
[0095] Casting material: QT500-7;
[0096] Casting weight: 142kg;
[0097] Maximum dimensions of the casting: 371mm × 338mm × 200mm;
[0098] Minimum casting hole size: 4mm;
[0099] Longest core length: 428mm;
[0100] Maximum wall thickness of casting: 90mm;
[0101] The casting process for the integrated hydraulic multi-way valve for excavators in this embodiment includes:
[0102] Step 1: Based on the internal oil passage structure of the valve body, construct a three-dimensional model of the sand core and a three-dimensional model of the valve body's external sand mold in the three-dimensional modeling software, and design the casting system.
[0103] Step 2: Decompose the sand core 3D model to obtain the upper main sand core 1 3D model, the lower main sand core 4 3D model, the first partial sand core 2 3D model, the second partial sand core 3 3D model, the third partial sand core 5 3D model, the fourth partial sand core 6 3D model, and the fifth partial sand core 7 3D model.
[0104] Step 3: Based on the 3D model of the upper main sand core 1, manufacture the upper sand core box mold 20; based on the 3D model of the lower main sand core 4, manufacture the lower sand core box mold 21; based on the 3D models of the first partial sand core 2, the second partial sand core 3, the third partial sand core 5, the fourth partial sand core 6, and the fifth partial sand core 7, respectively, manufacture the first partial sand core 2 box mold, the second partial sand core 3 box mold, the third partial sand core 5 box mold, the fourth partial sand core 6 box mold, and the fifth partial sand core 7 box mold; based on the 3D model of the valve body outer sand mold, manufacture the mold plate mold; set 8 venting columns and 10 overflow columns on the mold plate mold; the distribution position of the venting columns corresponds to the edge of the overall sand core 10; the cross-sectional area of the venting columns is larger than the cross-sectional area of the venting holes of the overall sand core 10; the overflow columns are distributed at the edge of the forming area of the valve body casting 12; the mold plate mold, venting columns, and overflow columns are molded using furan resin sand.
[0105] Step 4: The upper main sand core 1, lower main sand core 4, first partial sand core 2, second partial sand core 3, third partial sand core 5, fourth partial sand core 6, and fifth partial sand core 7 are manufactured separately using the core shooting process. The raw materials for the upper main sand core 1, lower main sand core 4, first partial sand core 2, second partial sand core 3, third partial sand core 5, fourth partial sand core 6, and fifth partial sand core 7 are ceramic sand coated with sand, and the heating temperature of the core box mold is 205℃.
[0106] Step 5: Place the first partial sand core 2 and the second partial sand core 3 at the reserved fixed position of the upper sand core box mold 20 for secondary core shooting to form the upper secondary core sand core 8; place the third partial sand core 5 and the fourth partial sand core 6 at the reserved fixed position of the lower sand core box mold 21 for secondary core shooting to form the lower secondary core sand core 9.
[0107] Step 6: Combine the upper secondary core shot sand core 8, the lower secondary core shot sand core 9 and the fifth partial sand core 7 to obtain the integral sand core 10 and open the sand core vent hole 11. Apply a water-based casting coating with a Baume degree of 28°Bé to the surface of the integral sand core 10.
[0108] Step 7: After the water layer of water-based casting coating on the surface of the integral sand core 10 has evaporated, a second coating of casting coating with a Baume degree of 32°Bé is applied, and the integral sand core 10 is placed in a drying oven to dry. The drying temperature is controlled at 190 degrees Celsius and the drying time is 35 minutes.
[0109] Step 8: Based on the mold plate, the upper box sand mold 22 and the lower box sand mold 23 are manufactured using the mixed furan resin self-hardening sand. At the same time, the sand mold vent hole 14, overflow hole 17 and gating system are formed. The heating riser sleeve 15 and the chill 18 are placed simultaneously. The chill 18 is placed below the casting forming area, and the heating riser sleeve 15 is located above the casting forming area. The gating system includes a sprue 16, a runner 13 and an ingate 19. The ratio of the cross-sectional area of the sprue 16, the runner 13, the flow-blocking section and the ingate 19 is ΣFsprue:ΣFrunner:ΣFflow-blocking:ΣFingate = 1.1:1.4:1:2. The thickness of the chill 18 is 100mm. The heating riser sleeve 15 is selected with an effective modulus of 42mm.
[0110] Step 9: Apply casting alcohol-based coating to the contact surfaces of the upper sand mold 22 and the lower sand mold 23 with the molten iron, and then ignite the casting alcohol-based coating to dry it.
[0111] Step 10: Place the integral sand core 10 in the lower sand mold 23, and place the upper sand mold 22 on top of the lower sand mold 23 using positioning pins to form a complete casting cavity.
[0112] Step 11-1: Add pig iron, scrap steel, recycled materials, silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper to an induction furnace for melting. Based on the total mass of all materials entering the furnace, the mass fraction of pig iron is 48%, the mass fraction of scrap steel is 15%, the mass fraction of recycled materials is 36.8%, and the remaining components consist of silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper. The melting temperature of the induction furnace is controlled at 1580℃, and the melting time is 10 minutes. The chemical composition of the molten iron in the induction furnace is controlled as follows (by mass percentage): C=3.72%, Si=1.54%, Mn=0.3%, P=0.042%, S=0.012%, with the remainder being Fe and unavoidable impurities.
[0113] Step 11-2: Spheroidize the molten iron at a temperature of 1490℃. Then, add 0.02% tin alloy and 0.6% primary inoculant to the ladle. Finally, pour the spheroidized molten iron into the ladle.
[0114] The chemical composition of the molten iron in the ladle, by mass percentage, is as follows: C=3.68%, Si=1.67%, Mn=0.4%, P=0.04%, S=0.010%, Mg=0.045%, residual rare earth content is 0.0026%, Cu=0.045%, Sn=0.023%, and the remainder is Fe and unavoidable impurities.
[0115] Step 12: Pour the molten iron and simultaneously add the inoculant. The molten iron enters the cavity from the bottom of the forming area of the valve body casting 12. The pouring temperature is controlled at 1385℃. The amount of inoculant added is 0.02% of the total mass of the valve body casting 12. After the molten iron cools in the casting cavity, it is shaken off to obtain the valve body casting 12.
[0116] Testing revealed that the matrix hardness of the valve body casting reached 210 HBW.
[0117] Step 13: Remove the horizontal sprue 13, sprue 16, ingate 19 and residual heat-generating riser sleeve 15 connected to the valve body casting 12.
[0118] Step 14: Perform shot blasting on the outer surface of the valve body casting 12.
[0119] Step 15-1: Clamp the valve body casting 12 on the vibratory core remover, vibrate for 20 minutes and blow high-pressure air into the valve hole that communicates with the outside.
[0120] Step 15-2: After flipping the valve body casting 12, vibrate it again for 25 minutes and blow high-pressure air into the valve hole that communicates with the outside.
[0121] Step 16: The oil passages of the valve body casting 12 are shot peened with steel shot with a diameter of 0.3 mm and inspected with an endoscope. Areas where residual sand is still present are shot peened again until the residual sand on the surface of the oil passages of the valve body casting 12 is completely removed.
[0122] Step 17: Perform a quality inspection on the valve body casting 12.
[0123] The valve body casting 12 was visually inspected and found to be clean and with a shape accuracy of CT9. The oil passages of the valve body casting 12 were inspected using an endoscope and found to be free of residual sand, with an internal oil passage accuracy of CT8. Through CT scanning, the appearance and internal oil passages of the valve body casting 12 were compared with the valve body design model and were found to be consistent in shape with no defects such as broken cores. The valve body casting 12 was cross-sectioned and found to have a dense matrix with no shrinkage porosity or shrinkage defects.
Claims
1. A casting process for an integral hydraulic multi-way valve for excavators, characterized in that, Includes the following steps: Step 1: Based on the internal oil passage structure of the valve body, construct a three-dimensional model of the sand core and a three-dimensional model of the valve body's external sand mold in three-dimensional modeling software, and design the casting system; Step 2: Decompose the sand core 3D model into an upper main sand core 3D model and a lower main sand core 3D model, and further decompose the local structures in the upper main sand core 3D model and the lower main sand core 3D model that cannot be formed by core shooting in one time to obtain several independent local sand core 3D models. Local structures that cannot be formed in one shot include: structures that interfere with each other after being integrally shot with adjacent structures and cannot be demolded; local structures with undercut and concave features; and structures with multi-directional intersecting oil channels at corners. Step 3: Based on the three-dimensional model of the upper main sand core, the three-dimensional model of the lower main sand core, and the three-dimensional model of the local sand core, manufacture the core box mold; based on the three-dimensional model of the valve body outer sand mold, manufacture the mold plate mold; set the exhaust column and overflow column on the mold plate mold. Step 4: Using the core shooting process, the upper main sand core, the lower main sand core, and various local sand cores are manufactured separately using a core box mold; Step 5: Place each local sand core at the corresponding fixed position of the core box mold corresponding to the upper main sand core or the corresponding fixed position reserved in the core box mold corresponding to the lower main sand core, and then perform secondary core shooting to obtain the upper secondary core shooting sand core and the lower secondary core shooting sand core. Local sand cores that do not meet the conditions for secondary core shooting will not participate in secondary core shooting. The reasons why some sand cores do not meet the conditions for secondary core shooting include: interference with the demolding path after secondary core shooting of the main sand core, resulting in the inability to demold; insufficient placement space; inability to design reliable positioning in the upper or lower main sand core; and insufficient bonding surface with the upper or lower main sand core or lack of geometric overlap transition. Step 6: Combine the upper secondary core shooting sand core, the lower secondary core shooting sand core, and the local sand cores that do not meet the secondary core shooting conditions into a whole sand core and open the vent holes. Apply water-based casting coating to the surface of the whole sand core. Step 7: After the water layer of water-based casting coating on the surface of the integral sand core has evaporated, apply casting coating a second time and place the integral sand core in a drying oven to dry. Step 8: Based on the mold plate, manufacture the upper and lower sand molds, simultaneously forming the sand mold vent holes, overflow holes, and gating system, and simultaneously place the heating riser sleeve and chills; Step 9: Apply a casting alcohol-based coating to the contact surfaces of the upper and lower sand molds with the molten iron, and then ignite the casting alcohol-based coating to dry it. Step 10: Place the integral sand core in the lower sand mold, and place the upper sand mold on top of the lower sand mold using positioning pins to form a complete casting cavity; Step 11: Melt the molten iron; Step 12: Pour the molten iron and simultaneously sprinkle in an inoculant. After the molten iron cools in the casting cavity, remove the sand to obtain the valve body casting. Step 13: Remove the gating system and any remaining hot riser sleeves that are connected to the valve body casting; Step 14: Perform shot blasting on the outer surface of the valve body casting; Step 15: Perform a core vibration operation on the valve body casting; Step 16: Shot peening the oil passages of the valve body casting and inspecting them with an endoscope. For areas where residual sand is still present, shot peening is performed again until the residual sand on the surface of the oil passages of the valve body casting is completely removed. Step 17: Perform a quality inspection on the valve body casting.
2. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, In step 3, there are 8 exhaust columns, and their distribution positions correspond to the edge of the integral sand core. The cross-sectional area of the exhaust column is larger than the cross-sectional area of the exhaust hole of the integral sand core. There are 10 overflow columns, which are distributed at the edge of the valve body casting forming area. The mold plate, exhaust columns and overflow columns are molded using furan resin sand.
3. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, In step 4, the raw materials for the upper main sand core, the lower main sand core and each local sand core are ceramic sand coated sand, and the heating temperature of the core box mold is 190-210℃. In step 5, ceramsite sand coated with a film is used for secondary core shooting.
4. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, In step 8, the chill is placed below the casting forming area, the heating riser sleeve is located above the casting forming area, and the raw materials for the upper and lower sand molds are furan resin self-hardening sand.
5. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, Step 11 includes the following steps: Step 11-1: Add pig iron, scrap steel, recycled materials, silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper to an induction furnace for melting. Based on the total mass of all materials entering the furnace, the mass fraction of pig iron is 48%, the mass fraction of scrap steel is 15%, the mass fraction of recycled materials is 36.8%, and the remaining components consist of silicon carbide, recarburizing agent, 75% ferrosilicon, 75% ferromanganese, and pure copper. Control the chemical composition of the molten iron in the induction furnace to the following mass percentages: C=3.7-3.75%, Si=1.5-1.55%, Mn=0.25-0.35%, P≤0.05%, S=0.006-0.015%, with the remainder being Fe and unavoidable impurities. Step 11-2: Spheroidize the molten iron, then add 0.02% tin alloy and 0.6% primary inoculant by mass of the molten iron to the casting ladle, and then pour the spheroidized molten iron into the casting ladle.
6. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 5, characterized in that, In step 11, the chemical composition of the molten iron in the ladle is controlled by mass percentage as follows: C=3.65-3.70%, Si=1.65-1.70%, Mn=0.35-0.40%, P≤0.05%, S=0.008-0.015%, Mg=0.035-0.045%, residual rare earth content≤0.003%, Cu=0.045-0.055%, Sn=0.020-0.025%, with the remainder being Fe and unavoidable impurities.
7. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, In step 12, molten iron enters the mold cavity from the bottom of the valve body casting forming area, the pouring temperature is controlled at 1360-1400℃, and the amount of inoculant added is 0.02% of the total mass of the valve body casting.
8. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, Step 15 includes the following steps: Step 15-1: Clamp the valve body casting on the vibratory core remover, vibrate for 20-25 minutes, and blow high-pressure air into the valve hole that communicates with the outside. Step 15-2: After flipping the valve body casting, vibrate it again for 20-25 minutes and blow high-pressure air into the valve hole that communicates with the outside.
9. The casting process for the integrated hydraulic multi-way valve for excavators according to claim 1, characterized in that, In step 16, steel shot with a diameter of 0.3 mm is used for shot peening.