Alkali-free low-temperature microcrystalline glass binder containing high-entropy nucleating agent and its preparation process
By employing the Bi2O3-CaF2 composite flux and the synergistic enhancement mechanism of high-entropy polycrystalline seeds, combined with the whole-process process of pre-prepared high-entropy nucleating agents, the problem of existing binders being unable to balance sintering temperature and chemical stability has been solved. This has resulted in a high-density and high-stability microcrystalline glass binder, which improves the grinding accuracy and lifespan of semiconductor wafer thinning processes.
Patent Information
- Application Number
- CN202611573034.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing microcrystalline glass binders for diamond grinding wheels have difficulty balancing sintering temperature and chemical stability, have a single crystal phase enhancement mechanism, and insufficient raw material homogenization scale, resulting in insufficient grinding accuracy and stability during semiconductor wafer thinning.
An alkali-free low-temperature glass system using Bi2O3-CaF2 composite flux was developed, and a high-entropy polycrystalline seed synergistic enhancement mechanism was introduced. Through a full-process process of pre-prepared high-entropy nucleating agent block material melt doping, melting and water quenching refinement, forming, muffle furnace segmented gradient sintering, and annealing, a polycrystalline seed binder with a sintering temperature not exceeding 820℃ was prepared, achieving interfacial thermal matching and high density.
It significantly improves the mechanical and chemical holding ability of the binder for diamond abrasive grains, thereby enhancing the service stability and service life of the grinding wheel under the conditions of thinning third-generation semiconductor wafers.
Smart Images

Figure CN123103532A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor wafer processing technology, and specifically relates to a microcrystalline glass binder for ultrafine diamond prepared by induction of a pre-prepared multi-component high-entropy nucleating agent and its preparation process. Background Technology
[0002] With the large-scale application of third-generation semiconductor (SiC, GaN) power devices in new energy vehicles, 5G communications, and fast charging, and the evolution of advanced packaging (Chiplet, 2.5 / 3D) towards smaller sizes and higher I / O densities, wafer thinning and back-side grinding have placed unprecedented demands on the processing accuracy, surface integrity, and batch consistency of diamond grinding wheels. Wafer thickness has advanced from 200 μm to 50 μm or even thinner limits. Any abrasive grain shedding, surface sub-damage, or wheel profile drift during thinning can lead to wafer breakage or device failure, posing a systemic challenge to the sintering temperature control, mechanical properties, interface holding ability, and resistance to acid and alkali grinding fluid corrosion of the binder. Glass binders, due to their combination of low-temperature fluidity of the glass phase and the strengthening and toughening effect of the crystal phase, are one of the most widely used systems in diamond grinding wheels. Most existing research focuses on the basic component formulation, crystallization behavior control, sintering densification, and heat treatment regime optimization of microcrystalline glass binders, attempting to improve the overall performance of grinding wheels through material design. However, existing binders still have several shortcomings for semiconductor wafer thinning applications: most studies only use a single nucleating agent, lacking a high-entropy polycrystalline phase synergistic strengthening design; the matrix grain boundaries are susceptible to corrosion by acid and alkali grinding media, resulting in significant degradation of mechanical properties after corrosion; and research on nanoscale fine dispersion of raw materials, homogenization control of multi-component composition, and graded release of residual internal stress after sintering-crystallization is relatively scarce. Therefore, it is necessary to optimize the binder formulation system and the entire preparation process in a targeted manner, taking into account the actual service requirements of diamond grinding wheels and the needs for low-temperature sintering, mechanical toughening, and chemical corrosion resistance, to improve its applicability under precision thinning and high-stability grinding conditions.
[0003] Analysis of existing microcrystalline glass binders for diamond grinding wheels reveals three main shortcomings: First, it is difficult to balance sintering temperature and chemical stability. While alkali metal binders can achieve low-temperature densification, alkali metal oxides (Na₂O, K₂O) significantly reduce chemical durability, acid and alkali corrosion resistance, and electrical insulation, posing a risk of ion migration and wafer contamination. Some publicly available alkali-free low-temperature binders avoid the alkali metal problem, but their fluxing methods are limited, resulting in relatively high sintering temperatures (typically above 850℃). They lack precise temperature-time matching for the diamond's thermal stability window, leading to oxidation, carbonization, and strength degradation in the diamond. Furthermore, most binders are not designed for thermal expansion matching of diamond, resulting in significant differences in thermal expansion coefficients. This leads to residual internal stress at the interface after cooling, inducing interfacial microcracks, insufficient interfacial wettability and mechanical bonding, and a need to improve holding power. Second, the crystal phase reinforcement mechanism is singular, lacking a synergistic design of polycrystalline phases and high-entropy effects. Existing microcrystalline glass binders mostly use a single nucleating agent or a few simple combinations, resulting in a limited variety of main crystalline phases precipitated (mostly single zinc aluminum silicate or cordierite phases). The grains are coarse and unevenly distributed, making it impossible to utilize the strengthening effects of polycrystalline phase interfaces, cross-pinning, and microcrack toughening. Furthermore, the high-entropy "cocktail effect" and lattice distortion strengthening have not been incorporated into the crystal phase design, and there is a lack of systematic utilization of the synergistic enhancement of multiple transition metal oxide components through solid solution. The matrix has many interconnected pores, making it easy for acid and alkali grinding media to penetrate and erode along the grain boundaries, causing grain boundary dissolution. After corrosion, the residual bending strength decreases significantly, further deteriorating the reliability of the grinding wheel. This makes it difficult to improve the bending strength, hardness, and density of the matrix, and it is impossible to form a sufficiently rigid three-dimensional anchoring structure around the abrasive grains. Under high load thinning, abrasive grain detachment and bonding layer damage are likely to occur. Thirdly, the raw material homogenization scale is insufficient, and the residual stress control methods are crude. Existing mixing processes mostly rely on conventional planetary ball milling or simple mechanical mixing, which can only achieve micron-level dispersion. Multi-component, multi-nucleating agent systems are prone to agglomeration and component segregation due to differences in density, hardness, and surface energy, resulting in uneven sintering and large performance fluctuations. Moreover, after sintering and crystallization, direct air cooling or single-temperature furnace cooling is generally used, which lacks a staged stress release mechanism. The residual internal stress caused by the thermal expansion mismatch between the crystalline phase and the glass phase is frozen in large quantities. Under the coupled action of grinding load and thermal shock, microcracks are easily induced to initiate and propagate, leading to increased brittleness, decreased resistance to edge chipping and fatigue, which restricts the machining accuracy and service life of grinding wheels.
[0004] The purpose of this invention is to address the aforementioned shortcomings by constructing an alkali-free low-temperature glass system with Bi2O3-CaF2 composite flux, introducing a high-entropy polycrystalline synergistic enhancement mechanism, and innovating a complete process of pre-prepared high-entropy nucleating agent block material melt doping-melting and water quenching refinement-forming-muffle furnace segmented gradient sintering-annealing. This results in the development of an alkali-free low-temperature polycrystalline binder for diamond grinding wheels with a sintering temperature not exceeding 820℃, no carbonization damage to diamond, a thermal expansion coefficient slightly higher than that of diamond to achieve interface thermal matching, high bending strength, high hardness, high density, and low residual stress. This meets the high precision, long life, and high stability requirements of grinding wheels in third-generation semiconductor wafer thinning and high-end precision grinding. Summary of the Invention
[0005] The inventive principle, namely the composition and effects of the glass raw materials used in this invention: SiO2: The basic glass network forging, which constructs a highly polymerized silicon-oxygen network framework to ensure the chemical and thermal stability of the matrix; B2O3: A basic glass network forging that reduces the high-temperature viscosity of the melt and improves the spreading and wetting ability of the glass melt on the diamond surface; ZnO: a basic glass network intermediate that regulates glass structural units, enhances sintering activity, and participates in the construction of zinc-aluminum spinel crystal phase; Al2O3: Strengthens the silicon-oxygen network, enhances the mechanical strength of the matrix, synergistically regulates the thermal expansion coefficient of the system, achieves interfacial thermal matching, and provides an aluminum source for the spinel crystal phase; CaO and MgO: These are basic glass network-modifying oxides that regulate thermal expansion behavior, promote sintering densification, and provide Ca²⁺ for calcium magnesium feldspar (Ca₂MgSi₂O₇). + Mg² + source; CaF2:F - Utilizing the glass network's disintegration function, it synergistically achieves low-temperature fluxing with Bi2O3; Ca² + It participates in the interfacial reaction and, during the sintering process, synergistically with Bi2O3 to generate a bismuth-rich fluoride oxide transition layer in situ at the diamond-binder interface, improving interfacial wettability and forming mechanical interlocking. Bi2O3:Bi³ + It has high polarizability, disrupts the symmetry of the glass network, significantly reduces the melt viscosity, and enables low-temperature sintering below 820℃; at the same time, it participates in the formation of the bismuth-rich fluoride oxide transition layer at the interface, improving the binder's holding force and compatibility with diamond abrasive grains. TiO2, ZrO2, P2O5: Basic nucleating agents that reduce crystallization activation energy, induce crystal nucleation, and promote the precipitation of main crystalline phases such as calcium magnesium feldspar, zinc aluminum spinel, etc. Cr2O3, MnO2, NiO: High-entropy nucleation components, multiple metal ions with different ionic radii, valence states and field strengths enter the crystal phase lattice and undergo solid solution, utilizing the high-entropy "cocktail effect" to generate lattice distortion, hindering dislocation movement and abnormal grain growth, and inducing the synergistic precipitation of multiple high-strength main crystalline phases; the interlocking of polycrystalline phases can significantly reduce the interconnected porosity, block the penetration channels of acid and alkali grinding fluids along grain boundaries, and improve the residual bending strength and strength retention rate after corrosion. In the above formulation, the mass percentage of each component can be appropriately fluctuated without changing the basic technical concept of the present invention. Moreover, the nucleating components are not strictly limited to TiO2, ZrO2, P2O5, Cr2O3, MnO2, and NiO selected in this embodiment. Without changing the concept of the present invention, at least five of the following can be used as substitutes: Group IVB HfO2; Group VA V2O5; Group VIB Fe2O3; Group VIIB CoO; and Group VIII CuO and FeO. When replacing, at least five equivalent oxides of the same group are selected to replace the original nucleating component. The mass percentage of each substitute oxide component is controlled at 1~2wt%, and the fluctuation of each component is ±1.0~±1.5wt%. The total mass percentage of the system is 100%, and no alkali metal oxides such as Na2O, K2O, and Li2O are introduced into the system throughout the process.
[0006] This invention is implemented according to the following technical solution: The preparation process of an alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent includes the following steps: 1) Add Bi2O3-CaF2 modifier to a glass binder raw material that does not contain alkali metal oxides, wherein the modifier has a composition of 2 wt% CaF2 and 4 wt% Bi2O3, to obtain a modified glass raw material; 2) The modified glass raw material is ball-milled, melted, water-quenched, and ball-milled to obtain binder powder; a high-entropy nucleating agent is added during the melting stage; 3) The binder powder is granulated, dry-pressed, sintered, and annealed to prepare an alkali-free low-temperature microcrystalline glass binder.
[0007] Preferably, the modified glass raw material has the following composition and mass percentage: SiO2 38%~42%, B2O3 2%~5%, ZnO 10%~16%, Al2O3 10%~16%, CaO 3%~6%, MgO 2%~4%, CaF2 1%~2%, Bi2O3 3%~4%, with the balance being a high-entropy nucleating agent. The mass percentage is based on the total mass of the modified glass raw material and the high-entropy nucleating agent.
[0008] Preferably, the high-entropy nucleating agent is a multi-component high-entropy nucleating agent, wherein the raw materials of the multi-component high-entropy nucleating agent are selected from five or more oxides of Ti, Zr, P, Cr, Mn, Ni and their equivalent elements in the same group.
[0009] Preferably, the high-entropy nucleating agent is composed of TiO2, ZrO2, P2O5, Cr2O3, MnO2 and NiO, and the number of each cation is equal, and the amount of each oxide is 0.2 wt% to 3 wt%.
[0010] Preferably, the high-entropy nucleating agent is a pre-formed block high-entropy nucleating agent, which is obtained by mixing and sintering the raw materials of the multi-component high-entropy nucleating agent.
[0011] Preferably, the mixing and sintering process is as follows: the nucleating raw material is mixed in a high-energy ball mill at 1050~1300 r / min for 5~20 min, and the mixed nucleating raw material is solid-state sintered at 650~950℃ for 2~4 h.
[0012] Preferably, in step 3), the sintering is a three-stage sintering process: the first stage is the nucleation stage, where the temperature is increased to 680-720°C at a rate of 6-10°C / min and held for 30-50 min; the second stage is the crystallization stage, where the temperature is increased to 750-780°C at a rate of 4-8°C / min and held for 60-80 min; and the third stage is the densification stage, where the temperature is increased to 780-820°C at a rate of 3-7°C / min and held for 45-65 min.
[0013] Preferably, the annealing process is as follows: after sintering and holding, the temperature is lowered to 630~670℃ at a rate of less than or equal to 2℃ / min and held for 60~180 min.
[0014] Preferably, in step 2), the melting is a three-stage melting: in the first stage, the temperature is raised from room temperature to 400~500℃ and held for 20~40 min; in the second stage, the temperature is raised to 850~950℃ and held for 20~40 min; in the third stage, the temperature is raised to 1380~1420℃ at a rate of 15℃ / min.
[0015] Preferably, the addition stage of the pre-formed blocky high-entropy nucleating agent is the third stage of melting in step 2).
[0016] Preferably, in step 2), the refining process is as follows: the glass slag obtained by water quenching is dried and coarsely crushed, and then refined and dispersed using a high-energy ball mill; the ball milling speed is 1000 r / min, and the ball milling time is 5~20 min, to obtain a binder powder with uniform particle size.
[0017] Preferably, in step 3), the granulation process is as follows: the binder powder is added to 3-7 wt% PVA solution to form a wet material; the wet material is sieved and granulated to obtain granular powder with a particle size controlled at 75-150 μm.
[0018] Preferably, in step 3), the dry pressing process is as follows: the granulated granular powder is loaded into a Φ20mm circular cemented carbide mold, and dry pressed under a pressure of 22~35MPa. After holding the pressure for 25~50s, the mold is removed to obtain a molded blank.
[0019] The present invention also includes an alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent prepared by the above method, wherein the binder contains at least two main crystalline phases selected from quartz, calcium magnesium feldspar and zinc aluminum spinel.
[0020] The beneficial effects of this invention are: The microcrystalline glass binder provided by this invention uses alkali-free zinc-aluminum-calcium-silicon microcrystalline glass as a matrix, and regulates the glass network structure through Bi2O3-CaF2 composite flux modification components; introduces multiple groups of transition metal oxides to construct a high-entropy polycrystalline seed system; prepares pre-formed blocky multi-component high-entropy nucleating agents, and puts them into the molten glass to achieve melting and diffusion, thereby constructing a high-entropy polycrystalline seed system. With the high-entropy "cocktail effect" and lattice distortion, multiple high-strength main crystalline phases such as quartz, calcium magnesium feldspar, and zinc-aluminum spinel are synergistically precipitated and cross-pinned. Through precise control of the entire process of water quenching, powder refinement, molding, muffle furnace segmented gradient sintering and annealing, a microcrystalline glass binder with a sintering temperature not exceeding 820℃, high density, high bending strength, and resistance to acid and alkali corrosion is obtained, thereby significantly improving its mechanochemical synergistic holding ability for diamond abrasive grains and enhancing the service stability and service life of the grinding wheel under the thinning conditions of third-generation semiconductor wafers. Attached Figure Description
[0021] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0022] Figure 1 Flowchart of the preparation process of alkali-free low-temperature microcrystalline glass binder containing high-entropy nucleating agent.
[0023] Figure 2 Bar chart of flexural strength of microcrystalline glass binders prepared at different sintering temperatures.
[0024] Figure 3 XRD patterns of microcrystalline glass binders prepared at different sintering temperatures.
[0025] Figure 4 Differential scanning calorimetry (DSC) curve of the microcrystalline glass binder prepared by the present invention.
[0026] Figure 5 The residual flexural strength retention rate of microcrystalline glass binders prepared at different sintering temperatures after 40 days of acid and alkali corrosion. (a) is the test environment with pH=4, and (b) is the test environment with pH=10.
[0027] Figure 6 SEM images of the microcrystalline glass binder prepared in this invention: (a) is an SEM image at 5000x magnification, and (b) is an SEM image at 10000x magnification.
[0028] Figure 7 Comparison chart of the flexural strength and residual flexural strength retention rate of the microcrystalline glass binders prepared in Examples 2 and 3-4 of the present invention after 40 days of acid and alkali corrosion.
[0029] Figure 8 Linear shrinkage and volume shrinkage of microcrystalline glass binders prepared at different sintering temperatures before and after sintering, (a) is linear shrinkage; (b) is volume shrinkage. Detailed Implementation
[0030] The present invention will now be described in further detail with reference to specific embodiments. It should be understood that the specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention.
[0031] There are no particular limitations on the purity of any raw materials used in this invention; the purity used is conventional and employed in the field. Similarly, the apparatus used in this invention, unless otherwise specified, employs commonly used apparatus in the field.
[0032] Example 1 like Figure 1 The diagram shown is a flow chart of an alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent and its preparation process, including the following steps: 1) Preparation of pre-formed blocky multi-component high-entropy nucleating agent Weigh out the following components by mass percentage: TiO2 1.5%, ZrO2 1.5%, P2O5 1.5%, Cr2O3 1.5%, MnO2 1.5%, and NiO 1.5%, as raw materials for the high-entropy nucleating agent. Add the raw materials of the high-entropy nucleating agent to a high-energy ball mill and mix thoroughly for 10 min at a speed of 1200 r / min. Place the ball-milled nucleating raw materials in a high-temperature muffle furnace and sinter them in solid state at 800℃ for 2 h to allow the nucleating raw materials to undergo an ion solid solution reaction, forming ion-solidified blocky materials, and obtain a single-phase solid solution pre-prepared blocky multi-component high-entropy nucleating agent for later use. The mass percentages mentioned in this embodiment refer to the total mass of the high-entropy nucleating agent and the modified glass raw materials.
[0033] 2) Raw material weighing and protective premixing The components and their mass percentages of the modified glass raw material are as follows: SiO2 40%, B2O 35%, ZnO 15%, Al2O3 15%, CaO 6%, MgO 4%, CaF 22%, Bi2O 34%. The raw materials are accurately weighed and mixed according to the above mass percentages. The modified glass raw material is then fed into a planetary ball mill, using anhydrous ethanol as the dispersion medium. The ball-to-material mass ratio is controlled at 3:1. Graded zirconia grinding balls are used, with the mass ratio of large, medium, and small grinding balls being 20%:30%:50%. The ball milling speed is set to 220 r / min, and the milling time is 5 h. The graded grinding balls ensure thorough and uniform mixing of the components of the base glass, suppressing component segregation during the subsequent melting stage.
[0034] 3) Vacuum drying to remove solvent After ball milling, the modified glass raw material was transferred to a tray and placed in a vacuum drying oven for drying. The drying temperature was set to 75℃ and the vacuum degree to -0.085MPa. Drying continued until the anhydrous ethanol was completely evaporated, yielding the dried glass raw material. Vacuum drying avoids the volatilization loss of volatile components such as B, Bi, and F under normal pressure and high temperature drying, ensuring that the actual material ratio is consistent with the designed formula.
[0035] 4) Preparation of glass slag by melting and water quenching The dried modified glass raw material was placed in a crucible for a three-stage melting process: the heating rate was kept constant at 15℃ / min throughout the process; first, the temperature was raised from room temperature to 450℃ and held for 30 min to promote the decomposition of borate-related components and complete the pre-reaction; then, the temperature was raised to 900℃ and held for 30 min to promote the complete decomposition of carbonate components; finally, the temperature was raised to 1400℃, at which point the pre-prepared blocky multi-component high-entropy nucleating agent prepared in step 1) was added, and the temperature was held for another 120 min to allow the pre-prepared blocky high-entropy nucleating agent and the modified glass raw material to fully melt and diffuse into the melt, resulting in a mixed melt. After melting, the resulting mixed melt was quickly poured into deionized water for water quenching to inhibit crystallization and obtain amorphous glass slag.
[0036] 5) High-energy ball milling for refining The amorphous glass slag obtained by water quenching was dried and then coarsely crushed before being fed into a high-energy ball mill for fine dispersion. The ball milling speed was 1000 r / min and the milling time was 10 min. The strong impact and shearing action of the high-energy ball milling completed the deagglomeration and refinement of the glass slag, resulting in a binder powder with uniform particle size.
[0037] 6) Granulation The binder powder obtained above was mixed with 5 wt% PVA solution as a binder and thoroughly stirred to form a wet material. The wet material was then sieved and granulated to obtain granular powder with excellent flowability and pressing performance, with the particle size controlled between 75 and 150 μm. Compared with simple manual mixing, granulation can reduce powder agglomeration and result in a more uniform distribution of components within the pressed green body.
[0038] 7) Dry pressing The granulated powder is loaded into a Φ20mm circular cemented carbide mold and dry-pressed under a pressure of 30MPa. After holding the pressure for 40s, it is demolded to obtain a green blank for subsequent sintering.
[0039] 8) Segmented gradient sintering crystallization The shaped green blank was placed in an alumina crucible and then placed in a muffle furnace. A segmented gradient sintering process was adopted: Nucleation stage: the temperature was increased to 700℃ at 8℃ / min and held for 40min to activate and form a large number of nuclei; Crystallization stage: the temperature was increased to 770℃ at 6℃ / min and held for 70min to drive the synergistic precipitation and cross-growth of the first batch of main crystalline phases, quartz and calcium magnesium feldspar; Densification stage: the temperature was increased to 780℃ at 5℃ / min and held for 55min to induce the concentrated precipitation of the second batch of main crystalline phases, zinc aluminum spinel, while densification of the green blank was achieved by utilizing the viscous flow of the residual glassy phase. The maximum sintering temperature throughout the process was controlled not to exceed 820℃ to avoid graphitization damage to the diamond abrasive grains during subsequent diamond wheel preparation. The segmented gradient heating reduced the internal temperature difference of the green blank, suppressed local abnormal grain growth, and ensured uniform precipitation of various crystalline phases.
[0040] 9) Annealing treatment After sintering and holding, the furnace is cooled to 650℃ for annealing and held for 120 minutes. After annealing, the cooling rate is controlled to be ≤2℃ / min and the furnace is slowly cooled to room temperature. Annealing eliminates some of the residual internal stress generated by sintering, reduces the brittleness of the matrix, and improves the resistance to edge chipping.
[0041] 10) Analysis, characterization, and performance testing.
[0042] Differential thermal analysis (DSC) was used to test the thermal behavior of the precursor glass powder, confirming that the system possesses multi-step crystallization characteristics. The entire crystallization process can be completed below 820℃, providing a temperature basis for the sintering process. XRD phase analysis was used to examine the sintered samples, revealing that the main precipitates were quartz, calcium magnesium feldspar, and zinc aluminum spinel. These phases intergrow and form a cross-pinned microstructure. Through the synergistic effect of polycrystalline phases and the lattice distortion effect of high-entropy nucleation components, the mechanical and corrosion resistance of the matrix is improved. Scanning electron microscopy was used to observe the microstructure and grain structure of the samples. The Archimedes' displacement method was used to test the bulk density. A universal testing machine was used to test the original flexural strength. Static acid and alkali immersion tests were conducted to test the residual flexural strength after corrosion and calculate the strength retention rate to evaluate the acid and alkali corrosion resistance. Based on the comprehensive testing, the binder prepared in this study can meet the requirements of high strength, high density, and resistance to acid and alkali coolant corrosion for diamond grinding wheels used in the thinning of third-generation semiconductor wafers.
[0043] Example 2 The difference between this embodiment and Embodiment 1 is that, in step 8), the sintering temperature of the densification stage is 800°C.
[0044] Example 3 The difference between this embodiment and Embodiment 1 is that, in step 8), the sintering temperature of the densification stage is 820°C.
[0045] Comparative Example 1 The difference between this comparative example and Example 1 is that, in step 8), the sintering temperature of the densification stage is 760°C.
[0046] Comparative Example 2 The difference between this embodiment and Embodiment 1 is that, in step 8), the sintering temperature of the densification stage is 840°C.
[0047] Comparative Example 3 The difference between this comparative example and Example 2 is that no Bi2O3-CaF2 modifier was added to the binder. The composition and mass percentage of the glass raw material are 46% SiO2, 5% B2O3, 15% ZnO, 15% Al2O3, 6% CaO, and 4% MaO. The composition and mass percentage of the high-entropy nucleating agent used are the same as those in Example 1, with the mass percentage referring to the total mass of the glass raw material and the high-entropy nucleating agent.
[0048] Comparative Example 4 The difference between this comparative example and Example 2 is that the binder uses a single-component high-entropy nucleating agent, whose glass raw material composition and mass percentage are 46% SiO2, 5% B2O3, 15% ZnO, 15% Al2O3, 6% CaO, and 4% MaO, and the multi-component high-entropy nucleating agent composition and mass percentage are 9% TiO2, with the mass percentage referring to the total mass of the glass raw material and the high-entropy nucleating agent.
[0049] Performance Evaluation like Figure 2 The figure shows a bar chart of the flexural strength of microcrystalline glass binders prepared at different sintering temperatures. The test results show that when the sintering temperature is 760℃, the sintering temperature is too low, and the system is not sufficiently crystallized. The flexural strength of the binder in Comparative Example 1 is only 96.0875 MPa, indicating poor densification of the glass phase inside the binder, numerous porosity defects, and low mechanical properties. When the sintering temperature is in the range of 780~820℃ (Examples 1~3), as the sintering temperature increases, the prepared binder continuously completes sintering densification and controllable crystallization, with uniform precipitation of the crystalline phase. The glass phase and the crystalline phase form a tight interfacial bond, reducing internal porosity and effectively improving the matrix's load-bearing capacity. When the sintering temperature is further increased to 840℃, the flexural strength of the binder in Comparative Example 2 drops to 122.98 MPa. This is because the sintering temperature is too high, causing abnormal grain growth, microcracks at grain boundaries, and excessive precipitation of some crystalline phases, leading to internal stress and a decrease in the material's mechanical properties.
[0050] like Figure 3 The figures show the XRD patterns of microcrystalline glass binders prepared at different sintering temperatures. The binder prepared at 760℃ (Comparative Example 1) exhibits weak diffraction peaks, dominated by the glass phase, with minimal crystalline phase precipitation. At 840℃ (Comparative Example 2), although the second crystallization peak is exceeded, abnormal grain growth and partial remelting weaken the diffraction peaks. The binders prepared at 780~820℃ (Examples 1~3) clearly show characteristic diffraction peaks of SiO2, Ca2MgSi2O7, and ZnAl2O4. With increasing sintering temperature, the intensity of the crystalline phase diffraction peaks gradually increases, indicating improved crystallinity. Above 820℃, the crystalline phases remelt, and their content decreases. Within the sintering range of 780~820℃, the system can precipitate multiple crystalline phases. The synergistic effect of the crystalline and glass phases forms the basis for the material's high flexural strength and excellent corrosion resistance.
[0051] like Figure 4 As shown in the figure, the DSC curve of the microcrystalline glass binder raw material is as follows: glass transition temperature T g =654℃; T N1 The first nucleation temperature is approximately 740℃. C1 The first exothermic crystallization peak is approximately 770℃; T N2The second nucleation temperature is approximately 795℃. C2 The second crystallization exothermic peak is approximately 815℃. Based on the thermal analysis results, it was determined that the sintering range should cover the crystallization range of 770~815℃. Therefore, 780℃, 800℃, and 820℃ were selected as the sintering temperatures for the examples. 760℃ did not fully enter the crystallization range, and 840℃ exceeded the second crystallization peak. These were used as comparative examples to corroborate the aforementioned XRD and mechanical results.
[0052] like Figure 5 As shown in the figure, (a) and (b) represent the flexural strength retention rates of the samples after corrosion in acidic environments (pH=4) and alkaline environments (pH=10) for 10–40 days, respectively. With prolonged corrosion time, the flexural strength retention rates of all binder groups decreased slightly. Under the same corrosion conditions, the strength retention rates of the binder samples prepared at 780–820℃ (Examples 1–3) were generally higher than those prepared in Comparative Examples 1–2. The strength retention rates of all samples were generally better in alkaline environments than in acidic environments. The microcrystalline glass binder matrix prepared at 780–820℃ has a dense structure, effectively blocking the penetration of corrosive media and exhibiting superior resistance to acid and alkali corrosion.
[0053] like Figure 6 The image shown is an SEM image of the binder prepared in Example 1. The results confirm the above performance characteristics: the microcrystalline glass binder prepared in the preferred temperature range (780~820℃) has a dense matrix structure, uniform grain distribution, and few defects. After long-term acid and alkali corrosion, the integrity of the matrix structure is better maintained, and it has both excellent mechanical properties and acid and alkali corrosion resistance.
[0054] like Figure 7 As shown in (a), at the same sintering temperature (800℃), the flexural strength of Example 2 reached 144.75 MPa, significantly higher than that of Comparative Example 3 (79.80 MPa) without Bi2O3-CaF2 modifier and Comparative Example 4 (108.05 MPa) using a single-component nucleating agent. Comparative Example 3 lacked a composite flux, resulting in poor glass melt fluidity, insufficient densification of the green body, and a significant decrease in mechanical properties. Comparative Example 4 used only a single-component nucleating agent, leading to an imbalance between nucleation and grain growth, resulting in larger grain size and reduced flexural strength. Figure 7 As shown in (b) and (c), the strength retention rate of the three groups of samples gradually decreased with the extension of corrosion time. However, the strength retention rate of Example 2 was always higher than that of Comparative Example 3 and Comparative Example 4, indicating that the corrosion resistance of Comparative Example 3 and Comparative Example 4 was not as good as that of Comparative Example 2.
[0055] like Figure 8As shown, within the sintering temperature range of 760~840℃, the shrinkage rate gradually increases with increasing temperature; insufficient densification occurs at 760℃, over-burning occurs at 840℃, and 780~820℃ is the suitable sintering range for equilibrium between the crystalline phase and the glassy phase. At 800℃, the flexural strength of Example 2 is significantly higher than that of Comparative Example 3 (without Bi2O3-CaF2 modifier) and Comparative Example 4 (with a single-component nucleating agent). Within the sintering window of 780~820℃, the Bi2O3-CaF2 modifier and the multi-component high-entropy nucleating agent produce a synergistic effect, improving both the degree of sintering densification and precisely controlling microcrystal precipitation, enabling the microcrystalline glass binder to simultaneously possess high flexural strength and excellent resistance to acid and alkali corrosion.
[0056] The scope of protection of this invention is not limited to the specific embodiments described above. All equivalent modifications made based on the technical solutions of this invention fall within the scope of protection of this invention.
Claims
1. A preparation process for an alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent, characterized in that, Includes the following steps: 1) Add Bi2O3-CaF2 modifier to a glass binder raw material that does not contain alkali metal oxides, wherein the modifier has a composition of 2 wt% CaF2 and 4 wt% Bi2O3, to obtain a modified glass raw material; 2) The modified glass raw material is ball-milled, melted, water-quenched, and ball-milled to obtain binder powder; a high-entropy nucleating agent is added during the melting stage; 3) The binder powder is granulated, dry-pressed, sintered, and annealed to prepare an alkali-free low-temperature microcrystalline glass binder.
2. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 1, characterized in that, The modified glass raw material has the following composition and mass percentage: SiO2 38%~42%, B2O3 2%~5%, ZnO 10%~16%, Al2O3 10%~16%, CaO 3%~6%, MgO 2%~4%, CaF2 1%~2%, Bi2O3 3%~4%, with the balance being a high-entropy nucleating agent. The mass percentage is based on the total mass of the modified glass raw material and the high-entropy nucleating agent.
3. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 1, characterized in that, The high-entropy nucleating agent is a multi-component high-entropy nucleating agent, and the raw materials of the multi-component high-entropy nucleating agent are selected from five or more oxides of Ti, Zr, P, Cr, Mn, Ni and their equivalent elements in the same group.
4. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 1, characterized in that, The high-entropy nucleating agent is composed of TiO2, ZrO2, P2O5, Cr2O3, MnO2 and NiO, and the number of each cation is equal, and the amount of each oxide is 0.2 wt% to 3 wt%.
5. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 3, characterized in that, The high-entropy nucleating agent is a pre-formed blocky high-entropy nucleating agent, which is obtained by ball milling, mixing and sintering the raw materials of the multi-component high-entropy nucleating agent.
6. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 1, characterized in that, In step 3), the sintering is a three-stage sintering process, with the first stage temperature being 680~720℃; the second stage temperature being 750~780℃; and the third stage temperature being 780~820℃.
7. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 1, characterized in that, In step 2), the melting is a three-stage melting: the first stage temperature is 400~500℃; the second stage temperature is 850~950℃; and the third stage temperature is 1380~1420℃.
8. The preparation process of the alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 7, characterized in that, The addition stage of the pre-formed blocky high-entropy nucleating agent is the third stage of melting in step 2).
9. An alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 8.
10. The alkali-free low-temperature microcrystalline glass binder containing a high-entropy nucleating agent according to claim 9, characterized in that, The binder contains at least two main crystalline phases selected from quartz, calcium magnesium feldspar, and zinc aluminum spinel.