A method for automatic welding of small-diameter stainless steel pipes in all positions
By machining axial longitudinal grooves at the tip of the tungsten electrode and combining them with internal and external cooling systems, the problems of arc drift and heat accumulation in the welding of small-diameter stainless steel pipes were solved. This achieved full cross-sectional penetration of complex joints and improved the density and mechanical properties of the welded joints, meeting the sealing requirements of high-pressure clean pipeline systems.
Patent Information
- Application Number
- CN202611579095.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-17
AI Technical Summary
Small-diameter stainless steel pipes are prone to arc drift and excessive heat accumulation during automatic welding. Furthermore, complex joints such as those with varying wall thicknesses or corner joints are difficult to achieve complete penetration across the entire cross-section, resulting in poor weld formation and failure to meet the sealing requirements of high-pressure clean pipeline systems.
By employing a synergistic mechanism of a tungsten electrode with a specific surface microstructure and an internal and external dual cooling system, and by machining axial longitudinal grooves at the tip of the tungsten electrode and combining them with internal and external cooling channels, the thermodynamic and electromagnetic states during the welding process are precisely controlled. Combined with a pipe clamp assembly adapted to complex spaces and preset welding parameters, stable arc focusing and narrowing of the heat-affected zone are achieved.
It achieves stable arc focusing, avoids grain coarsening in the heat-affected zone caused by excessive heat accumulation, ensures the density and mechanical properties of the welded joint, solves the problem of full cross-section penetration in complex joints, and meets the sealing requirements of high-pressure clean pipeline systems.
Smart Images

Figure CN123103129A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of automatic welding technology, and in particular to an automatic welding method for small-diameter stainless steel pipes in all positions. Background Technology
[0002] Small-diameter stainless steel pipes are widely used in fluid transport networks in aerospace, semiconductor manufacturing, and biomedicine industries. In the assembly and installation of pipeline systems, all-position automated tungsten inert gas welding (TIG) is the core technology for achieving high-quality connections between pipe fittings.
[0003] However, small-diameter stainless steel pipes are characterized by thin walls and low heat capacity, presenting inherent technical bottlenecks when welding under space-constrained conditions. Conventional tungsten electrode fabrication processes generate circumferential grinding textures on the electrode tip surface. This microstructure leads to an imbalance in the electric field distribution, causing the cathode spot to jump laterally in the circumferential direction, resulting in arc drift and uneven weld penetration. Under continuous welding conditions, limited by the heat transfer path of a single pipe wall, heat is rapidly conducted axially along the pipe wall and accumulates in large quantities. This heat accumulation not only easily leads to thermal deformation of thin-walled pipes but also causes the heat-affected zone to remain at high temperatures for too long, resulting in austenite grain coarsening and a decline in the overall mechanical properties of the joint.
[0004] Furthermore, actual engineering projects involve numerous non-standard assembly nodes such as reducing joints, short straight pipes, and short elbows. Conventional standard welding clamps are prone to physical interference when dealing with these complex geometries, making it difficult to maintain the coaxiality of the joined pipe fittings. When there are differences in wall thickness or fillet welds between the assembled pipe fittings, the heat capacity of the base materials on both sides is severely unbalanced. Due to the lack of a targeted heat input focus adjustment mechanism in existing technologies, thin-walled areas are prone to thermal collapse under continuous arc action, while the thick-walled side and deep joints cannot obtain sufficient heat, leaving defects such as incomplete penetration, incomplete fusion, or porosity. At the same time, under the all-position rotary welding trajectory, the liquid metal is prone to sag due to gravity, and conventional continuous heating modes cannot maintain the stability of the molten pool in various spatial positions, ultimately leading to poor weld formation and failure to meet the stringent sealing requirements of high-pressure clean pipeline systems. Summary of the Invention
[0005] The purpose of this invention is to provide an automatic welding method for small-diameter stainless steel pipes in all positions, which solves the problems of arc drift and excessive heat accumulation that easily occur during automatic welding of small-diameter thin-walled stainless steel pipes, as well as the difficulty in achieving full cross-section penetration in complex joints such as those with different wall thicknesses or corner joints.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] This invention provides an automatic welding method for small-diameter stainless steel pipes in all positions, employing the following technical solution:
[0008] The end face of the pipe is cut and smoothed, the inner and outer peripheries of the pipe opening are deburred and polished, and the end face and the inner and outer peripheries of the pipe opening are wiped clean with organic solvent.
[0009] The two sections of the pipe fittings are coaxially connected and spot-welded for positioning along the circumferential direction of the joint;
[0010] The tip of the tungsten electrode is ground into a cone shape and axial longitudinal grooves are machined on the cone surface. The tungsten electrode is then inserted into the chuck of an all-position automatic welding clamp.
[0011] The pipe fitting, after being spot-welded and positioned, is placed in the pipe clamp assembly for clamping and securing; both ends of the pipe fitting are sealed and protective gas is introduced into the pipe fitting;
[0012] The cooling circuit is activated, allowing the coolant to circulate through the cooling channel inside the all-position automatic welding gun, while the water-cooling module is attached to the outer wall surface of the pipe for localized cooling.
[0013] Input preset parameters into the welding machine control system to generate a welding program, and start the welding program to drive the tungsten electrode to rotate around the circumference of the pipe to perform automatic welding.
[0014] By adopting the above technical solution, the thermodynamic and electromagnetic states during the welding process can be precisely controlled due to the synergistic mechanism of the tungsten electrode with a specific surface microstructure and the internal and external dual cooling system. Therefore, a dense welding effect with stable arc focusing, narrow heat-affected zone, and no incomplete fusion or porosity defects in the joint is obtained.
[0015] Its core mechanism and reaction process are as follows:
[0016] Cathode electron emission channel reconfiguration mechanism:
[0017] Traditional grinding processes leave circumferential mechanical grooves on the tungsten electrode surface, causing the electric field distribution to lose its axisymmetry and resulting in lateral drift of the arc spot. This solution involves machining axial longitudinal grooves on the conical surface of the tungsten electrode, creating metal ridges along the axial direction at the microscopic level. Based on the tip effect of the microscopic electric field, electric field lines accumulate at high density at these axial ridge locations.
[0018] When an arc-ignition voltage is applied to the system, the electric field intensity distribution changes, and the energy barrier for electrons to overcome the work function at the material surface decreases. The emission process follows the Richardson-Douchman equation, with electrons preferentially forming directional emission channels along axial micro-ridges. This channel structure blocks the disordered jumping of the cathode spot in the circumferential direction, concentrating the energy density of the plasma arc highly along the central axis and maintaining the consistency of the weld pool geometry.
[0019] Dual thermodynamic dynamic equilibrium mechanism:
[0020] When an all-position automatic welding gun operates continuously within a confined pipe space, the system's heat input primarily comes from arc radiation heat and Joule heat generated by conductive components. The heat conduction mechanism of a single pipe wall causes heat to rapidly diffuse to the base material on both sides.
[0021] This scheme establishes a dual heat dissipation model: the internal cooling channel forcibly removes the accumulated heat of the core components of the equipment through convection heat transfer; the water-cooled module attached to the outer wall of the pipe adds an additional heat exchange boundary at the solid-liquid interface.
[0022] This mechanism limits the heating range of the base material to the periphery of the weld, avoiding the precipitation of chromium carbide and grain coarsening caused by excessively long high-temperature residence time in austenitic stainless steel, thus ensuring the room temperature and high-temperature mechanical properties of the joint area.
[0023] Preferably, the end face of the pipe fitting is cut and smoothed, specifically as follows:
[0024] The end face is cut using a pipe cutting machine, and the perpendicularity error between the rotation axis of the cutter head and the axis of the pipe is controlled to be less than or equal to 0.1°; the polishing is done using wet sandpaper or a pneumatic stainless steel wire brush; the wiping and cleaning is done using a non-woven cloth soaked in the organic solvent, wherein the organic solvent is acetone or anhydrous ethanol.
[0025] By adopting the above technical solution, a chemical pretreatment mechanism for removing porosity nucleation sources was established. Controlling perpendicularity error during the pipe cutting process eliminated macroscopic geometric gaps at the mating ends, preventing air entrapment. Grinding removed the dense oxide film from the pipe surface. Wiping with acetone or anhydrous ethanol removed residual cutting fluid and hydrocarbon grease.
[0026] Under the high temperature of an electric arc, any residual hydrocarbons will undergo thermal decomposition. The generated hydrogen gas dissolves in the molten pool and cannot completely escape during the rapid solidification of the molten pool, forming macroscopic volumetric porosity defects inside the weld.
[0027] The pretreatment steps of this scheme cut off the gas evolution source from both physical boundaries and chemical composition, ensuring the compactness of the internal structure of the weld.
[0028] Preferably, when two pipe sections are coaxially connected, the gap between the two pipe sections is less than or equal to 0.05 mm, the radial misalignment is less than or equal to 10% of the pipe wall thickness, and the number of spot welding positions along the circumferential direction of the joint is 2 to 4 points, with a single-point arc ignition time of 0.5 s to 1.5 s.
[0029] By adopting the above technical solution, the gap and misalignment are limited, eliminating geometric stress concentration points at the bonding interface. The limited misalignment allows the arc heat to be evenly distributed to the end faces of both pipe walls.
[0030] The set number of spot weld positions and short-time arc ignition parameters, while establishing the initial connection strength, minimize the local heat input and thermal stress generated by spot welding, preventing the pipe fitting from warping and deforming due to thermal expansion during subsequent continuous welding heating.
[0031] Preferably, the tungsten electrode is a cerium tungsten electrode, the cone angle of the cone is 20° to 30°, and the surface roughness of the axial longitudinal groove is 0.4μm to 1.6μm; the all-position automatic welding clamp has a drive half tooth, and after being inserted into the chuck of the all-position automatic welding clamp, the tail end of the tungsten electrode does not protrude beyond the outer edge of the drive half tooth.
[0032] By adopting the above technical solution, the doping of cerium oxide in the cerium-tungsten electrode reduces the electron work function and improves the arc ignition success rate. The 20°–30° cone angle setting optimizes the morphology of the arc plasma flow, enabling the arc to maintain sufficient penetration depth while possessing a suitable weld width coverage. A surface roughness of 0.4μm–1.6μm limits the geometric size of the axial longitudinal micro-protrusions; excessively large sizes can easily lead to overheating and melting at the tip, while excessively small sizes cannot form an electric field concentration effect. Controlling the tungsten electrode tail end to not protrude beyond the drive half-tooth eliminates the potential for mechanical interference and jamming of rotating components within the enclosed welding clamp cavity.
[0033] Preferably, the pipe clamp assembly includes a standard pipe clamp, a specially made thin pipe clamp, and a short elbow clamp, wherein the axial thickness of the specially made thin pipe clamp is less than that of the standard pipe clamp; when the straight section length of the pipe fitting is greater than a preset threshold, the standard pipe clamp with an inner diameter consistent with the outer diameter of the pipe fitting is used; when the straight section length of the pipe fitting is less than the preset threshold, the specially made thin pipe clamp is used; when the outer diameters of the two pipe fittings are inconsistent, pipe clamps corresponding to their respective pipe diameters are respectively assembled on both sides of the all-position automatic welding clamp; when the pipe fitting includes a short elbow, the standard pipe clamp is installed on the upper part of the all-position automatic welding clamp near the elbow, and the short elbow clamp with an arc-shaped notch is installed on the lower part.
[0034] By adopting the above technical solutions, a dynamic clamping system adapted to complex spatial pipe network topologies was constructed. By configuring specially designed thin-walled pipe clamps with reduced axial dimensions, the physical interference problem caused by insufficient assembly length in valve joints or short straight pipe areas was solved. For asymmetrical structures, the system uses reducing pipe clamps or short elbow clamps with arc-shaped notches to achieve precise clamping and centering of various non-standard geometric pipe fittings while ensuring the coaxiality of the pipe fittings and the clamping force, thus guaranteeing the consistency between the tungsten electrode rotation trajectory and the circumference of the weld seam.
[0035] Preferably, air plugs are used to seal both ends of the pipe fitting, and the expansion diameter of the air plugs ranges from 80% to 120% of the inner diameter of the pipe fitting; the cooling circuit is connected to a forced water cooler, and the internal cooling channel includes a water tank and a water-carrying cable, and the coolant flows sequentially through the forced water cooler, the water tank, the water-carrying cable, and the forced water cooler to form a circulation; the coolant is a mixture of deionized water and ethylene glycol, wherein the volume percentage of ethylene glycol is 20% to 50%.
[0036] By adopting the above technical solution, the expansion size of the air plug limits the sealing area inside the pipe fitting, and the introduced protective gas displaces residual air, preventing oxidation and discoloration of the weld back side at high temperatures. Deionized water in the coolant provides a high specific heat capacity as the basic heat transfer medium, removing free ions and preventing electrochemical corrosion within the cooling circuit. Adding 20%–50% by volume of ethylene glycol lowers the coolant's freezing point to meet the requirements of low-temperature construction environments, while also adjusting the fluid's kinematic viscosity and heat transfer coefficient. This avoids cavitation phenomena caused by pure water in small channels, maintaining stable flow and pressure output in the cooling system.
[0037] Preferably, the preset parameters input into the welding machine control system include: pipe material, pipe outer diameter, pipe wall thickness, welding clamp model, and shielding gas type.
[0038] By adopting the above technical solution, a systematic association is established between the physical properties of the pipe fittings and the equipment operating parameters. Based on the above input variables, the control system calls upon the built-in expert process database to calculate and output the optimal current pulse sequence and rotation speed that match the thermal characteristics and geometric dimensions of the material, thus eliminating parameter setting deviations in the manual trial-and-error process.
[0039] Preferably, when there is a difference in wall thickness between the two sections of the pipe fittings being joined, during the automatic welding process, the axis of the tungsten electrode tip is axially offset toward the pipe fitting with the thicker wall thickness, and the offset distance is set to 0.5mm to 1.5mm.
[0040] By adopting the above technical solution, the thermodynamic imbalance problem during the connection of thick-walled pipes with different wall thicknesses was solved.
[0041] If the heat source is arranged symmetrically, it will cause overheating and collapse on the thin-walled side while the thick-walled side fails to reach the solidus temperature. By offsetting the tungsten electrode by 0.5mm to 1.5mm, the landing point coordinates of the electric arc heat flow are adjusted, causing the high-density energy region to be biased towards the thick-walled side. The heat energy is conducted to the thin-walled region through the metal lattice, forcing the base materials on both sides to melt synchronously, eliminating the unfused interface at the junction, and ensuring the integrity of the metallurgical bond.
[0042] Preferably, when the joint of the pipe fitting is a fillet weld, the all-position automatic welding clamp has a rotary drive shaft inside, and an adapter is installed between the chuck and the rotary drive shaft so that the axis of the tungsten electrode forms an angle of 40° to 50° with the axis of the rotary drive shaft.
[0043] By adopting the above technical solution, the jet vector direction of the electric arc plasma flow is changed, taking into account the geometric characteristics of the inside angle formed by the intersection of the straight pipe and the short bend. The electric arc emitted by the conventional vertically set tungsten electrode is constrained by the geometric shielding of the outer wall of the bend, and the heat accumulates on the surface, preventing the apex of the joint root from melting through.
[0044] The assembly adapter forces the tungsten electrode to tilt, aligning the arc centerline directly with the deep gap of the joint along the bisector of the 40°–50° angle. The dynamic pressure of the plasma jet displaces the liquid metal on the surface, delivering the heat input focus to the bottom corner, achieving full-section deep melting penetration of the corner joint and cutting off potential high-pressure fluid leakage channels.
[0045] Preferably, the execution parameters for the automatic welding are set as follows: peak welding current of 20A to 150A; base current of 10A to 50A; pulse width duty cycle of 20% to 50%; pulse frequency of 1.0Hz to 5.0Hz; and rotational linear speed of the tungsten electrode of 50mm / min to 200mm / min.
[0046] By employing the above technical solution, the pulse current cycle creates a thermodynamic cycle of alternating heating and cooling in the molten pool region. During the peak current phase, high-density energy is output to break through the pipe wall and achieve full melting; during the base current phase, heat input is reduced, maintaining the arc while promoting solidification and crystallization of the liquid molten pool. The duty cycle and pulse frequency, combined with the set rotational linear velocity, control the overlap rate between adjacent melting points.
[0047] This parameter combination transforms continuous linear energy input into discontinuous point energy input, limiting the linear energy per unit length. From the system control level, it prevents the molten pool from collapsing due to gravity, ensuring that the weld surface is smooth and uniform at all positions and spatial angles.
[0048] In summary, the present invention has at least one of the following beneficial technical effects:
[0049] 1. This invention processes axial longitudinal grooves on the conical surface of the tungsten electrode tip and utilizes the cooling channel inside the all-position automatic welding gun in conjunction with an external water-cooling module to implement dual cooling. This allows electrons to be emitted directionally along the microscopic axial structure to concentrate arc energy, while simultaneously cutting off the axial conduction path of heat along the pipe wall. Therefore, it eliminates the arc drift phenomenon during the welding process, avoids grain coarsening in the heat-affected zone caused by excessive heat accumulation, and thus ensures the joint density and mechanical properties of small-diameter stainless steel pipe welds.
[0050] 2. This invention provides a pipe clamp assembly that includes a standard pipe clamp, a specially designed thin pipe clamp, and a short elbow clamp for different assembly scenarios. This allows the welding clamp system to adapt to the complex geometry of reducing joints or short pipes in confined spaces, solving the mechanical interference problem that easily occurs when assembling narrow pipe networks. Therefore, it can accurately maintain the coaxiality and clamping force of the assembled pipe fittings, ensuring that the circumferential rotation trajectory of the tungsten electrode coincides with the gap to be welded, and avoiding weld deviation and poor forming caused by misalignment.
[0051] 3. When dealing with thick-walled pipes with different wall thicknesses, this invention sets the tungsten electrode to be biased towards the thick-walled side. When dealing with fillet welds, it uses an adapter to make the tungsten electrode tilt at a specific angle and performs automatic welding in conjunction with preset pulse current parameters. This guides the arc heat flow to focus directly on the large heat capacity area or the deep root of the joint, while establishing a dynamic balance between the heating and solidification of the molten pool. Therefore, it overcomes the technical bottleneck of conventional processes that cannot completely penetrate complex asymmetrical joints, and prevents local collapse defects caused by gravity when the liquid metal is welded in all positions. Attached Figure Description
[0052] Figure 1 This is the overall process of the automatic welding method of the present invention. Detailed Implementation
[0053] The following is in conjunction with the appendix Figure 1 The present invention will be further described in detail below.
[0054] This invention provides an automatic welding method for small-diameter stainless steel pipes in all positions.
[0055] Preparation Example 1:
[0056] This preparation example provides a method for preparing a tungsten electrode with a specific cone angle and axial longitudinal striations, including the following steps:
[0057] A cerium-tungsten electrode with a diameter of 1.6 mm was selected. A tungsten electrode grinder equipped with a diamond grinding wheel with a grit size of 150 mesh was used. The axis of rotation of the grinding wheel was kept parallel to the axis of the cerium-tungsten electrode. The tip of the cerium-tungsten electrode was ground into a cone shape, and the cone angle was controlled to be 20°. A structure with axial longitudinal grooves was machined on the cone surface, and the surface roughness of the axial longitudinal grooves was controlled to be 0.4 μm.
[0058] Preparation Example 2:
[0059] This preparation example provides a method for preparing a tungsten electrode with a specific cone angle and axial longitudinal striations, including the following steps:
[0060] A cerium-tungsten electrode with a diameter of 2.4 mm was selected. A tungsten electrode grinder equipped with a diamond grinding wheel with a grit size of 180 mesh was used. The axis of rotation of the grinding wheel was kept parallel to the axis of the cerium-tungsten electrode. The tip of the cerium-tungsten electrode was ground into a cone shape, and the cone angle was controlled to be 25°. A structure with axial longitudinal grooves was machined on the cone surface, and the surface roughness of the axial longitudinal grooves was controlled to be 1.0 μm.
[0061] Preparation Example 3:
[0062] This preparation example provides a method for preparing a tungsten electrode with a specific cone angle and axial longitudinal striations, including the following steps:
[0063] A cerium-tungsten electrode with a diameter of 2.4 mm was selected. A tungsten electrode grinder equipped with a diamond grinding wheel with a grit size of 200 mesh was used. The axis of rotation of the grinding wheel was kept parallel to the axis of the cerium-tungsten electrode. The tip of the cerium-tungsten electrode was ground into a cone shape, and the cone angle was controlled to be 30°. A structure with axial longitudinal grooves was machined on the cone surface, and the surface roughness of the axial longitudinal grooves was controlled to be 1.6 μm.
[0064] Preparation Example 4:
[0065] This preparation example provides a method for preparing coolant for a cooling circuit, including the following steps:
[0066] Measure 20 parts by volume of ethylene glycol and 80 parts by volume of deionized water, mix the ethylene glycol and deionized water and stir evenly to obtain a coolant with a volume percentage of 20% ethylene glycol.
[0067] Preparation Example 5:
[0068] This preparation example provides a method for preparing coolant for a cooling circuit, including the following steps:
[0069] Measure 35 parts by volume of ethylene glycol and 65 parts by volume of deionized water, mix the ethylene glycol and deionized water and stir evenly to obtain a coolant with a volume percentage of 35% ethylene glycol.
[0070] Preparation Example 6:
[0071] This preparation example provides a method for preparing coolant for a cooling circuit, including the following steps:
[0072] Measure 50 parts by volume of ethylene glycol and 50 parts by volume of deionized water, mix the ethylene glycol and deionized water and stir evenly to obtain a coolant with a volume percentage of 50% ethylene glycol.
[0073] Example 1:
[0074] See attached document Figure 1 This embodiment provides an automatic welding method for small-diameter stainless steel pipes in all positions, including the following steps:
[0075] Two 316L stainless steel pipes with an outer diameter of 6.35 mm and a wall thickness of 0.5 mm were selected. The straight section lengths of both pipe fittings were greater than a preset threshold, which is the minimum assembly length required for the standard pipe clamp. In this embodiment, it is set to 30 mm. The actual straight section lengths of both pipe fittings were 50 mm.
[0076] When using a pipe cutter to cut the end face of a pipe fitting, the perpendicularity error between the rotation axis of the cutter head and the axis of the pipe fitting should be controlled to be 0.05°.
[0077] Use a scraper to deburr the inner and outer perimeter of the pipe opening on the end face, polish it with 400-grit wet sandpaper, and wipe the end face and the inner and outer perimeter of the pipe opening with a non-woven cloth soaked in acetone.
[0078] Two pipe sections are coaxially joined using a pipe fitting assembly, with the joint gap between the two sections controlled at 0.02mm and the radial misalignment at 5% of the pipe wall thickness. Spot welding is then performed along the circumferential direction of the joint, with two spot welds at a current of 15A and a single-point arc ignition time of 0.5s.
[0079] Using the tungsten electrode provided in Preparation Example 1, it is inserted into the chuck of an all-position automatic welding clamp, such that the tail end of the tungsten electrode does not protrude beyond the outer edge of the drive half-tooth of the all-position automatic welding clamp.
[0080] Select a standard pipe clamp with an inner diameter that matches the outer diameter of the pipe fitting, and place the spot-welded and positioned pipe fitting into the standard pipe clamp for clamping and securing.
[0081] Use gas plugs to seal both ends of the pipe and introduce high-purity argon gas into the pipe, controlling the expansion diameter of the gas plugs to be 80% of the inner diameter of the pipe.
[0082] The cooling circuit is started, and the coolant provided in Preparation Example 4 is used to make the coolant flow through the forced water cooler, the water tank inside the all-position automatic welding gun, the water cable and the forced water cooler in sequence to form a circulation. At the same time, the water cooling module is attached to the outer wall surface of the pipe for local cooling.
[0083] Input preset parameters (pipe material is 316L, pipe outer diameter is 6.35mm, pipe wall thickness is 0.5mm, welding clamp model and shielding gas type is high-purity argon) into the welding machine control system to generate the welding program.
[0084] Start the welding program to perform automatic welding. The execution parameters are set as follows:
[0085] The welding peak current is 20A, the base current is 10A, the pulse width duty cycle is 20%, the pulse frequency is 1.0Hz, and the tungsten electrode rotation speed is 50mm / min.
[0086] Example 2:
[0087] This embodiment provides an automatic all-position welding method for small-diameter stainless steel pipes, including the following steps:
[0088] Select a section of 316L stainless steel pipe with an outer diameter of 12.7mm and a wall thickness of 1.0mm and a section of 316L stainless steel pipe fitting with a wall thickness of 1.5mm. The straight section lengths of both pipe fittings are less than the preset threshold.
[0089] In this embodiment, a preset threshold of 30mm is set, and the actual straight segment length of the pipe is only 20mm due to space constraints. A pipe cutter is used to cut the end face, and the perpendicularity error between the cutter head rotation axis and the pipe axis is controlled to be 0.1°.
[0090] After deburring with a scraper, polish with a pneumatic stainless steel wire brush and wipe clean with a non-woven cloth soaked in anhydrous ethanol.
[0091] Two pipe sections are coaxially joined, with the joint gap controlled at 0.04 mm and the radial misalignment at 8% of the wall thickness of the thinner pipe section. Spot welding is performed along the circumference of the joint for positioning, with 3 spot welds, a spot welding current of 25 A, and a single spot arc ignition time of 1.0 s.
[0092] The tungsten electrode provided in Preparation Example 2 is inserted into the chuck of the all-position automatic welding clamp, with its tail end not protruding beyond the outer edge of the drive half-tooth.
[0093] A specially designed thin-walled pipe clamp is used to clamp and secure the spot-welded pipe fitting. Both ends of the pipe fitting are sealed with gas plugs, and high-purity argon gas is introduced; the expansion diameter of the gas plugs is 100% of the inner diameter of the pipe fitting.
[0094] The cooling circuit is activated, and the coolant provided in Preparation Example 5 is used to circulate inside the system. The water-cooled module is attached to the outer wall surface of the pipe for local cooling.
[0095] Input preset parameters to generate a welding program and start automatic welding.
[0096] Because there is a 0.5mm difference in wall thickness between the two pipe sections, during the automatic welding process, the axis of the tungsten electrode tip is axially offset towards the pipe section with the thicker wall, with the offset distance set to 1.0mm. The execution parameters are set as follows:
[0097] The welding peak current is 85A, the base current is 30A, the pulse width duty cycle is 35%, the pulse frequency is 3.0Hz, and the tungsten electrode rotation speed is 125mm / min.
[0098] Example 3:
[0099] This embodiment provides an automatic all-position welding method for small-diameter stainless steel pipes, including the following steps:
[0100] Select a pipe fitting with an outer diameter of 25.4 mm and a wall thickness of 4.0 mm, and a stepped reducer fitting with an outer diameter of 50.0 mm and an end face wall thickness of 4.0 mm. Use a pipe cutter to cut the end faces, with a perpendicularity error of 0.08°.
[0101] After deburring, sand with 600-grit wet sandpaper and wipe clean with a non-woven cloth soaked in acetone.
[0102] Two pipe sections are coaxially connected, with the joint gap controlled at 0.05mm and the radial misalignment at 10% of the pipe wall thickness. Spot welding is performed along the circumference of the joint for positioning, with 4 spot welds, a spot welding current of 35A, and a single spot arc ignition time of 1.5s.
[0103] The tungsten electrode provided in Preparation Example 3 is inserted into the clamp, with the tail end not protruding. Since the outer diameters of the two pipe sections are different, pipe clamps corresponding to their respective pipe diameters are installed on both sides of the all-position automatic welding clamp to clamp and secure the pipe sections.
[0104] Both ends are sealed with gas plugs and high-purity argon gas is introduced. The expansion diameter of the gas plugs is 120% of the inner diameter of the pipe.
[0105] The cooling circuit is activated, and the coolant provided in Preparation Example 6 is used for internal circulation and local cooling of the externally attached water-cooled module.
[0106] Input preset parameters to generate a welding program and start automatic welding. The execution parameters are set as follows:
[0107] The welding peak current is 150A, the base current is 50A, the pulse width duty cycle is 50%, the pulse frequency is 5.0Hz, and the tungsten electrode rotation speed is 200mm / min.
[0108] Example 4:
[0109] This embodiment provides an automatic all-position welding method for small-diameter stainless steel pipes (welding of short elbows and fillet welds), including the following steps:
[0110] A straight pipe with an outer diameter of 12.7 mm and a short elbow fitting with an outer diameter of 12.7 mm were selected for fillet weld butt joint. The pretreatment, spot welding positioning, pneumatic sealing and double cooling steps were the same as in Example 2.
[0111] The tungsten electrode provided in Preparation Example 2 was used. When assembling the all-position automatic welding clamp, a standard pipe clamp was installed on the upper part of the all-position automatic welding clamp near the short elbow, and a short elbow clamp with an arc-shaped notch was installed on the lower part to clamp and secure the pipe fitting.
[0112] Since the joint is a fillet weld, an adapter is installed between the chuck inside the all-position automatic welding clamp and the rotary drive shaft, so that the axis of the tungsten electrode and the axis of the rotary drive shaft form a 45° angle.
[0113] Input preset parameters to generate a welding program and start automatic welding. The execution parameter settings are the same as in Example 2.
[0114] Comparative Example 1:
[0115] Compared with Example 1, the difference is that after cutting and smoothing the end face of the pipe fitting and deburring it, water sandpaper is not used for polishing, and non-woven cloth soaked in organic solvent is not used to wipe and clean the inner and outer perimeter of the pipe opening. Instead, the butt joint and spot welding are performed directly. All other aspects are the same.
[0116] Comparative Example 2:
[0117] Compared with Example 1, the difference is that when grinding the tip of the tungsten electrode, the grinding texture processed on the conical surface is a circumferential horizontal line; and after the tungsten electrode is installed in the chuck of the all-position automatic welding clamp, the tail end of the tungsten electrode protrudes beyond the outer edge of the drive half tooth, and the rest are the same.
[0118] Comparative Example 3:
[0119] Compared with Example 3, the difference is that when the cooling circuit is started, the coolant is only allowed to flow through the cooling channel inside the all-position automatic welding gun for internal circulation, and the water cooling module is not attached to the outer wall surface of the pipe for local cooling. All other aspects are the same.
[0120] Comparative Example 4:
[0121] Compared with Example 2, the difference is that during the automatic welding process, the tungsten electrode tip is aligned with the center of the joint, and the axis of the tungsten electrode tip is not axially offset towards the pipe with thicker wall. All other aspects are the same.
[0122] Comparative Example 5:
[0123] Compared with Example 4, the difference is that no adapter is installed between the chuck and the rotary drive shaft, and the axis of the tungsten electrode is welded at a 90° right angle to the axis of the rotary drive shaft. All other aspects are the same.
[0124] Test Example 1:
[0125] Arc ignition tests were conducted using the all-position automatic welding clamps assembled in Examples 1 to 4 and their corresponding preset programs. Continuous high-frequency arc ignition commands were set in the welding machine control system. Each example performed 100 automatic arc ignitions, and the number of times a stable arc was successfully established was recorded to calculate the arc ignition success rate.
[0126] During the stable pulse welding phase, a high-frequency data acquisition module is connected in parallel to the output of the welding machine. The sampling frequency is set to 1000Hz, and the arc voltage signal is continuously acquired within 60 seconds. The mean square error of the arc voltage during this time period is calculated to characterize the drift amplitude during the arc operation.
[0127] Samples of pipe fittings welded in Examples 1 to 4 were extracted, one end was sealed, and the pipe fittings were connected to the vacuum system of a helium mass spectrometer leak detector. The inside of the pipe fittings was evacuated until the background pressure was less than the set detection threshold. High-purity helium gas was sprayed into the weld area outside the pipe fittings, and the steady-state helium leakage rate displayed by the leak detector was recorded.
[0128] One end of the leak-tested pipe sample is sealed with a blind flange, and the other end is connected to a hydraulic burst test bench. Water is injected into the pipe and the air is purged. The pressure is slowly increased at a rate of 1.5 MPa / min until the pipe yields or the weld breaks. The highest critical burst pressure displayed on the instrument is recorded.
[0129] Table 1. Test data of electric arc physical properties and macroscopic physical properties of pipe fittings in Examples 1-4
[0130] Test Project Arc ignition success rate (%) Mean square deviation of arc voltage (V) Helium leakage rate (Pa·m³ / s) Burst pressure (MPa) Example 1 99 0.14 2.6×10 -9 35.2 Example 2 97 0.17 3.4×10 -9 38.7 Example 3 100 0.12 1.8×10 -9 82.4
[0131] in conclusion:
[0132] According to the data in Table 1, the arc ignition success rate of Examples 1 to 4 was maintained above 97%, and the arc voltage variance was controlled in the low range of 0.12V to 0.19V, indicating that the arc state during the welding process was in a highly stable state.
[0133] In this scheme, the axial longitudinal grooves processed on the conical surface of the tungsten electrode tip change the electron emission mechanism under the action of the electric field. The axial micro-texture, as the preferred channel for electron emission, increases the local current density at the tip and physically suppresses the phenomenon of arc spots wandering and scattering laterally on the conical surface. This allows the arc energy to be focused precisely and continuously towards the center of the joint, reducing the fluctuation amplitude of the voltage signal.
[0134] In terms of macroscopic physical properties, the helium leakage rate of the fittings in each embodiment reached 10%. -9 The leakage rate is orders of magnitude lower than the standard required for conventional industrial vacuum-grade pipelines, proving that the weld is densely formed in all positions and there are no penetrating micropores or lack of fusion defects. The burst pressure data reflects the mechanical bearing limit of the pipe fitting joint. Among them, the burst pressure of the thick pipe fitting in Example 3 reached 82.4 MPa, and the burst pressure of the other thin-walled pipe fittings was also greater than 35 MPa. The fracture points were all located in the base material area rather than the weld area during the test.
[0135] The pressure-bearing capacity demonstrates that the dual water-cooling mechanism employed in this solution, combined with the set pulse parameters, controls the heat input per unit length while ensuring complete root penetration. This prevents grain coarsening and embrittlement in the heat-affected zone due to overheating, resulting in the macroscopic strength and tensile yield strength of the welded joint area matching the strength of the base material. The above data collectively verify the feasibility of this invention in a closed-loop, all-position automated welding process for small-diameter stainless steel pipes.
[0136] Test Example 2:
[0137] From the sample batches of automatically welded samples in Example 1, Comparative Example 1, and Comparative Example 2, pipe fitting samples were randomly selected for X-ray non-destructive testing. Following the standard for radiographic testing of pipeline welds, the pipe fittings were fixed on a radiography stage, and the focal length and exposure time were controlled for radiographic imaging to obtain the weld film.
[0138] After rinsing, place the flaw detection film under a viewing lamp and mark a continuous 100mm evaluation zone on the weld image. Use a magnifying glass with a scale to observe the image within the evaluation zone, count the total number of black circular porosity defects, and measure the image size of the largest diameter porosity, recording it as the maximum porosity equivalent size.
[0139] Macroscopic geometric dimensions of the weld seams on the outer surface of the above-extracted samples were measured. Using a dial caliper with an accuracy of 0.02 mm, the weld width on the front side was measured every 30° along the circumference of the pipe fitting. The maximum and minimum weld width values in the entire circumference measurement data were recorded, and the difference between the two was calculated to quantify the degree of fluctuation in weld width.
[0140] Table 2. Comparison of macroscopic defects and weld width fluctuations in Example 1 and Comparative Examples 1 and 2
[0141] Test Project Number of pores per 100 mm Maximum equivalent pore size (mm) Maximum and minimum weld width difference on the front side (mm) Example 1 1 0.15 0.22 Comparative Example 1 14 1.52 0.58 Comparative Example 2 3 0.28 1.87
[0142] in conclusion:
[0143] According to the data in Table 2, Comparative Example 1 had 14 pores per 100 mm, with a maximum equivalent pore size of 1.52 mm, which is higher than the test value of Example 1. This indicates that the pipe surface, which had not undergone mechanical polishing and organic solvent degreasing, retained oil, moisture, and dense oxides generated during machining. Under the high temperature of the welding arc, impurities such as hydrocarbons on the pipe surface rapidly decomposed, releasing gases such as hydrogen and carbon monoxide.
[0144] In all-position automated welding, the molten pool is small and solidifies rapidly. Precipitated gases cannot completely escape the surface before the molten pool crystallizes, remaining trapped inside the weld metal and forming numerous macroscopic porosity defects. This result indicates that a deep pretreatment process based on wet sandpaper polishing and acetone wiping is a necessary step to control internal porosity sources.
[0145] The number of pores in Comparative Example 2 was relatively controllable, but the difference between its maximum and minimum weld width reached 1.87 mm, which was drastic compared to 0.22 mm in Example 1. The physical mechanism was that the circumferential transverse grooves processed on the electrode cone surface changed the microscopic electric field distribution at the tip. When electrons escaped from the cathode surface, they were blocked by the transverse mechanical grooves, causing the arc emission spot to jump irregularly laterally on the cone surface.
[0146] This physical drift of the electric arc along the circumference causes the heat distribution in the input pipe material to lose its asymmetry, resulting in irregular changes in local penetration depth and width. This directly leads to a formation defect in the macroscopic weld, with inconsistent widths. The axial longitudinal striation structure used in Example 1 provides a continuous axial channel for electron emission, fixes the position of the arc root, and maintains the stability of the thermodynamic state of the molten pool, thereby obtaining a weld with uniform width.
[0147] Test Example 3:
[0148] Pipe samples from Examples 3 and 3, after welding and natural cooling to room temperature, were placed under standard industrial lighting. The distance between the boundaries of the oxidized discoloration areas on both sides of the weld seam on the outer surface of the pipe was measured using vernier calipers. Four measurement points were evenly distributed along the circumference of the pipe to obtain the total width data, and the arithmetic mean of the four measurement points was calculated as the final recorded value of the total width of the macroscopic heat-affected zone.
[0149] The automatic welding clamp systems of Example 3 and Comparative Example 3 were connected to the test station, and a welding program for thick pipe fittings with a peak current of 150A and a duty cycle of 50% was loaded into the welding machine control panel. The equipment was turned on and set to continuous cycle operation mode to simulate continuous full-load construction operation.
[0150] Thermocouple sensors were attached to the housing and chuck transmission parts of the automatic welding clamp, and connected to a temperature recorder. The system test cycle was set to 60 minutes. During the test cycle, the number of times the system automatically cut off the arc and triggered the shutdown protection due to the monitored temperature reaching the set safety threshold was recorded.
[0151] After the system triggers an overheat shutdown, keeping the environmental conditions constant, record the time required from the moment the system shuts down and the current is cut off until the thermocouple feedback temperature drops to the lower limit of the safe temperature for restarting the arc. All waiting times within the test cycle are accumulated and counted as the total forced shutdown cooling waiting time.
[0152] Table 3. Data on the width of the heat-affected zone and continuous operation shutdown test in Example 3 and Comparative Example 3
[0153] Test Project Total width of the macroscopic heat-affected zone (mm) Number of times the machine is stopped due to continuous operation at full load (times / hour) Total waiting time for forced shutdown and cooling (min) Example 3 12.4 0 0 Comparative Example 3 31.7 3 43
[0154] in conclusion:
[0155] According to the data in Table 3, the measured total width of the macroscopic heat-affected zone in Comparative Example 3 was 31.7 mm, while the measured value in Example 3 was 12.4 mm. The heat input per unit time was high when performing 150 A peak current all-position welding on a 4.0 mm thick stainless steel pipe fitting.
[0156] Comparative Example 3 relies solely on the internal water-cooling channel of the welding clamp to dissipate some heat. A large amount of residual heat conducted from the weld pool to the outside diffuses axially along the stainless steel pipe wall towards both ends, causing the base material at a location far from the weld joint to heat up and exceed the surface oxidation critical point, forming a wide discoloration band.
[0157] Example 3 establishes an additional solid-liquid heat exchange contact surface on the base material by attaching a water-cooled module connected to the cooling circuit to the outer wall of the pipe fitting. The circulating coolant carries away the conductive heat outside the pipe fitting, interrupting the axial extension path of heat conduction, compressing the overall heated area of the pipe fitting to the area near the joint, and controlling the volume of the heat-affected zone.
[0158] In the full-load continuous operation test, Comparative Example 3 experienced three overheating shutdowns within one hour, with a cumulative forced cooling waiting time of 43 minutes. Example 3 did not trigger the shutdown protection mechanism. When the automatic welding clamp performs high-current pulse output for a long time in a closed pipeline space, the jacket, tungsten electrode, and conductive structural components absorb arc radiation heat and generate Joule heat.
[0159] In Comparative Example 3, the single internal cooling water tank is limited by the internal volume of the welding clamp shell, resulting in a fixed heat exchange area and a critical value for its maximum heat dissipation power per unit time. When the rate of heat generation exceeds the rate of heat loss from the water tank, heat accumulation occurs, triggering the sensor to shut down the system logic.
[0160] In Example 3, the external water-cooling module is connected in series with the cooling system, increasing the heat exchange area of the entire fluid circulation loop and the amount of coolant involved in the system. The internal and external water-cooling modules share the heat load in parallel, improving the overall heat dissipation power of the system and achieving a dynamic balance between the heat input to the system and the heat dissipated, ensuring that the automatic welding machine maintains continuous operation at the rated duty cycle under extreme parameter conditions.
[0161] Test Example 4:
[0162] Straight pipe sections containing welds were cut from the completed welding batches of Examples 2 and 4. Both ends of the pipe section specimens were fixed in the upper and lower clamps of a universal tensile testing machine. The testing machine was controlled to apply a tensile load along the axial direction of the pipe at a constant tensile speed until the specimen fractured. The peak breaking force output by the testing machine control system was recorded, and the tensile strength was calculated based on the original cross-sectional area of the thin-walled side of the pipe. The location of the fracture was observed to confirm whether the fracture occurred in the base metal region or the weld joint region.
[0163] Longitudinal cuts were made along the axial direction of the specimens reserved in Example 2 and Comparative Example 4 to prepare strip-shaped bending specimens with widths meeting the standard requirements. The specimens were placed on cylindrical supports of a bending test bench, and a downward pressure was applied to the center of the weld using a pressure head of specified diameter. Face bending tests were performed with the tension surface on the front of the pipe fitting, and back bending tests were performed with the tension surface on the back of the inner wall of the pipe fitting, applying pressure until the bending angle of the specimen reached 180°. The specimens were removed, and macroscopic cracks appearing on the tension surface were observed using a graduated magnifying glass. Crack dimensions exceeding the upper limit of the acceptable standard were recorded.
[0164] The short elbows and straight pipe angle joints welded together in Example 4 and Comparative Example 5 were connected to the hydraulic test bench circuit via threaded connectors. Blind flanges were used to seal the remaining end openings of the pipe fittings. Pure water was injected into the pipeline to purge any trapped air.
[0165] Start the pressure testing pump and gradually increase the water pressure inside the pipeline according to the set pressure gradient. Maintain a constant system pressure for 10 minutes after each pressure increase, and visually observe and record the critical gauge pressure values at which water seepage occurs on the surface of the fillet weld and at the joint root. If no leakage occurs even after visible expansion and deformation of the pipe body, record the ultimate burst pressure of the system at this point.
[0166] Table 4. Mechanical Properties and Hydraulic Bearing Test Data of Fillet Weld Joints with Different Wall Thicknesses
[0167] Test Project Tensile strength (MPa) Tensile fracture location Macroscopic crack characteristics of a bending tensile surface Critical pressure for water leakage / burst (MPa) Example 2 517.4 Tensile fracture of 1.0mm thick side base material No visible cracks were found on the face and back bending surfaces under tension. / Comparative Example 4 289.6 Cracking occurred at the interface between the weld and the 1.5mm thick side pipe fitting. The tension surface under backbend exhibits a main crack with a length of 5.7 mm. / Example 4 / / / 34.1 (The pipe body expanded and deformed, but no water pressure leakage occurred) Comparative Example 5 / / / 8.3 (Water droplet leakage and pressure relief at the root of fillet weld)
[0168] Note: " / " indicates "not applicable" or "this test was not performed".
[0169] in conclusion:
[0170] According to the data in Table 4, the tensile strength of Comparative Example 4 is 289.6 MPa. The specimen fractured at the interface between the weld and the 1.5 mm thick pipe under tensile conditions and produced a 5.7 mm macroscopic crack in the back bending test.
[0171] In Example 2, the tensile strength reached 517.4 MPa. The specimen fractured in the 1.0 mm thick base material region, and no cracks appeared on the bending test surface. In the butt joint configuration of stainless steel pipes with different wall thicknesses, the thicker-walled section has a larger cross-sectional area, resulting in a larger heat capacity, while the thinner-walled section has a smaller heat capacity.
[0172] In Comparative Example 4, during the welding process, the tungsten electrode was aligned with the exact center of the joint, and the arc heat was symmetrically distributed to both sides. When the metal on the thin-walled side absorbed heat and reached its melting point, turning into a liquid state, the heat absorbed by the metal on the thick-walled side was insufficient to break through the solidus line. As a result, after the molten pool cooled and solidified, an unfused interface remained at the joint surface of the thick tube. When tensile stress and bending deformation occurred, the external force caused stress concentration at this unfused boundary, which promoted the rapid propagation of microcracks inside the material into through-cracks and ultimately led to failure.
[0173] In Example 2, the tungsten electrode axis was offset by 1.0 mm towards the thick-walled tube side, adjusting the spatial coordinates of the heat source input. This concentrated the high-density arc energy onto the thick-walled tube region with a large heat capacity. The heat energy was conducted to the thin-walled tube region through the metal lattice, causing the base materials on both sides to melt and converge synchronously, establishing a stable metallurgical bonding interface, eliminating stress concentration defects, and improving the joint's load-bearing capacity.
[0174] In the fillet weld test, Comparative Example 5 showed root leakage under 8.3 MPa water pressure, while Example 4 showed plastic expansion deformation of the base material under 34.1 MPa pressure but no leakage. The straight pipe and the short elbow intersect to form a 90° inside angle.
[0175] In Comparative Example 5, the tungsten electrode axis is set at a right angle to the jacket rotation drive shaft. The direction of the arc plasma jet is directed towards the outer wall of the straight pipe. Due to the geometric obstruction of the outer wall of the elbow, the arc heat accumulates on the surface of the pipe fitting and cannot be conducted to the root apex deep within the corner joint. The metal at the bottom of the joint does not melt, forming a gap that runs through the inside and outside. Pressurized water seeps outward along the unfused gap.
[0176] In Example 4, the tungsten electrode is tilted at a 45° angle by using an adapter, ensuring that the center line of the electric arc emitted from the tungsten electrode is directly aligned with the deepest part of the joint gap along the angle bisector. The dynamic pressure of the plasma jet displaces the surface liquid metal, delivering the heat input focus to the bottom corner position, achieving full-section penetration and closure of the pipe wall metal. The dense crystalline structure seals the fluid leakage channels, meeting the high-pressure requirements of the pipeline.
Claims
1. A method for automatic welding of small-diameter stainless steel pipes in all positions, characterized in that, Includes the following steps: The end face of the pipe is cut and smoothed, the inner and outer peripheries of the pipe opening are deburred and polished, and the end face and the inner and outer peripheries of the pipe opening are wiped clean with organic solvent. The two sections of the pipe fittings are coaxially connected and spot-welded for positioning along the circumferential direction of the joint; The tip of the tungsten electrode is ground into a cone shape and axial longitudinal grooves are machined on the cone surface. The tungsten electrode is then inserted into the chuck of an all-position automatic welding clamp. The pipe fitting, after being spot-welded and positioned, is placed in the pipe clamp assembly for clamping and securing. Seal both ends of the pipe fitting and introduce protective gas into the pipe fitting; The cooling circuit is activated, allowing the coolant to circulate through the cooling channel inside the all-position automatic welding gun, while the water-cooling module is attached to the outer wall surface of the pipe for localized cooling. Input preset parameters into the welding machine control system to generate a welding program, and start the welding program to drive the tungsten electrode to rotate around the circumference of the pipe to perform automatic welding.
2. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, The end face of the pipe fitting is cut and smoothed, specifically as follows: The end face is cut using a pipe cutting machine, and the perpendicularity error between the rotation axis of the cutter head and the axis of the pipe is controlled to be less than or equal to 0.1°. The polishing is done using wet sandpaper or a pneumatic stainless steel wire brush. The wiping and cleaning process uses a non-woven fabric soaked in the organic solvent, which is acetone or anhydrous ethanol.
3. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, When two pipe sections are coaxially connected, the gap between the two pipe sections is less than or equal to 0.05 mm, and the radial misalignment is less than or equal to 10% of the pipe wall thickness. The number of spot welding positions along the circumference of the joint is 2 to 4, and the arc ignition time for each spot is 0.5s to 1.5s.
4. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, The tungsten electrode is a cerium-tungsten electrode, the cone angle of the cone is 20° to 30°, and the surface roughness of the axial longitudinal groove is 0.4 μm to 1.6 μm; The all-position automatic welding clamp has a drive half-tooth. After being inserted into the chuck of the all-position automatic welding clamp, the tail end of the tungsten electrode does not protrude beyond the outer edge of the drive half-tooth.
5. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, The pipe clamp assembly includes a standard pipe clamp, a specially made thin pipe clamp, and a short elbow clamp, wherein the axial thickness of the specially made thin pipe clamp is smaller than that of the standard pipe clamp. When the length of the straight section of the pipe fitting is greater than a preset threshold, a standard pipe clamp with an inner hole size that is consistent with the outer diameter of the pipe fitting is used. When the length of the straight section of the pipe fitting is less than a preset threshold, the specially made thin pipe clamp is used; When the outer diameters of the two pipe sections are inconsistent, pipe clamps corresponding to their respective pipe diameters are installed on both sides of the all-position automatic welding clamp. When the pipe fitting includes a short elbow, the standard pipe clamp is installed on the upper part of the all-position automatic welding clamp near the elbow, and the short elbow clamp with an arc-shaped notch is installed on the lower part.
6. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, The two ends of the pipe are sealed with air plugs, and the expansion diameter of the air plugs is 80% to 120% of the inner diameter of the pipe. The cooling circuit is connected to a forced water cooler, and the internal cooling channel includes a water tank and a water-carrying cable. The coolant flows sequentially through the forced water cooler, the water tank, the water-carrying cable, and the forced water cooler to form a circulation. The coolant is a mixture of deionized water and ethylene glycol, wherein the volume percentage of ethylene glycol is 20% to 50%.
7. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, The preset parameters input into the welding machine control system include: Pipe material, outer diameter, wall thickness, welding clamp type, and shielding gas type.
8. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, When there is a difference in wall thickness between the two pipe sections being connected, during the automatic welding process, the axis of the tungsten electrode tip is axially offset toward the pipe section with the thicker wall, and the offset distance is set to 0.5mm to 1.5mm.
9. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, When the joint of the pipe fitting is a fillet weld, the all-position automatic welding clamp has a rotary drive shaft inside. An adapter is installed between the chuck and the rotary drive shaft so that the axis of the tungsten electrode forms an angle of 40° to 50° with the axis of the rotary drive shaft.
10. The method for automatic welding of small-diameter stainless steel pipes in all positions according to claim 1, characterized in that, The execution parameters for the automatic welding are set as follows: The peak welding current is 20A to 150A; the base current is 10A to 50A. The pulse width duty cycle is 20% to 50%; the pulse frequency is 1.0 Hz to 5.0 Hz; and the linear speed of the tungsten electrode rotation is 50 mm / min to 200 mm / min.