A method for preparing ferrous phosphide / carbon composite materials using Joule heating of waste lithium iron phosphate

By employing Joule heating technology and resistance feedback control strategy, ferrous phosphide/carbon composite materials can be directly prepared using waste lithium iron phosphate, solving the problems of high energy consumption and phase agglomeration, and realizing the preparation of ferrous phosphide/carbon composite materials with high efficiency and low cost.

CN123105569APending Publication Date: 2026-11-17XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611438554.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing ferrous phosphide/carbon composites suffer from high energy consumption, prolonged high-temperature treatment leading to lithium salt volatilization and phase aggregation, and traditional methods use dangerous and expensive phosphorus sources.

Method used

Joule heating technology was used to encapsulate waste lithium iron phosphate and control the resistance change. A resistance feedback control strategy was used to achieve rapid heating and prepare ferrous phosphide/carbon composite material, avoiding the defects of high-temperature sintering, and using Fe-P elements in waste batteries as raw materials.

Benefits of technology

The rapid preparation of high-purity ferrous phosphide/carbon composite material was achieved, reducing energy consumption, avoiding lithium salt volatilization and phase agglomeration, and forming microcrystalline Fe2P particles uniformly dispersed in the carbon matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105569A_ABST
    Figure CN123105569A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing ferrous phosphide / carbon composite materials from waste lithium iron phosphate using Joule heating. The method involves encapsulating waste black powder containing iron phosphate and graphite within conductive carbon paper; applying two high-power Joule pulse discharges under an inert protective atmosphere, utilizing the rapid temperature rise from Joule heating to trigger a vigorous carbothermic reduction reaction, driving the lithium iron phosphate to transform into a high-purity ferrous phosphide / carbon composite material. This invention overcomes the drawbacks of traditional high-temperature sintering methods, such as long processing time, high energy consumption, and easy particle coarsening and agglomeration, achieving a high-value green recycling of valuable iron and phosphorus elements from waste batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of battery recycling and high-value resource utilization of waste, specifically relating to a method for preparing ferrous phosphide / carbon composite material by using Joule heating of waste lithium iron phosphate. Background Technology

[0002] With the rapid development of the new energy vehicle industry, the number of retired lithium iron phosphate (LiFePO4) batteries has exploded. The "black powder" obtained from the mixed crushing of retired positive and negative electrodes is rich in valuable metal elements such as iron, phosphorus, and lithium, as well as highly conductive graphite negative electrodes. Traditional wet recycling processes consume large amounts of concentrated inorganic acids (such as concentrated sulfuric acid) and strong hydrogen peroxide reducing agents. Not only is the purification of iron and phosphorus precipitation in the leachate complex, but it also generates a large amount of hazardous acidic wastewater containing heavy metals. Traditional pyrometallurgical high-temperature reduction phase inversion (such as muffle furnace or tube furnace sintering) requires continuous high-temperature baking for several hours to tens of hours, with an extremely slow heating rate (usually <10℃ / min). This not only consumes a lot of energy, but also causes uncontrolled vaporization and volatilization of lithium salts due to prolonged high temperatures, making the phases easily agglomerate and form a mixture of impurities that are difficult to separate.

[0003] Ferrous phosphide (Fe2P) is considered a promising high-performance electrode material due to its metalloid-like high conductivity, excellent theoretical lithium / sodium storage capacity, and good intrinsic activity in electrocatalysis. However, current artificial synthesis of Fe2P typically relies on white phosphorus, red phosphorus, or highly toxic hypophosphite as phosphorus sources, which are extremely dangerous and costly processes. If the Fe-P elements readily available in waste LiFePO4 black powder could be used as raw materials and directly converted into nano-Fe2P / C composite materials in situ using associated graphite carbon, the dual value of "waste treatment and high-value regeneration" could be achieved. Joule heating technology utilizes the material's own ohmic resistance for instantaneous discharge, achieving heating rates of several thousand degrees per second. However, waste lithium iron phosphate itself has uneven conductivity, making it prone to localized thermal runaway and ejection under Joule thermal shock, and the volatilization and phase evolution of lithium are difficult to control precisely. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing ferrous phosphide / carbon composite materials by using Joule heating of waste lithium iron phosphate. This method eliminates the drawbacks of traditional high-temperature sintering, such as long time consumption, high energy consumption, and easy coarsening and agglomeration of particles, and realizes the high-value green recycling of valuable iron and phosphorus elements in waste batteries.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing ferrous phosphide / carbon composite materials using Joule heating of waste lithium iron phosphate includes the following steps:

[0007] (1) The waste lithium iron phosphate battery is placed in a conductive carbon carrier for encapsulation to form the reactant;

[0008] (2) The reactant is placed in the Joule heating reaction chamber, and the two ends of the reactant are electrically connected to the power supply electrodes, and an inert protective gas is introduced into the Joule heating reaction chamber.

[0009] (3) Apply voltage and current to the reactant to perform the first stage of Joule heating, and simultaneously collect the voltage across the reactant and the current through the reactant to determine the real-time resistance of the reactant; determine the reaction state of the reactant based on the change of the real-time resistance R relative to the initial resistance / R0 R / R0 and / or the rate of change of the real-time resistance dR / dt; when R / R0 and / or dR / dt reach a first preset threshold, convert the first stage of Joule heating to the second stage of Joule heating;

[0010] (4) During the second stage of Joule heating, when at least one of R / R0 and dR / dt reaches the second preset threshold, Joule heating is stopped, and the reaction products are collected under an inert protective atmosphere to obtain the Fe2P / C composite material.

[0011] Preferably, before step (1), a delithiation pretreatment step is also included: placing the waste lithium iron phosphate battery raw material in an acidic or neutral leachate containing an oxidant for oxidative leaching, so that lithium ions are transferred into the liquid phase, and iron and phosphorus are retained in the filter residue and converted into iron phosphate; after solid-liquid separation, the lithium-rich filtrate is collected, and the washed and dried filter residue is used as the waste lithium iron phosphate battery in step (1), wherein the filter residue contains iron phosphate and carbon.

[0012] Preferably, the oxidant in the leachate is selected from at least one of ammonium persulfate, sodium persulfate, and hydrogen peroxide; the leaching temperature is 25–80°C, the solid-liquid ratio is 10–100 g / L, and the reaction time is 0.5–4 h.

[0013] Preferably, the first preset threshold is R / R0 ≤ 0.9 and / or dR / dt ≤ -0.05Ω / s; the second preset threshold is at least one of R / R0 ≤ 0.3 and |dR / dt| ≤ 0.01Ω / s.

[0014] Preferably, the supply voltage of the first stage is 10-20V and the supply current of the first stage is 10-30A; the supply voltage of the second stage is 25-50V and the supply current of the second stage is 50-80A.

[0015] Preferably, the material equilibrium temperature in the first stage is 400–800°C and the heating time is 5–30 seconds; the material equilibrium temperature in the second stage is 1000–1400°C and the heating time is 10–90 seconds.

[0016] Preferably, in step (1), the conductive carbon carrier is selected from at least one of carbon paper, graphite paper, carbon cloth, carbon felt or graphene paper.

[0017] Preferably, in step (2), the inert atmosphere is selected from nitrogen or argon, and the gas flow rate is 50 to 500 mL / min.

[0018] The present invention also proposes a ferrous phosphide / carbon composite material prepared by the above method, wherein the ferrous phosphide / carbon composite material consists of microcrystalline Fe2P particles uniformly dispersed in a carbon matrix.

[0019] The present invention further proposes an electrode sheet for an electrochemical energy storage device, comprising a current collector and an active material layer disposed on the current collector, wherein the active material layer comprises the aforementioned ferrous phosphide / carbon composite material.

[0020] Compared with existing technical solutions, the present invention has the following advantages:

[0021] (1) The present invention uses Joule heating to prepare Fe2P / C composite material. The preparation process takes tens of seconds and the reaction cycle is short: traditional furnace tube reduction takes 6-12 hours, which greatly reduces the preparation cost.

[0022] (2) The Fe2P / C composite material prepared by this invention has high phase purity and excellent microstructure: rapid heating and cooling avoid the defects of excessive growth and agglomeration of iron and phosphorus particles in conventional sintering. The graphite carbon and carbon paper substrate limit grain coarsening and form a unique structure of Fe2P active microspheres. Attached Figure Description

[0023] Figure 1 The images show the microstructure of the Fe2P / C composite material prepared in Example 1 under a scanning electron microscope (SEM), where a is an SEM image at a scale of 20 μm and b is an SEM image at a scale of 10 μm.

[0024] Figure 2 The X-ray diffraction (XRD) phase pattern of the Fe2P / C composite material prepared in Example 1. Detailed Implementation

[0025] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0026] Example 1

[0027] A method for preparing ferrous phosphide / carbon composite materials using Joule heating of waste lithium iron phosphate includes the following steps:

[0028] (1) Take 2.0g of industrial black powder (mainly LiFePO4 and graphite) from waste lithium iron phosphate battery raw materials after discharge, crushing, sorting and passing through a 200-mesh sieve; prepare a composite oxidation system of ammonium persulfate and hydrogen peroxide, add the industrial black powder to the above composite oxidation system, the solid-liquid ratio is 500g / L, and stir at 40-60℃ for 2h to transfer lithium ions in the black powder into the liquid phase, and oxidize and delithiate LiFePO4 to FePO4 and leave it in the filter residue; collect the lithium-rich filtrate after solid-liquid separation, and precipitate it as lithium carbonate after subsequent treatment; use the washed and dried filter residue as waste lithium iron phosphate battery, the filter residue contains iron phosphate and carbon.

[0029] Take a flexible, highly conductive carbon paper with a thickness of 0.2 mm, spread waste lithium iron phosphate battery powder evenly in the center of the carbon paper, and tightly roll it up to form a cylindrical reactant.

[0030] (2) Place the reactant into a custom Joule heating reaction chamber. The two ends of the reactant are clamped with graphite clamp electrodes. After evacuation, high-purity nitrogen gas (flow rate 150 mL / min) is introduced to maintain a slightly positive pressure protective environment.

[0031] (3) To further improve process controllability, the present invention adopts a resistance feedback control strategy.

[0032] The power supply parameters for the first and second stages of Joule heating are set: the supply voltage for the first stage is 10–20V, and the supply current is 10–30A; the supply voltage for the second stage is 25–50V, and the supply current is 50–80A. At the instantaneous start of the first stage of Joule heating, the loop resistance is collected as the initial resistance R0. As the heating time progresses, the voltage across the reactant and the current flowing through it are collected in real time to calculate the instantaneous resistance R. Furthermore, the normalized resistance R / R0 and the rate of change of resistance dR / dt are calculated. When R / R0 drops to the first preset threshold (e.g., 0.9) or dR / dt is lower than the first preset threshold (e.g., -0.05Ω / s), the reaction is determined to have started. The programmable power supply automatically increases the supply voltage and current, switches to the second stage of Joule heating, and simultaneously collects the voltage across the reactant and the current through the reactant in real time, calculates the instantaneous resistance R, and further calculates the normalized resistance R / R0 and the rate of change of resistance dR / dt. When R / R0 drops to the second preset threshold (e.g., 0.3) and dR / dt is lower than the second preset threshold (e.g., 0.01Ω / s), the reaction is determined to be complete, the programmable power supply automatically terminates the output, and the total heating time does not exceed 80s.

[0033] The carbon paper acts as an external heating element, rapidly heating up and radiating heat inwards. The reactant particles instantly cross the carbothermic reduction thermodynamic phase transition threshold (>776℃). The residual graphite carbon inside the reactant particles works synergistically with the outer carbon paper to rapidly disrupt the original olivine lattice of iron phosphate, completely reducing pentavalent phosphorus and stripping oxygen atoms. This induces iron and phosphorus atoms to reconstruct a stable hexagonal phase of ferrous phosphide (Fe2P), which is then uniformly dispersed in the carbon matrix.

[0034] In the first stage of Joule heating, low-power heating is used, with a reaction temperature of 400-600℃. This allows the entire reactant to heat up first, resulting in a gradual change in the resistance of the reactant. In the first stage, the contact state between particles tends to be uniform, and the conductivity is homogenized. This avoids excessive local current density in the reactant, which could cause local instantaneous overheating and thus prevent incomplete reaction.

[0035] During the second stage of Joule heating, the carbothermic reduction reaction is initiated, and a dazzling white light is rapidly emitted in the reaction chamber. The reaction temperature instantly soars to 1250–1350°C. After the reaction body undergoes a violent carbothermic reduction phase transition, in the later stage of the second stage of Joule heating, Fe2P formation tends to be complete and dispersed in the carbon matrix. The conductive network is stable, the decrease of R / R0 slows down, and the absolute value of dR / dt decreases and approaches zero.

[0036] (4) After the reaction is completed, the power is automatically cut off and the solid is cooled to room temperature in situ under nitrogen flow. The solid is taken out, ground and sieved to obtain dark gray powder, i.e. Fe2P / C composite material.

[0037] SEM testing of Fe2P / C composite materials (e.g.) Figure 1 As can be seen, the Fe2P particles are submicron to micron in size and dispersed in a carbon matrix.

[0038] XRD tests were performed on the Fe2P / C composite material (e.g. Figure 2 The X-ray diffraction (XRD) pattern showed characteristic diffraction peaks of the Fe2P / C crystal plane at 2θ = 40.3°, 44.4°, 47.3°, and 52.8°. Furthermore, the diffraction peaks perfectly matched the standard card JCPDS No. 51-0943 (hexagonal Fe2P), and no residual lithium compound characteristic peaks were observed, confirming that the original phase had completely transformed into pure crystalline Fe2P / C.

[0039] The downstream of the reaction device is connected to a gas phase condensation recovery device or an acidic tail gas absorption bottle; in step (2), the lithium element volatilized during the Joule heating process enters the absorption device for recovery under the influence of the gas flow.

[0040] The above are merely preferred embodiments of the present invention and do not constitute any limitation on the present invention. Any equivalent substitutions or modifications made by those skilled in the art to the technical solutions and content disclosed in the present invention without departing from the scope of the present invention shall be deemed to have remained within the protection scope of the present invention.

Claims

1. A method for preparing ferrous phosphide / carbon composite material using Joule heating of waste lithium iron phosphate, characterized in that, Includes the following steps: (1) The waste lithium iron phosphate battery is placed in a conductive carbon carrier for encapsulation to form the reactant; (2) The reactant is placed in the Joule heating reaction chamber, and the two ends of the reactant are electrically connected to the power supply electrode, and an inert protective gas is introduced into the Joule heating reaction chamber. (3) Apply voltage and current to the reactant to perform the first stage of Joule heating, and simultaneously collect the voltage across the reactant and the current through the reactant to determine the real-time resistance of the reactant; determine the reaction state of the reactant based on the change of the real-time resistance R relative to the initial resistance / R0 R / R0 and / or the rate of change of the real-time resistance dR / dt; when R / R0 and / or dR / dt reach a first preset threshold, convert the first stage of Joule heating to the second stage of Joule heating; (4) During the second stage of Joule heating, when at least one of R / R0 and dR / dt reaches the second preset threshold, Joule heating is stopped, and the reaction products are collected under an inert protective atmosphere to obtain the Fe2P / C composite material.

2. The method according to claim 1, characterized in that, Prior to step (1), a delithiation pretreatment step is also included: Waste lithium iron phosphate battery raw materials are placed in an acidic or neutral leachate containing an oxidant for oxidation leaching, so that lithium ions are transferred into the liquid phase, while iron and phosphorus are retained in the filter residue and converted into iron phosphate; after solid-liquid separation, lithium-rich filtrate is collected, and the washed and dried filter residue is used as the waste lithium iron phosphate battery in step (1), wherein the filter residue contains iron phosphate and carbon.

3. The method according to claim 2, characterized in that, The oxidant in the leachate is selected from at least one of ammonium persulfate, sodium persulfate, and hydrogen peroxide; the leaching temperature is 25–80°C, the solid-liquid ratio is 10–100 g / L, and the reaction time is 0.5–4 h.

4. The method according to claim 1, characterized in that, The first preset threshold is R / R0 ≤ 0.9 and / or dR / dt ≤ -0.05Ω / s; The second preset threshold is at least one of R / R0≤0.3 and |dR / dt|≤0.01Ω / s.

5. The method according to claim 1, characterized in that, The supply voltage for the first stage is 10-20V, and the supply current for the first stage is 10-30A; the supply voltage for the second stage is 25-50V, and the supply current for the second stage is 50-80A.

6. The method according to claim 1, characterized in that, The material equilibrium temperature in the first stage is 400–800℃, and the heating time is 5–30s; the material equilibrium temperature in the second stage is 1000–1400℃, and the heating time is 10–90s.

7. The method according to claim 1, characterized in that, In step (1), the conductive carbon carrier is selected from at least one of carbon paper, graphite paper, carbon cloth, carbon felt or graphene paper.

8. The method according to claim 1, characterized in that, In step (2), the inert atmosphere is selected from nitrogen or argon, and the gas flow rate is 50 to 500 mL / min.

9. A ferrous phosphide / carbon composite material prepared by the method according to any one of claims 1-8, characterized in that, The ferrous phosphide / carbon composite material consists of microcrystalline Fe2P particles uniformly dispersed in a carbon matrix.

10. An electrode sheet for an electrochemical energy storage device, characterized in that, It includes a current collector and an active material layer disposed on the current collector, the active material layer comprising the ferrous phosphide / carbon composite material of claim 9.