Welding process for sealing surfaces of small-diameter valves

By pre-processing hard alloy sealing rings and using brazing technology combined with medium- and high-frequency induction heating and infrared temperature measurement control, the operational difficulties and quality instability in welding the sealing surfaces of small-diameter valves have been solved, achieving efficient and stable welding results, extending the service life of valves and reducing production costs.

CN123103231APending Publication Date: 2026-11-17JIANGNAN VALVE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611622635.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing welding methods for small-diameter valve sealing surfaces suffer from problems such as high operational difficulty, unstable quality, low finished product qualification rate, short service life, and high production cost. In particular, the fusion welding method is prone to welding defects and valve body deformation in narrow spaces.

Method used

The sealing ring is pre-processed using cemented carbide welding wire or Stellite cemented carbide bar. The sealing ring is then joined to the valve body by brazing. After ensuring the surface quality through penetrant testing and flux treatment, brazing is performed. The welding temperature is controlled by medium- and high-frequency induction heating and infrared temperature measurement to avoid the defects of traditional overlay welding and achieve uniformity and stability of the sealing surface.

Benefits of technology

It improves welding efficiency and quality stability, reduces operational technical requirements, ensures uniform hardness of the sealing surface, extends service life, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103231A_ABST
    Figure CN123103231A_ABST
Patent Text Reader

Abstract

A welding process for the sealing surface of small-diameter valves is disclosed. This process involves pre-machining a hard alloy sealing ring, which is then brazed to the valve body. This eliminates the need for welding within the narrow cavity of the valve body, avoiding welding defects caused by limited operating space, reducing the technical requirements for operators, increasing welding efficiency, and improving quality stability during mass production. Pre-machining the sealing ring allows for early defect detection, screening out substandard sealing blanks and avoiding subsequent waste processing. Simultaneously, the brazing heating process ensures uniform heating, minimizing overall valve body deformation, resulting in a more uniform hardness and stress distribution on the sealing surface, leading to a higher yield rate. The resulting sealing surface is less prone to cracking and leakage during long-term use, extending its service life and effectively reducing the processing and production costs of sealing surfaces for small-diameter valves.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of valve technology, and specifically to a welding process for the sealing surface of a small-diameter valve. Background Technology

[0002] In existing technologies, small-diameter gate valves are typically welded using fusion welding. However, due to the small diameter and deep sealing surface, fusion welding is difficult to perform, and the arc crater cracks at the weld neck are difficult to repair, resulting in a low first-pass yield and requiring multiple reworks. Direct fusion welding cannot meet production quality and delivery time requirements. Furthermore, the narrow welding space and limited welding torch movement easily lead to defects such as uneven weld layer thickness, incomplete fusion, and slag inclusions. Simultaneously, the heat concentrated in a localized area of ​​the valve body during welding can cause deformation, resulting in uneven sealing surface hardness after subsequent finishing, a low finished product yield, and increased susceptibility to cracking and leakage due to uneven stress during later use, leading to a shorter service life. In addition, direct welding requires highly skilled operators, has low welding efficiency, poor quality stability in mass production, and high production costs. Summary of the Invention

[0003] In view of this, the present invention provides a welding process for the sealing surface of a small-diameter valve.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] A welding process for the sealing surface of a small-diameter valve includes the following steps:

[0006] Step 1: Preparation of the sealing ring. Use cemented carbide welding wire and argon arc welding to build up a long strip of cemented carbide round bar, or directly use Stellite cemented carbide bar material, then process it into the required sealing ring size. Step 2: Penetrant testing. Spray penetrant onto the surface of the sealing ring from Step 1 and leave it for at least 15 minutes. Wipe off the surface penetrant, then spray colorant onto the sealing ring surface and check the surface quality to ensure there are no defects. Step 3: Machining the sealing ring groove. Machining a sealing ring groove on the valve body for placing the sealing ring. The bottom of the sealing ring groove also has an annular storage groove with a depth of 0.2~0.5mm and a width of 0.5~1.2mm. The bottom or side wall of the sealing ring groove also has at least two blind venting micro-grooves with a width of 0.1~0.2mm and a depth of 0.1~0.15mm, evenly distributed along the circumference and not penetrating the valve body wall. The total volume of the brazing groove is 1.2 to 2.0 times the volume of the gap between the outer ring side of the sealing ring and the side wall of the sealing ring groove; Step 4: Cleaning the workpiece, using organic solvent to clean the surface of the sealing ring; Step 5: Applying flux, applying flux to the inside of the sealing ring groove, and placing the cleaned sealing ring in the sealing ring groove, so that the sealing ring is in close contact with the inner wall of the sealing ring groove; Step 6: Heating, heating the valve body to 50-100℃ higher than the melting point of the brazing filler metal; Step 7: Filling the brazing wire, immediately filling the brazing wire manually after the valve body temperature rises to the welding temperature of the brazing filler metal, visually until the wire melts and fills the gap; Step 8: Rough machining inspection, after the valve body cools, rough machining is performed on the sealing surface, and the penetration inspection in Step 2 is repeated; Step 9: Fine machining inspection, machining the remaining dimensions of the valve body according to the drawings, and repeating the penetration inspection in Step 2; Step 10: Water pressure test, after completing the overall assembly of the valve, the sealing surface is pressure tested, and it is qualified if there is no leakage.

[0007] Preferably, after the sealing ring is placed in the sealing ring groove, a gap is formed between the outer ring side of the sealing ring and the side wall of the sealing ring groove, the size of the gap being 0.2-0.3mm, the depth of the sealing ring groove being 0.1-0.2mm greater than the thickness of the sealing ring, and a transition fillet being formed between the side wall of the sealing ring groove and the bottom surface, the transition fillet being R0.5~R1.0mm.

[0008] Preferably, the cemented carbide welding wire contains more than 44% cobalt, the hardness requirement after welding is HRC35-42, the flux is a silver brazing solvent, the brazing wire is a silver-based brazing wire, and the melting point of the brazing wire is 620℃-650℃.

[0009] Preferably, in step six, a medium-to-high frequency induction heater is used, with a frequency of 20~50kHz and a power of 10~25kW, suitable for small-diameter workpieces; the heating temperature is set 60~90℃ higher than the melting point of the brazing filler metal; and an infrared thermometer is used to continuously monitor the temperature at the bottom of the valve body groove.

[0010] Preferably, in step four, the organic solvent used is thinner. After soaking and cleaning for 5-10 minutes, the ring is taken out and dried to remove oil stains, metal shavings, and residual processing coolant from the surface of the sealing ring, ensuring that the surface of the sealing ring is clean and free of impurities.

[0011] Preferably, in step one, the diameter of the Stellite cemented carbide bar is reserved with a machining allowance of 3~5mm according to the size of the finished ring; DC argon arc welding is used, with a welding current of 80~120A, an argon flow rate of 8~12 L / min, an interpass temperature controlled at ≤150℃, and a weld thickness of not less than 1.2 times the thickness of the finished ring.

[0012] Preferably, in step eight, the sealing surface is rough-machined on a lathe to remove excess brazing filler metal and oxide scale, leaving a finishing allowance of 0.2~0.3mm and a surface roughness Ra≤6.3μm.

[0013] Preferably, in step five, powdered silver-based soldering flux FB105 type borax-based flux is selected. Before use, it is mixed with distilled water to form a paste with a water-to-powder ratio of about 1:2. Then, a small stainless steel scraper or a special brush is used to evenly fill the bottom and sidewalls of the groove with the flux paste. The coating thickness is about 0.3~0.5mm, ensuring no missed areas or accumulation.

[0014] The beneficial effects of this invention are as follows: This process changes the traditional welding concept. A hard alloy sealing ring is pre-processed, and then brazed to join the sealing ring to the valve body. The valve's sealing surface welding can be completed using brazing alone, eliminating the need for welding within the narrow cavity of the valve body as in existing technologies. This avoids various defects that can easily occur during welding due to limited operating space, reduces the technical requirements for operators, increases welding efficiency, and improves quality stability in mass production. Pre-processing the sealing ring allows for early defect detection, screening out unqualified sealing blanks and avoiding subsequent waste processing. Simultaneously, the brazing heating process ensures uniform heating, resulting in minimal overall valve body deformation. The hardness of the sealing surface after processing is uniform, with more even stress distribution, leading to a higher finished product qualification rate. The resulting sealing surface is less prone to cracking and leakage during long-term use, extending its service life and effectively reducing the processing and production costs of sealing surfaces for small-diameter valves. Attached Figure Description

[0015] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0016] Appendix Figure 1 This is a schematic diagram of the valve and sealing ring assembly. Detailed Implementation

[0017] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0018] The present invention will now be further described with reference to the accompanying drawings.

[0019] This invention provides the following technical solution:

[0020] This invention discloses a welding process for the sealing surface of a small-diameter valve, comprising the following steps:

[0021] Step 1: Preparation of the sealing ring. Use cemented carbide welding wire and argon arc welding to build up a long strip of cemented carbide round bar, or directly use Stellite cemented carbide bar material, then process it to the required sealing ring 1 size. Step 2: Penetrant testing. Spray penetrant onto the surface of the sealing ring 1 from Step 1 and leave it for at least 15 minutes. Wipe off the surface penetrant, then spray colorant onto the surface of the sealing ring 1 to check the surface quality and ensure there are no defects. In this step, coloring can visually identify whether there are microcracks, pores, or other internal hidden defects on the surface of the sealing ring 1 that are difficult to distinguish with the naked eye. This allows for the early rejection of unqualified workpieces, avoiding the waste of time and materials caused by discovering defects only after subsequent welding, effectively improving the yield rate. The penetrant is JYBL-4, and the colorant is the matching JYBL-4 developer. Step 3: Machining the sealing ring groove 2. Machining the groove on the valve body 3... Step 4: Cleaning the workpiece. Use an organic solvent to clean the surface of the sealing ring 1. In this step, remove residual oil, processing debris, and coolant impurities from the surface of the sealing ring 1 to avoid impurities affecting the bonding strength of subsequent brazing, and to prevent problems such as weak bonding and residual air bubbles in the gaps after the sealing surface is welded, ensuring the tightness and stability of the welded part. Step 5: Applying flux. Apply flux to the sealing ring groove 2 and place the cleaned sealing ring 1 in the sealing ring groove 2, so that the sealing ring 1 is in close contact with the inner wall of the sealing ring groove 2. Specifically, in this step, use powdered silver-based brazing flux FB105 type borax-based flux. Before use, mix it with distilled water to form a paste with a water-to-powder ratio of about 1:2. Then use a small stainless steel scraper or a special brush to evenly fill the bottom and side walls of the groove with the paste flux, ensuring a coating thickness of about 0.3~0.5mm, to ensure no missing coating or flux accumulation in the entire brazing area. The flux can remove oxides on the welding surface, improve the flow and wetting performance of the brazing filler metal, and avoid inclusion and incomplete fusion defects at the welded part; Step 6: Heating, heat the valve body 3 to 50-100°C above the melting point of the brazing filler metal. In this step, medium-high frequency induction heating can perform precise concentrated heating on the seal ring groove 2, featuring fast heating speed and small heat-affected zone, which will not cause excessive thermal stress deformation to the overall structure of the valve body 3, and is adapted to the structural characteristics of the small-caliber valve body 3. Meanwhile, continuous temperature monitoring through an infrared temperature measuring gun can accurately control the heating temperature, avoid insufficient temperature leading to insufficient melting of the brazing filler metal, or excessive temperature causing flux burning loss and coarse base material grains, so as to ensure stable welding quality; Step 7: Filling brazing filler wire, manually fill the brazing filler wire immediately after the temperature of the valve body 3 rises to the welding temperature 50-100°C above the melting point of the brazing filler metal, until the wire melts and fills the gap visually on the valve body 3; Step 8: Rough machining and inspection, perform rough machining on the sealing surface after the valve body 3 cools down, and repeat the penetration inspection in Step 2; Step 9: Finish machining and inspection, machine the remaining dimensions of the valve body 3 according to the drawing, and repeat the penetration inspection in Step 2; Step 10: Hydrostatic pressure test, complete the overall assembly of the valve, then conduct a sealing surface pressure test, and it is qualified if there is no leakage.

[0022] Further, after the seal ring 1 is placed in the seal ring groove 2, a gap is formed between the outer ring side of the seal ring 1 and the side wall of the seal ring groove 2, the size of the gap is 0.2-0.3mm, the depth of the seal ring groove 2 is 0.1-0.2mm greater than the thickness of the seal ring 1, a transition fillet is formed between the side wall and the bottom surface of the seal ring groove 2, and the transition fillet is R0.5~R1.0mm. Specifically, the reserved gap can ensure that the molten brazing filler metal can uniformly fill the entire mating surface, avoiding poor flow of the brazing filler metal leaving voids. Meanwhile, the transition fillet can avoid stress concentration, reduce the risk of cracking of the seal ring groove 2 during the use of the valve body 3, and also allow the brazing filler metal to be uniformly filled at the fillet, avoiding residual air bubbles in dead corners.

[0023] Further, the cobalt content of the hard alloy welding wire is more than 44%, the hardness requirement after surfacing is HRC35-42, the brazing flux is a silver brazing flux, the brazing filler wire is a silver-based brazing filler wire, and the melting point of the brazing filler wire is 620°C-650°C. Specifically, the hard alloy seal ring 1 with high cobalt content has more excellent toughness and impact resistance, which is suitable for the working scenario where the sealing surface is repeatedly impacted during valve opening and closing. The hardness range of HRC35-42 not only ensures the wear resistance of the sealing surface, but also avoids brittle fracture of the sealing surface caused by excessive hardness. The silver-based brazing filler wire has a moderate melting point, which will not cause overburning damage to the hard alloy seal ring 1 during welding, and the strength of the welded joint meets the pressure-bearing use requirements of the valve.

[0024] Furthermore, in step six, a medium-to-high frequency induction heater is used, with a frequency of 20~50kHz and a power of 10~25kW, suitable for small-diameter workpieces; the heating temperature is set 60~90℃ higher than the melting point of the brazing filler metal; and an infrared thermometer is used to continuously monitor the temperature at the bottom of the groove in the valve body 3. Specifically, these frequency and power parameters enable precise and concentrated heating of the sealing ring groove 2 area of ​​the small-diameter valve, without affecting other unrelated parts of the valve body 3. This allows for rapid heating to the target welding temperature while minimizing thermal deformation of the valve body 3, ensuring the dimensional accuracy of subsequent assembly. Continuous infrared temperature measurement allows for real-time control of the heating process, preventing temperature fluctuations from affecting the brazing quality.

[0025] Furthermore, in step four, thinner is selected as the organic solvent. After soaking and cleaning for 5-10 minutes, it is taken out and dried to remove oil stains, metal shavings and residual processing coolant from the surface of the sealing ring 1, ensuring that the surface of the sealing ring 1 is clean and free of impurities.

[0026] Furthermore, in step one, the diameter of the Stellite cemented carbide bar is adjusted to allow for a machining allowance of 3-5 mm based on the finished ring size. DC TIG welding is used with a welding current of 80-120 A, an argon flow rate of 8-12 L / min, and an interpass temperature controlled at ≤150℃. The weld thickness is no less than 1.2 times the thickness of the finished ring. Specifically, allowing sufficient machining allowance ensures a uniform microstructure in the subsequently machined sealing ring 1 blank, preventing surface welding defects from affecting the performance of the finished sealing ring 1. The DC TIG welding parameters, combined with low interpass temperature control, reduce heat input during the welding process, preventing coarse grains in the weld layer, ensuring the strength and toughness of the cemented carbide weld layer, and meeting the performance requirements of the sealing ring 1.

[0027] Furthermore, in step eight, the sealing surface is rough-machined on a lathe to remove excess brazing filler metal and oxide scale, leaving a finishing allowance of 0.2~0.3mm and a surface roughness Ra≤6.3μm. Specifically, leaving sufficient finishing allowance provides ample room for correction in subsequent finishing processes, removes excess brazing filler metal and oxide scale in advance, avoids excessive wear on finishing tools due to large residual material from rough machining, and controls surface roughness to provide a good machining foundation for finishing, ensuring that the final dimensional accuracy of the sealing surface meets the machining requirements.

[0028] Furthermore, an annular solder storage groove 4 is provided at the bottom of the sealing ring groove 2. The depth of the annular solder storage groove 4 is 0.2~0.5mm and the width is 0.5~1.2mm. At least two blind exhaust micro-grooves (not shown in the figure) are also provided at the bottom or side wall of the sealing ring groove 2. The exhaust micro-grooves are 0.1~0.2mm wide and 0.1~0.15mm deep, evenly distributed along the circumference, and do not penetrate the valve body 3 wall. The total volume of the annular solder storage groove is 1.2~2.0 times the volume of the gap between the outer ring side of the sealing ring 1 and the side wall of the sealing ring groove 2. Before brazing, a silver-based solder ring, solder wire ring or solder foil is pre-placed in the annular solder storage groove. The amount of pre-placed solder matches the gap and the volume of the solder storage groove. Specifically, in this embodiment, the annular brazing groove can store a fixed amount of brazing filler metal in advance, avoiding the problem of inaccurate control of the amount of brazing filler metal when manually filling the wire, and ensuring that the amount of brazing filler metal in the mating gap is sufficient. The blind venting micro-groove can smoothly expel the air accumulated in the gap when the brazing filler metal is filled into the gap, avoiding the formation of air pore defects due to air residue. At the same time, since the venting micro-groove is a non-through blind groove, it will not affect the overall pressure bearing performance of the valve body 3. It is easy to process and highly practical.

[0029] Example 1:

[0030] Step 1: Use hard alloy welding wire (45% cobalt content) for argon arc welding, current 80A, argon flow rate 8 L / min, interpass temperature ≤150℃, weld thickness is 1.2 times the thickness of the finished ring, to process into sealing ring 1; Step 2: Penetrant testing, spray penetrant on the surface of sealing ring 1 from step 1 and keep it for more than 15 minutes, wipe off the surface penetrant, then spray colorant on the surface of sealing ring 1, check the surface quality to ensure that there are no defects; Step 3: Machining sealing ring groove 2, machining sealing ring groove 2 for placing sealing ring 1 on valve body 3; Step 4: Cleaning the workpiece, use thinner, soak and clean for 5 minutes, then take it out and let it dry; Step 5: The inner gap of sealing ring groove 2 is 0.2 mm, the groove depth is 0.1 mm larger than the ring thickness, the transition radius R0.5 mm; the flux (FB105, water-to-powder ratio 1:2) is applied to a thickness of about 0.3 mm; Step 6: Medium and high frequency induction heating, frequency 50 kHz, power 10kW, set temperature 50℃ higher than the melting point of the brazing filler metal (620℃), then heat to 670℃; Step 7: Fill with silver-based brazing wire (raise the temperature of valve body 3 to the melting point of 620℃); Step 8: Rough machining with a allowance of 0.2 mm, roughness Ra≤6.3 μm; Step 9: Finishing inspection, process the remaining dimensions of valve body 3 according to the drawing, and repeat step 2 for penetration inspection; Step 10: Water pressure test, complete the overall assembly of the valve, and then conduct a sealing pressure test. No leakage indicates it is qualified.

[0031] In this embodiment, the heating temperature of 670 ℃ in step six reduces the heat-affected zone of the valve body 3 substrate, effectively avoiding grain coarsening and sensitization of austenitic stainless steel or low alloy steel, which is beneficial to maintaining the mechanical properties of the valve body 3; in step five, the gap between the sealing ring 1 and the side wall of the sealing ring groove 2 is 0.2 mm, which, together with the thin flux layer, makes the capillary effect stronger, the brazing filler ...

[0032] Example 2:

[0033] The difference between Example 2 and Example 1 is that: Stellite cemented carbide rods are used directly, with a 5 mm machining allowance for the finished ring diameter, without weld overlay. The gap between the sealing ring 1 and the sidewall of the sealing ring groove 2 is 0.3 mm, the groove depth is 0.2 mm greater than the ring thickness, and the transition fillet radius is R1.0 mm; the flux coating thickness is approximately 0.5 mm; the heating frequency is 20 kHz, the power is 25 kW, and the set temperature is 100 ℃ higher than the melting point of the brazing filler metal. If the melting point of the brazing filler metal is 650 ℃, then it is heated to 750 ℃; silver-based brazing wire (melting point 650 ℃) is used; a rough machining allowance of 0.3 mm is left, and the surface roughness Ra≤6.3 μm.

[0034] The specific steps of Example 2 are as follows:

[0035] Step 1: Preparation of Sealing Ring 1. Stellite carbide bar stock is used directly. The bar diameter is adjusted according to the finished ring size, allowing a 5 mm machining allowance. No welding is performed. The ring is then machined to the required size. Step 2: Penetrant Testing. A penetrant is sprayed onto the surface of the sealing ring 1 from Step 1 and left for at least 15 minutes. The penetrant is then wiped off. A colorant is then sprayed onto the surface of the sealing ring 1. The surface quality is checked to ensure there are no defects. Step 3: Machining the Sealing Ring Groove 2. A sealing ring groove 2 is machined into the valve body 3 to house the sealing ring 1. The inner clearance of the sealing ring groove 2 is 0.3 mm, and the groove depth is 0.2 mm greater than the ring thickness. The transition radius between the sidewall and bottom surface of the sealing ring groove 2 is R1.0. mm; Step 4: Cleaning the workpiece. Immerse the surface of the sealing ring 1 in an organic solvent (thinner) for 5-10 minutes, then remove and air dry to remove oil, metal shavings, and residual coolant; Step 5: Applying flux. Use powdered silver-based brazing flux FB105 type borax-based flux, mix with distilled water to form a paste (water-to-powder ratio approximately 1:2), and use a small stainless steel scraper or special brush to evenly fill the bottom and sidewalls of the sealing ring groove 2 with the paste flux, with a coating thickness of approximately 0.5 mm, ensuring no missed areas or accumulation; then place the cleaned sealing ring 1 in the sealing ring groove 2, ensuring that the sealing ring 1 is in close contact with the inner wall of the sealing ring groove 2; Step 6: Heating. Use a medium-high frequency induction heater with a frequency of 20 kHz and a power of 25 kW, setting the heating temperature to be 100 ℃ higher than the melting point of the brazing filler metal (if the melting point of the brazing filler metal is 650 ℃, then heat to 750 ℃). Step 7: Fill with brazing wire. After the valve body 3 temperature rises to the welding temperature, immediately fill with silver-based brazing wire (melting point 650 ℃) manually until the wire melts and fills the gap. Step 8: Rough machining inspection. After the valve body 3 cools down, rough machine the sealing surface with a lathe to remove excess brazing material and oxide scale, leaving a finishing allowance of 0.3 mm and a surface roughness Ra≤6.3 μm. Repeat the penetration test in Step 2. Step 9: Finishing inspection. Machin the remaining dimensions of the valve body 3 according to the drawings and repeat the penetration test in Step 2. Step 10: Water pressure test. After the valve is fully assembled, perform a sealing pressure test. If there is no leakage, it is qualified.

[0036] This embodiment directly uses Stellite rod stock, avoiding problems such as internal porosity and dilution rate in the weld overlay. The sealing ring 1 has uniform material and optimal density, stable hardness and resistance to erosion and corrosion. The 0.3mm gap and R1.0 radius significantly reduce the requirements for assembly accuracy. The brazing filler metal has low flow resistance, making it particularly suitable for complex shapes or manual operation conditions, and the filling reliability is high. The heating temperature of 750℃ enhances the wettability and spreadability of the brazing filler metal, but expands the heat-affected zone, and the valve body 3 may experience significant thermal deformation, requiring strict control of the cooling rate. At the same time, high-power heating requires more precise temperature control, otherwise overheating is likely. The rough machining allowance of 0.3 mm is beneficial for subsequent correction of thermal deformation.

[0037] Example 3:

[0038] The difference between Example 3 and Example 1 is as follows: Hard alloy welding wire (48% cobalt content) is used for surfacing, with a current of 120A, an argon flow rate of 12 L / min, an interpass temperature ≤150℃, and a surfacing thickness 1.3 times the thickness of the finished ring; the gap between the sealing ring 1 and the sidewall of the sealing ring groove 2 is 0.25 mm, the groove depth is 0.15 mm greater than the ring thickness, and the transition radius R is 0.75 mm; the flux coating thickness is approximately 0.4 mm, and the water-to-powder ratio is the same as before; the heating frequency is 35 kHz, the power is 18 kW, and the set temperature is 75℃ higher than the melting point of the brazing filler metal (if the melting point of the brazing filler metal is 635℃, then heat to 710℃); silver-based brazing wire (melting point 635℃) is used; a roughing allowance of 0.25 mm is left, and the surface roughness Ra ≤ 6.3 μm.

[0039] The specific steps of Example 3 are as follows:

[0040] Step 1: Preparation of Sealing Ring 1. A long strip of cemented carbide round bar is surfacing using argon arc welding with cemented carbide welding wire (48% cobalt content). DC argon arc welding is used, with a welding current of 120 A, an argon flow rate of 12 L / min, and an interpass temperature controlled at ≤150 ℃. The surfacing thickness is no less than 1.3 times the thickness of the finished ring. Then, it is machined to the required dimensions of Sealing Ring 1. Step 2: Penetrant Testing. A penetrant is sprayed onto the surface of Sealing Ring 1 from Step 1 and left for at least 15 minutes. The penetrant is then wiped off, and a colorant is sprayed onto the surface of Sealing Ring 1. The surface quality is checked to ensure there are no defects. Step 3: Machining Sealing Ring Groove 2. A Sealing Ring Groove 2 for placing Sealing Ring 1 is machined on the valve body 3. The inner gap of Sealing Ring Groove 2 is 0.25 mm, and the groove depth is 0.15 mm greater than the ring thickness. The transition radius between the sidewall and bottom surface of Sealing Ring Groove 2 is R0.75. mm; Step 4: Cleaning the workpiece. Immerse the surface of the sealing ring 1 in an organic solvent (thinner) for 10 minutes, then remove and air dry to remove oil, metal shavings, and residual coolant; Step 5: Applying flux. Use powdered silver-based brazing flux FB105 type borax-based flux, mix with distilled water to form a paste (water-to-powder ratio approximately 1:2), and use a small stainless steel scraper or special brush to evenly fill the bottom and sidewalls of the sealing ring groove 2 with the paste flux, with a coating thickness of approximately 0.4 mm, ensuring no missed areas or accumulation; then place the cleaned sealing ring 1 in the sealing ring groove 2, ensuring that the sealing ring 1 is in close contact with the inner wall of the sealing ring groove 2; Step 6: Heating. Use a medium-high frequency induction heater with a frequency of 35 kHz and a power of 18 kW, setting the heating temperature to be higher than the melting point of the brazing filler metal by 75 ℃ (if the melting point of the brazing filler metal is 635 ℃, then heat to 710 ℃). Step 7: Fill with brazing wire. After the valve body 3 temperature rises to the welding temperature, immediately fill with silver-based brazing wire (melting point 635 ℃) manually until the wire melts and fills the gap. Step 8: Rough machining inspection. After the valve body 3 cools down, rough machine the sealing surface with a lathe to remove excess brazing material and oxide scale, leaving a finishing allowance of 0.25 mm and a surface roughness Ra≤6.3 μm. Repeat the penetration test in Step 2. Step 9: Finishing inspection. Machin the remaining dimensions of the valve body 3 according to the drawings and repeat the penetration test in Step 2. Step 10: Water pressure test. After the valve is fully assembled, perform a sealing pressure test. If there is no leakage, it is qualified.

[0041] In this embodiment, a welding method is used to ensure material utilization, while increasing the welding current (120 A) makes the hardness of the cemented carbide layer closer to the upper limit (approximately HRC 42), resulting in excellent wear resistance. The 0.25mm gap and fillet radius (R0.75) achieve a balance between capillary filling efficiency and assembly tolerance, preventing both clogging and incomplete filling. The heating temperature of 710℃ makes the heat-affected zone controllable, with deformation between that of Embodiments 1 and 2. With moderate frequency and power, stable heating efficiency, and easy matching of infrared thermometry, this solution has low dependence on operator proficiency, a wide process window, a high finished product qualification rate, and the most balanced comprehensive performance (strength, wear resistance, dimensional accuracy), making it suitable for the mass production of most small-diameter gate valves.

[0042] Example 4:

[0043] Step 1: Use hard alloy welding wire (45% cobalt content) for argon arc welding, current 80A, argon flow rate 8 L / min, interpass temperature ≤150℃, weld thickness is 1.2 times the thickness of the finished ring, to process into sealing ring 1; Step 2: Penetrant testing, spray penetrant on the surface of sealing ring 1 from step 1 and keep it for more than 15 minutes, wipe off the surface penetrant, then spray colorant on the surface of sealing ring 1, check the surface quality to ensure that the surface is free of defects; Step 3: Machining sealing ring groove 2, machining sealing ring groove 2 on valve body 3, the gap between the outer ring side of sealing ring 1 and the groove sidewall is 0.25mm, the groove depth is 0.15mm greater than the ring thickness, and the transition radius R0.75mm. Machining an annular storage groove at the bottom of the groove, 0.8mm wide and 0.3mm deep; machining 4 blind exhaust micro-grooves at the bottom of the groove, 0.15mm wide and 0.12mm deep, evenly distributed along the circumference, not penetrating the valve body wall. The total volume of the brazing groove is 1.5 times the gap volume; Step 4: Clean the workpiece, use thinner, soak and clean for 5 minutes, then take it out and let it dry; Step 5: The gap in the sealing ring groove 2 is 0.2 mm, the groove depth is 0.1 mm larger than the ring thickness, and the transition radius R is 0.5 mm; the flux (FB105, water-to-powder ratio 1:2) is applied with a thickness of about 0.3 mm; Step 6: Medium and high frequency induction heating, frequency 50 kHz, power 10 kW, set the temperature 50 ℃ higher than the melting point of the brazing filler metal, the melting point of the brazing filler metal is 620 ℃, then heat to 670 ℃; Step 7: Fill with silver-based brazing wire (raise the temperature of valve body 3 to the melting point 620 ℃); Step 8: Rough machining with a allowance of 0.2 mm, roughness Ra≤6.3 μm; Step 9: Finish machining and inspection, machine the remaining dimensions of valve body 3 according to the drawing, repeat step 2 penetration inspection; Step 10: Water pressure test, complete the overall assembly of the valve, and then perform a sealing pressure test, no leakage is acceptable.

[0044] The difference between this embodiment and Embodiment 1 lies in the fact that this embodiment has an annular brazing filler groove and multiple blind venting micro-grooves at the bottom of the sealing ring groove 2. The annular brazing filler groove can pre-store sufficient brazing filler metal. The advantage of this structural design is that the annular brazing filler groove can store excess brazing filler metal, and can continuously replenish brazing filler metal to the mating gap during brazing, avoiding gap shortage caused by brazing filler metal cooling and shrinkage, and ensuring that the brazing seam is always filled with sufficient brazing filler metal. The blind venting micro-grooves can smoothly expel the air accumulated inside the gap during the process of brazing filler metal filling the gap, avoiding the formation of brazing defects such as pores and looseness caused by air blocking inside the gap, and further improving the tightness of the brazing seam. At the same time, because the venting micro-grooves are blind grooves that do not penetrate the valve body wall, they will not have an adverse effect on the overall pressure bearing capacity and structural strength of the valve body 3.

[0045] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A welding process for the sealing surface of a small-diameter valve, characterized in that: The process includes the following steps: Step 1: Preparation of the sealing ring. Hard alloy welding wire is used to weld the ring into a long strip of hard alloy round bar using argon arc welding, or Stellite hard alloy bar material is used directly, and then processed into the required sealing ring size. Step 2: Penetrant testing. A penetrant is sprayed onto the surface of the sealing ring from Step 1 and left for at least 15 minutes. The penetrant is then wiped off, and a colorant is sprayed onto the surface of the sealing ring. The surface quality is checked to ensure there are no defects. Step 3: Machining the sealing ring groove. A sealing ring groove for placing the sealing ring is machined on the valve body. The bottom of the sealing ring groove also has an annular storage groove with a depth of 0.2~0.5mm and a width of 0.5~1.2mm. At least two blind venting micro-grooves are also provided at the bottom or sidewall of the sealing ring groove. The venting micro-grooves have a width of 0.1~0.2mm and a depth of 0.1~0.15mm, are evenly distributed along the circumference, and do not penetrate the valve body wall. The total volume of the annular brazing groove is 1.2 to 2.0 times the volume of the gap between the outer ring side of the sealing ring and the side wall of the sealing ring groove; Step 4: Cleaning the workpiece, using organic solvent to clean the surface of the sealing ring; Step 5: Applying flux, applying flux to the inside of the sealing ring groove, and placing the cleaned sealing ring in the sealing ring groove, so that the sealing ring is in close contact with the inner wall of the sealing ring groove; Step 6: Heating, heating the valve body to 50-100℃ above the melting point of the brazing filler metal; Step 7: Filling brazing wire, immediately filling the brazing wire manually after the valve body temperature rises to a welding temperature 50-100℃ above the melting point of the brazing filler metal, visually until the wire melts and fills the gap; Step 8: Rough machining inspection, after the valve body cools, rough machining is performed on the sealing surface, and the penetration inspection in Step 2 is repeated; Step 9: Fine machining inspection, machining the remaining dimensions of the valve body according to the drawings, and repeating the penetration inspection in Step 2; Step 10: Water pressure test, after completing the overall assembly of the valve, the sealing surface is pressure tested, and it is qualified if there is no leakage.

2. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: After the sealing ring is placed in the sealing ring groove, a gap is formed between the outer ring side of the sealing ring and the side wall of the sealing ring groove. The size of the gap is 0.2-0.3 mm. The depth of the sealing ring groove is greater than the thickness of the sealing ring by 0.1-0.2 mm. A transition fillet is formed between the side wall of the sealing ring groove and the bottom surface. The transition fillet is R0.5~R1.0 mm.

3. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: The cemented carbide welding wire contains more than 44% cobalt, and the hardness requirement after welding is HRC35-42. The flux is a silver brazing solvent, and the brazing wire is a silver-based brazing wire with a melting point of 620℃-650℃.

4. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: In step six, a medium-high frequency induction heater is used with a frequency of 20~50kHz and a power of 10~25kW; the heating temperature is set to be 60~90℃ higher than the melting point of the brazing filler metal; and an infrared thermometer is used to continuously monitor the temperature at the bottom of the valve body groove.

5. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: In step four, thinner is used as the organic solvent. After soaking and cleaning for 5-10 minutes, the ring is taken out and dried to remove oil, metal shavings and residual processing coolant from the surface of the sealing ring, ensuring that the surface of the sealing ring is clean and free of impurities.

6. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: In step one, the diameter of the Stellite cemented carbide bar is reserved with a machining allowance of 3~5mm according to the size of the finished ring; DC argon arc welding is used, with a welding current of 80~120A, an argon flow rate of 8~12 L / min, an interpass temperature controlled at ≤150℃, and a weld thickness of not less than 1.2 times the thickness of the finished ring.

7. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: In step eight, the sealing surface is rough-machined on a lathe to remove excess brazing filler metal and oxide scale, leaving a finishing allowance of 0.2~0.3mm and a surface roughness Ra≤6.3μm.

8. The welding process for the sealing surface of a small-diameter valve according to claim 1, characterized in that: In step five, powdered silver-based soldering flux FB105 type borax-based flux is selected. Before use, it is mixed with distilled water to form a paste with a water-to-powder ratio of about 1:

2. Then, a small stainless steel scraper or a special brush is used to evenly fill the bottom and sidewalls of the groove with the flux paste. The coating thickness is about 0.3~0.5mm, ensuring no missed areas or accumulation.