High-efficiency surface strengthening method and special friction strip for grooved parts
By combining customized friction strips and linear friction welding equipment, the accessibility and uniformity of surface strengthening of irregular grooved parts were solved, achieving efficient and uniform surface strengthening effect, and improving surface quality and production efficiency.
Patent Information
- Application Number
- CN202611277991.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for surface strengthening of grooved parts suffer from problems such as poor tool accessibility, uneven modified layer, difficulty in controlling surface roughness, and low strengthening efficiency, especially for irregularly shaped grooves.
Customized friction strips are used, designed according to the shape of the groove. A strengthening layer is formed on the surface of the groove by combining vibration and upsetting force through linear friction welding equipment. The frictional heat and mechanical force are used to achieve uniform strengthening of the entire cross section, dynamic recrystallization and grain refinement, and avoid metallurgical bonding.
It achieves uniform reinforcement of the entire cross section of irregular grooves, improves surface hardness, wear resistance and fatigue resistance, reduces surface roughness and improves production efficiency, and is particularly suitable for difficult-to-machine materials such as titanium alloys.
Smart Images

Figure CN123103154A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of surface modification technology for metal parts, and more specifically, to a method for efficient surface strengthening of grooved parts and a special friction strip. Background Technology
[0002] In the fields of aerospace, automotive manufacturing, and precision machinery, many critical load-bearing components contain complex groove structures, such as tenons, oil grooves, and guide rail grooves. These groove surfaces typically serve as mating surfaces or friction pairs, and have extremely high requirements for wear resistance, fatigue resistance, and surface roughness.
[0003] Traditional methods for strengthening the surface of trenches mainly include shot peening, surface rolling, laser hardening, micro-arc oxidation, and physical vapor deposition (PVD) coatings. However, these methods have the following limitations: 1. Poor accessibility: For deep and narrow grooves or grooves with specific cross-sections (such as trapezoidal or semi-circular), the shot peening projectiles or rolling rollers have difficulty reaching the root of the groove, resulting in a reinforcement blind zone.
[0004] 2. Shallow modified layer: The modified layer obtained by laser quenching and coating technology is usually thin, which is prone to peeling under heavy load or impact conditions.
[0005] 3. Deterioration of surface quality: Although shot peening and rolling processes can improve surface hardness, they often damage the original texture of the machined surface, increase surface roughness, and even introduce microcracks, which in turn affect the fitting accuracy.
[0006] 4. Limitations of Friction Stir Processing: Although friction stir processing (FSP) can achieve excellent grain refinement, its tool probe is usually cylindrical, which is mainly suitable for flat surfaces or curved surfaces with small curvature. It cannot adapt to the contouring of irregular grooves, and the probe is prone to interference in narrow spaces. Summary of the Invention
[0007] (a) Technical problems to be solved The technical problem to be solved by the present invention is: the technical problems of poor tool accessibility, uneven modified layer, difficulty in controlling surface roughness and low strengthening efficiency in the surface strengthening of grooved parts in the prior art. The present invention provides a method for high-efficiency surface strengthening of grooved parts that can adapt to irregular groove contours, achieve uniform strengthening of the whole cross section and improve surface quality.
[0008] (II) Technical Solution To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a method for efficient surface strengthening of grooved structure parts, comprising the following steps: S1. According to the groove cross-sectional shape of the part to be reinforced, a friction strip is processed and prepared; the friction end shape of the friction strip matches the groove shape. S2. The clamping end of the friction bar is rigidly clamped to the vibration side of the linear friction welding equipment; the part to be reinforced in the groove is fixed to the upsetting side of the linear friction welding equipment, so that the friction end of the friction bar is aligned with the groove. S3. Start the equipment and control the vibration side to drive the friction strip to reciprocate along the set direction at a preset frequency and amplitude; at the same time, control the upsetting side to apply upsetting force to the vibration side, so that the friction strip contacts the groove surface and generates relative motion, and a reinforcing layer is formed on the groove surface by means of frictional heat and mechanical force.
[0009] In the above technical solution, the shape of the friction end matches the shape of the groove, allowing the friction strip to fully adhere to the groove surface, including areas inaccessible by traditional tools such as the bottom corners of trapezoidal grooves and the arc bottoms of semi-circular grooves, achieving uniform strengthening of the entire cross-section of the groove. Reciprocating vibration generates frictional heat, bringing the surface metal of the groove to a thermoplastic state; simultaneously, the upsetting force provides mechanical force, causing intense plastic deformation of the surface metal. Under the combined effect of thermo-mechanical forces, the surface metal of the groove undergoes dynamic recrystallization and grain refinement, thus forming a strengthening layer in situ without the need for additional materials or subsequent heat treatment. During the reciprocating vibration process, the friction strip can complete full-surface strengthening along the length of the groove in one pass, eliminating the need for point-by-point impact like shot peening or multiple passes like friction stir processing, significantly improving production efficiency.
[0010] Preferably, in step S1, the material hardness of the friction strip is higher than that of the material hardness of the groove part to be strengthened; and at the friction welding process temperature, metallurgical bonding is not easily formed between the friction strip material and the material of the groove part to be strengthened.
[0011] In the above technical solution, the friction strip material and the workpiece material are not easily metallurgically bonded, meaning that they will not weld together under frictional heat. This is a key prerequisite for achieving "surface treatment" rather than "welding," ensuring the repeatability and stability of the process. The friction strip is harder than the workpiece material, and during the treatment process, it can act as an "ironing" agent on the groove surface. As a relatively hard "mold," the friction strip flattens the microscopic protrusions on the groove surface under heat, reducing surface roughness and improving the sealing and lubrication performance of the mating surfaces. This contrasts sharply with shot peening, which leads to a deterioration in surface roughness (Ra increases from 0.4 μm to 3~6 μm).
[0012] Preferably, the material of the grooved part to be reinforced is titanium alloy, and the material of the friction strip is selected from high-strength steel or high-temperature alloy.
[0013] In the aforementioned technical solutions, titanium alloys are typical difficult-to-machine materials due to their low thermal conductivity and severe work hardening. High-strength steel or high-temperature alloys have much higher hardness than titanium alloys and low miscibility with titanium alloys at friction welding temperatures, making them ideal material choices for friction strips. This material combination breaks through the bottleneck of traditional heat treatment for complex irregular-shaped titanium alloy parts, providing a new surface strengthening solution for grooved titanium alloy parts widely used in the aerospace field.
[0014] Preferably, in step S3, the groove includes a long, straight trapezoidal groove or a semi-circular groove. This effectively strengthens materials that are difficult to process.
[0015] In the above technical solution, the long, straight trapezoidal groove and the semi-circular groove represent two typical irregular groove cross-sections. The trapezoidal groove has sharp bottom corners, and the semi-circular groove has a continuous arc-shaped bottom surface. These two cross-sections are precisely the typical shapes that traditional processes such as shot peening, rolling, and friction stir processing are difficult to handle. This method can handle these two types of grooves, proving its universality for irregular grooves. In the prior art, no method can simultaneously achieve uniform reinforcement of the entire cross-section of these two types of irregular grooves; this invention fills this technological gap.
[0016] Preferably, in step S3, during the linear friction treatment, the surface of the groove undergoes dynamic recrystallization under frictional heat, resulting in grain refinement and a reduction in surface micro-unevenness. Grain refinement leads to an improvement in overall mechanical properties. In the above technical solution, dynamic recrystallization significantly refines the grains on the surface of the trench, producing a fine-grain strengthening effect, which greatly improves surface hardness, wear resistance, and fatigue resistance. The "reduction of surface micro-unevenness" indicates that this method improves surface quality while strengthening, which is fundamentally different from processes such as shot peening and rolling that "sacrifice surface roughness for increased hardness," and is one of the core advantages of this method.
[0017] Preferably, in step S3, the friction strip completes full surface reinforcement along the length of the groove in one go during the reciprocating vibration process.
[0018] In the above technical solution, one-time completion means that there is no need for segmented processing or multiple repetitions. For long grooves (such as a trapezoidal groove with a length of 200mm), full surface strengthening can be completed in a few seconds to tens of seconds. The production efficiency is much higher than shot peening (which requires point-by-point coverage) and friction stirring (which requires multiple overlapping passes). One-time continuous processing avoids the overlapping or transition areas that may be generated by segmented processing, ensuring the uniformity and consistency of the strengthened layer along the length of the groove.
[0019] Secondly, the present invention also provides a special friction strip for implementing the method, comprising a clamping end and a friction end; the friction end has a geometric profile adapted to the cross-sectional shape of the groove in the part to be reinforced, for fitting the surface of the groove; the clamping end is used to connect to the vibration side clamp of a linear friction welding equipment.
[0020] Preferably, the surface roughness Ra of the friction end is ≤1.6μm.
[0021] (III) Beneficial Effects The above-described technical solution of the present invention has at least the following advantages: 1. This invention uses a custom-designed friction strip whose contour can perfectly fit the groove cross-section, solving the problem that traditional tools cannot reach the root of the groove (such as the bottom corner of a trapezoidal groove or the arc bottom of a semi-circular groove), achieving uniform reinforcement of the entire cross-section of the groove, and completely eliminating reinforcement blind spots.
[0022] 2. This invention utilizes the high-temperature thermoplastic effect generated by linear friction to induce dynamic recrystallization of the surface metal of the groove, significantly refining the grains (referring to the microstructure of a titanium alloy linear friction welded joint, the grains in the dynamic recrystallization zone can be refined to the order of 4~6 μm), eliminating casting or machining defects, and greatly improving surface hardness, wear resistance and fatigue resistance.
[0023] 3. Unlike traditional shot peening or rolling, this invention strengthens the surface while reducing microscopic unevenness due to the friction strip's higher hardness and surface roughness Ra ≤ 1.6 μm under the effect of frictional-thermal coupling. This helps improve the sealing and lubrication performance of the mating surfaces and avoids the roughness deterioration problem caused by shot peening.
[0024] 4. The friction strips are made of materials that do not easily form metallurgical bonds with the workpiece, which avoids the adhesion between the tool and the workpiece and ensures the stability of the process; and can complete the continuous processing of long grooves in one go, with high production efficiency and suitable for mass production.
[0025] 5. This invention is particularly suitable for groove strengthening of difficult-to-machine materials such as titanium alloys, breaking through the bottleneck of traditional heat treatment in handling complex irregular parts; the friction strip profile can be customized as needed, and can adapt to various groove cross-sectional shapes such as long straight trapezoidal grooves and semi-circular grooves. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0027] Figure 1 This is a schematic diagram of the structure of the grooved part to be strengthened according to Embodiment 1 of the present invention.
[0028] Figure 2 This is a schematic diagram of the friction strip provided in Embodiment 1 of the present invention.
[0029] Figure 3 This is a schematic diagram of the structure of the grooved part to be reinforced provided in Embodiment 2 of the present invention.
[0030] Figure 4 This is a schematic diagram of the friction strip provided in Embodiment 2 of the present invention.
[0031] Figure 5 This is one of the implementation structural diagrams of the efficient surface strengthening method for grooved parts provided in Embodiment 2 of the present invention.
[0032] Figure 6 This is the second implementation structural diagram of the efficient surface strengthening method for grooved parts provided in Embodiment 2 of the present invention.
[0033] The labels for the attached figures are as follows: 1. Trapezoidal groove part to be strengthened; 2. Trapezoidal friction strip; 3. Semicircular groove part to be strengthened; 4. Semicircular friction strip; 11. Trapezoidal groove; 21. Semicircular groove; 31. First clamping end; 32. First friction end; 41. Second clamping end; 42. Second friction end. Detailed Implementation
[0034] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.
[0035] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention, and do not indicate that the device or element must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the present invention.
[0036] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating relative importance or the number of technical features. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified. The specific implementation of this invention will be described in more detail below with reference to specific embodiments: Example 1: Surface strengthening of titanium alloy parts with long, straight trapezoidal grooves 1. Parameters of parts and friction strips The part to be strengthened is a long, straight trapezoidal groove part 1 made of titanium alloy (TC4, Ti-6Al-4V). The groove is 200mm long, and the trapezoidal cross-section has an upper base of 8mm, a lower base of 4mm, and a depth of 6mm.
[0037] Custom-made trapezoidal friction strips 2 according to the cross-sectional shape of the groove to be reinforced: The cross-sectional profile of the first friction end 32 is completely consistent with the trapezoidal groove 11, and the surface roughness Ra≤1.6μm; The first clamping end 31 has a rectangular cross section and is used for rigid connection with the vibration side clamp of the linear friction welding equipment. The friction strip material is made of high-strength steel (such as 300M steel), which has a higher hardness than TC4 titanium alloy and is less likely to undergo metallurgical bonding with TC4 at the friction welding process temperature.
[0038] 2. Clamping The first clamping end 31 of the trapezoidal friction bar is installed into the vibration side of the linear friction welding equipment and rigidly clamped; the trapezoidal groove part 1 to be strengthened is installed on the forging side of the equipment, and the position is adjusted so that the first friction end 32 of the friction bar is aligned with the trapezoidal groove 11.
[0039] 3. Linear friction treatment Start the equipment and set the process parameters: Vibration frequency: 13.6~43Hz (preferably 30Hz); amplitude: 1.5~3mm (preferably 2mm); friction pressure f: 20~80MPa (preferably 60MPa); upsetting pressure P: 60~160MPa (preferably 80MPa); friction time: 1.5~20s (preferably 5s).
[0040] Parameter selection principles: Friction pressure and reciprocating frequency are the main influencing factors of heat input. Increased frequency and / or pressure significantly increase welding heat input; however, excessive pressure will affect the stability of the specimen's reciprocating motion and also increase the outflow of ductile metal, so excessively high pressure values should be avoided. Specific parameters need to be comprehensively set based on the groove size, part material, and friction strip material to ensure that the friction strip completes full surface strengthening along the groove length in one continuous reciprocating vibration process.
[0041] 4. Processing Results Under the action of frictional heat and mechanical force, dynamic recrystallization occurs on the surface of trapezoidal groove 11, the grains are refined to the order of 4~6μm, the micro-unevenness of the surface is significantly reduced, a uniform thickness and fine grain reinforcement layer are formed in situ on the surface of the groove, and there is no reinforcement blind zone at the root of the groove.
[0042] Example 2: Surface strengthening of titanium alloy parts with semi-circular grooves 1. Parameters of parts and friction strips The part to be strengthened is a semi-circular groove part 3 made of titanium alloy (TC17), with a groove length of 150mm and a semi-circular cross-sectional radius of 5mm.
[0043] Custom-made semi-circular friction strip 4: The cross-section of the second friction end 42 is semi-circular, which is completely in contact with the arc surface of the semi-circular groove 21, and the surface roughness Ra≤1.6μm; The contour of the second friction end 42 of the semi-circular friction strip 4 is strictly matched with the cross-sectional shape of the semi-circular groove 21 to ensure that: The second friction end 42 is fully in contact with the surface of the semi-circular groove 21 to ensure uniform transfer of frictional heat and mechanical force. Uniform reinforcement can also be achieved in areas inaccessible to conventional tools, such as the root and rounded corners of the semi-circular groove 21; The outline of the semi-circular friction strip 4 has a certain "contour ironing" effect on the surface of the semi-circular groove 21, reducing surface roughness.
[0044] The design of the second clamping end 41 must meet the interface requirements of the vibration side clamp of the linear friction welding equipment to ensure rigid clamping and avoid loosening or phase shift under high-frequency reciprocating vibration.
[0045] The material of the semi-circular friction strip 4 is a high-temperature alloy (such as GH4169), which has a higher hardness than TC17 titanium alloy and is not easily metallurgically bonded with TC17 at the friction welding process temperature.
[0046] 2. Clamping and processing The clamping method is the same as in Embodiment 1. The second clamping end 41 of the semi-circular friction strip 4 is rigidly clamped to the vibration side of the equipment, and the semi-circular groove part 3 is fixed to the upsetting side. Friction pressure F is applied to the semi-circular friction strip 4.
[0047] Start the equipment and control the vibration side to drive the semi-circular friction strip 4 to reciprocate along the set direction at a preset frequency and amplitude f. At the same time, the upsetting side applies upsetting pressure P, so that the second friction end 42 contacts the arc surface of the semi-circular groove 21 and generates relative motion.
[0048] 3. Processing Results During the reciprocating vibration process, the semi-circular friction strip 4 completes the full surface strengthening of the 150mm long semi-circular groove in one go. A uniform dynamic recrystallization and grain refinement strengthening layer is formed at the bottom of the groove and the rounded corners on both sides, and the surface roughness is significantly reduced compared with that before treatment.
[0049] Those skilled in the art should understand that the specific process parameters in the above embodiments are merely preferred examples, and can be adjusted in actual production based on the following factors: The key principle is that frictional pressure and reciprocating motion frequency are the main influencing factors of heat input. Under the premise of ensuring stable vibration and not producing excessive flash, heat input should be controlled by adjusting the frequency and amplitude to induce full dynamic recrystallization of the trench surface.
[0050] Compared with the prior art, the technical effects of the present invention can be reflected in the following dimensions: 1. Under the action of thermo-mechanical coupling, the surface metal of the trench undergoes dynamic recrystallization, and the grains are refined to the micron level, forming a fine grain strengthening effect; at the same time, the "ironing" effect of the friction strip significantly reduces the surface roughness, and the surface integrity is better than that of shot peening and rolling processes.
[0051] 2. The friction strip completes full surface strengthening along the length of the groove in one pass, eliminating the need for point-by-point impact like shot peening or multiple passes like friction stir processing, thus significantly improving production efficiency.
[0052] 3. By replacing friction strips with different contours, it can be adapted to various groove cross sections such as trapezoidal grooves and semi-circular grooves, breaking through the geometric adaptability limitations of traditional processes.
[0053] 4. It is particularly suitable for difficult-to-machine materials such as titanium alloys. High-strength steel or high-temperature alloys are selected as friction strip materials, which not only ensures the wear resistance of the friction strip itself, but also avoids metallurgical bonding with titanium alloy workpieces. It has a wide process window and good stability.
[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for efficient surface strengthening of grooved parts, characterized in that, Includes the following steps: S1. According to the groove cross-sectional shape of the part to be reinforced, a friction strip is processed and prepared; the friction end shape of the friction strip matches the groove shape. S2. The clamping end of the friction bar is rigidly clamped to the vibration side of the linear friction welding equipment; the part to be reinforced in the groove is fixed to the upsetting side of the linear friction welding equipment, so that the friction end of the friction bar is aligned with the groove. S3. Start the equipment and control the vibration side to drive the friction strip to reciprocate along the set direction at a preset frequency and amplitude; at the same time, control the upsetting side to apply upsetting force to the vibration side, so that the friction strip contacts the groove surface and generates relative motion, and a reinforcing layer is formed on the groove surface by means of frictional heat and mechanical force.
2. The method for high-efficiency surface strengthening of grooved structure parts as described in claim 1, characterized in that, In step S1, the material hardness of the friction strip is higher than that of the material hardness of the groove part to be strengthened; and at the friction welding process temperature, metallurgical bonding is not easily formed between the friction strip material and the material of the groove part to be strengthened.
3. The method for high-efficiency surface strengthening of grooved structure parts as described in claim 2, characterized in that, The material of the grooved part to be strengthened is titanium alloy, and the material of the friction strip is selected from high-strength steel or high-temperature alloy.
4. The method for high-efficiency surface strengthening of grooved structure parts as described in claim 1, characterized in that, In step S3, the groove includes a long straight trapezoidal groove or a semi-circular groove.
5. The method for high-efficiency surface strengthening of grooved structure parts as described in claim 1, characterized in that, In step S3, during the linear friction treatment, the surface of the groove undergoes dynamic recrystallization under the action of frictional heat, resulting in grain refinement and a reduction in surface micro-unevenness.
6. The method for high-efficiency surface strengthening of grooved structure parts as described in claim 1, characterized in that, In step S3, the friction strip completes full surface reinforcement along the length of the groove in one go during the reciprocating vibration process.
7. A dedicated friction strip for implementing the method according to any one of claims 1 to 6, characterized in that, It includes a clamping end and a friction end; the friction end has a geometric profile adapted to the cross-sectional shape of the groove in the part to be reinforced, for fitting the surface of the groove; the clamping end is used to connect to the vibration side clamp of the linear friction welding equipment.
8. The special friction strip according to claim 7, characterized in that, The surface roughness Ra of the friction end is ≤1.6μm.