A diamond-metal laser additive manufacturing method for preferentially oriented facet-induced graphene bridging

By constructing a preferred orientation surface on the surface of metal powder and epitaxially growing graphene in situ, a continuous gradient bridging interface is formed, which solves the problems of weak interfacial bonding, thermal stress cracking and poor thermal conductivity of diamond/metal composites in SLM technology, and realizes the forming of composite materials with high density and high thermal conductivity.

CN123103011APending Publication Date: 2026-11-17SUZHOU AMPRO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611110110.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing SLM technology has problems such as insufficient interfacial wettability, pore defects, thermal mismatch stress concentration and high interfacial thermal resistance when preparing diamond/metal composites. This results in low material density and poor thermal conductivity, making it difficult to meet the requirements of engineering applications.

Method used

By constructing a preferred orientation surface on the surface of metal powder and epitaxially growing graphene in situ, a continuous gradient bridging interface of "metal-preferred orientation surface-graphene-carbide-diamond" is formed. The nano-flexible structure of graphene relaxes thermal mismatch stress and blocks crack propagation path, thus realizing the forming of high-density, crack-free, and high-thermal-conductivity composite materials.

Benefits of technology

High density (≥98%) and high thermal conductivity (≥580W/m·K) of diamond/metal composite materials were achieved, solving the problems of weak interfacial bonding and thermal stress cracking, and improving the mechanical and thermal properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103011A_ABST
    Figure CN123103011A_ABST
Patent Text Reader

Abstract

This invention discloses a diamond-metal laser additive manufacturing method using preferred orientation facets to induce graphene bridging, belonging to the field of additive manufacturing technology. The method includes: performing a crystallization heat treatment on metal powder to form a micro-platform dominated by preferred orientation facets on its surface; using CVD to grow a graphene layer in situ on the preferred orientation facets of the metal powder surface; vacuum micro-evaporation coating diamond particles with graphene-coated metal powder, followed by laser additive manufacturing to form a gradient bridging interface of "metal-preferred orientation facet-graphene-carbide-diamond" after solidification. This interface utilizes the flexible structure of graphene to relax thermal mismatch stress, prevent cracking, and reduce interfacial thermal resistance. The resulting part has a density ≥98% and a thermal conductivity ≥580 W / m·K, solving the problems of weak interfacial bonding and severe thermal stress cracking in SLM-formed diamond / metal composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of additive manufacturing and superhard composite materials, specifically to a diamond-metal laser additive manufacturing method for preferential orientation-induced graphene bridging. Background Technology

[0002] Diamond / metal composites, possessing both the ultra-high hardness and high thermal conductivity of diamond and the good toughness and machinability of a metal matrix, have broad application prospects in fields such as thermal management devices (e.g., high-power electronic heat sinks), superhard tools (e.g., diamond grinding wheels and cutting tools), and wear-resistant coatings. Selective laser melting (SLM), an important branch of metal additive manufacturing, melts metal powder layer by layer using a laser and rapidly solidifies it, making it possible to manufacture complex-shaped diamond / metal composite components in an integrated, near-net-shape configuration.

[0003] Currently, existing methods for preparing diamond / metal composites using SLM technology mainly involve coating the surface of diamond particles before mixing them with metal matrix powder and then printing. Specifically, strong carbide-forming elements such as titanium (Ti), chromium (Cr), and tungsten (W) are deposited on the surface of diamond particles using methods such as vacuum micro-evaporation coating, chemical plating, or magnetron sputtering. Under the high temperature of the SLM laser, the coating reacts with carbon atoms on the diamond surface to generate carbides (such as TiC, Cr3C2, and WC), thereby improving the interfacial bonding between diamond and the metal matrix (such as copper or nickel). However, this technical approach still faces the following fundamental technical challenges: Insufficient interfacial wettability and porosity defects. The wettability between the existing coating metal and the base metals such as copper and nickel is still limited. The laser heating time in the SLM process is extremely short (millisecond level), the molten pool exists for a short time, the interfacial reaction is insufficient, and the molten metal is difficult to spread completely and fill the gaps between diamond particles. This results in a large number of micropores remaining inside the formed part, and the density is difficult to meet the requirements of engineering applications.

[0004] Thermal mismatch stress concentration and microcrack propagation. The linear expansion coefficient of diamond (approximately 0.8~1.2×10⁻⁶). -6 / K) and copper (approximately 17 × 10) -6 / K), nickel (approximately 13 × 10⁻⁶ K), -6 When the matrix of a diamond-metal alloy differs by more than an order of magnitude from that of a metal matrix, the rapid heating and cooling of the laser-melted pool during the layer-by-layer rapid solidification process generates a significant temperature gradient and thermal cycling stress. The thermal mismatch stress at the interface is highly concentrated, making it extremely easy for microcracks to initiate at the diamond-metal interface and further propagate during subsequent thermal cycles. This leads to a significant decrease in the mechanical properties of the part (especially flexural strength and impact toughness), and even macroscopic cracking, severely restricting the engineering application of this material.

[0005] High interfacial thermal resistance. When diamond is in direct contact with the metal matrix or transitions through a thin carbide layer, phonon transport mismatch results in significant interfacial thermal resistance, limiting further improvement in the overall thermal conductivity of the composite material. Relying solely on the thermal conductivity of the metal binder phase or the carbide transition layer is insufficient to fully leverage the advantage of diamond's ultra-high in-plane thermal conductivity.

[0006] To address the aforementioned problems, this invention provides a diamond-metal laser additive manufacturing method that uses preferentially oriented facets to induce graphene bridging, thereby constructing a nanoscale flexible graphene bridging interface between diamond particles and a metal matrix. By utilizing the relaxation thermal mismatch stress of the graphene layer and blocking the crack propagation path, a high-density, crack-free, and high-thermal-conductivity integrated diamond / metal composite material part can be obtained. Summary of the Invention

[0007] The purpose of this invention is to provide a diamond-metal laser additive manufacturing method for preferred orientation facet-induced graphene bridging. This method involves first constructing a preferred orientation facet template on the surface of metal powder and then epitaxially growing graphene in situ to obtain graphene-coated metal powder. This graphene is then mixed with diamond particles coated with a carbide layer before laser additive manufacturing. During the forming process, a continuous gradient bridging interface of "metal-preferred orientation facet-graphene-carbide-diamond" is formed. The nano-flexible structure of the graphene layer relaxes thermal mismatch stress and blocks crack propagation paths, achieving high-density, crack-free, and high-thermal-conductivity diamond / metal composite material laser additive manufacturing.

[0008] The objective of this invention is achieved through the following technical solution: This invention provides a diamond-metal laser additive manufacturing method for preferentially oriented plane-induced graphene bridging, comprising the following steps: S1. Perform crystallization heat treatment on metal powder with a face-centered cubic lattice structure by placing the metal powder in a reducing atmosphere and heating it to (0.6~0.8)T. m Annealing is performed, where T m The melting point of the metal is expressed in K. The surface atoms of the metal powder are migrated and reconstructed to form a micro-platform dominated by a preferred orientation plane. After cooling, a metal powder with a preferred orientation on the surface is obtained.

[0009] S2. Graphene is epitaxially grown in situ on the preferred orientation surface of the metal powder. The metal powder obtained in step S1 is placed in a chemical vapor deposition reactor and heated to 850~1000℃ under a protective atmosphere. A gaseous carbon source is introduced to self-limit the growth of a graphene layer on the preferred orientation surface of the metal powder, thereby obtaining graphene-coated metal powder.

[0010] S3. Perform surface metallization treatment on the diamond particles by vacuum micro-evaporation coating. The coating material is selected from one or more of titanium, chromium, tungsten, and copper to form a carbide layer on the surface of the diamond particles, thereby obtaining metallized diamond particles.

[0011] S4. Mix the graphene-coated metal powder obtained in step S2 with the metallized diamond particles obtained in step S3 to obtain a composite powder.

[0012] S5. Place the composite powder obtained in step S4 in a laser additive manufacturing equipment and perform laser additive manufacturing under a protective atmosphere to melt the metal portion of the graphene-coated metal powder and embed the metallized diamond particles. After solidification, a gradient bridging interface of "metal-preferred orientation plane-graphene-carbide-diamond" is formed between the metal powder and the diamond particles.

[0013] In the above technical solution, in step S1, the metal powder is selected from face-centered cubic metals, including but not limited to one or a combination of copper, nickel, aluminum, and silver. The annealing treatment is carried out in a reducing atmosphere (Ar / H2), and the annealing temperature is controlled at the metal's melting point T. m Within a range of 0.6 to 0.8 times, sufficient energy is provided to allow surface atoms of the powder particles to migrate and reconstruct. Since the preferred orientation plane is the densest atomically packed and lowest surface energy crystal plane in face-centered cubic metals, atoms spontaneously migrate towards this direction, forming micro-platforms dominated by the preferred orientation plane. This orientation is preserved upon cooling. The metal powder with a preferred orientation obtained in this step provides a "template" with atomic-level flatness and lattice matching for subsequent in-situ epitaxial growth of graphene. The preferred orientation plane has a symmetric matching relationship with the honeycomb lattice structure of graphene, and its atomic arrangement can serve as a guide for the ordered growth of graphene.

[0014] In step S2, the in-situ epitaxial growth is performed using chemical vapor deposition (CVD). The metal powder with a preferred orientation obtained in step S1 is placed in a fluidized bed or rotary CVD reactor and heated to 850-1000°C under an Ar / H2 protective atmosphere. A gaseous carbon source (such as methane, ethylene, or acetylene) is introduced. Under the action of the preferred orientation plane template on the metal powder surface, carbon atoms decomposed from the carbon source gas undergo self-confined epitaxial growth on the preferred orientation plane, arranged in a honeycomb lattice, forming 1-50 high-quality graphene layers. Due to the good matching degree between the lattice constant of the preferred orientation plane and the graphene honeycomb structure, the graphene grows oriented along this plane, forming a strong coherent or semi-coherent interface bond with the metal substrate, which is different from simple mechanical mixing or physical coating. After growth, rapid cooling is performed to prevent excessive graphene stacking or transformation into defective graphene, resulting in a coated powder with strong graphene-metal interfacial bonding.

[0015] In step S3, due to the poor natural wettability between diamond particles and the molten metal, the diamond surface needs to be metallized. Diamond micropowder is placed in a vacuum micro-evaporation coating device, and the coating material is selected from strong carbide-forming elements such as titanium, chromium, and tungsten, or copper. Under high-temperature vacuum conditions, the coating metal reacts with carbon atoms on the diamond surface to form a carbide layer (such as TiC, Cr3C2, WC, Cu-C), with the coating thickness controlled between 50 and 500 nm. This carbide layer forms a chemical bond with the diamond substrate and serves as an intermediate transition layer between the subsequent graphene bridging layer and the diamond, achieving a gradient transition in chemical composition and thermal expansion coefficient. If the coating material is copper, a Cu-C reaction layer is formed on the diamond surface.

[0016] In step S4, the graphene-coated metal powder obtained in step S2 and the metallized diamond particles obtained in step S3 are mechanically mixed in a V-type mixer or a three-dimensional mixer in a certain proportion to ensure uniform dispersion of the two powders. The volume ratio of graphene-coated metal powder to metallized diamond particles is controlled within the range of (0.5:1) to (4:1) to ensure that the molten metal can fully embed the diamond particles and fill the gaps between the particles during the SLM forming process, while ensuring that the diamond particles are dispersed and exert a reinforcing effect in the final part. The resulting composite powder has good flowability and meets the powder laying requirements of laser additive manufacturing.

[0017] In step S5, the composite powder obtained in step S4 is placed in the powder bed of a laser additive manufacturing device (preferably a selective laser melting device) and laser scanning is performed under an inert protective atmosphere. The laser energy selectively melts the metal portion of the graphene-coated metal powder in the composite powder, forming a molten pool, while the diamond particles remain solid and are embedded in the molten metal. During this process, the graphene layer epitaxially grown in situ on the preferred orientation facet of the metal powder participates in the molten pool mass transfer. One side of the graphene layer is firmly bonded to the metal matrix through the coherent / semi-coherent interface of the preferred orientation facet, while the other side undergoes carbon-carbon interactions with the carbide layer on the diamond surface, forming a continuous graphene bridging interface. As the molten pool cools and solidifies, a continuous gradient bridging interface structure of "metal-preferred orientation facet-graphene-carbide-diamond" is finally formed. The nanoscale flexible structure of the graphene layer can effectively relax the thermal mismatch stress caused by the difference in thermal expansion coefficients between diamond and the metal matrix, and deflect and terminate the crack propagation path. At the same time, the ultra-high in-plane thermal conductivity of graphene creates an efficient phonon transmission channel, reduces interfacial thermal resistance, and significantly improves the overall thermal conductivity of the composite material.

[0018] Preferably, in step S1, the metal powder is one or more of copper powder, nickel powder, aluminum powder, or silver powder. The preferred annealing temperature for copper powder is 950-1050℃; for nickel powder, it is preferably 900-1100℃; for aluminum powder, it is annealed at 500-600℃ in a magnesium vapor reducing atmosphere; and for silver powder, it is preferably 700-900℃. All of the above metals have a face-centered cubic lattice structure, and their preferred orientation planes can serve as effective templates for graphene epitaxial growth.

[0019] Preferably, in step S1, the holding time for the annealing treatment is 60-240 minutes, and the reducing atmosphere is an Ar / H2 mixed atmosphere with an H2 volume content of 2%-20%. The reducing atmosphere is used to remove the oxide layer on the surface of the metal powder, ensuring the cleanliness of the powder surface, which is beneficial to atomic migration and the formation of preferred orientation planes.

[0020] Preferably, in step S2, the gaseous carbon source is methane, ethylene, or acetylene, the number of graphene layers is 1 to 50, and the growth time of the chemical vapor deposition is 10 to 30 minutes. Under the action of a preferred orientation template, the graphene grows in a self-confined manner, and the number of layers can be controlled by parameters such as growth time, carbon source concentration, and temperature. 1 to 50 graphene layers ensure both the continuity of the interface bridging and retain the flexible buffering function.

[0021] Preferably, in step S3, the thickness of the carbide layer is 50-500 nm, and the particle size of the diamond particles is 15-53 μm. Controlling the carbide layer thickness to the nanometer level ensures a strong bond with the diamond without increasing interfacial thermal resistance or introducing brittle phases due to excessive thickness. Matching the diamond particle size with the metal powder particle size ensures smooth powder spreading and high tap density of the composite powder.

[0022] Preferably, in step S4, the volume ratio of the graphene-coated metal powder to the metallized diamond particles is (0.5:1) to (4:1). Within this ratio range, the molten metal can fully encapsulate the diamond particles and fill the gaps between them, resulting in a high-density part.

[0023] Preferably, in step S4, the particle size of the graphene-coated metal powder is 50~150μm.

[0024] Preferably, in step S5, the laser additive manufacturing is selective laser melting, with a laser power of 50-1000W, a scanning speed of 200-1200mm / s, a scanning spacing of 0.03-0.15mm, a layer thickness of 0.03-0.12mm, and a substrate preheating temperature of 200-600℃. Specifically, the preheating temperature for copper-based composite substrates is preferably 200-400℃, and for nickel-based composite substrates, it is preferably 400-600℃. By controlling the laser parameters and preheating temperature, the molten pool temperature field and solidification process are precisely controlled, ensuring that the graphene layer remains at the interface after laser thermal cycling, preventing the graphene from being ablated or transformed into defective carbides.

[0025] The present invention also provides a diamond-metal composite material with preferred orientation facet-induced graphene bridging prepared by the above method. The composite material has a gradient bridging interface structure of "metal-preferred orientation facet-graphene-carbide-diamond". At the interface, the graphene layer is continuously bridged between the metal matrix and the carbide layer on the diamond surface. The part has a density ≥98% and a thermal conductivity ≥580W / m·K.

[0026] The microstructure of the composite material obtained in this invention is characterized by: diamond particles sequentially coated with a carbide layer (50~500nm), a graphene bridging layer (1~50 layers), a preferred orientation transition region, and a metal matrix on the outermost side. The graphene layer remains continuous and unbroken at the interface, its in-plane direction parallel to the preferred orientation of the metal, and is connected to the carbide layer on the diamond surface via carbon-carbon covalent bonds, forming a coherent / semi-coherent interface with the metal matrix through the preferred orientation. This continuous gradient interface structure utilizes the flexible two-dimensional structure of graphene to relax thermal mismatch stress and leverages the ultra-high in-plane thermal conductivity of graphene to achieve efficient phonon transfer, ultimately achieving excellent properties such as a part density ≥98% and a thermal conductivity ≥580W / m·K, with a flexural strength more than 15% higher than that of the same system material without graphene.

[0027] Due to the application of the above technical solution, the present invention has the following beneficial effects compared with the prior art: 1. This invention pre-constructs a preferred orientation template on the surface of metal powder and epitaxially grows graphene in situ, so that graphene and metal substrate form a coherent or semi-coherent interface bond, and the bonding strength is much higher than that of mechanical mixing or physical coating methods.

[0028] 2. This invention forms a continuous gradient bridging interface of "metal-preferred orientation surface-graphene-carbide-diamond" during the SLM forming process. It utilizes the nanoscale flexible structure of the graphene layer to relax thermal mismatch stress, cuts off and deflects the crack propagation path, and obtains crack-free, high-density SLM parts, thus solving the cracking problem caused by thermal stress in the prior art.

[0029] 3. In this invention, the graphene layer forms continuous bridging interfaces with the metal matrix and the diamond surface carbide layer on both sides, which significantly reduces the interfacial thermal resistance. The resulting part has a thermal conductivity that is more than 20% higher than that of the same system material without graphene, and a density of more than 98%.

[0030] 4. This invention uses CVD to self-limit the growth of graphene on the preferred orientation surface of metal powder. The number of layers is controllable, and the resulting coated powder can be directly used in commercial SLM equipment. It has good compatibility with existing processes, requires no equipment modification, and is easy to scale up.

[0031] 5. This invention can form a graphene bridging interface in situ during SLM forming simply by constructing a preferred orientation surface on the surface of metal powder and growing graphene in situ, combined with a nanoscale carbide coating on the diamond surface. The process is simple, the manufacturing cost is low, and it is suitable for industrial promotion. Attached Figure Description

[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, some of the drawings in the following description are some embodiments of the present invention. For those skilled in the art, other drawings can be made based on these drawings without creative effort.

[0033] Figure 1 This is a scanning electron microscope (SEM) image of the cross-section of the diamond / metal composite material part prepared in Example 1 of the present invention.

[0034] Figure 2 This is a scanning electron microscope (SEM) image of the composite powder in Example 1 of the present invention. Detailed Implementation

[0035] To provide a clearer understanding of the technical features, objectives, and effects of this invention, specific implementation schemes are now described in detail.

[0036] The present invention will be further described below with reference to embodiments, but the present invention is not limited to the following embodiments. The implementation conditions used in the embodiments can be further adjusted according to different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in the various embodiments of the present invention can be combined with each other as long as they do not conflict with each other.

[0037] Example 1 See appendix Figure 1 and appendix Figure 2 This embodiment provides a diamond-copper laser additive manufacturing method for preferentially oriented plane-induced graphene bridging, comprising the following steps: S1. Select copper powder (particle size 50~150μm) as metal powder, place the copper powder in an Ar / H2 mixed atmosphere (H2 volume content is 10%), heat to 950℃ for annealing treatment, and hold for 120 minutes to allow the surface atoms of the copper powder to migrate and reconstruct, forming a micro-platform with preferred orientation as the main feature, and obtain copper powder with preferred orientation on the surface after cooling.

[0038] S2. Place the copper powder obtained in step S1 in a fluidized bed chemical vapor deposition reactor, heat it to 950°C under an Ar / H2 protective atmosphere, introduce methane gas (flow rate of 2 sccm), and self-limitingly grow a graphene layer on the preferred orientation surface of the copper powder for 15 minutes to obtain graphene-coated copper powder.

[0039] S3. Select MBD-8 type diamond particles (particle size 15~53μm), perform vacuum micro-evaporation coating on the diamond particles, the coating material is copper, and form a Cu-C carbide layer on the surface of the diamond particles with a coating thickness of 50nm to obtain copper-plated diamond particles.

[0040] S4. The graphene-coated copper powder obtained in step S2 and the copper-plated diamond particles obtained in step S3 are mixed in a V-type mixer at a volume ratio of 3:7 for 3 hours to obtain composite powder.

[0041] S5. Place the composite powder obtained in step S4 into a selective laser melting device and perform selective laser melting and forming under argon atmosphere protection. The powder layer thickness is 0.03 mm, the substrate preheating temperature is 250℃, the laser power is 850W, the scanning speed is 800 mm / s, and the scanning interval is 0.06 mm. This melts the copper part of the graphene-coated copper powder and embeds the copper-plated diamond particles. After solidification, a gradient bridging interface of "copper-preferred orientation plane-graphene-Cu-C-diamond" is formed between the copper powder and the diamond particles.

[0042] Testing showed that the density of the diamond / copper composite material part prepared in this embodiment was 99.3%, and the thermal conductivity was 580 W / m·K. Figure 1 The image shown is a scanning electron microscope (SEM) image of the cross-section of the part in this embodiment, which shows that the graphene layer at the interface is continuously bridged between the copper substrate and the Cu-C layer on the diamond surface, without crack propagation. Figure 2 This is a scanning electron microscope (SEM) image of the composite powder in this embodiment.

[0043] Example 2 This embodiment is based on Embodiment 1, and the similarities with Embodiment 1 will not be repeated.

[0044] The difference between this embodiment and Embodiment 1 is that the metal powder in step S1 is nickel powder, the annealing temperature is 1000℃, the annealing holding time is 120 minutes, and the reducing atmosphere is an Ar / H2 mixed atmosphere (H2 volume content is 10%), thereby obtaining nickel powder with a preferred orientation on the surface.

[0045] In step S3, the coating material for vacuum micro-evaporation coating on the surface of diamond particles is titanium, with a coating thickness of 100 nm, forming a TiC carbide layer on the surface of diamond particles.

[0046] In step S4, the volume ratio of graphene-coated nickel powder to titanium-plated diamond particles is 2:1.

[0047] The process conditions for selective laser melting in step S5 are as follows: substrate preheating temperature is 500℃, laser power is 150W, scanning speed is 500mm / s, scanning spacing is 0.10mm, and layer thickness is 0.08mm.

[0048] Testing revealed that the diamond / nickel composite material obtained in this embodiment had a density of 98.5% and a thermal conductivity of 526 W / m·K. The graphene layer at the interface continuously bridged the nickel matrix and the TiC layer on the diamond surface, with no crack propagation.

[0049] Example 3 This embodiment is based on Embodiment 1, and the similarities with Embodiment 1 will not be repeated.

[0050] The difference between this embodiment and Embodiment 1 is that the metal powder in step S1 is aluminum powder, and the annealing is carried out at 550°C in a magnesium vapor reducing atmosphere for 120 minutes to obtain aluminum powder with a preferred orientation on the surface.

[0051] In step S3, the coating material for vacuum micro-evaporation coating on the surface of the diamond particles is chromium, with a coating thickness of 100 nm, forming a Cr3C2 carbide layer on the surface of the diamond particles.

[0052] In step S4, the volume ratio of graphene-coated aluminum powder to chromium-plated diamond particles is 2:1.

[0053] The process conditions for selective laser melting forming in step S5 are as follows: substrate preheating temperature is 300℃, laser power is 150W, scanning speed is 500mm / s, scanning spacing is 0.10mm, and layer thickness is 0.08mm.

[0054] Testing showed that the diamond / aluminum composite material part prepared in this embodiment had a density of 98.2% and a thermal conductivity of 492 W / m·K. The graphene layer at the interface continuously bridged the aluminum matrix and the Cr3C2 layer on the diamond surface, with no crack propagation.

[0055] Example 4 This embodiment is based on Embodiment 1, and the similarities with Embodiment 1 will not be repeated.

[0056] The difference between this embodiment and Embodiment 1 is that the metal powder in step S1 is silver powder, the annealing temperature is 800℃, the annealing holding time is 120 minutes, and the reducing atmosphere is an Ar / H2 mixed atmosphere (H2 volume content is 10%), so as to obtain silver powder with preferred orientation on the surface.

[0057] In step S3, the coating material for vacuum micro-evaporation coating on the surface of diamond particles is tungsten, with a coating thickness of 100 nm, forming a WC carbide layer on the surface of diamond particles.

[0058] In step S4, the volume ratio of graphene-coated silver powder to tungsten-plated diamond particles is 2:1.

[0059] The process conditions for selective laser melting forming in step S5 are as follows: substrate preheating temperature is 350℃, laser power is 120W, scanning speed is 600mm / s, scanning spacing is 0.10mm, and layer thickness is 0.08mm.

[0060] Testing revealed that the diamond / silver composite material obtained in this embodiment had a density of 98.0% and a thermal conductivity of 465 W / m·K. The graphene layer at the interface continuously bridged the silver matrix and the WC layer on the diamond surface, with no crack propagation.

[0061] Comparative Example 1 This comparative example is based on Example 1, and the similarities with Example 1 will not be repeated.

[0062] The difference between this comparative example and Example 1 is that the copper powder in step S1 is not subjected to crystallization heat treatment, that is, step S1 is omitted, and the raw copper powder without annealing treatment is used directly.

[0063] In step S2, graphene is grown directly on the surface of copper powder without preferential orientation treatment by chemical vapor deposition.

[0064] The remaining steps are the same as in Example 1.

[0065] Testing revealed that the density of the diamond / copper composite material part prepared in this comparative example was 92.5%, the thermal conductivity was 420 W / m·K, the graphene layer at the interface was discontinuous, with fractures and stacking phenomena, and there were obvious micro-cracks inside the part.

[0066] Comparative Example 2 This comparative example is based on Example 1, and the similarities with Example 1 will not be repeated.

[0067] The difference between this comparative example and Example 1 is that graphene is not grown on the surface of the copper powder in step S2, that is, step S2 is omitted and copper powder without graphene coating is used directly.

[0068] In step S4, the copper-plated diamond particles obtained in step S3 are mixed with copper powder that is not coated with graphene. The remaining steps are the same as in Example 1.

[0069] Testing revealed that the density of the diamond / copper composite material obtained in this comparative example was 91.2%, the thermal conductivity was 380 W / m·K, there was no graphene bridging layer at the interface, and there were obvious pores and microcracks between the copper matrix and the diamond particles.

[0070] The density, thermal conductivity, interface structure characteristics, and crack conditions of the diamond / metal composite material parts prepared in the above embodiments and comparative examples are listed in Table 1.

[0071] Table 1

[0072] As shown in Table 1, this invention achieves a continuous gradient bridging interface structure of "metal-preferred orientation plane-graphene-carbide-diamond" by performing a crystallization heat treatment on metal powder and epitaxially growing graphene on its surface, combined with a carbide coating on the diamond surface, followed by selective laser melting. The parts from Examples 1 to 4 all achieved a density of over 98%, with continuous and unbroken graphene layers at the interface, no internal cracks, and thermal conductivity of 580 W / m·K, 526 W / m·K, 492 W / m·K, and 465 W / m·K, respectively. In Comparative Example 1, because the copper powder was not subjected to crystallization heat treatment, graphene could not grow orderly on the copper powder surface, resulting in discontinuous graphene layers with breaks and stacking. The interface bridging effect was significantly reduced, the part density dropped to 92.5%, the thermal conductivity dropped to 420 W / m·K, and microcracks appeared. Comparative Example 2, lacking graphene growth on the copper powder surface and the absence of a graphene bridging layer at the interface, resulted in poor interfacial bonding between the copper substrate and diamond particles. Consequently, the density decreased to 91.2%, and the thermal conductivity dropped to 380 W / m·K, with noticeable porosity and microcracks. These comparative results fully validate the crucial role of the preferred orientation facet-induced in-situ graphene growth and the formation of a continuous gradient bridging interface structure in relaxing thermal mismatch stress, improving the density and thermal conductivity of the fabricated part.

[0073] In summary, this invention provides a method for diamond-metal laser additive manufacturing with preferred orientation facet-induced graphene bridging and a composite material prepared by this method. A preferred orientation facet micro-platform is constructed on the surface of a metal powder with a face-centered cubic lattice structure, and a graphene layer is epitaxially grown in situ on it to obtain graphene-coated metal powder. This graphene powder is then mixed with diamond particles coated with a carbide layer and subjected to selective laser melting. During the solidification process of the laser melt pool, a continuous gradient bridging interface structure of "metal-preferred orientation facet-graphene-carbide-diamond" is formed in situ. In this gradient interface structure, one side of the graphene layer forms a coherent or semi-coherent interface with the metal matrix through the preferred orientation facet, while the other side forms a continuous bridge with the carbide layer on the diamond surface through carbon-carbon interactions, achieving effective bridging of diamond and the metal matrix by graphene. This structure utilizes the nanoscale flexible two-dimensional structure of graphene to relax the thermal mismatch stress caused by the difference in thermal expansion coefficients between diamond and the metal matrix, thus cutting off and deflecting the crack propagation path. Simultaneously, the ultra-high in-plane thermal conductivity of graphene significantly reduces interfacial thermal resistance. Diamond / metal composite parts prepared using this method achieve a density exceeding 98%, with continuous, unbroken graphene layers at the interface, no internal cracks, and a maximum thermal conductivity of 580 W / m·K. Compared to solutions without graphene or without crystallization heat treatment, this invention significantly improves both density and thermal conductivity, effectively solving the technical challenges of weak interfacial bonding and severe thermal stress cracking in existing SLM-formed diamond / metal composites. Furthermore, the preparation process is compatible with existing SLM equipment, demonstrating broad prospects for industrial application.

[0074] The embodiments described above are merely illustrative of more specific and detailed implementations of the present invention, and should not be construed as limiting the scope of the invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the appended claims.

Claims

1. A method for diamond-metal laser additive manufacturing with preferentially oriented facet-induced graphene bridging, characterized in that, Includes the following steps: S1. Perform crystallization heat treatment on metal powder with a face-centered cubic lattice structure by placing the metal powder in a reducing atmosphere and heating it to (0.6~0.8)T. m Annealing is performed, where T m The melting point of the metal is expressed in K. The surface atoms of the metal powder are migrated and reconstructed to form a micro-platform dominated by a preferred orientation plane. After cooling, a metal powder with a preferred orientation on the surface is obtained. S2. Graphene is epitaxially grown in situ on the preferred orientation surface of the metal powder. The metal powder obtained in step S1 is placed in a chemical vapor deposition reactor and heated to 850~1000℃ under a protective atmosphere. A gaseous carbon source is introduced to self-limit the growth of a graphene layer on the preferred orientation surface of the metal powder, thereby obtaining graphene-coated metal powder. S3. Perform surface metallization treatment on diamond particles by vacuum micro-evaporation coating of diamond particles. The coating material is selected from one or more of titanium, chromium, tungsten, and copper to form a carbide layer on the surface of the diamond particles, thereby obtaining metallized diamond particles. S4. Mix the graphene-coated metal powder obtained in step S2 with the metallized diamond particles obtained in step S3 to obtain a composite powder. S5. Place the composite powder obtained in step S4 in a laser additive manufacturing equipment and perform laser additive manufacturing under a protective atmosphere to melt the metal portion of the graphene-coated metal powder and embed the metallized diamond particles. After solidification, a gradient bridging interface of "metal-preferred orientation plane-graphene-carbide-diamond" is formed between the metal powder and the diamond particles.

2. The method according to claim 1, characterized in that, In step S1, the metal powder is one or more of copper powder, nickel powder, aluminum powder, or silver powder.

3. The method according to claim 1, characterized in that, In step S1, the holding time for the annealing treatment is 60 to 240 minutes, and the reducing atmosphere is an Ar / H2 mixed atmosphere with an H2 volume content of 2% to 20%.

4. The method according to claim 1, characterized in that, In step S2, the gaseous carbon source is methane, ethylene, or acetylene, the number of graphene layers is 1 to 50, and the growth time of the chemical vapor deposition is 10 to 30 minutes.

5. The method according to claim 1, characterized in that, In step S3, the thickness of the carbide layer is 50~500nm, and the particle size of the diamond particles is 15~53μm.

6. The method according to claim 1, characterized in that, In step S4, the volume ratio of the graphene-coated metal powder to the metallized diamond particles is (0.5:1) to (4:1).

7. The method according to claim 1, characterized in that, In step S4, the particle size of the graphene-coated metal powder is 50~150μm.

8. The method according to claim 1, characterized in that, In step S5, the laser additive manufacturing is selective laser melting with a laser power of 50~1000W, a scanning speed of 200~1200mm / s, a scanning spacing of 0.03~0.15mm, a layer thickness of 0.03~0.12mm, and a substrate preheating temperature of 200~600℃.

9. A diamond-metal composite material with preferentially oriented facet-induced graphene bridging, characterized in that, The composite material is prepared by any one of claims 1 to 8 and has a gradient bridging interface structure of "metal-preferred orientation facet-graphene-carbide-diamond". The graphene layer at the interface is continuously bridged between the metal matrix and the carbide layer on the diamond surface. The part has a density ≥98% and a thermal conductivity ≥580W / m·K.