A method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology
By employing multi-metal laser powder bed fusion additive manufacturing technology, laser-guided lap remelting is used to form a shared molten pool, enabling wide-area diffusion and integrated forming of tungsten-copper heterogeneous components. This solves the problem of poor interfacial bonding quality in tungsten-copper heterogeneous components and improves interfacial bonding stability and thermal stress relief capabilities.
Patent Information
- Application Number
- CN202611320639.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to achieve wide-area diffusion and integrated forming of tungsten-copper heterogeneous components, resulting in poor interfacial bonding quality, concentrated thermal stress, and difficulty in applying them to complex, lightweight, and integrated thermal components.
By employing multi-metal laser powder bed fusion additive manufacturing technology, an overlapping area is set at the junction of tungsten and copper heterogeneous interfaces. The copper area is scanned first, followed by the tungsten area. Laser-guided overlapping and remelting are used to form a shared molten pool, achieving bidirectional wide-area diffusion of tungsten and copper elements and forming a continuously gradient metallurgical bonding interface.
A metallurgical bonding with a diffusion width of nearly 700 μm at the interface of tungsten-copper heterostructure components, continuous and gradual changes in composition, no abrupt changes, and no defects was achieved, which improved the interface compatibility and bonding stability and alleviated the problem of thermal stress concentration.
Smart Images

Figure CN123103013A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology. Background Technology
[0002] Tungsten-copper dissimilar components combine the high radiation resistance and high melting point of tungsten with the high thermal and electrical conductivity of copper, making them irreplaceable in fusion reactor divertors, high heat flux components, and aerospace thermal management systems. However, tungsten and copper have extremely mismatched physical properties: a melting point difference exceeding 2000℃, extremely low room temperature solubility, and a large difference in thermal expansion coefficients. They are typical dissimilar metals that are difficult to weld, and the bonding quality and diffusion range of their dissimilar interface directly determine the thermal stability, mechanical properties, and service life of the tungsten-copper dissimilar components.
[0003] Currently, tungsten-copper heterostructures are mainly connected using brazing and hot isostatic pressing (HIP). Brazing relies on an intermediate filler metal layer to indirectly connect the tungsten and copper substrates. However, after forming, the interface develops a multi-layered complex structure, easily generating brittle intermetallic compounds and low-melting-point brittle phases, severely damaging the high-temperature mechanical properties and continuous heat conduction channels of the interface, significantly weakening the high-temperature service reliability of tungsten-copper heterostructures. HIP involves applying high temperature and high pressure simultaneously in a closed cavity for a long period of steady-state action, relying on solid-state atomic diffusion to achieve metallurgical bonding of the tungsten-copper substrate. However, the solid-state diffusion kinetic rate is low, only achieving shallow atomic migration at the interface, resulting in a final interface diffusion layer thickness of only 5-8 μm. The diffusion transition range is extremely narrow, causing abrupt changes in physical properties on both sides of the interface, leading to high thermal stress concentration during service. Under high-low temperature cycling and instantaneous high-heat-flux impact conditions, the interface of tungsten-copper heterostructures is highly susceptible to failure behaviors such as microcracks and delamination.
[0004] In addition, brazing and hot isostatic pressing are composite forming processes involving separate splicing and overall pressure, which make it difficult to integrally form tungsten-copper precision components with complex irregular transition interfaces, thus limiting the application of tungsten-copper heterostructures in complex, lightweight, and integrated thermal components. Summary of the Invention
[0005] Purpose of the invention: The purpose of this invention is to provide a method for constructing tungsten-copper heterostructures that can achieve wide-area diffusion at the tungsten-copper heterostructure interface and can be directly integrally formed into complex irregular components. This method can form a tungsten-copper heterostructure interface with continuous gradual changes in composition, no abrupt changes, and no defects, and the effective diffusion width of the interface is nearly 700 μm.
[0006] Technical solution: The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to the present invention includes the following steps:
[0007] (1) Construct a three-dimensional CAD model of the tungsten-copper heterogeneous component, and divide it into tungsten and copper regions according to the component's function; slice the CAD model into layers, with the layer thickness set to 20~50μm according to the component's accuracy requirements; wherein, the laser power of the tungsten region is 400~500W, the laser scanning speed is 400~600mm / s, and the scanning line spacing is 0.05~0.08mm, and the laser power of the copper region is 300~450W, the laser scanning speed is 500~700mm / s, and the scanning line spacing is 0.09~0.11mm; the tungsten region adopts... High power (400~500W), slow scanning speed (400~600mm / s), and small line spacing (0.05~0.08mm) are used to ensure the full melting and shaping of high-melting-point tungsten metal. Compared with the tungsten region, the copper region is scanned with lower power (300~450W), faster scanning speed (500~700mm / s), and larger scanning line spacing (0.09~0.11mm) to avoid overheating, ablation, and spheroidization of the high thermal conductivity copper metal. At the same time, an overlap area of 0.05~0.15mm is set at the junction of the tungsten and copper heterogeneous interface.
[0008] (2) Import the slice file into the multi-metal laser powder bed melting and forming equipment, and then lay a copper powder layer of preset thickness in the area to be formed. According to the preset laser forming process parameters of the copper area, start the laser beam to perform selective melting and scanning to complete the forming of the current layered copper area entity (the current layered copper area entity covers an overlap area of 0.05~0.15mm, that is, the 0.05~0.15mm overlap area is the CuCrZr copper alloy entity); after the forming is completed, clean up the excess powder around this layer to leave room for the tungsten powder to be laid; after the single layer forming of the copper area is completed, lay a tungsten powder layer of corresponding thickness in the area to be formed of the tungsten area. According to the preset laser forming process parameters of the tungsten area, the laser beam completes the melting and forming of the current layered tungsten area along the preset tungsten area scanning trajectory; the tungsten area scanning trajectory covers an overlap area of 0.05~0.15mm, so that the high temperature melting zone of the tungsten side boundary and the remelted liquid zone of the copper side merge with each other, forming a continuous shared metallurgical pool at the tungsten-copper heterogeneous interface;
[0009] (3) After the laser leaves the interface, the molten pool cools rapidly to obtain a wide-area diffusion metallurgical bonding interface; after completing the additive manufacturing of the current layer, the forming platform descends by a preset layer thickness and stacks layer by layer to complete the preparation of the entire tungsten-copper heterostructure.
[0010] In step (1), the thickness of the slice layer is preferably 25~30μm; the laser power in the tungsten region is preferably 450~500W, the laser scanning speed is preferably 500~550mm / s, and the scanning line spacing is preferably 0.06mm; the laser power in the copper region is preferably 350~400W, the laser scanning speed is preferably 600~700mm / s, and the scanning line spacing is preferably 0.1mm; and an overlapping area with a width of preferably 0.1~0.12mm is set at the junction of the tungsten-copper heterogeneous interface.
[0011] In step (2), the copper powder is spherical CuCrZr copper alloy powder with a particle size of 15~53μm; the tungsten powder is spherical pure tungsten powder with a particle size of 15~53μm. During the laser forming process, the oxygen content of the processing environment is ≤100ppm, the circulating protective gas is argon, and the laser spot diameter is not higher than 75μm.
[0012] When scanning the tungsten region, the laser beam precisely overlaps the copper region by 0.05~0.15mm along a preset path, achieving secondary laser remelting of the copper interface edge. This invention utilizes laser-directed overlap remelting to rapidly absorb laser energy at the preset overlap edge of the copper region, causing instantaneous remelting and transforming it from a solid to a molten liquid state. Because the scanning trajectory of the tungsten region covers the overlap area, the high-temperature molten zone at the tungsten boundary and the remelted liquid region on the copper side adhere and fuse together, breaking the traditional solid-solid connection boundary and forming a continuous shared metallurgical pool at the tungsten-copper heterogeneous interface. This shared pool achieves direct liquid bonding of the two dissimilar metals. Inside the shared pool formed by laser overlap remelting, a high-intensity convection flow effect with multiple driving forces is simultaneously generated, completely different from the low-speed solid-phase diffusion of traditional processes, achieving large-scale, deep, bidirectional diffusion of tungsten and copper elements. The specific mechanisms are as follows: First, the melting point of tungsten (3410℃) differs greatly from that of copper (1083℃). During laser scanning, the temperature on the tungsten side of the molten pool is much higher than that on the copper side, creating a large instantaneous temperature gradient within the narrow shared molten pool. This drives the molten metal to flow directionally from the high-temperature tungsten side to the low-temperature copper side. Second, the uneven temperature distribution on the molten pool surface generates a surface tension gradient, inducing the Marangoni convection effect and accelerating the circulation and disturbance of the fluid within the molten pool. Third, the high temperature of the laser causes a small amount of evaporation on the metal surface, and the resulting vapor backflow pressure further impacts the molten pool fluid, enhancing the disturbance effect. Under the multiple coupled driving forces of temperature gradient, surface tension gradient, and vapor backflow pressure, a high-speed, bidirectional, and circulating coupled convection flow field is formed within the shared molten pool, completely breaking the static distribution state of the metal within the molten pool. Strong convection continuously drives the deep migration and penetration of liquid copper elements from the copper side into the high-temperature region of the tungsten side. Simultaneously, trace amounts of tungsten elements diffuse and transition into the copper interface, achieving bidirectional wide-area diffusion of these two dissimilar metals. This effectively broadens the interface diffusion width, constructs a gradual elemental distribution structure, and eliminates abrupt compositional defects at the interface. This coupled convection-diffusion mechanism transforms the tungsten-copper interface from a sharply defined, spliced interface into a continuously gradually changing diffusion transition interface, significantly improving interface compatibility and bonding stability. After the laser leaves the interface, the molten pool cools rapidly, ultimately constructing a wide-area diffusion metallurgical bonding interface that is wider than that of traditional solid-state bonding processes.
[0013] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: The present invention adopts a sequential scanning method of scanning the copper region first and then the tungsten region, so that the copper side edge will be locally remelted during the scanning of the tungsten region, forming a continuous liquid connection zone at the heterogeneous interface. The continuous liquid connection zone can effectively reduce the interface non-fusion defects, improve the wetting and filling ability of liquid copper on tungsten particles, and form a continuous metallurgical bond at the interface, thereby improving the bonding quality of the interface. Finally, a high-quality metallurgical bonding interface with continuous gradual change in composition, no abrupt change, and no defects is formed. The effective diffusion width of the tungsten-copper heterogeneous component interface is nearly 700μm. This structure can effectively alleviate the problem of interface thermal stress concentration caused by the difference in thermophysical properties between tungsten and copper dissimilar metals. Attached Figure Description
[0014] Figure 1 SEM images of the spherical pure tungsten powder and the spherical CuCrZr copper alloy powder used in this invention;
[0015] Figure 2 A three-dimensional CAD model of the tungsten-copper heterostructure constructed for Example 1;
[0016] Figure 3 This is a schematic diagram of the shared molten pool formed during the laser forming process in Example 1;
[0017] Figure 4 These are photographs of tungsten and copper being formed during the laser forming process in Example 1.
[0018] Figure 5 Photographs and SEM images of the interface of the tungsten-copper heterostructure obtained in Example 1 are shown.
[0019] Figure 6 SEM image of the interface of the tungsten-copper heterostructure obtained in Comparative Example 1;
[0020] Figure 7 SEM image of the non-spherical pure tungsten powder used in Comparative Example 2;
[0021] Figure 8 SEM image of the interface of the tungsten-copper heterostructure obtained in Comparative Example 2;
[0022] Among them, copper region 101; overlapping region 102; tungsten region 103; laser 201; molten pool 202; tungsten solid 203; tungsten powder 204; interface diffusion mixed solid 205; CuCrZr powder 206; fluid flow inside the molten pool 207; copper solid 208. Detailed Implementation
[0023] Example 1
[0024] This invention relates to a method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology, comprising the following steps:
[0025] (1) Select spherical pure tungsten powder with a particle size of 15~53μm and spherical CuCrZr copper alloy powder with a particle size of 15~53μm. The microstructure of the powder is as follows: Figure 1 As shown;
[0026] (2) Construct a standardized 3D CAD model of the tungsten-copper heterostructure. The model adopts a regular and symmetrical structural design. The length, width, and height of the pure tungsten functional area and the CuCrZr copper alloy functional area are uniformly set to 10mm×5mm×3mm. An overlapping area is directly set at the junction of the tungsten and copper areas, with a width of 0.1mm. The model structure and area division are as follows: Figure 2 As shown in Table 1, after completing the model construction and functional area division, the overall heterogeneous model was sliced using multi-metal laser powder bed melting (LPBF) slicing software, with a single powder layer thickness of 30 μm. The process parameters for laser forming of the tungsten and copper regions are shown in Table 1. The laser power for the pure tungsten region was 450 W, the laser scanning speed was 500 mm / s, and the scanning line spacing was 0.06 mm, corresponding to a laser volumetric energy density of 500 J / mm². 3 This energy density range effectively avoids powder fusion defects caused by low energy density, while also preventing forming problems such as violent molten pool fluctuations, metal splashing, and internal porosity caused by high energy density, ensuring the compactness and stability of the tungsten region formation; the laser power in the CuCrZr copper alloy region is 400W, the laser scanning speed is 600mm / s, and the scanning line spacing is 0.1mm, corresponding to a laser volumetric energy density of approximately 222J / mm². 3 This parameter can be adapted to the high thermal conductivity of copper alloys, effectively suppressing defects such as spheroidization, ablation, and porosity, and achieving high-quality dense forming of copper regions.
[0027] Table 1 shows the processing parameters during the laser forming process in Example 1.
[0028]
[0029] (3) Import the pre-processed slice forming file into the multi-metal laser powder bed melting forming equipment, and complete the pre-processing operations such as equipment optical path calibration, powder spreading system debugging, protective gas circulation and oxygen content detection in advance to ensure that the equipment is in a stable working state; during the forming process, the CuCrZr copper alloy region and the pure tungsten region are sequentially melted and formed in the same powder spreading layer, that is, the CuCrZr copper alloy region is formed first and the pure tungsten region is formed later, so as to achieve precise construction of the same layer partition of two dissimilar metal materials; since the pure tungsten region uses higher laser power, With a lower scanning speed and a significantly higher overall laser energy input density than the copper alloy region, the high-energy-density laser beam can cover the 0.1mm overlap area (the 0.1mm overlap area being the pre-formed CuCrZr copper alloy entity) when scanning the tungsten-copper interface overlap region. This allows for sufficient secondary remelting of the already formed CuCrZr copper alloy side interface edge, eliminating defects such as interface incomplete fusion, micropores, and cracks that are easily encountered in traditional tungsten-copper heterogeneous forming. Simultaneously, relying on the shared molten pool formed by the overlap remelting and the multi-field coupled convection diffusion effect (such as... Figure 3 As shown in the figure, bidirectional wide-area diffusion of tungsten and copper is achieved;
[0030] (3) After completing the additive manufacturing of the current layer according to step (2), the forming platform descends by a preset layer thickness and stacks the layers one by one to complete the preparation of the entire tungsten copper heterostructure.
[0031] The effective diffusion width at the interface of the tungsten-copper heterostructure finally prepared in Example 1 was approximately 693 μm (e.g., Figure 5 As shown in the figure, compared with the narrow diffusion interface of traditional solid-state bonding and conventional laser splicing processes, the diffusion area is greatly widened. At the same time, the interface formed in Example 1 is a metallurgical bonding interface with continuous gradual change in composition, no abrupt changes, and no defects.
[0032] Comparative Example 1
[0033] Comparative Example 1 was prepared using the same method as Example 1, except that the processing parameters during the laser forming process were changed from 450W laser power and 500mm / s for the tungsten region and 400W laser power and 600mm / s for the copper region to 350W laser power and 700mm / s for the tungsten region and 250W laser power and 900mm / s for the copper region; finally, a tungsten-copper heterostructure was obtained.
[0034] Table 2 shows the processing parameters during the laser forming process in Comparative Example 1.
[0035]
[0036] The effective diffusion width at the interface of the tungsten-copper heterostructure prepared in Comparative Example 1 was 483 μm (e.g., Figure 6As shown in the figure, compared to Example 1, the interface width of Comparative Example 1 decreased. This is because the laser power and scanning speed were reduced, resulting in a smaller molten pool size and faster solidification time, which in turn narrowed the interface diffusion width. Furthermore, it can be observed that there are pore defects on the tungsten side and crack defects on the copper side.
[0037] Comparative Example 2
[0038] Comparative Example 2 was prepared using the same method as Example 1, the only difference being that the raw material was changed from spherical pure tungsten powder with a particle size of 15-53 μm to non-spherical pure tungsten powder with an equivalent particle size distribution of 8-28 μm. Figure 7 As shown. When using non-spherical powders, the heterogeneous interface lacks a clear and regular boundary, and the tungsten phase exhibits a distinctly discontinuous distribution, such as... Figure 8 As shown. This is because non-spherical powder particles have sharp edges and poor flowability, resulting in significant fluctuations in powder bed density during the powder spreading process. Under laser irradiation, the stability of the molten pool decreases, and the wetting behavior of tungsten particles in the copper melt deteriorates, making it difficult to form a continuous and dense tungsten skeleton. At the same time, irregular powder exacerbates molten pool disturbance and local element segregation, ultimately causing blurred interface contours and tungsten phase fracture and dispersion, making it difficult to obtain structurally controllable tungsten-copper integrated heterogeneous components.
Claims
1. A method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology, characterized in that, Includes the following steps: (1) Construct a three-dimensional CAD model of the tungsten-copper heterostructure and divide it into tungsten and copper regions according to the function of the component; slice the CAD model into layers with a layer thickness of 20~50μm; the laser power of the tungsten region is 400~500W, the laser scanning speed is 400~600mm / s, and the scanning line spacing is 0.05~0.08mm; the laser power of the copper region is 300~450W, the laser scanning speed is 500~700mm / s, and the scanning line spacing is 0.09~0.11mm; set an overlap area with a width of 0.05~0.15mm at the junction of the tungsten-copper heterostructure. (2) Import the slice file into the multi-metal laser powder bed melting and forming equipment, and then lay a copper powder layer of preset thickness in the area to be formed. According to the preset laser forming process parameters of the copper area, start the laser beam to perform selective melting and scanning to complete the forming of the current layered copper area. After the single-layer forming of the copper area is completed, lay a tungsten powder layer of corresponding thickness in the area to be formed of the tungsten area. According to the preset laser forming process parameters of the tungsten area, the laser beam completes the melting and forming of the current layered tungsten area along the preset tungsten area scanning trajectory. The tungsten area scanning trajectory covers an overlap area of 0.05~0.15mm, so that the high-temperature melting zone of the tungsten side boundary and the remelted liquid zone of the copper side merge with each other, forming a continuous shared metallurgical pool at the tungsten-copper heterogeneous interface. (3) After the laser leaves the interface, the molten pool cools rapidly to obtain a wide-area diffusion metallurgical bonding interface; after completing the additive manufacturing of the current layer, the forming platform descends by a preset layer thickness and stacks layer by layer to complete the preparation of the entire tungsten-copper heterostructure.
2. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (1), the thickness of the slice layer is set to 25~30μm.
3. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (1), the laser power in the tungsten region is 450~500W, the laser scanning speed is 500~550mm / s, and the scanning line spacing is 0.06mm.
4. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (1), the laser power in the copper region is 350~400W, the laser scanning speed is 600~700mm / s, and the scanning line spacing is 0.1mm.
5. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (1), an overlap area with a width of 0.1~0.12mm is set at the junction of the tungsten-copper heterogeneous interface.
6. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (2), the copper powder is spherical CuCrZr copper alloy powder with a particle size of 15~53μm.
7. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (2), the tungsten powder is spherical pure tungsten powder with a particle size of 15~53μm.
8. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (2), during the laser forming process, the oxygen content of the processing environment is ≤100ppm.
9. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (2), during the laser forming process, the circulating protective gas is argon.
10. The method for constructing tungsten-copper heterostructures based on multi-metal laser powder bed fusion additive manufacturing technology according to claim 1, characterized in that: In step (2), during the laser forming process, the diameter of the laser spot is no higher than 75 μm.