An inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel

By optimizing the inertial friction welding parameters and post-weld heat treatment, the problems of form controllability and residual stress in the welding process of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel were solved, improving the quality and mechanical properties of the welded joint, which is suitable for the manufacture of aero-engine components.

CN123103159APending Publication Date: 2026-11-17AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611539634.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the inertial friction welding process between K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, there are problems such as poor controllability of weld joint formation, unstable joint quality, and difficulty in eliminating residual stress, which makes it difficult to meet the usage requirements of aero-engine components.

Method used

By controlling the spindle speed, moment of inertia, and welding pressure in inertial friction welding, combined with the total shrinkage during welding, and performing segmented post-weld stress-relief heat treatment, welding parameters are optimized to match the differences in material plasticity, thereby improving the quality of interfacial bonding.

Benefits of technology

It improves the forming stability and mechanical properties of welded joints, reduces defects such as incomplete welding and cracks, and ensures the high quality and stability of the joints, making it suitable for the manufacture of aero-engine components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103159A_ABST
    Figure CN123103159A_ABST
Patent Text Reader

Abstract

This application discloses an inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, comprising: providing a first workpiece and a second workpiece to be welded, and machining and cleaning the end faces to be welded; clamping the first workpiece and the second workpiece to be welded in an inertial friction welding machine so that the end faces to be welded are centered and fitted together; setting the spindle speed to 1500 to 1700 r / min and the moment of inertia to 42 to 48 kg·m. 2 The welding pressure is 3 to 5 MPa, and inertial friction welding is performed, controlling the total shrinkage to be 4.36 to 4.92 mm. After welding, pressure holding and upsetting are performed. Post-weld stress-relief heat treatment is then carried out, heating to 560 to 600℃ and holding for 1.5 to 3 hours, then cooling to 530 to 570℃ and holding for 1.5 to 3 hours, followed by air cooling. This inertial friction welding method adapts to the high-temperature plasticity differences between the two materials through parameter combination control, improving flash formation and reducing defects such as incomplete welding and cracks. The two-stage heat treatment releases residual stress, stabilizes the joint microstructure, and improves the mechanical properties and process repeatability of the welded joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metal welding technology, and more specifically, to an inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel. Background Technology

[0002] K424 cast superalloy is a nickel-based cast superalloy with high high-temperature strength, creep resistance, and oxidation resistance. It is commonly used in hot-end components such as low-pressure turbine impellers in aero-engines. 1Cr11Ni2W2MoV heat-resistant steel is a martensitic heat-resistant stainless steel with good mid-temperature mechanical properties and corrosion resistance. It is commonly used in compressor discs and shaft-type load-bearing components. In the manufacturing of integrated aero-engine components, it is sometimes necessary to connect K424 cast superalloy with 1Cr11Ni2W2MoV heat-resistant steel to balance the performance requirements of different parts and manufacturing costs. However, the two materials have significant differences in physical properties and high-temperature plasticity, making reliable connection difficult.

[0003] Currently, dissimilar metals can be joined using fusion welding. Fusion welding involves heating the parts to be joined to a molten state and then solidifying to form a joint, and it is suitable for a variety of metal materials. However, when joining K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, the significant differences in the thermophysical properties and high-temperature plasticity of the two materials can easily lead to problems such as welding cracks, compositional segregation, and joint performance degradation during the welding process, making it difficult to meet the joint quality requirements.

[0004] Inertial friction welding (IFW), a solid-state welding technique, involves rotating the workpieces relative to each other and applying axial pressure during the welding process. Frictional heat softens the interface materials, causing plastic flow and forming a welded joint. IFW has advantages such as a narrow heat-affected zone and minimal microstructural distortion, making it suitable for joining dissimilar high-temperature alloys and heat-resistant steels. However, due to the significant difference in high-temperature plasticity between K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, poor joint formation controllability is a common problem during welding. Furthermore, residual stress at the dissimilar interfaces within the welded joint is difficult to eliminate completely, resulting in insufficient stability in joint quality and mechanical properties, hindering its application in engineering projects.

[0005] Therefore, how to improve the forming quality and mechanical properties of the inertial friction welded joint between K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel has become a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention

[0006] The purpose of this application is to disclose an inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, so as to improve the forming quality and mechanical properties of the inertial friction welded joint of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel.

[0007] A method for inertial friction welding of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, comprising: Step S10: Provide a first workpiece to be welded and a second workpiece to be welded. The first workpiece to be welded is made of K424 cast high-temperature alloy, and the second workpiece to be welded is made of 1Cr11Ni2W2MoV heat-resistant steel. The weldable end faces of the first workpiece to be welded and the weldable end faces of the second workpiece to be welded are machined flat and cleaned. Step S20: Clamp the first workpiece to be welded and the second workpiece to be welded on the inertial friction welding machine, so that the end face to be welded of the first workpiece to be welded and the end face to be welded of the second workpiece to be welded are aligned and fitted together. Step S30: Set the spindle speed of the inertial friction welding machine to 1500 r / min to 1700 r / min, the moment of inertia to 42 kg·m2 to 48 kg·m2, and the welding pressure to 3 MPa to 5 MPa. Start the inertial friction welding machine so that one of the first workpiece to be welded and the second workpiece to be welded rotates with the spindle while the other is fed and pressed along the axial direction to perform inertial friction welding. Control the total shrinkage of the inertial friction welding to 4.36 mm to 4.92 mm. After welding, hold the pressure and forge to obtain the welded joint. Step S40: Perform post-weld stress relief heat treatment on the welded joint. The post-weld stress relief heat treatment includes heating to 560°C to 600°C and holding for 1.5 hours to 3 hours, then cooling to 530°C to 570°C and holding for 1.5 hours to 3 hours. After the holding period, remove the joint from the furnace and air cool to room temperature.

[0008] In one possible implementation, in step S30, the total shrinkage of the weld is 4.50 mm to 4.80 mm.

[0009] In one possible implementation, in step S30, the spindle speed is 1600 r / min and the moment of inertia is 45 kg·m. 2 The welding pressure is 4 MPa.

[0010] In one possible implementation, in step S30, the upsetting pressure of the pressure holding upsetting is the same as the welding pressure, and the pressure holding time of the pressure holding upsetting is 3s to 8s.

[0011] In one possible implementation, in step S40, the post-weld stress relief heat treatment is as follows: the temperature is raised to 580°C and held for 2 hours, then lowered to 550°C and held for 2 hours, and after the holding period, the product is removed from the furnace and air-cooled to room temperature.

[0012] In one possible implementation, in step S40, the heating rate to 580°C is 5°C / min to 10°C / min, and the cooling rate from 580°C to 550°C is 2°C / min to 5°C / min.

[0013] In one possible implementation, in step S10, the first part to be welded is a turbine component made of K424 cast high-temperature alloy, and the second part to be welded is a load-bearing component made of 1Cr11Ni2W2MoV heat-resistant steel; the first part to be welded is in the casting state upon arrival, and the second part to be welded is in the forging state upon arrival.

[0014] In one possible implementation, in step S10, the surface roughness Ra of the end face to be welded is not greater than 3.2 μm, and the end face to be welded is ultrasonically cleaned with acetone or anhydrous ethanol before clamping.

[0015] In one possible implementation, in step S30, the material on one side of the second workpiece undergoes plastic flow and radial extrusion under the combined action of frictional heat and axial pressure, forming continuous flash; the material on one side of the first workpiece is splashed out from the welding interface, so that the weld joint forms the morphology of the flash on one side.

[0016] In one possible implementation, after step S40, the method further includes: Step S50: The welded joint is machined to remove the burrs from the welded joint; Step S60: Perform at least one of the following tests on the welded joint after machining: visual inspection, surface fluorescence inspection, and X-ray inspection.

[0017] Compared to related technologies, the inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel disclosed in this application combines and controls the spindle speed, moment of inertia, welding pressure, and total shrinkage during welding. This method allows for a match between the heat input at the friction interface and the axial pressure, adapting to the significant difference in high-temperature plasticity between K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel. It improves the plastic flow and flash formation of the material during welding, reduces joint quality fluctuations caused by poor formability, and helps reduce defects such as incomplete welding and cracks. After welding, pressure holding and upsetting further densifies the weld interface and improves the integrity of the interface bonding. Post-weld stress-relief heat treatment—first heating to 560℃ to 600℃ and holding for 1.5 to 3 hours, then cooling to 530℃ to 570℃ and holding for 1.5 to 3 hours—helps release residual welding stress, stabilize the joint microstructure, and improve the mechanical properties of the joint. Therefore, the resulting welded joint has stable forming and good process repeatability, and can be used for welding and manufacturing of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel components. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments or related technologies of this application, the accompanying drawings used in the description of the embodiments or related technologies will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a flowchart of the first inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel disclosed in the embodiments of this application; Figure 2 A flowchart of the second inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel; Figure 3 This is a schematic diagram of the structure of the welded joint disclosed in the embodiments of this application.

[0020] The attached figures are labeled as follows: 100, First part to be welded; 200, Second part to be welded; 300, Weld seam; 400, Flash. Detailed Implementation

[0021] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0022] In related technologies, the high-temperature plasticity of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel differs significantly, which can easily lead to problems such as poor joint formation controllability when using inertial friction welding. Moreover, due to the difference in thermal expansion coefficients, the interface between dissimilar materials is prone to residual large stresses, affecting the interface bonding quality and mechanical properties.

[0023] Based on this, this application provides an inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel. This method matches the spindle speed, moment of inertia, and welding pressure, and limits the total welding shrinkage within a set range, ensuring that the frictional heat input and the degree of interfacial plastic flow remain consistent even under dissimilar material conditions. Furthermore, a segmented heat treatment followed by post-weld stress relief is applied to release residual stress at the dissimilar interface in stages. This results in a metallurgical bond at the weld joint interface, with a joint load-bearing capacity no less than that of the base material.

[0024] See Figure 1 The inertial friction welding method of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel in this application includes steps S10 to S40.

[0025] Step S10: Provide a first workpiece 100 and a second workpiece 200 to be welded. The first workpiece 100 is made of K424 cast high-temperature alloy, and the second workpiece 200 is made of 1Cr11Ni2W2MoV heat-resistant steel. The weldable end faces of the first workpiece 100 and the second workpiece 200 are machined flat and cleaned. Optionally, both the first workpiece 100 and the second workpiece 200 can be round bars. The weldable end faces are precision machined to ensure flatness; machining can be performed by turning to achieve a flat surface. Cleaning can be done using ultrasonic cleaning with organic solvents to remove oil and oxide film from the end faces, which is beneficial for the subsequent metallurgical bonding at the friction interface. The flat and clean end faces of the workpieces to be welded ensure that the gaps between the first workpiece 100 and the second workpiece 200 are uniform at all points on the interface after they are bonded together. The interface contact state is consistent at the beginning of the friction, avoiding uneven heating caused by local non-contact. This provides uniform initial conditions for subsequent use of the shortening amount as a unified criterion.

[0026] Step S20: Clamp the first workpiece 100 and the second workpiece 200 on the inertial friction welding machine, so that the end face of the first workpiece 100 to be welded is aligned and in contact with the end face of the second workpiece 200 to be welded. Alignment and contact here means that the axes of the first workpiece 100 and the second workpiece 200 are coaxial and their end faces are in contact with each other. After clamping, the first workpiece 100 and the second workpiece 200 are located on the rotating side and the moving side of the inertial friction welding machine, respectively, or on the moving side and the rotating side, respectively. That is, one of the first workpiece 100 and the second workpiece 200 can rotate with the spindle, while the other can be fed and pressurized axially.

[0027] Step S30: Set the spindle speed of the inertial friction welding machine to 1500 r / min to 1700 r / min and the moment of inertia to 42 kg·m. 2 Up to 48 kg·m 2 The welding pressure is 3MPa to 5MPa. The inertial friction welding machine is started, causing one of the first workpiece 100 and the second workpiece 200 to rotate with the spindle while the other is fed axially under pressure for inertial friction welding. The total shrinkage during inertial friction welding is controlled to be 4.36mm to 4.92mm. After welding, pressure is maintained and upsetting is performed to obtain the welded joint. The total shrinkage refers to the difference between the sum of the lengths of the first workpiece 100 and the second workpiece 200 before welding and the length of the welded joint after welding. This value reflects the total axial displacement consumed by the extrusion of interface material to form flash and interface plasticization during the friction welding process. The control of the total shrinkage is exemplarily achieved by using a displacement detection element to monitor the axial displacement online. When the displacement reaches the set value, the welding machine automatically ends the friction stage and switches to upsetting.

[0028] By controlling the rotational speed, moment of inertia, welding pressure, and total welding shrinkage, the frictional heat input, interfacial plastic flow, and flash extrusion amount are simultaneously constrained within a set range. The rotational speed and moment of inertia determine the energy input level of the frictional interface, the welding pressure determines the extrusion rate of the interfacial plasticized layer, and the shrinkage controls the final flash extrusion amount. Therefore, even if the high-temperature plasticity difference between the first workpiece 100 and the second workpiece 200 is significant, a satisfactory bonding state can still be obtained, and the process repeatability is stable. After the welding reaches the set shrinkage amount, pressure holding and upsetting are performed, that is, under the condition of maintaining axial pressure, the interface is bonded under pressure to obtain a welded joint including weld 300 and flash 400.

[0029] Step S40: Perform post-weld stress-relieving heat treatment on the welded joint. The post-weld stress-relieving heat treatment includes heating to 560℃ to 600℃ and holding at that temperature for 1.5 to 3 hours, then cooling to 530℃ to 570℃ and holding at that temperature for 1.5 to 3 hours. After the holding period, remove the welded joint from the furnace and air-cool it to room temperature. This two-stage heat treatment reduces residual stress in the welded joint and stabilizes the interfacial structure.

[0030] Preferably, the total shrinkage during welding in step S30 can be between 4.50 mm and 4.80 mm. This range allows for a moderate amount of flash 400 extrusion and helps maintain process repeatability.

[0031] In one specific implementation, in step S30, the spindle speed is 1600 r / min and the moment of inertia is 45 kg·m. 2 The welding pressure is 4 MPa. This set of parameters matches the shrinkage range of 4.36 mm to 4.92 mm, and can stably achieve the set shrinkage in a single clamping.

[0032] In one specific embodiment, in step S30, the upsetting pressure during pressure holding is the same as the welding pressure, and the holding time is 3 to 8 seconds. Pressure holding upsetting allows axial pressure to continue being applied to the welding interface after the spindle stops rotating, further densifying the interface material under pressure. The fact that the upsetting pressure is the same as the welding pressure eliminates the need to re-establish pressure equilibrium at the interface during stage transitions, which helps maintain the continuity of the plastic flow layer at the interface. If the holding time is too short, the interface may not bond sufficiently. If the holding time is too long, it may affect the process cycle time. The range of 3 to 8 seconds can be matched with the aforementioned welding pressure to obtain a stable weld joint.

[0033] In one specific embodiment, the post-weld stress relief heat treatment is preferably performed by heating to 580°C and holding for 2 hours, then cooling to 550°C and holding for 2 hours, and finally removing the product from the furnace and air-cooling it to room temperature.

[0034] Furthermore, the heating rate to 580℃ can be 5℃ / min to 10℃ / min, and the cooling rate from 580℃ to 550℃ can be 2℃ / min to 5℃ / min. By controlling the heating and cooling rates, the additional thermal stress caused by excessively rapid temperature changes during heat treatment can be reduced.

[0035] In one specific embodiment, in step S10, the first weldment 100 is a turbine component made of K424 cast high-temperature alloy, and the second weldment 200 is a load-bearing component made of 1Cr11Ni2W2MoV heat-resistant steel. The first weldment 100 arrives in a cast state, and the second weldment 200 arrives in a forged state. There are differences between the cast and forged states in terms of microstructure density and high-temperature plasticity. The aforementioned load-bearing components are exemplary shaft-like, disc-like, or cylindrical components. The shapes of the first weldment 100 and the second weldment 200 are determined according to the actual structure of the parts to be connected. For example, one side of the turbine component may have a disc-shaped or annular weldable end face, and one side of the load-bearing component may have a round bar-shaped or shaft-shaped weldable end face.

[0036] In one specific implementation, in step S10, the surface roughness Ra of the end face to be welded is no greater than 3.2 μm, which helps to increase the actual contact area of ​​the interface after bonding and ensures uniform heat generation in the initial stage of friction. The surface face to be welded can be machined smoothly by turning, grinding, or milling. Before clamping, the end face to be welded can be ultrasonically cleaned with acetone or anhydrous ethanol. Acetone or anhydrous ethanol has a dissolving and peeling effect on oil and oxide films; combined with ultrasonic cleaning, it can remove residues in the micro-pits of the end face and reduce the risk of interface inclusions.

[0037] like Figure 3 As shown, in step S30, the material on one side of the second workpiece 200 undergoes plastic flow and radial extrusion under the combined action of frictional heat and axial pressure, forming continuous flash 400. The material on the one side of the first workpiece 100, due to its relatively low high-temperature plasticity, is ejected from the welding interface in the form of spatter. Ultimately, the welded joint forms a single-sided flash 400 morphology, meaning the second workpiece 200 side has a relatively continuous flash 400, while the first workpiece 100 side does not have a continuous flash 400. This single-sided flash 400 morphology indicates that the process parameters are adapted to the plasticity differences between the two materials, which is beneficial for improving the controllability of the joint formation.

[0038] like Figure 2 As shown, after step S40, steps S50 and S60 may also be included.

[0039] Step S50: Machining the welded joint removes the burrs 400 on the inner and outer sides. Machining removes the burrs 400 to restore the joint to a regular shape, facilitating subsequent assembly and inspection.

[0040] Step S60: Perform at least one of the following tests on the machined weld joint: visual inspection, surface fluorescence inspection, and X-ray inspection. For example, one, two, or three of these tests can be performed. Visual inspection can be used to observe whether there are defects such as cracks, incomplete fusion, porosity, burn-through, or inclusions on the surface of the weld 300. Surface fluorescence inspection can be used to detect defects on and near the surface of the weld 300. X-ray inspection can be used to detect internal defects in the weld joint. Through these tests, the quality of the weld joint can be evaluated.

[0041] The following describes the complete working process of the inertial friction welding method of the K424 nickel-based cast high-temperature alloy and 1Cr11Ni2W2MoV martensitic heat-resistant steel of this application, with reference to an embodiment.

[0042] The first workpiece 100 is cut from the turbine working wheel via wire cutting, and the base material is K424 nickel-based cast high-temperature alloy. The second workpiece 200 is formed by forging, and the base material is 1Cr11Ni2W2MoV martensitic heat-resistant steel. Both the first workpiece 100 and the second workpiece 200 are round bars. In the initial state, the end faces of the first workpiece 100 and the second workpiece 200 to be welded have been machined flat and cleaned.

[0043] The first workpiece 100 and the second workpiece 200 are clamped in an inertial friction welding machine so that the two end faces to be welded are centered and in contact. At this time, one of the first workpiece 100 and the second workpiece 200 is connected to the main shaft, and the other is connected to the axial feed mechanism.

[0044] In response to the start signal, the spindle of the inertial friction welding machine accelerates to the set speed, for example, to 1600 r / min. The flywheel stores rotational kinetic energy, with a moment of inertia of 45 kg·m. 2 Once the spindle reaches the set speed, the axial feed mechanism drives the other of the first and second workpieces to be welded, 100 and 200, to move axially toward the rotating side, bringing the two end faces into contact and applying welding pressure of 4 MPa. Under the combined action of frictional heat and axial pressure, the material near the end faces to be welded heats up and softens. As friction continues, the material on the side of the second workpiece 200 undergoes plastic flow and is extruded radially, forming continuous flash 400. The material on the side of the first workpiece 100 is ejected from the welding interface in the form of spatter. The total axial length of the first and second workpieces to be welded, 100 and 200, gradually shortens. When the total shortening reaches 4.36 mm to 4.92 mm, the spindle rotation is stopped or the spindle is disengaged from the flywheel, and pressure holding and upsetting are performed. During pressure holding and upsetting, the upsetting pressure can be maintained at the same level as the welding pressure, and the holding time can be 3 to 8 seconds. Under the action of pressure holding and upsetting, the welding interface is further densified, forming a weld 300. After the pressure holding period is completed, a welded joint is obtained.

[0045] Subsequently, the welded joint was placed in a heating furnace for post-weld stress-relieving heat treatment. The heating furnace was operated according to a procedure of holding at 580℃ for 2 hours, then cooling to 550℃ and holding for 2 hours. After the holding period, the joint was removed from the furnace and air-cooled to room temperature. During the heat treatment process, the residual stress in the welded joint was released, and the microstructure of the 300 interface of the weld tended to stabilize.

[0046] When necessary, the heat-treated welded joint is machined to remove the 400mm burrs on the inner and outer sides, restoring the welded joint to a regular shape. Then, the machined welded joint undergoes visual inspection, surface fluorescence inspection, and X-ray testing to finally obtain a welded joint with a regular shape that meets the inspection standards.

[0047] To verify the effectiveness of the inertial friction welding method for K424 nickel-based cast superalloy and 1Cr11Ni2W2MoV martensitic heat-resistant steel described in this application, three parallel experiments were conducted using the same welding parameters. The total lengths before welding were 160.96 mm, 165.24 mm, and 164.90 mm, respectively, and the total lengths after welding were 156.60 mm, 160.72 mm, and 159.98 mm, respectively, corresponding to total weld shrinkage of 4.36 mm, 4.52 mm, and 4.92 mm, respectively. The results show that the flash extrusion amount in all three experiments was moderate, and the flash formation was good. This indicates that the process repeatability is good within the range of 4.36 mm to 4.92 mm of total weld shrinkage.

[0048] Furthermore, the welded joints prepared using the above method were subjected to room temperature tensile tests and 450°C high-temperature tensile tests. Under exemplary test conditions, the tensile strengths of the room temperature tensile specimens were 816 MPa and 734 MPa, respectively, and the tensile strengths of the 450°C high-temperature tensile specimens were 850 MPa and 779 MPa, respectively. The fracture locations in both the room temperature and 450°C high-temperature tensile tests were located on the K424 cast superalloy base material side. This indicates that the strength of weld 300 is not lower than that of the K424 cast superalloy base material, and tensile fracture did not occur in the weld 300 region.

[0049] Furthermore, room temperature impact tests were conducted on the welded joints prepared using the above method. Weld 300 was located at the center of the specimen, and a total of four parallel specimens were tested. The fracture surfaces of the impact specimens were uneven, and the fracture locations were near the weld zone or within the base material of the K424 cast high-temperature alloy. No fracture occurred at the weld 300 interface. This indicates that the toughness of the welded joint meets the service requirements. Metallographic observation of the welded joints prepared using the above method revealed a dense microstructure in the weld zone and a metallurgical bond at the interface. All of the above results verify the interfacial bonding state and load-bearing capacity of the welded joint.

[0050] The terms "first" and "second," etc., used in this application are used to distinguish different objects, not to describe a specific order, and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units may include steps or units not listed, but rather steps or units not listed.

[0051] In the description of this application, it should be understood that the terms "height," "thickness," "upper," "lower," "top," "bottom," "inner," and "outer," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. In the description of this application, "a plurality of" means two or more, and "at least one" can mean one, two, or more, unless otherwise expressly specified.

[0052] The above description of the disclosed embodiments enables those skilled in the art to make or use this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Specific technical means in some embodiments may be incorporated, in whole or in part, into another embodiment unless explicitly excluded by another embodiment. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for inertial friction welding of K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel, characterized in that, include: Step S10: Provide a first workpiece to be welded (100) and a second workpiece to be welded (200). The first workpiece to be welded (100) is made of K424 cast high-temperature alloy, and the second workpiece to be welded (200) is made of 1Cr11Ni2W2MoV heat-resistant steel. The weldable end faces of the first workpiece to be welded (100) and the weldable end faces of the second workpiece to be welded (200) are machined flat and cleaned. Step S20: Clamp the first workpiece to be welded (100) and the second workpiece to be welded (200) on the inertial friction welding machine, so that the end face to be welded of the first workpiece to be welded (100) and the end face to be welded of the second workpiece to be welded (200) are aligned and fitted together; Step S30: Set the spindle speed of the inertial friction welding machine to 1500 r / min to 1700 r / min, the moment of inertia to 42 kg·m2 to 48 kg·m2, and the welding pressure to 3 MPa to 5 MPa. Start the inertial friction welding machine so that one of the first workpiece to be welded (100) and the second workpiece to be welded (200) rotates with the spindle and the other is fed and pressed along the axial direction to perform inertial friction welding. Control the total shrinkage of the inertial friction welding to 4.36 mm to 4.92 mm. After welding, hold the pressure and forge to obtain the welded joint. Step S40: Perform post-weld stress relief heat treatment on the welded joint. The post-weld stress relief heat treatment includes heating to 560°C to 600°C and holding for 1.5 hours to 3 hours, then cooling to 530°C to 570°C and holding for 1.5 hours to 3 hours. After the holding period, remove the joint from the furnace and air cool to room temperature.

2. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S30, the total shrinkage during welding is 4.50 mm to 4.80 mm.

3. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S30, the spindle speed is 1600 r / min and the moment of inertia is 45 kg·m. 2 The welding pressure is 4 MPa.

4. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S30, the upsetting pressure of the pressure holding upsetting is the same as the welding pressure, and the pressure holding time of the pressure holding upsetting is 3s to 8s.

5. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S40, the post-weld stress relief heat treatment is as follows: the temperature is raised to 580°C and held for 2 hours, then lowered to 550°C and held for 2 hours, and after the holding period, the product is removed from the furnace and air-cooled to room temperature.

6. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 5, characterized in that, In step S40, the heating rate to 580°C is 5°C / min to 10°C / min, and the cooling rate from 580°C to 550°C is 2°C / min to 5°C / min.

7. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S10, the first part to be welded (100) is a turbine component made of K424 cast high-temperature alloy, and the second part to be welded (200) is a load-bearing component made of 1Cr11Ni2W2MoV heat-resistant steel; the first part to be welded (100) is in the casting state upon arrival, and the second part to be welded (200) is in the forging state upon arrival.

8. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S10, the surface roughness Ra of the end face to be welded is not greater than 3.2 μm, and the end face to be welded is ultrasonically cleaned with acetone or anhydrous ethanol before clamping.

9. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in claim 1, characterized in that, In step S30, the material on one side of the second workpiece to be welded (200) undergoes plastic flow and radial extrusion under the combined action of frictional heat and axial pressure, forming a continuous flash (400); the material on one side of the first workpiece to be welded (100) is thrown out from the welding interface in the form of splash, so that the welded joint forms the morphology of the flash (400) on one side.

10. The inertial friction welding method for K424 cast high-temperature alloy and 1Cr11Ni2W2MoV heat-resistant steel as described in any one of claims 1-9, characterized in that, Following step S40, the method further includes: Step S50: The welded joint is machined to remove the burrs (400) of the welded joint. Step S60: Perform at least one of the following tests on the welded joint after machining: visual inspection, surface fluorescence inspection, and X-ray inspection.