Method and apparatus for improving radial non-uniformity of dissimilar metal inertial friction welding joints

By preparing an arc filler wire intermediate layer and knurling pretreatment during inertial friction welding, the radial non-uniformity problem of aluminum/steel dissimilar metal inertial friction welded joints is solved, and the radial uniformity and mechanical properties of the joints are improved, making it suitable for aerospace launch vehicle piping systems.

CN123103233APending Publication Date: 2026-11-17DALIAN UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611627909.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In aerospace launch vehicle piping systems, aluminum/steel dissimilar metal inertial friction welds suffer from radial microstructure and performance inhomogeneity, resulting in insufficient reliability of the joints and making it difficult to meet the requirements of high-density mass production.

Method used

By preparing an arc-filled additive intermediate layer during inertial friction welding, combined with knurling pretreatment and irregular end face design, the radial non-uniformity of the friction welded joint is optimized. The filler wire additive process is carried out simultaneously on the inertial friction welding machine using arc welding equipment to prepare a 2-5 mm thick copper-based intermediate layer. Combined with the friction upsetting process, the interface metallurgical behavior can be controlled.

Benefits of technology

It improves the radial uniformity of dissimilar metal inertial friction welding joints, enhances the mechanical properties of the joints, and solves defects such as excessive flash, uneven interface formation, and incomplete root fusion that exist in traditional processes, thereby improving production efficiency and joint reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103233A_ABST
    Figure CN123103233A_ABST
Patent Text Reader

Abstract

This invention provides a method and apparatus for improving radial non-uniformity in dissimilar metal inertial friction welding joints, relating to the field of precision machining technology for aerospace equipment. This invention abandons the traditional direct butt welding approach and innovatively introduces a pre-treatment process of pre-forming a gradient intermediate layer using arc-filled wire: A transition alloy wire with metallurgical compatibility matching the base materials on both sides is deposited onto the hard metal end faces to be welded using arc welding. By controlling the arc current, welding voltage, and wire feed speed, an intermediate layer with a thickness of 2-5 mm and a gradient hardness is prepared, effectively reducing the initial hardness difference between the two end faces to be welded. This improves the radial uniformity of frictional heat input during inertial friction welding from the source, suppresses the non-uniform precipitation of harmful intermetallic compounds at the interface, and ultimately reduces the radial mechanical property deviation of the dissimilar welded joint, improves the tensile strength of the joint, and meets the high reliability service requirements of aerospace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of precision machining technology for aerospace equipment, and more particularly to a method and apparatus for improving radial non-uniformity of dissimilar metal inertial friction welded joints. Background Technology

[0002] In the manufacturing of aerospace launch vehicle piping systems, the connection of dissimilar metals such as aluminum and steel has long relied on traditional brazing processes. This process requires the use of brazing filler metal to join the two metals, involves numerous steps, has a long production cycle, and suffers from risks such as corrosion due to moisture from chlorine-containing flux and insufficient reliability of the joints during service. It is no longer suitable for the current high-density mass production requirements of aerospace equipment. As the requirements for lightweight and highly reliable connections in aerospace equipment continue to increase, inertial friction welding, as a solid-state joining technology, is gradually becoming an alternative. This technology uses high-speed rotating friction to generate heat, bringing the materials at the interface to be welded into a plastic state. Under the action of upsetting force, a direct solid-state bond is achieved between the base materials, fundamentally avoiding the metallurgical defects caused by the large differences in melting points and thermophysical properties between aluminum and steel during the fusion welding process.

[0003] However, during the engineering application process, it was discovered that inertial friction welding resulted in dissimilar metal joints with significant differences in hardness and softness, exhibiting radial microstructure and performance inhomogeneity at the interface. This has become a core bottleneck restricting the large-scale implementation of this technology, leading to a continuous increase in the demand for technological iterations related to process optimization and structural improvement. Currently, relevant patents in the industry for aluminum / steel dissimilar metal inertial friction welding are gradually focusing on radial uniformity control. One patent (CN115026409B) proposes a two-step radial friction welding scheme for aluminum / steel dissimilar alloys. By pre-welding a Cu transition layer on the steel side before completing the aluminum alloy layer connection, the formation of hard and brittle Fe-Al intermetallic compounds can be effectively controlled, while reducing welding residual stress. This provides a new approach to transition layer design for optimizing the interface uniformity of aluminum-steel inertial friction welding. The emergence of this type of patented technology breaks the previous limitation that aluminum-steel friction welding could only achieve small-scale sample connections, gradually promoting the transition of this technology to engineering-grade product applications. However, the aforementioned patent adds a step before aluminum / steel inertial friction welding: first, a copper intermediate layer is prepared on the end face of the steel base material through a first inertial friction welding operation, and then the copper layer is connected to the aluminum base material through a second inertial friction welding operation. This increases the complexity of the aluminum / steel dissimilar metal inertial friction welding process and the probability of operational errors during industrialization. In contrast, this invention uses an external arc welding device to complete the preparation of the intermediate layer during the inertial friction welding process of dissimilar metals with large differences in hardness, eliminating the need for additional steps. This ensures the directness of the overall inertial friction welding process for dissimilar metals with large differences in hardness, facilitating industrialization. This method is not disclosed in the aforementioned patent. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a method and apparatus for improving the radial non-uniformity of dissimilar metal friction fusion welded joints. The invention primarily improves the radial non-uniformity of soft / hard dissimilar metal friction fusion welded joints and enhances the uniformity of the joint's mechanical properties by preparing an intermediate layer on the end face during the friction fusion welding process. Simultaneously, the soft / hard dissimilar metal rod-shaped base material undergoes simple processing before welding, ensuring a straight soft / hard dissimilar metal friction fusion welding interface under the reduced radial non-uniformity. Through this design, a soft / hard dissimilar metal friction fusion welded joint with superior radial uniformity is obtained, improving mechanical properties and resolving defects in current processes such as excessive flash, uneven interface formation, and incomplete root fusion caused by severe radial non-uniformity.

[0005] The technical means employed in this invention are as follows: A method for improving radial non-uniformity in dissimilar metal inertial friction welded joints includes the following steps: S1. Prepare the workpiece to be welded. The workpiece to be welded is a cylindrical base material of dissimilar metals with large differences in hardness, including a hard base material and a soft base material with a hardness difference. The end of the hard base material to be welded is a convex platform with a frustum-shaped protrusion. The end of the soft base material to be welded is a concave platform with a frustum-shaped pit inside. The end face of the hard base material to be welded is the front face of the convex platform. The end face of the soft base material to be welded is the bottom face of the pit. S2. Use a knurling machine to knurl the end face of the hard base material to be welded, so that its surface forms a uniformly distributed groove morphology. S3. Place the inertial friction welding machine and the arc welding equipment on the lathe, and clamp the hard base material and the soft base material in the corresponding tooling positions of the inertial friction welding machine respectively. S4. When the flywheel of the inertial friction welding machine enters the initial acceleration moment of the motor, the speed is 2-200 rpm, and it begins to store energy and drive the hard base material to rotate. Simultaneously, the arc welding equipment is started to carry out the filler wire additive process. Under certain welding parameters such as welding current, welding voltage, and wire feeding speed, filler wire additive deposition is carried out on the weldable end face of the hard base material with pre-made concave and convex groove morphology to prepare an intermediate layer with a thickness of 2-5 mm. The filler wire additive process continues to run until the energy storage stage of the flywheel is completely terminated and the flywheel speed reaches 500-3000 rpm. S5. After the energy storage phase is completely terminated and the filler wire additive manufacturing process is completed, the wire feeding device is immediately stopped, and the wire feeding device is removed from the work area. The arc ignition state of the electric arc welding equipment is maintained throughout the process without interruption, and the welding current is the same as the welding current in S4. At the same time, the traveling mechanism of the inertial friction welding machine is started to feed axially, driving the soft base material and the hard base material to gradually approach and contact each other, entering the friction upsetting process. First, friction heat is generated under a certain axial force. After the flywheel speed drops to zero, the upsetting and holding pressure process is carried out, thereby completing the welding of the hard base material and the soft base material, and obtaining the finished workpiece. The welded end face of the hard base material and the welded end face of the soft base material form a joint. During the entire upsetting pressure cycle, the electric arc welding equipment continuously outputs a low current to maintain arc stability until the flywheel speed drops to zero and comes to a complete stop, and then the arc extinguishing operation is performed. S6. After the friction upsetting process is completed and the joint is completely cooled to the temperature range allowed by the process, the finished workpiece is removed from the inertial friction welding machine to obtain an inertial friction welded joint of dissimilar metals with large differences in softness and hardness after improving the non-uniformity.

[0006] Furthermore, in S1, the hard base material is made of steel, titanium, or copper, and the soft base material is made of aluminum or magnesium. The hardness difference between the hard and soft base materials is 50-150 HV. The platform height of the convex platform morphology is 1-5 mm, and the diameter of the front end face of the convex platform morphology is 10-40 mm. The platform depth of the concave platform morphology is 1-5 mm, and the diameter of the bottom surface of the pit is 10-40 mm.

[0007] Furthermore, in step S2, during the knurling process, the hard base material is clamped onto the clamping device of the knurling machine. After the coaxiality and locking tightness are checked, the rolling mechanism of the knurling machine is driven to process a regular concave-convex groove shape on the end face of the hard base material to be welded. The depth of the concave-convex groove shape is 1-5mm, and the concave-convex groove shape is a quadrangular frustum groove with a spacing of 1-3mm, or a quadrangular pyramidal groove with no spacing or a spacing of 1-3mm, or a straight groove with a spacing of 1-3mm.

[0008] Furthermore, in S3, during the entire time-series operation cycle of inertial friction welding, all moving parts of the arc welding equipment do not have spatial interference with the overall mechanical structure of the inertial friction welding machine, and there is no physical collision; wherein the welding power source of the arc welding equipment is arranged outside the safe operating distance of the inertial friction welding machine, and the welding tungsten electrode, wire feeding device and wire filler of the arc welding equipment are all arranged in an upper position, approaching the welding operation position of the inertial friction welding machine from the vertical upward direction.

[0009] Furthermore, in S3, the hard base material is clamped in the flywheel fixture station of the inertial friction welding machine, and the end face of the hard base material to be welded is located in the working area directly below the tungsten electrode for welding; the soft base material is clamped in the fixed side clamping end of the inertial friction welding machine.

[0010] Furthermore, in S4, an electric arc is generated by a welding power source and a tungsten electrode for welding. The heat from the electric arc evenly covers the weldable end face area of ​​the hard base material. The welding current parameter is set to the lowest feasible value under the premise of meeting the melting conditions of the wire filler. The wire filler is fed to the weldable end face of the hard base material through a wire feeding device. The wire feeding device is triggered and started after the electric arc establishes a stable combustion state. The feed speed of the wire filler is dynamically matched and linked with the real-time rotation speed of the flywheel. The welding current of the arc welding equipment is 40-70A, the welding voltage is 5-10V, and the wire feeding speed is 0.05-0.2m / min.

[0011] Furthermore, in S5, after the wire filler completely and evenly covers the weldable end face of the hard base material, the power output of the wire feeding device is immediately shut off and it is moved to a safe avoidance position. The welding power supply is kept in a live output state throughout the process. By maintaining a preset low current arc, a directional heat source is supplemented to the central area of ​​the interface of the inertial friction welding during the entire upsetting process to compensate for the radial distribution difference of friction heat generation. The soft base material is slowly brought into contact with the hard base material by low-speed axial feeding through the walking mechanism, and then enters the friction upsetting process under continuous arc heating. After the friction upsetting process is completely completed, the output of the welding power supply is cut off to extinguish the arc.

[0012] Furthermore, in S5, the friction pressure of the friction upsetting process is 20-200 MPa, and the upsetting pressure is 50-400 MPa.

[0013] Furthermore, in step S6, after the workpiece has been air-cooled to room temperature, the finished workpiece is removed from the tooling station of the inertial friction welding machine.

[0014] The present invention also provides an apparatus for improving the radial non-uniformity of dissimilar metal inertial friction welded joints, and the method for implementing the above-mentioned method for improving the radial non-uniformity of dissimilar metal inertial friction welded joints includes: lathe; A knurling machine, mounted on a lathe, includes a clamping device and a rolling mechanism. The clamping device is used to clamp a hard base material, and the rolling mechanism is used to knurl the end face of the hard base material to be welded before welding. An inertial friction welding machine, mounted on a lathe, includes a motor, a spindle, a flywheel, a fixture, a traveling mechanism, and a fixed-side clamping end. The output end of the motor is connected to the input end of the spindle via a clutch. The flywheel is coaxially connected to the spindle and stores rotational kinetic energy during motor acceleration, releasing this energy during welding to complete the welding process. The fixture is fixedly connected to the flywheel and is used to clamp the knurled hard base material. The fixed-side clamping end faces the fixture and is used to clamp the soft base material. The traveling mechanism is connected to the fixed-side clamping end and drives it to axially feed the soft base material. An electric arc welding device, mounted on a lathe, is a filler wire electric arc TIG welding device, comprising a welding power source, a welding tungsten electrode, a wire feeding device, and filler wire. The welding power source is electrically connected to the welding tungsten electrode and the wire feeding device. The welding tungsten electrode is located directly above the end face of the hard base material to be welded, and the wire feeding device is located above the hard base material to push the filler wire to the end face of the hard base material to be welded.

[0015] Compared with the prior art, the present invention has the following advantages: This invention addresses the long-standing challenge of uneven radial microstructure and properties in the development process of inertial friction welding of dissimilar metals with significant differences in hardness. It deeply couples arc-filled wire additive manufacturing, workpiece end-face knurling pretreatment, and the design of irregular end-face configurations for dissimilar metals with significant differences in hardness with the acceleration and energy storage timing of the flywheel motor in inertial friction welding. Without changing the core framework of solid-state welding in traditional inertial friction welding, it overcomes the inherent technical bottlenecks of asynchronous frictional heat generation and uncoordinated plastic flow in dissimilar materials through multi-dimensional synergistic effects of interface pre-configuration control, transition layer composition design, and thermal field timing optimization. This provides a new technical path for the high-consistency manufacturing of dissimilar metal joints in aerospace vehicle pipelines.

[0016] First, it achieves efficient and coordinated integration of process timing, significantly improving the compactness of the manufacturing process. This invention fully embeds the process of preparing the copper-based intermediate layer using arc-filled wire additive manufacturing into the acceleration and energy storage range of the flywheel motor in inertial friction welding. Within the time window when the flywheel rises from rest to the preset welding speed, the deposition of the copper-based transition layer on the knurled end face of the hard base material is completed simultaneously. There is no need to set up an additional independent transition layer preparation station, which avoids the process redundancy and pollution emission problems caused by traditional electroplating and thermal spraying transition layer processes. Furthermore, it can rely on the centrifugal effect of the flywheel rotation to achieve uniform radial spreading of copper-based droplets on the steel end face, ensuring the radial consistency of the transition layer thickness from a timing perspective and improving overall production efficiency.

[0017] Secondly, the irregular end-face configuration optimizes the uniformity of frictional heat generation and plastic flow from a physical perspective. This invention processes the aluminum base material welding end into a concave configuration and the steel base material welding end into a convex configuration. This allows for full radial surface contact in the initial stage of friction welding, completely changing the heat imbalance problem of traditional flat-end friction welding where heat generation is only generated in the edge region during the initial stage. It reduces the difference in frictional heat input at different radial positions on the interface and guides the synchronous radial flow of plastic material on both sides. This avoids the defects of excessive material extrusion in the edge region and insufficient plastic deformation in the central region in traditional flat-end processes, fundamentally weakening the radial plastic deformation gradient.

[0018] Third, the knurled-arc filler wire composite transition layer enables the control of interfacial metallurgical behavior. The knurled texture pre-prepared on the steel end face can form a mechanical interlocking structure with the copper-based material deposited by the arc filler wire, which greatly improves the interfacial bonding strength between the transition layer and the hard base material, avoiding the risk of detachment failure of traditional planar transition layers under high-speed friction and shearing.

[0019] Fourth, multi-dimensional synergistic regulation significantly improves the consistency of radial performance of the joint. Through the triple effects of thermal field pre-compensation, plastic flow guidance, and metallurgical reaction restriction, it has extremely strong engineering adaptability.

[0020] Based on the above reasons, this invention can be widely promoted in fields such as automobile manufacturing, petrochemical power, heat exchange equipment, and aerospace. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 This is a radial cross-sectional view of the rigid base material and the soft base material in this invention, where (a) is the rigid base material and (b) is the soft base material.

[0023] Figure 2 This is a schematic diagram of the preparation of end face grooves on an end face knurling machine in the present invention using a rigid base material.

[0024] Figure 3 Examples of end face morphology of the hard rod-shaped base material after the knurling process in this invention are shown, wherein (a) is a frustum-shaped groove, (b) is a pyramidal groove, and (c) is a straight groove.

[0025] Figure 4 This is a schematic diagram of the preparation stage of the intermediate layer in the inertial friction welding of dissimilar metals with large differences in hardness and softness assisted by arc filler wire in this invention.

[0026] Figure 5 This is a schematic diagram of the upsetting stage of inertial friction welding of dissimilar metals with large differences in softness / hardness assisted by arc filler wire in this invention.

[0027] Figure 6 This is a schematic diagram of the arc welding equipment in this invention.

[0028] In the diagram: 1. Hard base material; 2. Soft base material; 3. Knurling machine; 301. Clamping device; 302. Rolling mechanism; 4. Inertial friction welding machine; 401. Flywheel; 402. Traveling mechanism; 403. Fixed side clamping end; 5. Arc welding equipment; 501. Welding power source; 502. Tungsten electrode for welding; 503. Wire feeding device; 504. Wire filler. Detailed Implementation

[0029] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0030] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0032] Unless otherwise specifically stated, the relative arrangement, numerical expressions, and values ​​of the components and steps described in these embodiments do not limit the scope of the invention. It should also be understood that, for ease of description, the dimensions of the various parts shown in the drawings are not drawn to actual scale. Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of the specification. In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters in the following figures denote similar items; therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.

[0033] In the description of this invention, it should be understood that the orientation or positional relationship indicated by directional terms such as "front, back, up, down, left, right", "horizontal, vertical, horizontal" and "top, bottom" is generally based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing this invention and simplifying the description. Unless otherwise stated, these directional terms do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on the scope of protection of this invention. The directional terms "inner" and "outer" refer to the inner and outer contours relative to the outline of each component itself.

[0034] For ease of description, spatial relative terms such as "above," "on top of," "on the upper surface of," "above," etc., are used herein to describe the spatial positional relationship of a device or feature as shown in the figures to other devices or features. It should be understood that spatial relative terms are intended to encompass different orientations in use or operation beyond the orientation of the device as described in the figures. For example, if the device in the figures were inverted, a device described as "above" or "on top of" other devices or structures would subsequently be positioned as "below" or "under" other devices or structures. Thus, the exemplary term "above" can include both "above" and "below." The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used herein will be interpreted accordingly.

[0035] Furthermore, it should be noted that the use of terms such as "first" and "second" to define components is merely for the purpose of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore should not be construed as limiting the scope of protection of this invention.

[0036] Traditional inertial friction welding relies on the rotational kinetic energy stored in a flywheel to drive the workpiece to rotate relative to each other. It utilizes interfacial frictional heat to raise the temperature of the area to be welded to a plastic state, and then applies axial upsetting force to complete the solid-state connection between the base materials. While this method has advantages such as short welding cycles and high degree of joint microstructure refinement, the radial inhomogeneity caused by the difference in hardness between dissimilar base metals is a core common problem restricting the consistency of joint performance. This inhomogeneity stems from the asymmetric distribution of interfacial thermal-mechanical-material behavior throughout the welding process. In the flywheel-driven frictional heat generation stage, the linear velocity of the interface to be welded exhibits a linear gradient distribution along the radial direction, with the linear velocity in the edge region being much higher than that in the center region. This results in significant differences in frictional heat input at different locations on the interface. The material in the edge region enters a fully thermoplastic state first, while the heat accumulation rate in the center region lags behind, resulting in insufficient plastic deformation. This creates a gradient difference between the temperature field and the plastic field along the radial direction. During the subsequent upsetting and holding stage, the differences in rheological resistance in different regions of the interface are further amplified. Under the action of axial upsetting force, a large amount of plasticized material in the edge region is extruded outward to form excessive flash. The material in the central region is constrained by the surrounding insufficiently plasticized matrix and cannot complete sufficient atomic diffusion and dynamic recrystallization. Ultimately, this results in obvious non-uniform characteristics in the thickness of the intermetallic compound layer, the size of the recrystallized grains, and the distribution of residual stress at different radial positions of the joint. This not only causes micro-defects such as local hard and brittle phase aggregation and insufficient bonding, but also directly causes high dispersion of the radial mechanical properties of the joint. Under alternating load service scenarios, fatigue cracks are prone to initiation from the weak central region, which greatly reduces the service reliability and service life of dissimilar metal joints.

[0037] Therefore, this invention provides a method and apparatus for improving the radial non-uniformity of dissimilar metal inertial friction welding joints, specifically a method and apparatus for improving the radial non-uniformity of soft / hard dissimilar metal inertial friction welding joints. It is a method and apparatus for improving joint strength in low-power laser-assisted small-diameter titanium / steel dissimilar metal inertial friction welding, involving a soft / hard large-difference dissimilar metal inertial friction welding process. This improves the radial non-uniformity generated during the welding process by preparing an intermediate layer using arc filler wire. It can be widely applied to various industrial scenarios such as the manufacturing of lightweight dissimilar components in automobiles, dissimilar shaft connections in petrochemical and power industries, welding of dissimilar tube sheets in high-efficiency heat exchange equipment, and high-precision forming of key rotating components in aerospace.

[0038] Addressing the common industry challenges of uneven radial distribution of frictional heat generation, asynchronous plastic flow of interfacial materials, and significant radial non-uniformity of weld microstructure during inertial friction welding of dissimilar metals with large differences in hardness / softness, this invention abandons the traditional direct butt welding approach and innovatively introduces a pre-treatment process of pre-forming a gradient intermediate layer using arc filler wire. On the hard side of the metal to be welded, a transition alloy wire with metallurgical compatibility matching the base materials on both sides is deposited using arc fusion. By controlling the arc current to 40-70A and the wire feed speed to 0.05-0.2m / min, an intermediate layer with a thickness of 2-5mm and a gradient hardness (gradient transition means the hardness of the intermediate layer is higher than that of the hard base material but lower than that of the soft base material) is prepared. This effectively reduces the initial hardness difference between the two sides of the welded end face, improves the radial uniformity of frictional heat input during inertial friction welding from the source, suppresses the non-uniform precipitation of harmful intermetallic compounds at the interface, and ultimately reduces the radial mechanical property deviation of the dissimilar weld joint, improves the tensile strength of the joint, and meets the high reliability service requirements of aerospace.

[0039] The present invention provides a method for improving radial non-uniformity in dissimilar metal inertial friction welding joints, comprising the following steps: S1. Prepare the workpieces to be welded. The workpieces are cylindrical base materials of dissimilar metals with significant differences in hardness and softness (diameter 1-50mm), including hard base material 1 and soft base material 2. The weldable end of hard base material 1 has a convex platform shape resembling a frustum. The weldable end face of hard base material 1 is the front face of the convex platform shape. The platform height is 1-5mm, and the diameter of the front face of the convex platform shape (i.e., the diameter of the weldable end face of hard base material 1, referring to the diameter of the upper surface of the convex platform shape, i.e., the smallest outer diameter on the convex platform shape) is 10-40mm. The weldable end of soft base material 2 has an internal frustum shape. The concave platform morphology of the pit is as follows: the welding end face of the soft base material 2 is the bottom surface of the pit; the platform depth of the concave platform morphology is 1-5mm; the diameter of the bottom surface of the pit (i.e., the diameter of the welding end face of the soft base material 2, referring to the diameter of the lower surface of the concave platform morphology, i.e., the smallest inner diameter on the concave platform morphology) is 10-40mm; the material of the hard base material 1 is steel, titanium or copper; the material of the soft base material 2 is aluminum or magnesium; then the dissimilar metal base materials with large differences in softness / hardness are aluminum / steel, aluminum / titanium, aluminum / copper, magnesium / steel, magnesium / titanium, magnesium / copper metal combinations; the hardness difference between the hard base material 1 and the soft base material 2 is 50-150HV. S2. During the pre-welding processing, an end-face knurling machine is used. The knurling machine 3, mounted on a lathe, knurls the end face (front face of the boss) of the hard base material 1 to be welded, creating a uniformly distributed groove morphology with a depth of 1-5mm. The groove morphology includes frustum-shaped grooves spaced 1-3mm apart, pyramidal grooves with no spacing or a spacing of 1-3mm, or straight grooves spaced 1-3mm apart. Specifically, such as... Figure 3As shown in (a), several frustum-shaped grooves are machined, with a spacing of 1-3 mm between two adjacent frustum-shaped grooves; Figure 3 As shown in (b), several pyramidal grooves are machined, with no spacing between the pyramidal grooves; as Figure 3 As shown in (c), several straight grooves are machined, and the spacing between the straight grooves is 1-3mm.

[0040] S3. The inertial friction welding equipment uses an inertial friction welding machine 4. The arc filling process uses a low current process (only melting the welding wire and not the hard base material). The wire material is copper-based, nickel-based, or aluminum-based. After completing the workstation layout plan, the inertial friction welding machine 4 and the arc welding equipment 5 are placed in designated workstations that meet the requirements of process flow and safety distance, with a safety distance of 1-2m. Then, the hard base material 1 with an outwardly convex platform shape and the soft base material 2 with an inwardly concave platform shape are respectively clamped and fixed to the corresponding tooling workstations of the inertial friction welding machine 4.

[0041] S4. When the flywheel 401 of the inertial friction welding machine 4 enters the initial acceleration phase of the motor, its speed is 2-200 rpm, and it begins to store energy, driving the hard base material 1 to rotate; simultaneously, the arc welding equipment 5 is triggered to start the filler wire additive process, with a welding current of 40-70A, a welding voltage of 5-10V, and a wire feeding speed of 0.05-0.2m / min (this set of welding parameters is to control the welding heat input, ensuring that only the filler wire is melted, and the hard base material 1 is not melted). Filler additive deposition is performed on the weldable end face of the hard base material 1 with concave and convex groove morphology to prepare a functional intermediate layer with a thickness of 2-5 mm (if the thickness of the intermediate layer is too thin, the filled intermediate layer will be completely extruded during the upsetting process; at the same time, the arc position is fixed when preparing the intermediate layer, making it difficult to prepare an excessively thick intermediate layer, so the thickness is limited to 2-5 mm). This filler additive process continues until the energy storage stage of the flywheel 401 is completely terminated, during which the speed of the flywheel 401 reaches 500-3000 rpm.

[0042] S5. After the energy storage phase is completely terminated and the filler wire additive manufacturing process is completed, immediately stop the wire feeding action of the wire feeding device 503 and remove the wire feeding device 503 from the work area at a safe distance of 1-2m. Maintain the arc ignition state of the arc welding equipment 5 throughout the process without interruption, and keep the current at 40-70A. At the same time, trigger the traveling mechanism 402 of the inertial friction welding machine 4 to start axial feeding at a speed of 5-50mm / s, driving the soft base material 2 and the hard base material 1 to gradually approach and contact each other, entering the friction upsetting process. The friction pressure is 20-200MPa, and the upsetting pressure is 50 MPa. At a pressure of -400MPa, frictional heating is first generated under a certain axial force. After the speed of flywheel 401 drops to zero, an upsetting and holding pressure process is performed to complete the welding of the hard base material 1 and the soft base material 2, resulting in a finished workpiece. The welded end faces of the hard base material 1 and the soft base material 2 form a joint (during welding, the convex platform shape is inserted into the concave platform shape, and the pits of the convex platform shape and the concave platform shape match). The joint refers to the entire structure of the hard base material 1 base material - the heat-affected zone of the hard base material 1 - the interface - the heat-affected zone of the soft base material 2 - the soft base material 2. Throughout the upsetting pressure cycle, the arc welding equipment 5 continuously outputs the low current specified by the process to maintain arc stability until the speed of flywheel 401 drops to zero and comes to a complete stop, at which point the arc is extinguished.

[0043] S6. After the friction upsetting and pressure holding process is completed and the joint is completely cooled to the temperature range allowed by the process, the finished workpiece is removed from the tooling station 4 of the inertial friction welding machine to obtain the soft / hard dissimilar metal inertial friction welded joint with improved non-uniformity.

[0044] Preferably, the hard base material 1 is knurled on the end face to be welded using a knurling machine 3 to form a uniformly distributed groove morphology with a depth of 1-5 mm on its surface, including: The hard base material 1 with the protruding end face is clamped onto the clamping device 301 of the knurling machine 3. After the coaxiality and locking degree are checked (this check process is existing technology, i.e., used to check whether the workpiece is clamped), the rolling mechanism 302 is driven to process the regular concave and convex groove shape with preset spacing parameters on the end face of the hard base material 1 to be welded.

[0045] Preferably, after completing the workstation layout plan, the inertial friction welding machine 4 and the arc welding equipment 5 are placed in designated workstations that meet the requirements of process flow and safety distance, with a safety distance of 1-2m; then, the hard base material 1 with an outwardly convex platform shape and the soft base material 2 with an inwardly concave platform shape are respectively clamped and fixed to the corresponding tooling workstations of the inertial friction welding machine 4, including: When positioning the workstations of the inertial friction welding machine 4 and the arc welding equipment 5, it is necessary to complete the simulation verification of the motion trajectory of the entire process (this verification process is existing technology, that is, a no-load test is performed before operation to ensure that there is no collision between the equipment), to ensure that during the entire time-series operation cycle of inertial friction welding, all moving parts of the arc welding equipment 5 and the overall mechanical structure of the inertial friction welding machine 4 do not have spatial interference or physical collision. Then, the hard base material 1 is coaxially clamped and fixed to the flywheel 401 tooling station of the inertial friction welding machine 4 (that is, the clamp fixedly connected to the flywheel 401, with the clamp facing the fixed side clamping end 403), and the soft base material 2 is positioned and locked on the fixed side clamping end 403 of the inertial friction welding machine 4.

[0046] Preferably, when positioning the workstations of the inertial friction welding machine 4 and the arc welding equipment 5, it is necessary to complete the simulation and verification of the motion trajectory of the entire process to ensure that, throughout the entire time-series operation cycle of inertial friction welding, all moving parts of the arc welding equipment 5 do not have spatial interference with the overall mechanical structure of the inertial friction welding machine 4 and do not experience physical collisions, including: The welding power source 501 of the arc welding equipment 5 needs to be located outside the safe operating distance of the inertial friction welding machine 4 to avoid the safety risks caused by electromagnetic interference, spatter and mechanical movement during the welding process; the welding tungsten electrode 502, the wire feeding device 503 and the wire filler 504 are all arranged in an upper position, approaching the welding work position of the inertial friction welding machine 4 from the vertical upward direction.

[0047] Preferably, the process of coaxially clamping and fixing the hard base material 1 to the flywheel 401 tooling station of the inertial friction welding machine 4, and positioning and locking the soft base material 2 on the fixed side clamping end 403 of the inertial friction welding machine 4 includes: After the hard base material 1 is clamped and locked on the flywheel 401 of the inertial friction welding machine 4, the station centering check needs to be performed (this check process is existing technology) to ensure that the end face of the pre-made concave and convex grooves of the weldable boss is in the working area directly below the welding tungsten electrode 502 of the arc welding equipment 5, so as to provide sufficient operating space and reference centering conditions for the subsequent adjustment of the posture and angle of the welding tungsten electrode 502, the wire feeding device 503 and the wire filler 504.

[0048] Preferably, when the flywheel 401 of the inertial friction welding machine 4 enters the motor acceleration start-up moment, its rotation speed is 2-200 rpm, synchronously triggering the start of the arc welding equipment 5, the welding current is 40-70A, the welding voltage is 5-10V, and the wire feed speed is 0.05-0.2m / min. Filler wire additive deposition is performed on the weldable end face of the pre-formed grooved hard base material 1 to prepare a 2-5mm thick functional intermediate layer. This additive process continues until the energy storage phase of the flywheel 401 is completely terminated. During this phase, the flywheel 401 rotation speed reaches 500-3000 rpm, including: The flywheel 401 drive motor of the arc welding equipment 5 and the inertial friction welding machine 4 performs synchronous start control (an arc is generated by the welding power source 501 and the welding tungsten electrode 502, and the welding power source 501 provides welding current and welding voltage). Through time-series linkage (the arc position remains unchanged, and the rotation of the flywheel 401 makes the heat evenly distributed on the end face of the hard base material 1 to be welded; when the speed of the flywheel 401 is sufficient, it can be approximated as uniform heating) to ensure that the arc heat evenly covers the end face area of ​​the hard base material 1 to be welded; the welding current parameter setting must be the lowest feasible value under the premise of meeting the melting conditions of the wire filler 504, so as to avoid the risk of oxidation of the hard base material and intrusion of impurity elements caused by excessive heat input from the source of the process.

[0049] The wire feeder 504 is fed to the weldable end face of the hard base material 1 via the wire feeder 503. The wire feeder 503 needs to be triggered and started after the electric arc has established a stable combustion state, and the feed speed of the wire feeder 504 needs to be dynamically matched and linked with the real-time rotation speed of the flywheel 401 (when the rotation speed of the flywheel 401 is low, the wire feed speed can be appropriately increased to ensure the coverage area of ​​the intermediate layer; after the rotation speed of the flywheel 401 is increased, the wire feed speed should be slowed down to prevent molten droplet splashing. The specific rotation speed and wire feed speed parameters are determined according to the actual working conditions).

[0050] Preferably, after the energy storage phase is completely terminated and the filler wire additive manufacturing process is completed, the wire feeding action of the wire feeding device 503 is immediately stopped, and the wire feeding device 503 is removed from the work area at a safe distance of 1-2m. The arc ignition state of the arc welding equipment 5 is maintained throughout the process without interruption, and the current is maintained at 40-70A. Simultaneously, the traveling mechanism 402 at the feed end of the inertial friction welding machine 4 is triggered to start axial feeding at a speed of 5-50mm / s, entering the friction upsetting process. The friction pressure is 20-200MPa, and the upsetting pressure is 50-400MPa. Throughout the entire upsetting pressure cycle, the arc welding equipment 5 continuously outputs the low current specified by the process to maintain arc stability until the flywheel 401 speed drops to zero and comes to a complete stop, at which point the arc extinguishing operation is performed, including: Once the wire filler 504 has completely and evenly covered the weldable end face of the hard base material 1, immediately shut off the power output of the wire feeding device 503 and move it to a safe avoidance position, keeping the welding power supply 501 in a live output state throughout the process.

[0051] After the wire feeding device 503 is removed, the traveling mechanism 402 of the inertial friction welding machine 4 is simultaneously triggered to feed axially at low speed, driving the soft base material 2 to slowly come into contact with the hard base material 1, and then enters the inertial friction welding upsetting process under the condition of continuous arc heating.

[0052] After the upsetting and holding pressure process is completely completed, the output of welding power supply 501 is finally cut off to extinguish the arc.

[0053] Preferably, after the wire filler 504 completely and evenly covers the weldable end face of the hard base material 1, the power output of the wire feeding device 503 is immediately shut off and it is moved to a safe avoidance position, while keeping the welding power supply 501 in a live output state throughout the process includes: This process involves shutting down the wire feeder 503 while maintaining continuous output from the welding power supply 501. The core objective is to maintain a preset low-current (welding current 40-70A) arc throughout the upsetting process, moving towards the center region of the inertial friction welding interface (i.e., the location where heat generation is insufficient in conventional inertial friction welding processes; in this embodiment, this is the center of the front end face of the soft / hard base material, as shown in the attached figure). Figure 3 The central area of ​​(a) / (b) / (c) is supplemented with a directional heat source to specifically compensate for the radial distribution difference of frictional heat generation, thereby effectively reducing the non-uniformity of the radial structure and properties of the joint.

[0054] Preferably, after the upsetting and holding pressure process is completed and the joint has completely cooled to the allowable temperature range of the process, the finished workpiece is removed from the tooling station 4 of the inertial friction welding machine to obtain an inertial friction welded joint of dissimilar metals with large differences in softness / hardness after improving the non-uniformity, including: After the upsetting and holding pressure process of inertial friction welding is completed, the joint can be removed from the tooling station of the inertial friction welding machine 4 only after the workpiece has been air-cooled to room temperature. The final product is the soft / hard dissimilar metal inertial friction welded joint with improved non-uniformity.

[0055] The present invention provides an apparatus for improving radial non-uniformity of dissimilar metal inertial friction welded joints, and the method for implementing the above-mentioned method for improving radial non-uniformity of dissimilar metal inertial friction welded joints includes: lathe; The knurling machine 3, mounted on a lathe, includes a clamping device 301 and a rolling mechanism 302. The clamping device 301 is used to clamp the hard base material 1, and the rolling mechanism 302 is used to perform knurling on the end face of the hard base material 1 to be welded before welding. In this embodiment, the knurling machine 3 can be an existing knurling machine, and its clamping device 301 and rolling mechanism 302 can adopt existing structural forms. An inertial friction welding machine 4, mounted on a lathe, includes a motor, a spindle, a flywheel 401, a fixture, a traveling mechanism 402, and a fixed-side clamping end 403. The output end of the motor is connected to the input end of the spindle via a clutch. The flywheel 401 is coaxially connected to the spindle and is used to store rotational kinetic energy during the motor acceleration phase, releasing the energy during welding to complete the welding process. The fixture is fixedly connected to the flywheel 401 (the fixture can be a fixture built into the flywheel 401) and is used to clamp the knurled hard base material 1. The fixed-side clamping end 403 is directly opposite the fixture. The machine is used to clamp the soft base material 2; the traveling mechanism 402 is connected to the fixed side clamping end 403 and is used to drive the fixed side clamping end 403 to carry the soft base material 2 axially (the soft base material remains fixed and does not rotate during the inertial friction welding process, and it is connected to the traveling mechanism 402 in the axial direction to perform axial translational movement); in this embodiment, the inertial friction welding machine 4 can be an existing inertial friction welding machine, and its flywheel 401, clamp, traveling mechanism 402 and fixed side clamping end 403 can adopt existing structural forms; Arc welding equipment 5, mounted on a lathe, includes a welding power source 501, a welding tungsten electrode 502, a wire feeder 503, and wire filler 504. The welding power source 501 is electrically connected to the welding tungsten electrode 502 and the wire feeder 503. The welding tungsten electrode 502 is positioned directly above the end face to be welded of the hard base material 1 (the welding tungsten electrode 502 does not perform welding during upsetting; it only serves as heat supplementation and should remain in place). The wire feeder 503 is positioned above the hard base material 1. Figure 4 Located to the right of the welding tungsten electrode 502, the wire filler 504 is pushed to the welding end face of the hard base material 1. In this embodiment, the arc welding equipment 5 can adopt an existing filler wire arc TIG welding equipment, and its welding power source 501, welding tungsten electrode 502, wire feeding device 503 and wire filler 504 can adopt existing structural forms. There are two reasons for the radial non-uniformity of the joint. One is that the hardness difference of the base material is large, and the extrusion amount is different during upsetting. The other is that inertial friction welding uses relative rotation to generate heat for welding, but due to the different linear velocities at the contact surface, almost no heat is generated at the center of the circular contact surface, thus causing radial non-uniformity. The welding tungsten electrode 502 of the present invention can serve two functions: preparing an intermediate layer before upsetting (solving the first problem) and providing additional heat during upsetting (solving the second problem).

[0056] Inertial friction welding is a typical energy storage solid-state joining process. Before welding, a drive motor accelerates the spindle and associated flywheel assembly to a preset speed, allowing the flywheel to store sufficient rotational kinetic energy before disconnecting the power connection. Subsequently, a preset upsetting pressure is applied axially to the axisymmetric workpieces to be welded, causing high-speed relative friction between the two workpiece end faces. The mechanical energy stored in the flywheel is continuously converted into interfacial frictional heat, rapidly heating the material near the weld seam to a thermoplastic state below its melting point. As the flywheel speed gradually decreases to zero due to frictional dissipation, the welding process enters a short-duration, high-pressure upsetting stage. Under high pressure, the plasticized metal undergoes large plastic deformation and interfacial extrusion, accompanied by the breakage of the interfacial oxide film, full element diffusion, and dynamic recrystallization, ultimately forming a dense, forged weld structure. This process features a short thermal cycle time, a narrow heat-affected zone, extremely low intermetallic compound formation, and excellent joint mechanical properties, making it particularly suitable for high-precision welding of high-temperature alloys and dissimilar metal rotating components.

[0057] In conventional inertial friction welding, after the flywheel completes energy storage and disengages from the drive motor, it enters the upsetting stage. When the hard base material end face and the soft base material end face directly contact and rub, due to the significant differences in the thermophysical properties and plastic deformation resistance of dissimilar materials, there is a significant asynchrony in the frictional heat generation rate, high-temperature residence time, and plastic metal flow behavior at different radial positions of the joint. This results in insufficient heat accumulation in the central region of the joint and incomplete extrusion of plastic metal, ultimately leading to a radially distributed residual stress gradient and uneven mechanical properties. The core advantage of this invention is that it completes the in-situ preparation of the intermediate layer during the flywheel energy storage stage of traditional inertial friction welding, eliminating the need for an additional independent intermediate layer prefabrication process, thus achieving control over the radial microstructure and property uniformity of the joint. The method of this invention utilizes the equipment idle window during the flywheel energy storage stage to deposit a uniformly thick transitional intermediate layer with a hardness between that of the soft and hard base materials on the friction end face of the hard base material to be welded through an arc additive manufacturing mechanism integrated on the side of the inertial friction welding machine head. The thermal conductivity and plastic deformation resistance of this intermediate layer material can be directionally matched according to the performance parameters of the two base materials. After the flywheel disengages from the drive motor and enters the friction upsetting stage, the system maintains a continuous and stable output of the electric arc, using the arc energy to supplement the heat in the joint center area where the friction interface heat generation efficiency is lowest. Throughout the subsequent friction heating and upsetting process of inertial friction welding, this intermediate layer acts as a performance buffer medium, simultaneously adjusting the friction heating efficiency and plastic rheological resistance at different radial positions of the joint. Combined with the heat input from the arc to the central area, it further reduces the temperature difference between the joint center and edge areas, promoting uniform radial flow of the plastic metal and full diffusion of elements. This avoids localized stress concentration and incomplete welding defects caused by abrupt changes in the properties of the soft and hard base materials. Ultimately, without altering the original overall inertial friction welding process framework, it achieves a uniform distribution of microstructure and mechanical properties along the radial direction of the soft / hard dissimilar metal joint, significantly improving the overall service reliability of dissimilar metal inertial friction welded joints.

[0058] Example 1 A method for improving radial non-uniformity in dissimilar metal inertial friction welded joints of aluminum (soft rod-shaped base material, referred to as Aluminum I, diameter 20 mm) / steel (hard rod-shaped base material, referred to as Steel I, diameter 20 mm) includes the following steps: Step 101: On the knurling machine 3, grooves are machined on the end face of the boss to be welded on steel I to increase the wettability between the molten droplets and the end face of steel I to be welded during the preparation of the intermediate layer.

[0059] Steel I is clamped on the clamping device 301 of the knurling machine 3, and the rolling mechanism 302 of the knurling machine 3 is used to process a truncated quadrangular groove with a spacing of 3mm on the end face of steel I to be welded, so that the surface of the boss has an uneven shape.

[0060] The end of steel I to be welded has an outwardly convex platform shape with a boss height of 2mm and a boss surface diameter of 16mm.

[0061] Step 102: Place the inertial friction welding machine 4 and the arc welding equipment 5 in a suitable relative position.

[0062] In this step, the welding power source 501 of the arc welding equipment 5 should be placed outside the safe working distance of the inertial friction welding machine 4. The welding tungsten electrode 502, the wire feeding device 503, and the wire filler 504 (here the wire filler is set to pure copper welding wire, referred to as copper I) of the arc welding equipment 5 should be placed above the inertial friction welding machine 4.

[0063] The arc welding here uses a 4mm diameter tungsten electrode 502 and a 1.2mm diameter copper electrode 1.

[0064] Step 103: Clamp steel I and aluminum I on the inertial friction welding machine 4 and adjust the relative position of the arc welding equipment 5.

[0065] Steel I is clamped on the flywheel 401 of the inertial friction welding machine 4, and aluminum I is clamped on the fixed side clamping end 403 of the inertial friction welding machine 4.

[0066] When clamping, it is necessary to ensure that the end face of steel I with the pre-machined groove is directly below the tungsten electrode 502 for welding, and the wire feeding device 503 is placed above the front end of steel I, and the wire feeding of copper I is performed from the front side of steel I.

[0067] The end of aluminum I to be welded has a concave platform shape with a pit depth of 2mm and a lower surface diameter of 16mm.

[0068] Step 104: Start the inertial friction welding machine 4 to put the flywheel 401 into the motor acceleration stage. At the same time, start the arc welding equipment 5 to prepare a pure copper intermediate layer on the end face of steel I to be welded.

[0069] In this step, it should be noted that although the motor of the inertial friction welding machine 4 starts synchronously with the arc welding equipment 5, wire feeding should only be performed after the arc has stabilized.

[0070] During arc welding, the welding current is 60A, the wire feed speed is 0.1m / min, and the welding voltage range is 5-7V.

[0071] After the intermediate layer is prepared, turn off and remove the wire feeding device 503 of the arc welding equipment 5, but do not turn off the welding power supply 501, so that the small current welding arc continues to heat the welding end face of steel I.

[0072] Step 105: Disconnect the connection between the flywheel 401 and the main shaft of the inertial friction welding machine 4, and begin upsetting.

[0073] During the upsetting process, it is important to note that aluminum I will slowly approach and contact steel I under the drive of the traveling mechanism 402 of the inertial friction welding machine 4.

[0074] During the upsetting process, the welding arc maintains a low current output, continuously providing additional heat to the center of the base material, which generates less heat in traditional inertial friction welding.

[0075] Step 106: After upsetting is completed, remove the joint.

[0076] After the flywheel 401 has exhausted its inertia, steel I will stop rotating. At this time, turn off the welding power supply 501 of the arc welding equipment 5, wait for the joint to cool down, remove the joint, and obtain the improved aluminum / steel dissimilar metal inertial friction welded joint.

[0077] This invention, during the flywheel motor acceleration stage of inertial friction welding of dissimilar metals with significant differences in hardness and softness, prepares an intermediate layer with thermophysical properties between aluminum and steel on the end face of the steel bar base material through arc-filled wire additive manufacturing. This reduces radial non-uniformity at the joint interface caused by excessive thermophysical property differences between the two dissimilar metals during the subsequent upsetting stage. Furthermore, in traditional inertial friction welding of dissimilar metals with significant differences in hardness and softness, the large thermophysical property differences during the upsetting stage result in a large amount of flash on the soft metal side, leading to significant material waste and considerable difficulties in subsequent machining. Therefore, by machining the end face of the soft base material to be welded into a concave shape and the end face of the hard base material to be welded into a boss shape before welding, the center position of the soft base material, which is less heated during inertial friction welding and prone to large extrusion, is hollowed out. This saves material and achieves a straight weld interface.

[0078] Example 2 A method for improving radial non-uniformity in dissimilar metal inertial friction welded joints of aluminum (soft rod-shaped base material, referred to as Aluminum I, diameter 18 mm) / titanium (hard rod-shaped base material, referred to as Titanium I, diameter 18 mm) includes the following steps: Step 101: On the knurling machine 3, grooves are machined on the end face of the boss to be welded of titanium I to increase the wettability between the molten droplets and the end face of titanium I to be welded during the preparation of the intermediate layer.

[0079] Steel I is clamped on the clamping device 301 of the knurling machine 3, and the rolling mechanism 302 of the knurling machine 3 is used to process a non-spaced quadrangular pyramidal groove on the end face of titanium I to be welded, so that the surface of the boss has an uneven shape.

[0080] The end of titanium I to be welded has an outward convex platform shape with a boss height of 3mm and a boss upper surface diameter of 12mm.

[0081] Step 102: Place the inertial friction welding machine 4 and the arc welding equipment 5 in a suitable relative position.

[0082] In this step, the welding power source 501 of the arc welding equipment 5 should be placed outside the safe working distance of the inertial friction welding machine 4. The welding tungsten electrode 502, the wire feeding device 503, and the wire filler 504 (here the wire filler is set as CuAl8 copper-based welding wire, referred to as copper II) of the arc welding equipment 5 should be placed above the inertial friction welding machine 4.

[0083] The arc welding here uses a 3mm diameter tungsten electrode 502 and a 1.2mm diameter copper electrode II.

[0084] Step 103: Clamp titanium I and aluminum I on the inertial friction welding machine 4 and adjust the relative position of the arc welding equipment 5.

[0085] Titanium I is clamped on the flywheel 401 of the inertial friction welding machine 4, and aluminum I is clamped on the fixed side clamping end 403 of the inertial friction welding machine 4.

[0086] When clamping, it is necessary to ensure that the end face of the titanium I with the groove already machined is placed directly below the tungsten electrode 502 for welding, and the wire feeding device 503 is placed above the front end of the titanium I, and the copper II wire is fed from the front side of the titanium I.

[0087] The end of aluminum I to be welded has a concave platform shape with a pit depth of 3mm and a lower surface diameter of 12mm.

[0088] Step 104: Start the inertial friction welding machine 4 to put the flywheel 401 into the motor acceleration stage. At the same time, start the arc welding equipment 5 to prepare a CuAl8 copper-based alloy intermediate layer on the titanium I end face to be welded.

[0089] In this step, it should be noted that although the motor of the inertial friction welding machine 4 starts synchronously with the arc welding equipment 5, wire feeding should only be performed after the arc has stabilized.

[0090] During arc welding, the welding current is 50A, the wire feed speed is 0.08m / min, and the welding voltage range is 8-10V.

[0091] After the intermediate layer is prepared, turn off and remove the wire feeding device 503 of the arc welding equipment 5, but do not turn off the welding power supply 501, so that the small current welding arc continues to heat the welding end face of titanium I.

[0092] Step 105: Disconnect the connection between the flywheel 401 and the main shaft of the inertial friction welding machine 4, and begin upsetting.

[0093] During the upsetting process, it is important to note that aluminum I will slowly approach and contact titanium I under the drive of the traveling mechanism 402 of the inertial friction welding machine 4.

[0094] During the upsetting process, the welding arc maintains a low current output, continuously providing additional heat to the center of the base material, which generates less heat in traditional inertial friction welding.

[0095] Step 106: After upsetting is completed, remove the joint.

[0096] After the inertia of flywheel 401 is exhausted, titanium I will stop rotating. At this time, turn off the welding power supply 501 of the arc welding equipment 5, wait for the joint to dissipate heat, remove the joint, and obtain the improved aluminum / titanium dissimilar metal inertial friction welded joint.

[0097] Example 3 A method for improving radial non-uniformity in dissimilar metal inertial friction welded joints of magnesium (soft rod-shaped base material, referred to as magnesium I, diameter 30 mm) / steel (hard rod-shaped base material, referred to as steel I, diameter 30 mm) includes the following steps: Step 101: On the knurling machine 3, grooves are machined on the end face of the boss to be welded on steel I to increase the wettability between the molten droplets and the end face of steel I to be welded during the preparation of the intermediate layer.

[0098] Steel I is clamped on the clamping device 301 of the knurling machine 3, and the rolling mechanism 302 of the knurling machine 3 is used to process a non-spaced quadrangular pyramidal groove on the end face of steel I to be welded, so that the surface of the boss has an uneven shape.

[0099] The end of steel I to be welded has an outwardly convex platform shape, with a boss height of 5mm and a top surface diameter of 20mm.

[0100] Step 102: Place the inertial friction welding machine 4 and the arc welding equipment 5 in a suitable relative position.

[0101] In this step, the welding power source 501 of the arc welding equipment 5 should be placed outside the safe working distance of the inertial friction welding machine 4. The welding tungsten electrode 502, the wire feeding device 503, and the wire filler 504 (here the wire filler is set to pure nickel welding wire, referred to as Nickel I) of the arc welding equipment 5 should be placed above the inertial friction welding machine 4.

[0102] The arc welding here uses a 4mm diameter tungsten electrode 502 and a 1.2mm diameter nickel electrode 1.

[0103] Step 103: Clamp steel I and magnesium I on the inertial friction welding machine 4 and adjust the relative position of the arc welding equipment 5.

[0104] Steel I is clamped on the flywheel 401 of the inertial friction welding machine 4, and magnesium I is clamped on the fixed side clamping end 403 of the inertial friction welding machine 4.

[0105] When clamping, it is necessary to ensure that the end face of steel I with the pre-machined groove is directly below the tungsten electrode 502 for welding, and the wire feeding device 503 is placed above the front end of steel I, and the wire feeding of copper II is performed from the front side of steel I.

[0106] The end of magnesium I to be welded has a concave platform shape with a pit depth of 5 mm and a lower surface diameter of 20 mm.

[0107] Step 104: Start the inertial friction welding machine 4 to put the flywheel 401 into the motor acceleration stage. At the same time, start the arc welding equipment 5 to prepare a pure nickel intermediate layer on the end face of steel I to be welded.

[0108] In this step, it should be noted that although the motor of the inertial friction welding machine 4 starts synchronously with the arc welding equipment 5, the wire feeding should only be carried out after the arc has stabilized.

[0109] During arc welding, the welding current is 55A, the wire feed speed is 0.15m / min, and the welding voltage range is 7.5-9.5V.

[0110] After the intermediate layer is prepared, turn off and remove the wire feeding device 503 of the arc welding equipment 5, but do not turn off the welding power supply 501, so that the small current welding arc continues to heat the welding end face of steel I.

[0111] Step 105: Disconnect the connection between the flywheel 401 and the main shaft of the inertial friction welding machine 4, and begin upsetting.

[0112] During the upsetting process, it is important to note that under the drive of the traveling mechanism 402 of the inertial friction welding machine 4, magnesium I slowly approaches and contacts steel I.

[0113] During the upsetting process, the welding arc maintains a low current output, continuously providing additional heat to the center of the base material, which generates less heat in traditional inertial friction welding.

[0114] Step 106: After upsetting is completed, remove the joint.

[0115] After the inertia of flywheel 401 is exhausted, steel I will stop rotating. At this time, turn off the welding power supply 501 of the arc welding equipment 5, wait for the joint to dissipate heat, remove the joint, and obtain the improved magnesium / steel dissimilar metal inertial friction welded joint.

[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for improving radial non-uniformity in dissimilar metal inertial friction welded joints, characterized in that, Includes the following steps: S1. Prepare the workpiece to be welded. The workpiece to be welded is a cylindrical base material of dissimilar metals with large differences in hardness and softness. It includes a hard base material (1) and a soft base material (2) with a hardness difference. The end of the hard base material (1) to be welded is a convex platform with a frustum shape. The end of the soft base material (2) to be welded is a concave platform with a frustum-shaped pit inside. The end face of the hard base material (1) to be welded is the front end face of the convex platform shape. The end face of the soft base material (2) to be welded is the bottom surface of the pit. S2. Use a knurling machine (3) to knurl the end face of the hard base material (1) to be welded, so that the surface of the material forms a uniformly distributed groove morphology. S3. Place the inertial friction welding machine (4) and the arc welding equipment (5) on the lathe, and clamp the hard base material (1) and the soft base material (2) in the corresponding tooling positions of the inertial friction welding machine (4); S4. When the flywheel (401) of the inertial friction welding machine (4) enters the motor acceleration start moment, the speed is 2-200 rpm, energy storage begins, and the hard base material (1) is rotated; the arc welding equipment (5) is started simultaneously to carry out the filler wire additive process. Under certain welding parameters such as welding current, welding voltage and wire feeding speed, filler wire additive deposition is carried out on the weldable end face of the hard base material (1) with pre-made concave and convex groove morphology to prepare a 2-5 mm thick intermediate layer. The filler wire additive process continues to run until the energy storage stage of the flywheel (401) is completely terminated, and the speed of the flywheel (401) reaches 500-3000 rpm. S5. After the energy storage stage is completely terminated and the filler wire additive process is completed, the wire feeding device (503) is immediately stopped from feeding the welding wire, and the wire feeding device (503) is removed from the work area. The arc ignition state of the arc welding equipment (5) is maintained throughout the process without being cut off, and the welding current is the same as the welding current in S4. At the same time, the walking mechanism (402) of the inertial friction welding machine (4) is started to feed axially, driving the soft base material (2) and the hard base material (1) to gradually approach and contact each other, and enter the friction upsetting process. Frictional heat is generated under a certain axial force. After the speed of the flywheel (401) drops to zero, the upsetting and holding pressure process is carried out to complete the welding of the hard base material (1) and the soft base material (2) to obtain the finished workpiece. The welded end face of the hard base material (1) and the welded end face of the soft base material (2) form a joint. During the entire upsetting pressure cycle, the arc welding equipment (5) continuously outputs a low current to maintain the arc stability until the speed of the flywheel (401) drops to zero and stops completely, and then the arc extinguishing operation is performed. S6. After the friction upsetting process is completed and the joint is completely cooled to the temperature range allowed by the process, the finished workpiece is removed from the inertial friction welding machine (4) to obtain the soft / hard large difference dissimilar metal inertial friction welding joint after improving the non-uniformity.

2. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 1, characterized in that, In S1, the hard base material (1) is made of steel, titanium or copper, and the soft base material (2) is made of aluminum or magnesium. The hardness difference between the hard base material (1) and the soft base material (2) is 50-150 HV. The platform height of the convex platform morphology is 1-5 mm, and the diameter of the front end face of the convex platform morphology is 10-40 mm. The platform depth of the concave platform morphology is 1-5 mm, and the diameter of the bottom surface of the pit is 10-40 mm.

3. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 1, characterized in that, In S2, during the knurling process, the hard base material (1) is clamped onto the clamping device (301) of the knurling machine (3). After the coaxiality and locking degree are checked, the rolling mechanism (302) of the knurling machine (3) is driven to process a regular concave-convex groove shape on the end face to be welded of the hard base material (1). The depth of the concave-convex groove shape is 1-5mm, and the concave-convex groove shape is a quadrangular frustum groove with a spacing of 1-3mm, or a quadrangular pyramidal groove with no spacing or a spacing of 1-3mm, or a straight groove with a spacing of 1-3mm.

4. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 1, characterized in that, In S3, during the full-time operation cycle of inertial friction welding, all moving parts of the arc welding equipment (5) do not have spatial interference with the overall mechanical structure of the inertial friction welding machine (4) and do not have physical collisions; wherein the welding power source (501) of the arc welding equipment (5) is arranged outside the safe operating distance of the inertial friction welding machine (4), and the welding tungsten electrode (502), wire feeding device (503) and wire filler (504) of the arc welding equipment (5) are all arranged in an upper position, approaching the welding operation position of the inertial friction welding machine (4) from the vertical upward direction.

5. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 4, characterized in that, In S3, the hard base material (1) is clamped in the flywheel (401) tooling station of the inertial friction welding machine (4), and the end face of the hard base material (1) to be welded is in the working area directly below the tungsten electrode (502) for welding; the soft base material (2) is clamped in the fixed side clamping end (403) of the inertial friction welding machine (4).

6. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 4, characterized in that, In S4, an electric arc is generated by a welding power source (501) and a welding tungsten electrode (502). The heat from the electric arc evenly covers the weldable end face area of ​​the hard base material (1). The welding current parameter is set to the lowest feasible value under the premise of meeting the melting conditions of the wire filler (504). The wire filler (504) is fed to the weldable end face of the hard base material (1) by a wire feeding device (503). The wire feeding device (503) is triggered to start after the electric arc establishes a stable combustion state. The feed speed of the wire filler (504) is dynamically matched and linked with the real-time rotation speed of the flywheel (401). The welding current of the arc welding equipment (5) is 40-70A, the welding voltage is 5-10V, and the wire feeding speed is 0.05-0.2m / min.

7. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 6, characterized in that, In S5, after the wire filler (504) completely and evenly covers the weldable end face of the hard base material (1), the power output of the wire feeding device (503) is immediately turned off and moved to a safe avoidance position. The welding power supply (501) is kept in the energized output state throughout the process. By maintaining the preset low current arc, a directional heat source is added to the central area of ​​the interface of the inertial friction welding during the entire upsetting process to compensate for the radial distribution difference of friction heat generation. The soft base material (2) is driven to slowly come into contact with the hard base material (1) by the low-speed axial feed of the walking mechanism (402), and enters the friction upsetting process under the condition of continuous arc heating; after the friction upsetting process is completely finished, the output of the welding power supply (501) is cut off to complete the arc extinguishing.

8. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 1, characterized in that, In S5, the friction pressure of the friction upsetting process is 20-200 MPa, and the upsetting pressure is 50-400 MPa.

9. The method for improving radial non-uniformity of dissimilar metal inertial friction welded joints according to claim 1, characterized in that, In step S6, after the workpiece has been air-cooled to room temperature, the finished workpiece is removed from the tooling station of the inertial friction welding machine (4).

10. An apparatus for improving radial non-uniformity of dissimilar metal friction welded joints, comprising the method for improving radial non-uniformity of dissimilar metal friction welded joints as described in any one of claims 1-9, characterized in that, include: lathe; A knurling machine (3) is mounted on a lathe and includes a clamping device (301) and a rolling mechanism (302). The clamping device (301) is used to clamp the hard base material (1), and the rolling mechanism (302) is used to knurl the end face of the hard base material (1) to be welded before welding. An inertial friction welding machine (4), mounted on a lathe, includes a motor, a spindle, a flywheel (401), a fixture, a traveling mechanism (402), and a fixed-side clamping end (403). The output end of the motor is connected to the input end of the spindle via a clutch. The flywheel (401) is coaxially connected to the spindle and is used to store rotational kinetic energy during the motor acceleration phase and release energy during welding to complete the welding. The fixture is fixedly connected to the flywheel (401) and is used to clamp the knurled hard base material (1). The fixed-side clamping end (403) is directly opposite the fixture and is used to clamp the soft base material (2). The traveling mechanism (402) is connected to the fixed-side clamping end (403) and is used to drive the fixed-side clamping end (403) to axially feed the soft base material (2). The arc welding equipment (5) is installed on a lathe and adopts a filler wire arc TIG welding equipment, including a welding power source (501), a welding tungsten electrode (502), a wire feeding device (503) and a wire filler (504). The welding power source (501) is electrically connected to the welding tungsten electrode (502) and the wire feeding device (503). The welding tungsten electrode (502) is located directly above the end face to be welded of the hard base material (1). The wire feeding device (503) is located above the hard base material (1) and is used to push the wire filler (504) to the end face to be welded of the hard base material (1).

Citation Information

Patent Citations

  • A high-strength and tough radial friction welding method for steel / aluminum heterogeneous difficult-to-weld alloys

    CN115026409B