A turbocharger welding device and its manufacturing process

By improving the turbocharger welding equipment and process, and utilizing the combined structure of cylinder, clamping block and top block, the problem of fixing irregular parts was solved, and efficient welding quality and joint performance were improved.

CN123103155APending Publication Date: 2026-11-17HARBIN WELDING INST LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611480943.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional inertial friction welding devices cannot properly fix irregularly shaped parts of turbochargers, resulting in insufficient upsetting force, which affects the performance and forming of the welded joint, and the manufacturing process is difficult to control.

Method used

The system employs a combination structure of cylinder, tailstock, first clamping block, second clamping block, and standard workpiece. Combined with the groove design of the top block and the coaxiality control of the spindle box, it achieves precise clamping and multi-point fixation of irregularly shaped workpieces, ensuring axis alignment and uniform heat input during the welding process.

Benefits of technology

It improves the welding quality of irregularly shaped workpieces, reduces the unevenness of weld flash, enhances the performance, tensile strength, and low-cycle fatigue performance of the joint, and achieves reliable solid-state bonding of complex structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103155A_ABST
    Figure CN123103155A_ABST
Patent Text Reader

Abstract

This invention proposes a turbocharger welding device and its manufacturing process, belonging to the field of inertial friction welding technology. It solves the problem that traditional inertial friction welding devices cannot effectively fix irregularly shaped parts such as turbine discs, resulting in insufficient upsetting force and consequently affecting the performance or weak formation of the welded joint. It includes a cylinder, a tailstock, a first clamping block, an irregularly shaped workpiece, a second clamping block, and a standard workpiece. The cylinder is installed inside the tailstock, and its telescopic end is connected to the second clamping block. The first clamping block is installed at the end of the tailstock, and the irregularly shaped workpiece is installed between the first and second clamping blocks. The end of the standard workpiece passes through the second clamping block and is welded to the irregularly shaped workpiece. It is mainly used for inertial friction welding of irregularly shaped parts such as turbochargers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inertial friction welding technology, and in particular relates to a turbocharger welding device and its manufacturing process. Background Technology

[0002] Inertial friction welding is a solid-state joining method. Most of the energy is converted into heat energy at the friction interface and then carried out of the interface by the high-temperature thermoplastic metal in the form of flash. The heat input at the joint interface is relatively small. The joint has a forged structure, stable and reliable joint performance, wide material adaptability, and simple welding process with a high degree of automation. Therefore, for welding cylindrical shaft structures, inertial friction welding technology can more efficiently obtain excellent joints.

[0003] However, due to the complexity of turbocharger blade structure, traditional inertial friction welding devices cannot effectively fix irregularly shaped parts such as turbine disks, resulting in insufficient upsetting force and thus affecting the performance of the welded joint or its weak formation. At the same time, due to the special nature of the material, its manufacturing process is also difficult to control. Therefore, this invention proposes a turbocharger welding device and its manufacturing process. Summary of the Invention

[0004] In view of this, the present invention aims to provide a turbocharger welding device and its manufacturing process to solve the problem that traditional inertial friction welding devices cannot properly fix irregular parts such as turbine discs, resulting in insufficient upsetting force and thus affecting the performance of the welded joint or its weak formation.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: A turbocharger welding apparatus includes a cylinder, a tailstock, a first clamping block, a shaped workpiece, a second clamping block, and a standard workpiece. The cylinder is installed inside the tailstock, and the telescopic end of the cylinder is connected to the second clamping block. The first clamping block is installed at the end of the tailstock. The shaped workpiece is installed between the first clamping block and the second clamping block. The end of the standard workpiece passes through the second clamping block and is welded to the shaped workpiece.

[0006] Furthermore, a top block is provided in the middle of the first clamping block, and the top block contacts the irregularly shaped workpiece.

[0007] Furthermore, a groove is provided on the end face of the top block, and the unwelded end of the top block is engaged in the groove.

[0008] Furthermore, it also includes a spindle box and a clamping mechanism, wherein the standard workpiece is installed in the clamping mechanism, and the clamping mechanism is installed on the spindle box.

[0009] Furthermore, the coaxiality error between the spindle box and the tailstock is ≤0.05mm.

[0010] Furthermore, the clamping mechanism is hydraulically driven or pneumatically driven.

[0011] Furthermore, a through hole is provided at the center of the second clamping block.

[0012] A manufacturing process for a turbocharger welding device employs inertial friction welding, and the welding formula is as follows: (1) The upsetting pressure is F=πD 2 / 4×P, where P represents the welding pressure of the turbocharger welding contact surface, and D represents the outer diameter of the contact surface shaft; (2) Moment of inertia I = M × R 2 Where M is the weight of the inertial disk and R is the radius of the inertial disk; (3) The total energy input for inertial friction welding is E=Q×S, where Q is the energy required per unit area and S is the area of ​​the welding contact surface; (4) The welding rotation speed n is calculated from the total energy obtained in (3) as follows: E=I×ω 2 / 2, where ω is the initial angular velocity of the inertial disk.

[0013] Furthermore, the pressure P required for inertial friction welding of the turbocharger is 300 MPa, the energy Q required per unit area during welding is 470 J, and the welding upsetting force F used in the inertial friction welding process is 33 t, with a rotational inertia I of 280 kg·m. 2 The total energy E is 516465.414 J, and the initial rotational speed is 580 r / min.

[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention achieves precise clamping and multi-point fixation of asymmetrical structures of irregular workpieces through the synergistic action of the first clamping block and the second clamping block, combined with the groove design on the end face of the top block. This effectively avoids the displacement or vibration of irregular workpieces caused by uneven force during welding. The groove structure of the top block can disperse the welding upsetting pressure and reduce the local plastic deformation of irregular workpieces, thereby significantly reducing the unevenness of weld flash.

[0015] 2. The coaxiality error between the spindle box and the tailstock of this invention is strictly controlled to ≤0.05mm, ensuring that the axes of standard workpieces and irregular workpieces are precisely aligned. This solves the problem of uneven heat input distribution caused by coaxial deviation when welding irregular workpieces and standard shafts, improves the symmetry of flash forming, refines the grain of the joint, and thus improves the performance of the joint.

[0016] 3. For turbochargers, this invention can achieve a reliable solid-state connection between complex structures and shafts. Using this clamping method can improve efficiency. Attached Figure Description

[0017] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a schematic diagram of the structure of a turbocharger welding device according to the present invention; Figure 2 This is a schematic diagram illustrating the welding and forming of GH4169+K447A material using a turbocharger welding device according to the present invention. Figure 1 ; Figure 3 This is a schematic diagram illustrating the welding and forming of GH4169+K447A material using a turbocharger welding device according to the present invention. Figure 2 ; Figure 4 Tensile test results for GH4169+K447A material Figure 1 ; Figure 5 Tensile test results for GH4169+K447A material Figure 2 ; Figure 6 This is a schematic diagram of a turbocharger.

[0018] In the picture: 1-Cylinder, 2-Tailstock, 3-First clamping block, 4-Irregular workpiece, 5-Second clamping block, 6-Standard workpiece, 7-Top block. Detailed Implementation

[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. It should be noted that, unless otherwise specified, the embodiments and features in the embodiments of the present invention can be combined with each other, and the described embodiments are only some embodiments of the present invention, not all embodiments.

[0020] Detailed Implementation Method 1: See Figure 1 This embodiment describes a turbocharger welding device, comprising a cylinder 1, a tailstock 2, a first clamping block 3, a shaped workpiece 4, a second clamping block 5, and a standard workpiece 6. The cylinder 1 is installed inside the tailstock 2, and the telescopic end of the cylinder 1 is connected to the second clamping block 5. The first clamping block 3 is installed at the end of the tailstock 2. The shaped workpiece 4 is installed between the first clamping block 3 and the second clamping block 5. The end of the standard workpiece 6 passes through the second clamping block 5 and is welded to the shaped workpiece 4.

[0021] The first clamping block 3 has a top block 7 in the middle, which contacts the irregular workpiece 4. The top block 7 has a groove on its end face, and the unwelded end of the top block 7 is engaged in the groove.

[0022] The standard workpiece 6 is fixed on the spindle box by the clamping mechanism, and the irregular workpiece 4 is installed between the first clamping block 3 and the second clamping block 5. The cylinder 1 is started to pull the second clamping block 5, so that the second clamping block 5 and the first clamping block 3 fix the irregular workpiece 4. The drive motor on the spindle box is started to make the standard workpiece 6 rotate at high speed. After reaching the preset speed, the drive motor disengages from the inertia disk. The inertia disk continues to rotate by inertia, moving the spindle box towards the tailstock 2 until the standard workpiece 6 and the irregular workpiece 4 come into contact. At this time, the standard workpiece 6 and the irregular workpiece 4 begin to perform friction welding. The kinetic energy of the inertia disk is gradually converted into heat energy, and the speed decreases. When the speed approaches zero, upsetting pressure is applied to form a uniform welded joint. After the joint cools down, the welding of the standard workpiece 6 and the irregular workpiece 4 is completed.

[0023] Through the synergistic action of the first clamping block 3 and the second clamping block 5, combined with the groove design on the end face of the top block 7, the precise clamping and multi-point fixation of the asymmetrical structure of the irregular workpiece 4 are achieved, effectively avoiding the displacement or vibration of the irregular workpiece 4 due to uneven force during the welding process. The groove structure of the top block 7 can disperse the welding upsetting pressure, reduce the local plastic deformation of the irregular workpiece, and thus significantly reduce the unevenness of the weld flash.

[0024] Detailed Implementation Method 2: See Figure 1 In this embodiment, a top block 7 is provided in the middle of the first clamping block 3. The top block 7 contacts the irregular workpiece 4. A groove is provided on the end face of the top block 7. The unwelded end of the top block 7 is engaged in the groove. Engaging the irregular workpiece 4 in the groove can increase the friction between the irregular workpiece 4 and the two clamping blocks, and prevent the position of the irregular workpiece 4 from shifting during the welding process.

[0025] Detailed implementation method 3: See Figure 1 This embodiment also includes a spindle box and a clamping mechanism. The standard workpiece 6 is installed in the clamping mechanism, which is installed on the spindle box. The coaxiality error between the spindle box and the tailstock 2 is ≤0.05mm. The clamping mechanism is hydraulically driven or pneumatically driven. A through hole is provided at the center of the second clamping block 5 to ensure that the axes of the standard workpiece 6 and the irregular workpiece 4 are accurately aligned. This solves the problem of uneven heat input distribution caused by coaxial deviation when welding the irregular workpiece 4 and the standard shaft, improves the symmetry of flash forming, refines the joint grains, and thus improves tensile strength and low-cycle fatigue performance.

[0026] Specific implementation method 4: Based on specific implementation methods 1-3, the device can also be used for welding gears and shafts, which can improve the joint performance of gear shafts.

[0027] Detailed implementation method 4: See Figure 1This embodiment describes a manufacturing process for a turbocharger welding device, which employs inertial friction welding. The welding formula is as follows: (1) The upsetting pressure is F=πD 2 / 4×P, where P represents the welding pressure of the turbocharger welding contact surface, and D represents the outer diameter of the contact surface shaft; (2) Moment of inertia I = M × R 2 Where M is the weight of the inertial disk and R is the radius of the inertial disk; (3) The total energy input for inertial friction welding is E=Q×S, where Q is the energy required per unit area and S is the area of ​​the welding contact surface; (4) The welding rotation speed n is calculated from the total energy obtained in (3) as follows: E=I×ω 2 / 2, where ω is the initial angular velocity of the inertial disk.

[0028] In this embodiment, the K447A-GH4169 simulated part was welded using this process. The test piece was welded according to the predetermined process parameters, as shown in the table below:

[0029] like Figure 2-3 As shown, a noticeable flash was formed on the right side of the weld joint at GH4169, while no noticeable flash was observed on the K447A side. During the welding process of the high-temperature alloy, the interface temperature exceeded 1200℃. K447A still maintained high strength at this temperature. Simultaneously, during welding, material in the friction interface area on the K447A side was extruded from the interface in the form of spatter, without the formation of a significant plastic layer, indicating poor plasticity of the material. The macroscopic joint morphology is as follows. Figure 2-3 .

[0030] Room temperature tensile tests were conducted on the post-weld GH4169+K447A inertial friction welded joint. During specimen preparation, the weld seam was positioned in the center of the specimen. The specimen preparation standard followed GB / T228.1-2010-φ10 tensile bar. Macroscopic photographs of the tensile joint are shown below. Figure 4-5 , Figure 4 The specimen broke at the weld. Figure 5 The specimen fractured at the K447A side of the base material, with no obvious plastic deformation at the fracture surface. The tensile properties are shown in the table below:

[0031] Based on the above simulation test results, the final parameters of the turbocharger are as follows: the pressure P required for inertial friction welding is 300 MPa; the energy Q required per unit area for inertial friction welding of the turbocharger is 470 J; the inertial friction welding process parameters are: welding upsetting force F 33 t; and rotational inertia I 280 kg·m. 2The total energy E is 516465.414 J, and the initial rotational speed is 580 r / min. Figure 6 The image shows a turbocharger component.

[0032] Furthermore, this manufacturing process and equipment can also be applied to the inertial friction welding manufacturing of irregularly shaped components such as gears.

[0033] The specific embodiments of the present invention disclosed above are merely illustrative of the invention. These embodiments do not exhaustively describe all details, nor do they limit the invention to the specific embodiments described. Many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.

Claims

1. A turbocharger welding apparatus, characterized in that: The device includes a cylinder (1), a tailstock (2), a first clamping block (3), a shaped workpiece (4), a second clamping block (5), and a standard workpiece (6). The cylinder (1) is installed inside the tailstock (2). The telescopic end of the cylinder (1) is connected to the second clamping block (5). The first clamping block (3) is installed at the end of the tailstock (2). The shaped workpiece (4) is installed between the first clamping block (3) and the second clamping block (5). The end of the standard workpiece (6) is inserted into the second clamping block (5) and welded to the shaped workpiece (4).

2. The turbocharger welding apparatus according to claim 1, characterized in that: The first clamping block (3) has a top block (7) in the middle, and the top block (7) is in contact with the irregular workpiece (4).

3. The turbocharger welding apparatus according to claim 2, characterized in that: A groove is provided on the end face of the top block (7), and the unwelded end of the top block (7) is engaged in the groove.

4. The turbocharger welding apparatus according to claim 1, characterized in that: It also includes a spindle box and a clamping mechanism, wherein the standard workpiece (6) is installed in the clamping mechanism, and the clamping mechanism is installed on the spindle box.

5. A turbocharger welding apparatus according to claim 4, characterized in that: The coaxiality error between the main spindle box and the tailstock (2) is ≤0.05mm.

6. The turbocharger welding apparatus according to claim 4, characterized in that: The clamping mechanism is hydraulically driven or pneumatically driven.

7. The turbocharger welding apparatus according to claim 1, characterized in that: The second clamping block (5) has a through hole at its center.

8. A manufacturing process for a turbocharger welding apparatus as described in any one of claims 1-7, characterized in that: Welding is performed using inertial friction welding, and the welding formula is as follows: (1) The upsetting pressure is F=πD 2 / 4×P, where P represents the welding pressure of the turbocharger welding contact surface, and D represents the outer diameter of the contact surface shaft; (2) Moment of inertia I = M × R 2 Where M is the weight of the inertial disk and R is the radius of the inertial disk; (3) The total energy input for inertial friction welding is E=Q×S, where Q is the energy required per unit area and S is the area of ​​the welding contact surface; (4) The welding rotation speed n is calculated from the total energy obtained in (3) as follows: E=I×ω 2 / 2, where ω is the initial angular velocity of the inertial disk.

9. The manufacturing process of the turbocharger welding device according to claim 8, characterized in that: The pressure P required for inertial friction welding of the turbocharger is 300 MPa, the energy Q required per unit area during welding is 470 J, and the welding upsetting force F is 33 t, with a moment of inertia I of 280 kg·m. 2 The total energy E is 516465.414 J, and the initial rotational speed is 580 r / min.