A porous nickel in-situ grown Ni3S2 / MoS2 material, its preparation method and application

By growing Ni3S2/MoS2 core-shell heterostructures in situ on a porous nickel substrate, the problem of poor stability of Ni3S2 electrocatalysts under high current density was solved, achieving high efficiency and long-term stability in water electrolysis for hydrogen production.

CN123102993APending Publication Date: 2026-11-17LONGMEN LAB
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611613397.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing Ni3S2 electrocatalysts exhibit poor stability at high current densities. Mo doping leads to lattice distortion and structural loss, affecting long-term operational stability.

Method used

A Ni3S2/MoS2 core-shell heterostructure was grown in situ on a porous nickel substrate. Ni3S2 nanorods were encapsulated in ultrathin MoS2 nanosheets through hydrothermal reaction and pretreatment to build a tight interface to enhance electron transfer and catalytic effects.

Benefits of technology

This improved the stability and catalytic performance of the electrocatalyst under industrial-grade high current density, reduced the hydrogen evolution overpotential, and extended the long-term service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102993A_ABST
    Figure CN123102993A_ABST
Patent Text Reader

Abstract

This invention relates to the field of electrochemical technology and discloses an in-situ grown porous nickel Ni3S2 / MoS2 material, its preparation method, and its application. The method involves mixing nickel powder and NaCl powder and sintering the mixture to obtain a porous nickel matrix. The porous nickel matrix is ​​then placed in a mixed solution A and continuously stirred to obtain pretreated porous nickel. Mixed solution A is prepared by dissolving ammonium molybdate tetrahydrate, ammonium fluoride, and polyvinylpyrrolidone in deionized water at a mass ratio of 20:10:1~5. The pretreated porous nickel is then placed in mixed solution B and subjected to a hydrothermal reaction at 140~160℃ to obtain the target product. Mixed solution B is prepared by dissolving ammonium molybdate tetrahydrate and thioacetamide in deionized water at a mass ratio of 1:1~5. This invention also utilizes MoS2 nanosheets to encapsulate Ni3S2 nanorods to form a core-shell heterostructure, reducing its performance under industrial-grade high current density (500 mA·cm⁻¹). ‑2 The hydrogen evolution overpotential under the specified conditions was reduced, and its stability under industrial-grade high current density was improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrochemical technology, specifically to a porous nickel in-situ grown Ni3S2 / MoS2 material, its preparation method, and its application. Background Technology

[0002] Hydrogen, as an ideal clean energy carrier, boasts advantages such as high energy density, pollution-free combustion products, and wide availability, and is considered a crucial component of the future energy system. Hydrogen production through water electrolysis converts electrical energy into chemical energy, splitting water into hydrogen and oxygen. It offers advantages such as high product purity and simple process. However, the electrolysis process requires an electrocatalyst, and the performance of the electrocatalyst directly determines the hydrogen production reaction kinetic rate, making it a core factor limiting the efficiency of water electrolysis. Currently, electrocatalysts are mostly noble metal-based, transition metal-based, or carbon-based electrocatalysts. However, noble metal-based electrocatalysts are expensive, while transition metal-based or carbon-based electrocatalysts have unsatisfactory performance and insufficient structural stability under long-term operating conditions, limiting their industrial application.

[0003] In existing technologies, Ni3S2, due to its unique metallic electronic structure and good intrinsic conductivity, is used in the electrocatalytic hydrogen evolution reaction. However, single Ni3S2 materials have drawbacks such as a limited number of active sites, low hydrogen adsorption free energy, and cumbersome preparation processes. Therefore, Chinese Invention Patent 202310761080.1 discloses a Mo-doped Ni3S2 nanorod self-supporting electrocatalyst and its preparation method. Mo is incorporated into the Ni3S2 lattice as a dopant, allowing Mo-doped Ni3S2 nanorods to grow on the surface of nickel foam, effectively exposing active sites. However, under high current density and strong polarization conditions, the Mo atoms doped in the lattice of this electrocatalyst are easily oxidized and dissolved, and are lost into the electrolyte in the form of molybdate ions, which aggravates the lattice distortion. At the same time, the leaching loss of sulfur elements in the sulfide body is accompanied by the gradual destruction of the nanorod microstructure and partial pulverization and shedding. The violent scouring of bubbles at the electrode-electrolyte interface under high current further aggravates the above-mentioned structural destruction behavior, resulting in a large loss of active sites originally modulated by Mo doping, deterioration of the electronic structure of the material, and ultimately leading to a continuous decline in catalytic performance. Therefore, its long-term operating stability under industrial high current density is low. Summary of the Invention

[0004] To address the poor stability of electrocatalysts at high current densities in existing technologies, this invention provides a porous nickel-grown in-situ Ni3S2 / MoS2 material, its preparation method, and its applications. MoS2 nanosheets are encapsulated on Ni3S2 nanorods to form a core-shell heterostructure, reducing its stability at industrial-grade high current densities (500 mA·cm⁻¹). -2 The hydrogen evolution overpotential under the specified conditions was reduced, and its stability under industrial-grade high current density was improved.

[0005] To achieve the above objectives, the specific solution adopted by the present invention is as follows: a porous nickel in-situ grown Ni3S2 / MoS2 material, comprising a porous nickel matrix and Ni3S2 / MoS2 grown in-situ on the porous nickel matrix, wherein Ni3S2 is a nanorod array structure and MoS2 is a nanosheet wrapped around the Ni3S2 nanorods to form a core-shell heterostructure.

[0006] A method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material involves mixing nickel powder and NaCl powder and sintering the mixture to obtain a porous nickel matrix. The porous nickel matrix is ​​then placed in a mixed solution A and continuously stirred to obtain pretreated porous nickel. Mixed solution A is prepared by dissolving ammonium molybdate tetrahydrate, ammonium fluoride, and polyvinylpyrrolidone in deionized water at a mass ratio of 20:10:1~5. The pretreated porous nickel is then placed in mixed solution B and subjected to a hydrothermal reaction at 140~160℃ to obtain the target product. Mixed solution B is prepared by dissolving ammonium molybdate tetrahydrate and thioacetamide in deionized water at a mass ratio of 1:1~5.

[0007] As an optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material: the sintering process of the mixture of nickel powder and NaCl powder is as follows: the temperature is raised to 640~660℃ at a rate of 40~60℃ / min in a vacuum environment, and sintered for 10~20min, with an axial pressure of 10~30MPa during the sintering process; after sintering, the material is cooled with the furnace.

[0008] As another optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material: in mixed solution A, the ratio of ammonium molybdate tetrahydrate to deionized water is 1g:20~30mL.

[0009] As another optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material: in mixed solution B, the ratio of ammonium molybdate tetrahydrate to deionized water is 1g:20~30mL.

[0010] As another optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material: after the hydrothermal reaction, the porous nickel after the reaction is washed with deionized water, ultrasonically cleaned and rinsed with anhydrous ethanol in sequence, and then vacuum dried at 50~70℃ for 10~14h to obtain the target product.

[0011] As another optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material: before mixing nickel powder and NaCl powder, ball milling pretreatment is carried out under argon protection. The ball milling parameters are: ball-to-material ratio of 10:1, rotation speed of 250~350 r / min, and ball milling time of 8~12 h.

[0012] As another optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material, the NaCl powder has a particle size of 0.3~0.6 mm and the nickel powder has a particle size of 90~120 μm.

[0013] As another optimized method for preparing the above-mentioned porous nickel in-situ grown Ni3S2 / MoS2 material, the mass ratio of nickel powder to NaCl powder is 1:0.8~2.

[0014] Application of a porous nickel in-situ grown Ni3S2 / MoS2 material in hydrogen evolution by water electrolysis. The porous nickel in-situ grown Ni3S2 / MoS2 material is prepared by the above-mentioned preparation method.

[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a method for preparing porous nickel in-situ grown Ni3S2 / MoS2 materials. First, nickel powder and NaCl powder are mixed and sintered to obtain a porous nickel matrix. Then, the porous nickel matrix is ​​pretreated with a mixed solution A. Finally, the pretreated porous nickel is subjected to a hydrothermal reaction with a mixed solution B to obtain the target product. The sintering process can suppress grain coarsening, obtaining a high-strength porous nickel framework that can withstand bubble erosion under high current density. NaCl can precisely control the pore structure, forming interconnected micron-sized channels in the porous nickel, improving the active area and gas-liquid mass transfer. The combination of pretreatment and hydrothermal reaction prepares the target product. During the pretreatment process, NH4F dissociates to generate F... - The method employs coordination etching to perform mild and controllable chemical etching on the porous nickel matrix under the synergistic effect of ammonium molybdate. This creates numerous microscopic defects and roughened surfaces on the inner walls of the porous nickel channels, breaking the dense passivation layer on the surface of the porous nickel matrix. This provides a large number of active sites for the in-situ heterogeneous nucleation of Ni3S2 nanorods in the subsequent hydrothermal reaction, avoiding the phenomenon of local agglomeration and lack of growth of hydrothermal products, and achieving uniform growth of the nanorod array throughout the three-dimensional porous nickel channels. Polyvinylpyrrolidone is adsorbed on the surface of the etched porous nickel matrix to regulate the nucleation and growth dynamics of MoS2, resulting in ultrathin, low-crystallinity, and amorphous MoS2 nanosheets, which are then uniformly coated on the Ni3S2 nanorods. This ultrathin amorphous MoS2 can expose a large number of edge active sites, constructing a tight Ni3S2 / MoS2 core-shell heterogeneous interface, enhancing the two-phase electron transfer and synergistic catalytic effect. This enhances the bonding force between the active components and the substrate, strengthens the long-term stability under high current conditions, and enables the target product of this invention to operate stably for more than 550 hours under industrial-grade high current conditions. Attached Figure Description

[0016] Figure 1 This is an SEM image of a porous nickel matrix.

[0017] Figure 2 This is a high-magnification scan image of porous nickel in-situ grown Ni3S2 / MoS2 material.

[0018] Figure 3 This is the X-ray diffraction pattern of the porous nickel in-situ grown Ni3S2 / MoS2 material.

[0019] Figure 4 This is the X-ray photoelectron spectroscopy of porous nickel in-situ grown Ni3S2 / MoS2 material; among which, Figure 4 (a) represents the total spectrum. Figure 4 (b) shows the high-resolution spectrum of Ni. Figure 4 (c) represents the high-resolution spectrum of Mo. Figure 4 In the middle (d), the high-resolution spectrum of S is shown.

[0020] Figure 5 This is a comparison of hydrogen evolution polarization curves and hydrogen evolution overpotentials for in-situ grown porous Ni3S2 / MoS2 materials, MoS2 / Ni, and porous Ni; among them, Figure 5 In the middle (a), the hydrogen evolution polarization curve is shown. Figure 5 (b) represents the hydrogen evolution overpotential at a current density of 500 mA / cm².

[0021] Figure 6 These are the results of water electrolysis stability tests on the materials prepared in Example 1, Comparative Example 1, and Comparative Example 2 at a current density of 500 mA / cm². Figure 6 (a) represents the test results for MoS2 / Ni; Figure 6 (b) represents the test results of in-situ grown porous nickel Ni3S2 / MoS2 material. Figure 6 (c) represents the test results of Mo-doped Ni3S2 nanorods. Detailed Implementation

[0022] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. Parts not described or disclosed in detail in the following embodiments of the present invention should be understood as prior art known or should be known by those skilled in the art.

[0023] A porous nickel in-situ grown Ni3S2 / MoS2 material includes a porous nickel matrix and Ni3S2 / MoS2 grown in-situ on the porous nickel matrix. Ni3S2 is a nanorod array structure, and MoS2 is a nanosheet wrapped around the Ni3S2 nanorods to form a core-shell heterostructure.

[0024] The porous nickel matrix, with its porous structure, facilitates the penetration and diffusion of electrolyte solutions, shortens ion diffusion distances, and promotes rapid desorption of bubbles generated during the electrocatalytic reaction, preventing bubble accumulation on the electrode surface and thus avoiding the covering of catalytic active sites. The heterostructure constructed from Ni3S2 and MoS2 produces a synergistic effect. Ni3S2 grows as a nanorod array on the porous nickel matrix, providing a large specific surface area and abundant active sites; MoS2 is uniformly coated on the Ni3S2 nanorods in the form of ultrathin nanosheets, forming a core-shell heterostructure. This enables the target product to operate stably for over 550 hours under industrial-grade high-current conditions, while reducing its performance at industrial-grade high-current densities (500 mA·cm⁻¹). -2 The hydrogen evolution overpotential under ( ).

[0025] This invention also provides a method for preparing porous nickel in-situ grown Ni3S2 / MoS2 materials, comprising the following steps: To prepare the porous nickel matrix, firstly, nickel powder is placed in a ball mill jar with a ball-to-powder ratio of 10:1. After sealing the ball mill jar, argon gas is introduced for protection. Then, the ball mill jar is placed in a planetary ball mill for ball milling for 8-12 hours at a speed of 250-350 r / min. The particle size of the nickel powder after ball milling is 90-120 μm.

[0026] Ball-milled nickel powder and NaCl powder are mixed at a mass ratio of 1:0.8~2 to form a mixed powder with a NaCl powder particle size of 0.3~0.6mm. The mixed powder is placed in a mold for pre-pressing and then placed in a spark plasma sintering furnace. Under vacuum, the temperature is raised to 640~660℃ at a rate of 40~60℃ / min and sintered for 10~20min, with an axial pressure of 10~30MPa during the sintering process. After sintering, the mixture is cooled with the furnace. The sintered body is immersed in deionized water for 24h to remove NaCl and then dried at 50~70℃ to obtain a porous nickel matrix.

[0027] For the pretreatment of porous nickel matrix, ammonium molybdate tetrahydrate, ammonium fluoride, and polyvinylpyrrolidone were dissolved in deionized water at a mass ratio of 20:10:1~5, and the solution was ultrasonically treated to ensure thorough dispersion of the solutes, resulting in mixed solution A. The ratio of ammonium molybdate tetrahydrate to deionized water was 1 g: 20~30 mL. The porous nickel matrix was placed in mixed solution A and continuously stirred magnetically for 6~8 h until mixed solution A turned light blue with a grayish-white precipitate, yielding pretreated porous nickel. The pretreated porous nickel was then removed and rinsed clean.

[0028] Ni3S2 / MoS2 was grown in situ. Ammonium molybdate tetrahydrate and thioacetamide were dissolved in deionized water at a mass ratio of 1:1~5 to obtain mixed solution B, in which the ratio of ammonium molybdate tetrahydrate to deionized water was 1g:20~30mL. The pretreated porous nickel was placed in the lining of a hydrothermal reactor, and then mixed solution B was poured in until the pretreated porous nickel was completely submerged. The hydrothermal reaction was carried out at 140~160℃ for 10~14h. The porous nickel after the reaction was taken out and rinsed repeatedly with deionized water, supplemented by ultrasonic cleaning, until no black substance was removed from the surface. Then it was rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 50~70℃ for 10~14h to obtain the target product.

[0029] Example 1

[0030] A method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material includes the following steps: S1, Preparation of porous nickel matrix: 28g of nickel powder was placed in a ball mill jar with a ball-to-powder ratio of 10:1. The jar was sealed and purged with argon gas for protection. The jar was then placed in a planetary ball mill for 10 hours at a speed of 300 r / min. The particle size of the nickel powder after milling was 90-120 μm. 1.1g of the milled nickel powder and 0.9g of NaCl powder were mixed to form a mixed powder. The mixed powder was placed in a Ф20mm mold and pre-pressed for 10 seconds. It was then placed in a spark plasma sintering furnace and sintered at 650℃ for 15 minutes under vacuum at a rate of 50℃ / min, with an axial pressure of 20MPa during sintering. After sintering, the sintered body was cooled in the furnace. The sintered body was then soaked in deionized water for 24 hours to remove NaCl and dried at 60℃ to obtain a porous nickel matrix. SEM images of the porous nickel matrix were obtained, as shown below. Figure 1 As shown, by Figure 1 It can be seen that the porous nickel matrix has a large number of interconnected micron-sized pores, and the pores are evenly distributed.

[0031] S2, Pretreatment of porous nickel matrix: Dissolve 1.0 g of ammonium molybdate tetrahydrate, 0.1 g of polyvinylpyrrolidone and 0.5 g of ammonium fluoride in 25 mL of deionized water and sonicate to obtain mixed solution A; place the porous nickel matrix in mixed solution A and stir magnetically for 7 h until mixed solution A turns light blue with grayish-white precipitate to obtain pretreated porous nickel; remove the pretreated porous nickel and rinse it clean.

[0032] S3, In-situ growth of Ni3S2 / MoS2: 0.35 g of ammonium molybdate tetrahydrate and 0.5 g of thioacetamide were dissolved in 25 mL of deionized water to obtain mixed solution B. Pretreated porous nickel was placed in the lining of a hydrothermal reactor, and then mixed solution B was poured in until the pretreated porous nickel was completely submerged. The hydrothermal reaction was carried out at 150 °C for 12 h. The porous nickel after the reaction was taken out and rinsed repeatedly with deionized water and ultrasonically cleaned until no black substance was removed from the surface. Then it was rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 60 °C for 12 h to obtain the target product, which is denoted as the in-situ grown porous nickel Ni3S2 / MoS2 material.

[0033] Obtain SEM images of the target product, such as... Figure 2 As shown, ultrathin amorphous MoS2 nanosheets are wrapped around Ni3S2 nanorods.

[0034] Obtain the XRD pattern of the target product, such as Figure 3 As shown, three strong diffraction peaks appear on the XRD pattern, corresponding to the (111), (200), and (220) crystal planes of face-centered cubic nickel (Ni), originating from a porous nickel substrate. The remaining XRD diffraction peaks match the standard PDF card for Ni3S2, proving that the hydrothermal sulfidation step successfully generated the Ni3S2 phase. The absence of obvious sharp MoS2 characteristic diffraction peaks in the pattern indicates that the generated MoS2 is an ultrathin amorphous nanosheet with low crystallinity and extremely thin layers, lacking a clear long-range ordered crystal structure. This characteristic, however, exposes more edge active sites, enhancing the hydrogen evolution catalytic performance.

[0035] Obtain the XPS full spectrum, Ni 2p high-resolution spectrum, Mo 3d high-resolution spectrum, and S 1s high-resolution spectrum of the target product, such as... Figure 4 As shown, where, Figure 4 In the middle (a), the XPS full spectrum is shown, which characterizes the detection of Ni, O, C, Mo and S elemental signals on the surface of the target product; Figure 4 (b) shows the high-resolution spectrum of Ni 2p. The characteristic peak at 852.9 eV is the hallmark signal of Ni3S2, while 855.2 eV and 873.1 eV are attributed to Ni. 2+ Ni 2p 3 / 2 and Ni 2p 1 / 2 Spin splitting peaks, with signals at 861.2 eV and 879.1 eV being typical companion peaks for nickel-orbiting satellites; Figure 4 (c) shows the high-resolution spectrum of Mo 3d, with 231.6 eV corresponding to Mo. 4+ 3D 3 / 2 This proves the formation of MoS2, and the peak at 234.8 eV is attributed to Mo. 6+ The spectrum simultaneously contains Mo 4+ with Mo 6+The two valence states indicate that the surface of MoS2 undergoes slight oxidation in air; Figure 4 The middle (d) image shows the high-resolution spectrum of S 1s, with peaks at 161.4 eV and 163.4 eV corresponding to S 1s, respectively. 2- S 2p 3 / 2 and S2p 1 / 2 The broad peak at 168.7 eV is a characteristic vibrational peak of the SO bond. These results further demonstrate that both Ni3S2 and MoS2 phases coexist in the prepared sample.

[0036] Example 2

[0037] A method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material includes the following steps: S1, Preparation of porous nickel matrix: 28g of nickel powder was placed in a ball mill jar with a ball-to-powder ratio of 10:1. The jar was sealed and purged with argon gas for protection. The jar was then placed in a planetary ball mill for 10 hours at a speed of 250 r / min. The particle size of the nickel powder after milling was 90~120μm. The milled nickel powder and NaCl powder were mixed at a mass ratio of 1:0.8 to form a mixed powder. The mixed powder was placed in a Ф20mm mold and pre-pressed for 10s. Then, it was placed in a spark plasma sintering furnace and heated to 640℃ at a rate of 40℃ / min under vacuum. Sintering was carried out for 10 minutes with an axial pressure of 10MPa. After sintering, the sintered body was cooled with the furnace. The sintered body was soaked in deionized water for 24 hours to remove NaCl and dried at 50℃ to obtain a porous nickel matrix.

[0038] S2, Pretreatment of porous nickel matrix: Ammonium molybdate tetrahydrate, ammonium fluoride, and polyvinylpyrrolidone were dissolved in deionized water at a mass ratio of 20:10:1, with the ratio of ammonium molybdate tetrahydrate to deionized water being 1 g:20 mL. The solution was then sonicated to obtain mixed solution A. The porous nickel matrix was placed in mixed solution A and continuously stirred magnetically for 6 hours until mixed solution A turned pale blue with a grayish-white precipitate, yielding pretreated porous nickel. The pretreated porous nickel was then removed and rinsed clean.

[0039] S3, In-situ growth of Ni3S2 / MoS2: Ammonium molybdate tetrahydrate and thioacetamide were dissolved in deionized water at a mass ratio of 1:1 to obtain mixed solution B, with the ratio of ammonium molybdate tetrahydrate to deionized water being 1 g: 20 mL. The pretreated porous nickel was placed in the lining of a hydrothermal reactor, and then mixed solution B was poured in until the pretreated porous nickel was completely submerged. The hydrothermal reaction was carried out at 140 °C for 10 h. The porous nickel after the reaction was taken out and rinsed multiple times with deionized water, supplemented by ultrasonic cleaning, until no black substance was removed from the surface. Then it was rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 50 °C for 10 h to obtain the target product.

[0040] Example 3

[0041] A method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material includes the following steps: S1, Preparation of porous nickel matrix: 28g of nickel powder was placed in a ball mill jar with a ball-to-powder ratio of 10:1. The jar was sealed and purged with argon gas for protection. The jar was then placed in a planetary ball mill for 10 hours at a speed of 350 r / min. The particle size of the nickel powder after ball milling was 90~120μm. The ball-milled nickel powder and NaCl powder were mixed at a mass ratio of 1:2 to form a mixed powder. The mixed powder was placed in a Ф20mm mold and pre-pressed for 10s. Then, it was placed in a spark plasma sintering furnace and heated to 660℃ at a rate of 60℃ / min under vacuum. Sintering was carried out for 20 minutes with an axial pressure of 30MPa. After sintering, the sintered body was cooled with the furnace. The sintered body was soaked in deionized water for 24 hours to remove NaCl and dried at 70℃ to obtain a porous nickel matrix.

[0042] S2, Pretreatment of porous nickel matrix: Ammonium molybdate tetrahydrate, ammonium fluoride, and polyvinylpyrrolidone were dissolved in deionized water at a mass ratio of 20:10:5, with the ratio of ammonium molybdate tetrahydrate to deionized water being 1 g:25 mL. The solution was then sonicated to obtain mixed solution A. The porous nickel matrix was placed in mixed solution A and continuously stirred magnetically for 8 hours until mixed solution A turned pale blue with a grayish-white precipitate, yielding pretreated porous nickel. The pretreated porous nickel was then removed and rinsed clean.

[0043] S3, In-situ growth of Ni3S2 / MoS2: Ammonium molybdate tetrahydrate and thioacetamide were dissolved in deionized water at a mass ratio of 1:5 to obtain mixed solution B, with the ratio of ammonium molybdate tetrahydrate to deionized water being 1 g: 30 mL. The pretreated porous nickel was placed in the lining of a hydrothermal reactor, and then mixed solution B was poured in until the pretreated porous nickel was completely submerged. The hydrothermal reaction was carried out at 160 °C for 14 h. The porous nickel after the reaction was taken out and rinsed multiple times with deionized water, supplemented by ultrasonic cleaning, until no black substance was removed from the surface. Then it was rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 70 °C for 10 h to obtain the target product.

[0044] Example 4

[0045] A method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material includes the following steps: S1, Preparation of porous nickel matrix: 28g of nickel powder was placed in a ball mill jar with a ball-to-powder ratio of 10:1. The jar was sealed and purged with argon gas for protection. The jar was then placed in a planetary ball mill for 10 hours at a speed of 300 r / min. The particle size of the nickel powder after ball milling was 90~120μm. The ball-milled nickel powder and NaCl powder were mixed at a mass ratio of 1:1 to form a mixed powder. The mixed powder was placed in a Ф20mm mold and pre-pressed for 10s. Then, it was placed in a spark plasma sintering furnace and heated to 650℃ at a rate of 60℃ / min under vacuum. Sintering was carried out for 15 minutes with an axial pressure of 20MPa. After sintering, the sintered body was cooled with the furnace. The sintered body was soaked in deionized water for 24 hours to remove NaCl and dried at 60℃ to obtain a porous nickel matrix.

[0046] S2, Pretreatment of porous nickel matrix: Ammonium molybdate tetrahydrate, ammonium fluoride, and polyvinylpyrrolidone were dissolved in deionized water at a mass ratio of 20:10:1, with the ratio of ammonium molybdate tetrahydrate to deionized water being 1 g:20 mL. The solution was then sonicated to obtain mixed solution A. The porous nickel matrix was placed in mixed solution A and continuously stirred magnetically for 7 hours until mixed solution A turned pale blue with a grayish-white precipitate, yielding pretreated porous nickel. The pretreated porous nickel was then removed and rinsed clean.

[0047] S3, In-situ Growth of Ni3S2 / MoS2: Ammonium molybdate tetrahydrate and thioacetamide were dissolved in deionized water at a mass ratio of 1:3 to obtain mixed solution B, with the ratio of ammonium molybdate tetrahydrate to deionized water being 1 g: 25 mL. The pretreated porous nickel was placed in the lining of a hydrothermal reactor, and then mixed solution B was poured in until the pretreated porous nickel was completely submerged. The hydrothermal reaction was carried out at 150 °C for 12 h. The porous nickel after the reaction was taken out and rinsed multiple times with deionized water, supplemented by ultrasonic cleaning, until no black substance was removed from the surface. Then it was rinsed with anhydrous ethanol. Finally, it was placed in a vacuum drying oven and dried at 60 °C for 10 h to obtain the target product.

[0048] Comparative Example 1 A method for preparing porous nickel in-situ grown MoS2 material includes the following steps: S1, Preparation of porous nickel matrix: 28g of nickel powder was placed in a ball mill jar with a ball-to-powder ratio of 10:1. The jar was sealed and purged with argon gas for protection. The jar was then placed in a planetary ball mill for 10 hours at a speed of 300 r / min. The particle size of the nickel powder after milling was 90~120μm. 1.1g of the milled nickel powder and 0.9g of NaCl powder were mixed to form a mixed powder. The mixed powder was placed in a Ф20mm mold and pre-pressed for 10s. Then it was placed in a spark plasma sintering furnace and heated to 650℃ at a rate of 50℃ / min under vacuum. Sintering was carried out for 15 minutes with an axial pressure of 20MPa. After sintering, the sintered body was cooled with the furnace. The sintered body was soaked in deionized water for 24 hours to remove NaCl and dried at 60℃ to obtain a porous nickel matrix.

[0049] S2, the porous nickel matrix obtained in S1 is placed in a tube furnace and calcined at 500°C for 2 hours. During the calcination process, H2 / Ar mixed gas is introduced to further solidify the porous nickel alloy and prevent the porous nickel from being sulfided.

[0050] S3, Pretreatment of porous nickel matrix after calcination: Dissolve 1.0 g of ammonium molybdate tetrahydrate, 0.03 g of polyvinylpyrrolidone and 0.075 g of ammonium fluoride in 25 mL of deionized water and sonicate to obtain mixed solution A; place the calcined porous nickel matrix in mixed solution A and stir magnetically for 7 h until mixed solution A turns light blue with grayish-white precipitate to obtain pretreated porous nickel; remove the pretreated porous nickel and rinse it clean.

[0051] S4, In-situ growth of MoS2: 0.35 g of ammonium molybdate tetrahydrate and 0.5 g of thioacetamide were dissolved in 25 mL of deionized water to obtain mixed solution B; pretreated porous nickel was placed in the lining of a hydrothermal reactor, and then mixed solution B was poured in until the pretreated porous nickel was completely submerged. The hydrothermal reaction was carried out at 150 °C for 12 h. The porous nickel after the reaction was taken out and rinsed repeatedly with deionized water and ultrasonically cleaned until no black substance was removed from the surface; then it was rinsed with anhydrous ethanol; finally, it was placed in a vacuum drying oven and dried at 60 °C for 10-14 h to obtain MoS2 / Ni material.

[0052] Comparative Example 2 Mo-doped Ni3S2 nanorods were prepared using the method disclosed in invention patent 202310761080.1.

[0053] Three-electrode systems were prepared and assembled using the porous nickel in-situ grown Ni3S2 / MoS2 material obtained in Example 1, the MoS2 / Ni material obtained in Comparative Example 1, and porous Ni. Electrolysis tests were conducted in 1 mol / L KOH alkaline electrolyte, and the results are as follows: Figure 5As shown, where Figure 5 Figure (a) shows the LSV curve at 500 mA·cm⁻¹. -2 At the specified current density, the overpotential of the in-situ grown Ni3S2 / MoS2 material curve is lower than that of the MoS2 / Ni curve and the porous Ni curve. This demonstrates that when producing the same volume of hydrogen, the in-situ grown Ni3S2 / MoS2 material requires a smaller applied voltage. This indicates that Ni3S2 and the heterostructure significantly reduce the resistance to the hydrogen evolution reaction, and greatly improve the HER catalytic kinetics. Figure 5 (b) shows an industrial-grade high-current 500 mA·cm -2 Under the given conditions, the overpotential of porous Ni is 395 mV, the overpotential of MoS2 / Ni material is 366 mV, and the overpotential of in-situ grown porous Ni3S2 / MoS2 material is 301 mV. This demonstrates that in-situ grown porous Ni3S2 / MoS2 heterostructures can effectively address the defects of poor HER activity, excessive hydrogen adsorption, and slow water dissociation in pure nickel substrates. By relying on the synergistic effect of Ni3S2 and MoS2, the overpotential of Ni3S2 / MoS2 heterostructures can be reduced in industrial-grade applications with high current densities (500 mA·cm⁻¹). -2 The hydrogen evolution overpotential under the specified conditions was reduced, and its stability under industrial-grade high current density was improved.

[0054] The porous nickel in-situ grown Ni3S2 / MoS2 material prepared in Example 1, the MoS2 / Ni material prepared in Comparative Example 1, and the Mo-doped Ni3S2 nanorod self-supporting electrode obtained in Comparative Example 2 were subjected to constant current stability tests. An AEM alkaline electrolytic cell was used, and a 1 mol / L KOH alkaline electrolyte was introduced. The cathodes were MoS2 / Ni, porous nickel in-situ grown Ni3S2 / MoS2 material, and Mo-doped Ni3S2 nanorod self-supporting electrode, respectively. The anode was a laboratory-prepared NiS2 / NiMoFe self-supporting electrode. A constant current density of 500 mA·cm⁻¹ was used. -2 The reaction proceeded continuously under the specified conditions, and the test results are shown in [the table]. Figure 6 . Figure 6 (a) shows that after 319 hours of water splitting stability testing, the voltage of MoS2 / Ni increased from 1.98V to 2.38V, with an hourly voltage increase of 1.25 millivolts. The voltage fluctuation was large, indicating insufficient stability. Figure 6 Image (b) shows that after 550 hours of water splitting stability testing, the voltage of the porous nickel in-situ grown Ni3S2 / MoS2 material electrode increased from 1.89V to 1.96V, with an hourly voltage increase of 0.13 mV. The voltage increase was very small, and no large-scale detachment or pulverization of the electrode active material was observed throughout the entire testing process. Figure 6Figure (c) shows that after 120 hours of water splitting stability testing, the voltage of the Mo-doped Ni3S2 nanorods increased from 1.94V to 2.01V, with an hourly voltage increase of 0.58 mV. This significant voltage fluctuation indicates insufficient stability. This demonstrates that the material of this invention can operate stably for over 550 hours under industrial-grade high-current conditions, exhibiting excellent long-term high-current operational stability.

[0055] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A porous nickel in-situ grown Ni3S2 / MoS2 material, characterized in that: It includes a porous nickel matrix and Ni3S2 / MoS2 grown in situ on the porous nickel matrix. Ni3S2 is a nanorod array structure, and MoS2 is a nanosheet wrapped around the Ni3S2 nanorods to form a core-shell heterostructure.

2. A method for preparing a porous nickel in-situ grown Ni3S2 / MoS2 material, characterized by: Nickel powder and NaCl powder are mixed and sintered to obtain a porous nickel matrix; the porous nickel matrix is ​​placed in a mixed solution A and stirred continuously to obtain pretreated porous nickel; the mixed solution A is obtained by dissolving ammonium molybdate tetrahydrate, ammonium fluoride and polyvinylpyrrolidone in deionized water at a mass ratio of 20:10:1~5. Pretreated porous nickel was placed in mixed solution B and subjected to a hydrothermal reaction at 140-160°C to obtain the target product. Mixed solution B was obtained by dissolving ammonium molybdate tetrahydrate and thioacetamide in deionized water at a mass ratio of 1:1-5.

3. The method for preparing a porous nickel in-situ grown Ni3S2 / MoS2 material according to claim 2, characterized in that: The sintering process of the mixture of nickel powder and NaCl powder is as follows: the temperature is raised to 640-660℃ at a rate of 40-60℃ / min in a vacuum environment, and sintering is carried out for 10-20 min, with an axial pressure of 10-30 MPa during the sintering process; after sintering, the mixture is cooled with the furnace.

4. The method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material as described in claim 2, characterized in that: In mixed solution A, the ratio of ammonium molybdate tetrahydrate to deionized water is 1g:20~30mL.

5. The method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material as described in claim 2, characterized in that: In mixed solution B, the ratio of ammonium molybdate tetrahydrate to deionized water is 1g:20~30mL.

6. The method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material as described in claim 2, characterized in that: After the hydrothermal reaction was completed, the porous nickel was sequentially washed with deionized water, ultrasonically cleaned, and rinsed with anhydrous ethanol, and then vacuum dried at 50-70℃ for 10-14 h to obtain the target product.

7. The method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material as described in claim 2, characterized in that: Before mixing nickel powder and NaCl powder, the mixture is pre-treated by ball milling under argon protection. The ball milling parameters are: ball-to-material ratio of 10:1, rotation speed of 250~350 r / min, and ball milling time of 8~12 h.

8. The method for preparing a porous nickel in-situ grown Ni3S2 / MoS2 material as described in claim 2, characterized in that: The particle size of NaCl powder is 0.3~0.6 mm; the particle size of nickel powder is 90~120 μm.

9. The method for preparing porous nickel in-situ grown Ni3S2 / MoS2 material as described in claim 2, characterized in that: The mass ratio of nickel powder to NaCl powder is 1:0.8~2.

10. The application of a porous nickel in-situ grown Ni3S2 / MoS2 material in hydrogen evolution through water electrolysis, characterized in that: The porous nickel in-situ grown Ni3S2 / MoS2 material was prepared by any of the preparation methods described in claims 2-9.

Citation Information

Patent Citations

  • Mo-doped Ni3S2 nanorod self-supporting electrocatalyst and preparation method thereof

    CN117107270A