A method for preparing a high-barrier polypropylene film

By utilizing the cation exchange reaction of nano-inorganic barrier agents and organic intercalating agents, and the ABA three-layer co-extrusion structure, combined with physical vapor deposition, the problems of insufficient barrier performance and poor coating adhesion of polypropylene films were solved, resulting in the preparation of polypropylene films with high barrier performance, suitable for high-end packaging materials.

CN123104128APending Publication Date: 2026-11-17HUBEI JIAYUE NEW MATERIALS SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611014328.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polypropylene films have insufficient barrier properties and poor coating adhesion, and single modification methods have limited effectiveness.

Method used

By conducting a cation exchange reaction between nano-inorganic barrier agents and organic intercalating agents to expand the interlayer spacing, and combining the ABA three-layer co-extrusion structure with physical vapor deposition, a high-barrier coating is formed, enhancing adhesion.

Benefits of technology

It achieves high barrier performance, strong coating adhesion, controllable cost, is suitable for high-end packaging materials, and is easy to recycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104128A_ABST
    Figure CN123104128A_ABST
Patent Text Reader

Abstract

This invention relates to the technical field of polymer materials and packaging technology, and particularly to a method for preparing a high-barrier polypropylene film. The method involves a cation exchange reaction between a nano-inorganic barrier agent and an organic intercalating agent to obtain an organically modified nano-barrier agent with an interlayer spacing increased to over 2.5 nm. The obtained organically modified nano-barrier agent, a first compatibilizer, and a polypropylene base material are mixed, melt-blended, extruded, and granulated to obtain a modified masterbatch, solving the industry problem of easy coating peeling. The introduction of PBAT, a biodegradable material, enhances the film's environmental properties. The three-layer co-extrusion structure design, with the modified masterbatch added only to the core layer, facilitates the recycling and reuse of the polypropylene film. The tensile strength is ≥140 MPa, and the elongation at break is ≥130%, meeting the requirements for packaging material processing and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of polymer materials and packaging technology, and more particularly to a method for preparing a high-barrier polypropylene film. Background Technology

[0002] Polypropylene (PP) film is widely used in packaging, electronics, and other fields due to its excellent physical properties, chemical stability, and good processability. However, ordinary polypropylene film has poor barrier properties and cannot meet the requirements of high-end packaging for oxygen and water vapor barrier functions.

[0003] Existing technologies for improving the barrier properties of polypropylene films mainly include blending modification, surface coating, and multilayer composites. Blending modification involves adding nanomaterials (such as montmorillonite) or polar polymers to the polypropylene matrix, utilizing the "maze effect" to extend the gas permeation path. However, this method suffers from uneven dispersion of the modifier, resulting in limited improvement in barrier performance. Surface coating technology significantly improves the barrier effect by depositing high-barrier coatings such as alumina and silica on the film surface, but the coating has poor adhesion to the polypropylene substrate, making it prone to cracking. Multilayer composite technology is complex and costly.

[0004] Therefore, developing a method for preparing polypropylene films that combines ultra-high barrier properties, good coating adhesion, and process economy has significant industrial value. Summary of the Invention

[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0006] In view of the problems existing in the above-mentioned methods for preparing high-barrier polypropylene films, the present invention is proposed.

[0007] Therefore, the purpose of this invention is to provide a method for preparing a high-barrier polypropylene film, which aims to solve the technical problems of insufficient barrier properties, poor coating adhesion, and limited effectiveness of single modification methods in existing polypropylene films.

[0008] To solve the above technical problems, the present invention provides the following technical solution: S1: A cation exchange reaction is carried out between a nano-inorganic barrier agent and an organic intercalating agent to obtain an organically modified nano-barrier agent, the interlayer spacing of which is increased to more than 2.5 nm; S2: The obtained organic modified nano barrier agent, the first compatibilizer and polypropylene base material are mixed, melt-blended and extruded, and granulated to obtain modified masterbatch; S3: The obtained modified masterbatch is mixed with polypropylene base resin, biodegradable polar polymer and second compatibilizer, and then melt-blended and extruded to obtain blended modified granules. S4: Using an ABA three-layer co-extrusion structure, polypropylene heat-sealing resin is used as the surface material and blended modified granules are used as the core material. Through multi-layer co-extrusion and casting, a three-layer co-extruded thick sheet is obtained. S5: The obtained three-layer co-extruded thick sheet is biaxially stretched to obtain a nano-modified polypropylene base film; S6: The obtained base film is surface activated, and then a high-barrier coating is deposited on the activated surface by physical vapor deposition to obtain a high-barrier polypropylene film.

[0009] In a preferred embodiment of the method for preparing the high-barrier polypropylene film of the present invention, the nano-inorganic barrier agent in step (1) is one or more of montmorillonite, vermiculite, or kaolinite; the organic intercalating agent is a long-chain alkyl quaternary ammonium salt with the general formula [R1R2R3R4N]. + X - R1 is a C12-C18 alkyl group, R2, R3, and R4 are methyl or ethyl groups, and X is Cl or Br.

[0010] As a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, wherein: the cation exchange reaction temperature in step (1) is 60-100℃ and the reaction time is 2-6 hours; the interlayer spacing of the organically modified nano-barrier agent is 2.5-3.5nm.

[0011] As a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, wherein: the first compatibilizer in step (2) is polypropylene grafted with maleic anhydride, with a grafting rate of 0.5%-1.5%; the mass ratio of the organic modified nano barrier agent, the first compatibilizer and the polypropylene base material is 5-20:2-8:72-93.

[0012] As a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, wherein: the biodegradable polar polymer in step (3) is one or more of PBAT, PBS or PLA; the second compatibilizer is polypropylene grafted with maleic anhydride or ethylene-acrylic acid copolymer; and the mass ratio of the modified masterbatch, the biodegradable polar polymer and the polypropylene base resin is 10-30:2-10:60-88.

[0013] As a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, wherein: in the three-layer co-extrusion structure of step (4), the thickness ratio of the surface layer A layer to the core layer B layer is 1:1-3:1, and the total thickness is controlled at 15-50μm; the polypropylene heat-sealing resin is a binary or ternary copolymer polypropylene, and the melt flow rate is 5-10 g / 10min.

[0014] As a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, wherein: the biaxial stretching in step (5) is to first stretch longitudinally and then stretch transversely; the longitudinal stretching ratio is 4-6 times, the stretching temperature is 120-140℃, the transverse stretching ratio is 8-10 times, the stretching temperature is 150-170℃, and after stretching, heat setting treatment is performed at a temperature of 160-170℃ for 5-15 seconds.

[0015] In a preferred embodiment of the method for preparing the high-barrier polypropylene film of the present invention, the surface activation treatment in step (6) is corona treatment or plasma treatment.

[0016] In a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, the high-barrier coating is an alumina coating or a silicon oxide coating, and the coating thickness is 20-100 nm; the physical vapor deposition is vacuum evaporation or magnetron sputtering.

[0017] As a preferred embodiment of the preparation method of the high-barrier polypropylene film of the present invention, the method further includes (7) a protective coating step after step (6): coating a layer of water-based polyurethane or acrylate protective coating on the surface of the film on which the high-barrier coating has been deposited, with a dry film thickness of 0.5-2 μm.

[0018] The beneficial effects of this invention are as follows: This invention achieves a synergistic effect through a dual barrier mechanism of "organic modified nanomaterial bulk modification + high-barrier surface coating". The organically modified montmorillonite forms an oriented "maze effect" after biaxial stretching, and the surface alumina coating forms a dense physical barrier, reducing oxygen permeability to as low as 0.5-0.8 cm⁻¹. 3 / (m 2(24h·0.1MPa), far superior to single modification methods. After plasma activation, the surface roughness and polar groups of the nano-modified base film increase, and the adhesion of the alumina coating reaches Grade 1 of the cross-cut adhesion test (GB / T 9286), solving the industry problem of easy coating peeling. The introduction of PBAT biodegradable material improves the environmental properties of the film; the three-layer co-extrusion structure design, in which the modified masterbatch is added only to the core layer, facilitates the recycling and reuse of polypropylene film. Tensile strength ≥140 MPa, elongation at break ≥130%, meeting the requirements for packaging material processing and use. Compatible with existing BOPP production lines, requiring no major equipment modifications, and with controllable costs. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a schematic diagram of the preparation method provided by the present invention. Detailed Implementation

[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] This invention provides a method for preparing a high-barrier polypropylene film, comprising the following steps: (1) Preparation of organic modified nano barrier agent: Disperse the nano inorganic barrier agent in a solvent, add an organic intercalating agent to carry out a cation exchange reaction, and obtain an organic modified nano barrier agent with an interlayer spacing of more than 2.5 nm. (2) Preparation of modified masterbatch: The organic modified nano barrier agent and the first compatibilizer obtained in step (1) are mixed with polypropylene base material, and then melt-blended and extruded, and granulated to obtain modified masterbatch; (3) Preparation of blended modified granules: The modified masterbatch obtained in step (2) is mixed with polypropylene base resin, biodegradable polar polymer and second compatibilizer, and then melt-blended and extruded to granulate to obtain blended modified granules. (4) Multi-layer co-extrusion casting: Using an ABA three-layer co-extrusion structure, polypropylene heat-sealing resin is used as the surface material, and the blended modified granules obtained in step (3) are used as the core material. After multi-layer co-extrusion and casting, a three-layer co-extrusion thick sheet is obtained. (5) Biaxial stretching: The three-layer co-extruded thick sheet obtained in step (4) is biaxially stretched to obtain a nano-modified polypropylene base film. (6) Surface activation and coating: The base film obtained in step (5) is surface activated, and then a high-barrier coating is deposited on the activated surface by physical vapor deposition. (7) Protective coating: A protective coating is applied to the surface of the film on which the high-barrier coating has been deposited to obtain a high-barrier polypropylene film.

[0022] Example 1

[0023] (1) Preparation of organically modified montmorillonite: 100 g of sodium-based montmorillonite (cation exchange capacity 100 mmol / 100 g) was dispersed in 2 L of deionized water and heated to 80 °C. 30 g of octadecyltrimethylammonium chloride was dissolved in 500 mL of deionized water and slowly added to the montmorillonite suspension, and the mixture was stirred for 4 hours. The reaction product was filtered, washed with deionized water until no chloride ions were detected (silver nitrate detection), dried at 60 °C for 24 hours, and ground through a 300-mesh sieve to obtain organically modified montmorillonite (OMMT). XRD analysis showed that the interlayer spacing of the modified montmorillonite increased from 1.2 nm to 2.9 nm.

[0024] (2) Preparation of modified masterbatch: Take 10 kg of OMMT, 5 kg of PP-g-MAH (grafting rate 1.0%), and 85 kg of polypropylene base material (F800E, MFR 3.0 g / 10min), and mix them in a high-speed mixer for 10 minutes. Then feed them into a twin-screw extruder with the following extrusion temperatures: Zone 1 170℃, Zone 2 185℃, Zone 3 195℃, Zone 4 200℃, Zone 5 205℃, Die head 210℃, Screw speed 300 rpm, and Feed rate 20 kg / h. Extrude and granulate to obtain the modified masterbatch.

[0025] (3) Preparation of blended modified granules: Take 20 kg of modified masterbatch, 5 kg of PBAT (C1200) and 75 kg of polypropylene base resin (F800E), mix them evenly, and then granulate them again through a twin-screw extruder at the same extrusion temperature to obtain the blended modified granules.

[0026] (4) Multi-layer co-extruded sheets: A three-layer co-extrusion casting unit was used. Extruder A (surface layer) added binary copolymer polypropylene heat-sealing resin (4% ethylene content, MFR 7 g / 10min), extruder B (core layer) added blended modified granules, and extruder C (another surface layer) was the same as A. Extrusion temperatures were: Zone 1 180℃, Zone 2 200℃, Zone 3 220℃, Zone 4 230℃, Zone 5 235℃; die temperature 240℃; extrusion pressure 12MPa. The melt flowed out through a T-die and was cast onto cooling rollers to obtain a three-layer sheet with a total thickness of 200μm. The thickness ratio of each layer was A:B:A = 1:3:1 (40μm for each surface layer and 120μm for the core layer).

[0027] (5) Biaxial tension: The thick sheet is fed into a biaxial stretching machine: it is stretched longitudinally by 5 times at 130°C, stretched transversely by 9 times at 160°C, and heat-set at 165°C for 10 seconds to obtain a three-layer co-extruded base film with a total thickness of 20μm (4μm for each surface layer and 12μm for the core layer).

[0028] (6) Surface activation and coating: The base film was subjected to plasma activation treatment in a vacuum coating machine: vacuum degree 10 Pa, argon atmosphere, power 500 W, time 30 seconds. Then, the vacuum was evacuated to 3 × 10⁻⁶ Pa. -4 Pa was used to evaporate alumina (99.99% purity) using an electron beam at an evaporation source temperature of 1800℃, a deposition rate of 2nm / s, and a coating thickness of 50nm.

[0029] (7) Applying a protective coating A water-based polyurethane protective coating was applied using a gravure coating machine and dried at 80°C after coating, with a coating thickness of 1μm. The film was then wound up and slit to obtain the finished film.

[0030] It should be noted that the interlayers of montmorillonite originally contained exchangeable Na. + Ca 2+ Isocations. In solution, organic quaternary ammonium salt cations enter the interlayer of montmorillonite via ion exchange:

[0031] After the reaction, organic long-chain alkylammonium cations are inserted between the montmorillonite layers, increasing the interlayer spacing from approximately 1.2 nm to over 2.5 nm. Regarding the compatibilization reaction mechanism of PP-g-MAH and PBAT: The maleic anhydride groups in PP-g-MAH can undergo esterification with the hydroxyl groups at the ends of PBAT to form a graft copolymer, thus improving the compatibility between the two phases. PP-g-MAH (containing maleic anhydride ring) + Example 2

[0032] The experiment was basically the same as in Example 1, except that the organically modified montmorillonite was replaced with nano-vermiculite (also organically modified), while other conditions remained unchanged.

[0033] Example 3

[0034] The method is basically the same as in Example 1, except that the amount of PBAT added is increased to 8 parts (correspondingly reducing the amount of base resin), while other conditions remain unchanged.

[0035] Comparative Example 1 Ordinary BOPP film (unmodified, uncoated).

[0036] Comparative Example 2 BOPP film with only unmodified montmorillonite (without organic intercalation).

[0037] Comparative Example 3 BOPP film with only aluminum oxide coating on the surface (no nano-modification).

[0038] Comparative Example 4 BOPP film with only PBAT added (no nanomaterials).

[0039] Performance test results

[0040] Table 1: Performance Test Table The preparation method of the high-barrier polypropylene film proposed in this invention has been described in detail above, and the principle and implementation of this invention have been explained. The above description of the embodiments is only for the purpose of helping to understand the method and core idea of ​​this invention. At the same time, for those skilled in the art, there will be changes in the specific implementation and application scope based on the idea of ​​this invention. Therefore, the content of this specification should not be construed as a limitation of this invention.

Claims

1. A process for the preparation of a high barrier polypropylene film, characterized in that: Includes the following steps: S1: The inorganic nano barrier agent and the organic intercalating agent are subjected to a cation exchange reaction to obtain an organically modified nano barrier agent with an interlayer spacing of more than 2.5 nm. S2: The obtained organic modified nano barrier agent, the first compatibilizer and polypropylene base material are mixed, melt-blended and extruded, and granulated to obtain modified masterbatch; S3: The obtained modified masterbatch is mixed with polypropylene base resin, biodegradable polar polymer and second compatibilizer, and then melt-blended and extruded to obtain blended modified granules. S4: Using an ABA three-layer co-extrusion structure, polypropylene heat-sealing resin is used as the surface material and blended modified granules are used as the core material. Through multi-layer co-extrusion and casting, a three-layer co-extruded thick sheet is obtained. S5: The obtained three-layer co-extruded thick sheet is biaxially stretched to obtain a nano-modified polypropylene base film; S6: The obtained base film is surface activated, and then a high-barrier coating is deposited on the activated surface by physical vapor deposition to obtain a high-barrier polypropylene film.

2. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: The nano-inorganic barrier agent in step (1) is one or more of montmorillonite, vermiculite or kaolin; the organic intercalating agent is a long-chain alkyl quaternary ammonium salt, with a general formula of [R1R2R3R4N] + X - wherein R1 is C12-C18 alkyl, R2, R3, R4 are methyl or ethyl, and X is Cl or Br.

3. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: The cation exchange reaction temperature in step (1) is 60-100℃ and the reaction time is 2-6 hours; the interlayer spacing of the organically modified nanobarrier is 2.5-3.5nm.

4. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: The first compatibilizer in step (2) is polypropylene grafted with maleic anhydride, with a grafting rate of 0.5%-1.5%; the mass ratio of the organic modified nano barrier agent, the first compatibilizer and the polypropylene base material is 5-20:2-8:72-93.

5. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: The biodegradable polar polymer in step (3) is one or more of PBAT, PBS or PLA; the second compatibilizer is polypropylene grafted with maleic anhydride or ethylene-acrylic acid copolymer; the mass ratio of the modified masterbatch, the biodegradable polar polymer and the polypropylene base resin is 10-30:2-10:60-88.

6. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: In step (4), the three-layer co-extrusion structure has a thickness ratio of surface layer A to core layer B of 1:1-3:1, and the total thickness is controlled at 15-50μm; the polypropylene heat-sealing resin is a binary or ternary copolymer polypropylene with a melt flow rate of 5-10 g / 10min.

7. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: In step (5), the bidirectional stretching is performed first in the longitudinal direction and then in the transverse direction. The longitudinal stretching ratio is 4-6 times and the stretching temperature is 120-140℃. The transverse stretching ratio is 8-10 times and the stretching temperature is 150-170℃. After stretching, heat setting is performed at a temperature of 160-170℃ for 5-15 seconds.

8. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: The surface activation treatment in step (6) is either corona treatment or plasma treatment.

9. The method for preparing a high-barrier polypropylene film according to claim 1, characterized in that: The high-barrier coating is an aluminum oxide coating or a silicon oxide coating, with a coating thickness of 20-100 nm; the physical vapor deposition is vacuum evaporation or magnetron sputtering.

10. The method for preparing a high-barrier polypropylene film according to claim 8, characterized in that: The step (6) is followed by (7) a protective coating coating step: a water-based polyurethane or acrylate protective coating is coated on the surface of the film on which the high-barrier coating has been deposited, with a dry film thickness of 0.5-2 μm.