A FePS3 carbon composite material, its preparation method and application
FePS3 carbon composite materials were prepared by temperature gradient reaction and low-temperature ball milling. By using graphite to buffer mechanical force and conductive carbon materials to construct a conductive network, the structural instability of FePS3 during ball milling was solved, and the conductivity and lithium/sodium ion transport efficiency were improved.
Patent Information
- Application Number
- CN202611244343.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, when FePS3 is combined with carbon materials, the mechanical force during ball milling causes the crystal structure to become unstable and easily decompose, affecting electrical conductivity and electrochemical performance.
Layered FePS3 crystals were prepared by temperature gradient reaction and then composited with graphite and conductive carbon materials at low temperature. The buffering effect of graphite and the conductive carbon materials were used to construct a three-dimensional conductive network, forming more conductive paths and improving conductivity.
By maintaining the layered crystal structure of FePS3, the electrical conductivity of the composite material and the transport kinetics of lithium/sodium ions were improved, thus enhancing the energy storage performance.
Smart Images

Figure CN123105571A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of energy materials technology, and in particular to a FePS3 carbon composite material, its preparation method, and its application. Background Technology
[0002] With the rapid development of energy storage technology, developing battery electrode materials with high energy density and excellent cycle stability has become an important direction for improving the performance of lithium-ion and sodium-ion batteries. Layered materials, due to their atomic-scale thickness, high specific surface area, and structural features conducive to ion transport, have attracted widespread attention in the energy storage field. Among them, metal phosphide chalcogenides (MPS)... x M (representing transition metals such as Fe, Co, Ni, Mn, Sn, and Bi) exhibits significant application potential in optoelectronic devices, catalysis, and battery anode materials due to its unique two-dimensional layered structure and abundant electrochemical active sites. In MPS... x In this structure, metal cations are located between sulfur atom layers, and phosphorus atoms are orderly embedded in the crystal lattice structure. This structure can provide active centers for phosphorus and sulfur dual anions and form ion transport channels, enabling the material to undergo alloying and conversion reactions during lithium / sodium ion storage, thus exhibiting a high theoretical specific capacity.
[0003] As a typical metal phosphochalcogenide compound, FePS3 exhibits excellent lithium / sodium storage performance. The Fe and P elements in FePS3 can participate in multi-electron transfer processes, providing abundant active sites for lithium / sodium ion insertion and reaction. Simultaneously, the high electronegativity of S element promotes lithium / sodium ion insertion and extraction. However, FePS3 still suffers from low conductivity and volume expansion during charge and discharge, leading to reduced charge transport efficiency and limiting its practical application in lithium / sodium ion batteries. Currently, combining FePS3 with carbon materials is considered an effective way to improve these problems. By constructing a conductive network using carbon materials, ion / electron transport efficiency can be improved, and volume changes during cycling can be mitigated, thereby improving the electrochemical performance of the electrode material.
[0004] Currently, the composite of FePS3 and carbon materials is typically achieved using methods such as ball milling. However, during ball milling, the high-speed movement of the milling media generates strong mechanical forces between the balls and the jar, while friction also generates heat. This makes it difficult to maintain the stability of the FePS3 crystal structure, and some FePS3 decomposes and transforms into Fe7S8, thus affecting the structural integrity and electrochemical performance of the composite material. Therefore, how to effectively composite FePS3 with carbon materials while maintaining the layered crystal structure of FePS3 and improving the electrical conductivity of the composite material is a pressing technical problem that needs to be solved. Summary of the Invention
[0005] To overcome the shortcomings of existing technologies, the purpose of this invention is to provide a FePS3 carbon composite material, its preparation method, and its application. By combining graphite with FePS3 layered crystals, the mechanical force during ball milling is buffered, preventing the decomposition of FePS3 during ball milling. At the same time, a three-dimensional conductive network is constructed using conductive carbon materials to form more conductive paths, thereby improving the conductivity of the composite material, enhancing the transport kinetics of lithium / sodium ions, and improving the lithium / sodium storage performance of the material.
[0006] To achieve the above objectives, the present invention provides the following solution: In a first aspect, the present invention provides a method for preparing FePS3 carbon composite material, comprising the following steps: S1. Iron source, phosphorus source, sulfur source and transport agent are added to the reaction vessel, and after vacuum sealing, a temperature gradient reaction is carried out. After cooling, layered FePS3 crystals are obtained. S2. The layered FePS3 crystals are mixed with carbon materials and ball-milled under an inert atmosphere and low temperature to combine the FePS3 crystals with the carbon materials, thereby obtaining FePS3 carbon composite materials.
[0007] Preferably, in step S1, the iron source is iron powder, the phosphorus source is phosphorus powder, the sulfur source is sulfur powder, the transport agent is iodine, the molar ratio of the iron powder, phosphorus powder and sulfur powder is 1:1:3, and the mass of the iodine accounts for 2 to 5% of the total mass of the iron powder, phosphorus powder and sulfur powder.
[0008] Preferably, in step S1, the temperature of the high-temperature zone of the temperature gradient reaction is 500~700℃, the temperature of the low-temperature zone is 500~650℃, and the temperature difference between the high-temperature zone and the low-temperature zone is not less than 30℃; during the reaction, the iron source, phosphorus source and sulfur source are placed in the high-temperature zone, and the reaction time is 48~120 hours.
[0009] Preferably, in step S2, the carbon material includes graphite and conductive carbon material, wherein the conductive carbon material is selected from at least one of carbon nanotubes, carbon fibers, superconducting carbon black, porous carbon, and graphene.
[0010] Preferably, the carbon material contains 60-90% graphite by mass.
[0011] Preferably, the mass ratio of the layered FePS3 crystals to the carbon material is 1:1 to 4:1.
[0012] Preferably, in step S2, the inert atmosphere is selected from one or more of argon and nitrogen, and the low temperature condition is that the ambient temperature is controlled not to exceed 30°C during the ball milling process.
[0013] Preferably, during the ball milling process, the ball-to-material ratio is 40-100:1, the ball milling speed is 300-700 r / min, and the ball milling time is 8-30 hours.
[0014] Secondly, the present invention provides a FePS3 carbon composite material prepared according to the above preparation method, wherein the FePS3 carbon composite material comprises layered FePS3 crystals and carbon material composited with the layered FePS3 crystals.
[0015] Thirdly, the present invention provides an application of the above-mentioned FePS3 carbon composite material, wherein the FePS3 carbon composite material is used as a negative electrode active material for preparing lithium-ion batteries or sodium-ion batteries.
[0016] Compared with the prior art, the present invention discloses at least the following technical effects: (1) The present invention combines graphite with FePS3 layered crystals. By utilizing the fact that both graphite and FePS3 have a layered structure and are connected by van der Waals forces, graphite can be combined with two-dimensional FePS3 layered crystals. During ball milling, the mechanical force is buffered, and FePS3 is prevented from decomposing due to mechanical action, which is beneficial to maintaining the FePS3 layered crystal structure.
[0017] (2) This invention combines FePS3 with carbon materials to construct a three-dimensional conductive network using conductive carbon materials, forming more conductive paths, improving the conductivity of the composite material, and providing more efficient ion transport channels, reducing the diffusion paths of lithium / sodium ions, enhancing the transport dynamics of lithium / sodium ions, thereby improving the lithium / sodium storage performance of the material.
[0018] (3) The present invention uses temperature gradient reaction to prepare layered FePS3 crystals and combines low temperature ball milling composite method to prepare FePS3 carbon composite material. The preparation process does not require complicated treatment and has the advantages of simple operation and high efficiency. Furthermore, the obtained FePS3 carbon composite material can be used as a negative electrode material for lithium-ion batteries and sodium-ion batteries, and has potential application value in other energy storage and electrochemical related fields. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 The X-ray diffraction pattern of the FePS3 crystal prepared in Example 1 of this invention is shown.
[0021] Figure 2 This is a scanning electron microscope image of the FePS3 crystal prepared in Example 1 of the present invention.
[0022] Figure 3 The X-ray diffraction pattern of the FePS3 carbon composite material prepared in Example 1 of this invention is shown.
[0023] Figure 4 This is a scanning electron microscope image of the FePS3 carbon composite material prepared in Example 1 of the present invention.
[0024] Figure 5 This is a transmission electron microscope image of the FePS3 carbon composite material prepared in Example 1 of the present invention.
[0025] Figure 6 The rate performance diagram shows the FePS3 carbon composite material prepared in Example 1 of this invention as the negative electrode of a lithium-ion battery.
[0026] Figure 7 The graph shows the rate performance of the FePS3 carbon composite material prepared in Example 2 of this invention as the negative electrode of a sodium-ion battery.
[0027] Figure 8 The X-ray diffraction pattern is shown for the material prepared in Comparative Example 1 of this invention. Detailed Implementation
[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] This invention prepares layered FePS3 crystals through a temperature gradient reaction, and then utilizes the layered buffering effect of graphite and the conductive network construction effect of conductive carbon materials to achieve stable composite of FePS3 and carbon materials under low-temperature ball milling conditions. This solves the problems of low conductivity of FePS3 and easy structural decomposition during ball milling composite process. The specific steps include the following: First, iron, phosphorus, sulfur and transport agent are added to the reaction vessel, and after vacuum sealing, a temperature gradient reaction is carried out. After cooling, layered FePS3 crystals are obtained.
[0030] Specifically, iron powder, phosphorus powder, and sulfur powder are selected as reaction raw materials, and iodine is used as a transport agent. The iron powder, phosphorus powder, and sulfur powder are mixed in a molar ratio of 1:1:3, and the amount of iodine added accounts for 2-5% of the total mass of the iron powder, phosphorus powder, and sulfur powder.
[0031] After the above raw materials are mixed evenly, they are placed in a reaction vessel, and then sealed after being vacuumed to avoid the influence of the external atmosphere on the crystal formation process during the reaction.
[0032] Subsequently, the sealed reaction vessel was placed in a temperature gradient reaction environment for reaction, wherein the temperature of the high-temperature zone was controlled at 500~700℃, the temperature of the low-temperature zone was controlled at 500~650℃, and the temperature difference between the high-temperature zone and the low-temperature zone was not less than 30℃. During the reaction, the iron source, phosphorus source and sulfur source were placed at the high-temperature end, and the reaction time was 48~120 hours.
[0033] Under the influence of a temperature gradient, the reactants react at the high-temperature end and generate a gas-phase transport process, and then deposit and grow in the lower-temperature region to form FePS3 crystals with a layered structure.
[0034] In this invention, FePS3 crystals possess a layered structure, providing abundant electrochemical active sites when used as a negative electrode material in lithium-ion or sodium-ion batteries. However, FePS3 itself has low electrical conductivity, and during the traditional ball milling composite process, the high-speed movement of the milling media generates significant mechanical forces and frictional heat, easily leading to the destruction of the FePS3 layered crystal structure and further decomposition to form Fe7S8, thus affecting material performance. Therefore, the obtained layered FePS3 crystals are mixed with carbon materials and ball-milled under an inert atmosphere and low-temperature conditions to fully composite the FePS3 crystals with the carbon materials, yielding a FePS3-carbon composite material.
[0035] Specifically, layered FePS3 crystals are mixed with carbon materials at a mass ratio of 1:1 to 4:1. The carbon materials include graphite and conductive carbon materials, with the conductive carbon materials selected from at least one of carbon nanotubes, carbon fibers, superconducting carbon black, porous carbon, and graphene. Furthermore, the mass percentage of graphite in the carbon materials is 60% to 90%.
[0036] The mixed FePS3 crystals and carbon materials were placed in a ball mill and milled under an inert atmosphere. The inert atmosphere was selected from one or more of argon and nitrogen to reduce the possibility of oxidation reactions during the ball milling process.
[0037] Meanwhile, the ambient temperature is controlled to be no higher than 30℃ during the ball milling process to reduce the impact of heat generated by friction during high-speed ball milling on the FePS3 crystal structure.
[0038] Furthermore, during the ball milling process, the ball-to-material ratio is controlled at 40~100:1, the ball milling speed is controlled at 300~700 r / min, and the ball milling time is controlled at 8~30 hours, so that the FePS3 crystals and carbon materials can fully contact each other and form a stable composite structure, thus obtaining the FePS3 carbon composite material.
[0039] Both graphite and FePS3 have a layered structure, and the layers are connected by van der Waals forces. Therefore, graphite can combine with the two-dimensional FePS3 layered crystals, buffering the external mechanical forces during ball milling, reducing the destructive effect of mechanical forces on the FePS3 crystal structure, preventing the decomposition of FePS3 during ball milling, and helping to maintain the FePS3 layered crystal structure.
[0040] Meanwhile, conductive carbon materials can construct a three-dimensional conductive network around FePS3 crystals, forming more conductive paths, improving the conductivity of the composite material, and providing more efficient transport paths for lithium / sodium ion migration, reducing diffusion barriers and enhancing ion transport kinetics. Therefore, through the protective effect of graphite structure and the conductivity-enhancing effect of conductive carbon materials, the resulting FePS3 carbon composite material possesses both structural integrity and excellent electrochemical transport performance.
[0041] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. The instruments used in the following embodiments are as follows: Small dual-temperature zone tube furnace OTF-1200X-S-II, Hefei Kejing Materials Technology Co., Ltd.; Low-temperature planetary ball mill XQM-2-DW, Changsha Tianchuang Powder Technology Co., Ltd.; Constant temperature testing integrated machine MIHW-200-160CH, Shenzhen Xinwei Electronics Co., Ltd.
[0042] Example 1 This embodiment provides a method for preparing FePS3 carbon composite material, the steps of which are as follows: 335.2 mg of iron powder (99.99%), 186 mg of red phosphorus (99.9%) and 576 mg of sulfur powder (99.99%) were used as raw materials for the reaction, and 20-30 mg of elemental iodine (99.9%) was added as a transport agent.
[0043] After mixing the above raw materials evenly, place them in a quartz tube and heat them at 5×10⁻⁶ mm. -5 Torr seals the quartz tube under high vacuum conditions.
[0044] Subsequently, the sealed quartz tube was placed in a dual-temperature zone tube furnace for a temperature gradient reaction, with the high-temperature zone at 600°C and the low-temperature zone at 550°C, for a reaction time of 72 hours, and the reaction raw materials were placed at the high-temperature end.
[0045] After the reaction was completed, the dual-temperature zone tube furnace was slowly cooled to room temperature over 8 hours, and layered FePS3 crystals were collected in the low-temperature zone.
[0046] The obtained FePS3 crystal was characterized by X-ray diffraction pattern, and the results are as follows: Figure 1As shown, the obtained diffraction peaks match the FePS3 standard PDF card (PDF#78-0496), and no obvious impurity peaks are observed, indicating that pure phase FePS3 crystals were successfully prepared through temperature gradient reaction.
[0047] The obtained FePS3 crystals were further characterized by scanning electron microscopy, and the results are as follows: Figure 2 As shown, FePS3 crystals exhibit a layered stacked structure with obvious layered structural characteristics.
[0048] Then, in an argon-filled glove box, 90g of zirconia grinding balls, 1.05g of the FePS3 crystals prepared above, 0.3g of graphite, and 0.15g of carbon nanotubes were added to a 50mL zirconia ball milling jar. The mass ratio of FePS3 crystals to carbon materials was 7:3, and the carbon materials consisted of graphite and carbon nanotubes.
[0049] After feeding, the ball mill jar was sealed to maintain an argon protective atmosphere inside. The sealed jar was then placed in a low-temperature planetary ball mill, and the internal temperature was controlled to not exceed 15°C using a cold air cooling system. The mill was then ball-milled at 400 r / min for 12 hours to obtain the FePS3 carbon composite material.
[0050] The obtained FePS3 carbon composite material was characterized by X-ray diffraction pattern, and the results are as follows: Figure 3 As shown, the obtained diffraction peaks still match the FePS3 standard PDF card (PDF#78-0496), and a characteristic peak of carbon material appears at about 26.5°, indicating that the FePS3 crystal structure is maintained during ball milling and that the FePS3 crystal and carbon material are effectively combined.
[0051] The obtained FePS3 carbon composite material was further characterized by scanning electron microscopy and transmission electron microscopy, and the results are as follows: Figure 4 and Figure 5 As shown, carbon materials and FePS3 sheet structures can be observed to combine with each other to form a composite structure.
[0052] Example 2 This embodiment differs from Embodiment 1 in that: 1.05g of FePS3 crystals and 0.45g of graphite were added to a 50mL zirconia ball milling jar in an argon-filled glove box. After sealing, the jar was placed in a low-temperature planetary ball mill and ball milling was performed under argon protection and an ambient temperature not exceeding 15°C. The ball milling speed was 400 r / min, and the milling time was 12 hours. After ball milling, a FePS3 / graphite composite material was obtained.
[0053] X-ray diffraction analysis was performed on the obtained material. The FePS3 / graphite composite material prepared in this embodiment is the same as that in Example 1, retaining the FePS3 crystal structure and without the corresponding diffraction peak of Fe7S8.
[0054] This further demonstrates that both graphite and FePS3 have a layered structure, and the layers are connected by van der Waals forces. Graphite can combine with the layered crystals of FePS3, which buffers the mechanical forces during ball milling and helps maintain the crystal structure of FePS3.
[0055] Example 3 This embodiment differs from Embodiment 1 in that: 1.05g of FePS3 crystals, 0.3g of graphite, and 0.15g of graphene were added to a 50mL zirconia ball mill jar in an argon-filled glove box. After sealing, the jar was placed in a low-temperature planetary ball mill and ball milling was performed under argon protection and low-temperature conditions at a speed of 400 r / min for 12 hours. After ball milling, a FePS3 / graphite / graphene composite material was obtained.
[0056] X-ray diffraction analysis of the obtained materials showed that the FePS3 / graphite / graphene composite material prepared in this embodiment was the same as that in Example 1, maintaining the FePS3 crystal structure. This demonstrates that the conductive carbon material in this invention is not limited to carbon nanotubes, and that other conductive carbon materials can also achieve stable composite of FePS3 crystals and carbon materials.
[0057] Comparative Example 1 The difference between this comparative example and Example 1 is that no graphite was added, but only 0.45g of carbon nanotubes were added as carbon material. All other preparation conditions were the same as in Example 1.
[0058] The obtained material was characterized by X-ray diffraction pattern analysis, and the results are as follows: Figure 8 As shown, diffraction peaks matching those of the Fe7S8 standard PDF card (PDF#76-2308) appear around 34.0° and 44.0°.
[0059] The results show that, in the absence of the protective effect of the graphite sheet structure, FePS3 crystals are affected by mechanical action during ball milling, resulting in structural damage and further decomposition to form Fe7S8.
[0060] Comparative Example 2 The difference between this comparative example and Example 1 is that the mass of graphite was adjusted to 0.15g and the mass of carbon nanotubes was adjusted to 0.3g, while all other preparation conditions were the same as in Example 1.
[0061] X-ray diffraction analysis of the obtained material showed that the material prepared in this comparative example was the same as that in Comparative Example 1, and also showed the diffraction peak corresponding to Fe7S8. This indicates that when the graphite ratio decreases, the buffering and protective effect of graphite on the layered structure of FePS3 weakens, leading to a decrease in the stability of the FePS3 crystal structure and decomposition.
[0062] Comparative Example 3 The difference between this comparative example and Example 1 is that the ball milling process does not use a cold air cooling method to control the ball milling environment temperature, while other preparation conditions are the same as in Example 1.
[0063] X-ray diffraction analysis of the obtained material showed that, like Comparative Example 1, the material obtained in this comparative example also exhibited diffraction peaks corresponding to Fe7S8. This further indicates that, in the absence of controlled low-temperature conditions, the frictional heat generated during ball milling promotes the destruction of the FePS3 crystal structure and leads to the decomposition of FePS3.
[0064] Application Example 1 This application example uses the FePS3 carbon composite material prepared in Example 1 as the negative electrode active material for lithium-ion battery performance testing. The steps are as follows: FePS3 carbon composite material, superconducting carbon black, and polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 7:2:1. An appropriate amount of N-methylpyrrolidone (NMP) was added and mixed evenly to obtain the electrode slurry.
[0065] The obtained electrode paste was uniformly coated onto the surface of copper foil and dried in a vacuum drying oven at 80°C for 12 hours to obtain the negative electrode sheet.
[0066] Battery assembly was performed using CR2032 button cell casings in an argon-filled glove box (with water and oxygen content both below 0.01 ppm).
[0067] The lithium-ion battery consists of a negative electrode, a Celgard 2500 separator, and a lithium metal sheet. The electrolyte is a 1 mol / L LiPF6 EC / DEC mixed solution, in which the volume ratio of EC to DEC is 1:1, and 5% fluoroethylene carbonate (FEC) and 1% vinylene carbonate (VC) are added.
[0068] After assembly, let the battery stand for at least 12 hours.
[0069] The rate performance of the obtained lithium-ion batteries was tested using a constant temperature testing machine MIHW-200-160CH.
[0070] Test results are as follows Figure 6As shown, the specific charging capacities of the FePS3 carbon composite material at current densities of 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 2A / g, 4A / g, and 8A / g are 940.9mAh / g, 822.5mAh / g, 733.3mAh / g, 643.4mAh / g, 512.8mAh / g, 362.3mAh / g, and 217.8mAh / g, respectively.
[0071] Application Example 2 This application example uses the FePS3 carbon composite material prepared in Example 1 as the negative electrode active material for sodium-ion battery performance testing. The steps are as follows: The preparation process of the negative electrode sheet is the same as in Application Example 1.
[0072] Sodium-ion batteries were assembled in an argon-filled glove box using CR2032 button cell casings, with a sodium metal sheet as the counter electrode, a glass fiber membrane as the separator, and a 1.0 mol / L NaClO4 propylene carbonate (PC) solution as the electrolyte.
[0073] After assembly, let the battery stand for at least 12 hours.
[0074] The rate performance was tested using a constant temperature testing machine MIHW-200-160CH.
[0075] Test results are as follows Figure 7 As shown, the reversible specific capacities at current densities of 0.1 A / g, 0.2 A / g, 0.5 A / g, 1.0 A / g, and 2.0 A / g are 528.2 mAh / g, 497.8 mAh / g, 468.1 mAh / g, 452.3 mAh / g, and 424.6 mAh / g, respectively.
[0076] Based on the results of Application Examples 1 and 2 above, the obtained FePS3 carbon composite material can be used as a negative electrode active material for lithium-ion batteries and sodium-ion batteries, and also has potential application value in other energy storage and electrochemical related fields.
[0077] Therefore, by employing the aforementioned FePS3 carbon composite material, its preparation method, and its application, the combination of graphite and FePS3 layered crystals buffers the mechanical force during ball milling, preventing the decomposition of FePS3 during the ball milling process. Simultaneously, the use of conductive carbon materials to construct a three-dimensional conductive network creates more conductive paths, improving the conductivity of the composite material, enhancing the transport kinetics of lithium / sodium ions, and improving the lithium / sodium storage performance of the material.
[0078] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0079] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of the present invention. Furthermore, those skilled in the art will recognize that, based on the ideas of the present invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for preparing FePS3 carbon composite material, characterized in that, Includes the following steps: S1. Iron source, phosphorus source, sulfur source and transport agent are added to the reaction vessel, and after vacuum sealing, a temperature gradient reaction is carried out. After cooling, layered FePS3 crystals are obtained. S2. The layered FePS3 crystals are mixed with carbon materials and ball-milled under an inert atmosphere and low temperature to combine the FePS3 crystals with the carbon materials, thereby obtaining FePS3 carbon composite materials.
2. The preparation method according to claim 1, characterized in that, In step S1, the iron source is iron powder, the phosphorus source is phosphorus powder, the sulfur source is sulfur powder, the transport agent is iodine, the molar ratio of the iron powder, phosphorus powder and sulfur powder is 1:1:3, and the mass of the iodine accounts for 2 to 5% of the total mass of the iron powder, phosphorus powder and sulfur powder.
3. The preparation method according to claim 1, characterized in that, In step S1, the temperature of the high-temperature zone of the temperature gradient reaction is 500~700℃, the temperature of the low-temperature zone is 500~650℃, and the temperature difference between the high-temperature zone and the low-temperature zone is not less than 30℃; during the reaction, the iron source, phosphorus source and sulfur source are placed in the high-temperature zone, and the reaction time is 48~120 hours.
4. The preparation method according to claim 1, characterized in that, In step S2, the carbon material includes graphite and conductive carbon material, wherein the conductive carbon material is selected from at least one of carbon nanotubes, carbon fibers, superconducting carbon black, porous carbon, and graphene.
5. The preparation method according to claim 4, characterized in that, The carbon material contains 60-90% graphite by mass.
6. The preparation method according to claim 1, characterized in that, The mass ratio of the layered FePS3 crystals to the carbon material is 1:1 to 4:
1.
7. The preparation method according to claim 1, characterized in that, In step S2, the inert atmosphere is selected from one or more of argon and nitrogen, and the low temperature condition is that the ambient temperature is controlled not to exceed 30°C during the ball milling process.
8. The preparation method according to claim 7, characterized in that, During the ball milling process, the ball-to-material ratio is 40~100:1, the ball milling speed is 300~700 r / min, and the ball milling time is 8~30 hours.
9. A FePS3 carbon composite material prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The FePS3 carbon composite material includes layered FePS3 crystals and carbon materials composited with the layered FePS3 crystals.
10. An application of the FePS3 carbon composite material according to claim 9, characterized in that, The FePS3 carbon composite material is used as a negative electrode active material to prepare lithium-ion batteries or sodium-ion batteries.