A method for continuous preparation of flower-like hydroxyapatite materials, its products and applications

By conducting low-temperature solvothermal reaction and spray drying in a dynamic tubular reactor, high-purity, high-specific-surface-area flower-like hydroxyapatite material was prepared, solving the problems of long preparation time, high pollution, high energy consumption and poor adsorption performance in traditional processes, and achieving efficient treatment of dye wastewater.

CN123105575APending Publication Date: 2026-11-17SHANDONG HAIHUA CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611635992.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to prepare flower-like hydroxyapatite materials with high purity, high specific surface area, and wide pore size range. Furthermore, traditional processes suffer from long reaction times, high environmental pollution, high energy consumption, and poor adsorption performance.

Method used

A low-temperature solvothermal reaction was carried out in a dynamic tubular reactor using a high-concentration calcium source solution and an ammonium phosphate solution, combined with spray drying. Crystal growth was controlled by adjusting the pH and viscosity of the solution to prepare flower-like hydroxyapatite materials.

Benefits of technology

The continuous large-scale preparation of flower-like hydroxyapatite materials has been achieved, which improves the purity and specific surface area of ​​the materials, enhances the adsorption performance of dye wastewater, and reduces environmental pollution and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105575A_ABST
    Figure CN123105575A_ABST
Patent Text Reader

Abstract

This invention provides a method for the continuous preparation of flower-like hydroxyapatite materials, along with the resulting products and applications, relating to the field of wastewater treatment materials. The method involves a high-concentration phosphorus-containing solution composed of ammonium phosphate, an ammonia modifier, and sugars; and a high-concentration calcium-containing solution composed of calcium acetate, an ammonia modifier, and aspartic acid. These solutions are then continuously subjected to a low-temperature solvothermal reaction in a dynamic tubular reactor to obtain a reaction slurry. The reaction slurry is then filtered, diluted, and spray-dried to achieve continuous, large-scale preparation of flower-like hydroxyapatite materials with high specific surface area, high hydrophilicity, and high purity; the specific surface area is 240.82–259.79 m². 2 It has a water contact angle of 54.1-71.2°, a purity of 99.02-99.28%, and an adsorption rate of 99.02-99.63% for dyes in wastewater, showing broad prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wastewater treatment materials, and in particular to a method for the continuous preparation of flower-like hydroxyapatite materials, as well as the products and applications thereof. Background Technology

[0002] Hydroxyapatite (Ca 10 Hydroxyapatite (PO4)6(OH)2, due to its excellent adsorption properties, has been widely used in environmental remediation, bioseparation, and heavy metal removal. However, the performance of the material is severely limited by its morphology and specific surface area. Among various morphological systems, flower-shaped hydroxyapatite has a large specific surface area and high surface activity, and is significantly superior to conventional morphologies such as rods, spheres, and sheets in terms of drug loading / release and adsorption, making it a research hotspot for high-performance functional materials.

[0003] The current preparation of flower-like hydroxyapatite mainly relies on a hydrothermal batch process. This process typically involves adding soft templates such as disodium ethylenediaminetetraacetate (EDTA), sodium citrate, or sodium tartrate to react with Ca in the solution. 2+ Complexation forces crystals to develop in a directional manner, assembling from linear or plate-like structures into flower-like morphologies. However, soft template agents such as EDTA are extremely chemically stable and difficult to degrade, causing secondary pollution to soil and groundwater. Furthermore, because this process uses a batch reactor for feeding, batch-to-batch variations often prevent it from meeting the requirements for continuous and stable industrial production.

[0004] Chinese invention patent document CN102556993A discloses a method for preparing hydroxyapatite with a three-dimensional nanoflower structure. The method involves dissolving calcium nitrate and diammonium hydrogen phosphate separately in a dilute nitric acid solution, then simultaneously adding them to an excess urea solution. The pH of the mixed solution is adjusted to 3-6 with ammonia, and the mixture is subjected to a hydrothermal reaction at 90-180℃ for 10-24 hours to obtain flower-like hydroxyapatite assembled from nanorods or nanosheets. This process utilizes the in-situ hydrolysis of excess urea to generate ammonia gas, thereby adjusting the pH of the reaction system and controlling the morphology of the hydroxyapatite. However, in this patent preparation, adjusting the pH of the system to the acidic range easily leads to the formation of miscible hydroxyapatite. Furthermore, the low concentrations of calcium and phosphorus sources, and the difficulty in achieving uniform mixing of the calcium and phosphorus sources at the interface in a batch reactor, result in a long reaction time. In addition, the drying method uses constant temperature drying, which is time-consuming and difficult to implement for continuous large-scale production.

[0005] Chinese invention patent document CN120270970A discloses a method for preparing low-crystallinity hydroxyapatite microspheres. The method involves adding a surfactant to a mixed solution of calcium and phosphorus source reagents, reacting at a constant temperature to generate a hydroxyapatite slurry, then adding water to obtain a hydroxyapatite microparticle suspension. Finally, the microparticle suspension is spray-dried to obtain low-crystallinity hydroxyapatite microspheres. The surfactant in this process has a dual function: firstly, it disperses the sieving and secondary dispersion steps; secondly, it reduces the crystallinity of hydroxyapatite. However, the use of polyethylene glycol (PEG) and polyvinylpyrrolidone (PVP) surfactants can cause environmental pollution. This process involves adding water to the reacted hydroxyapatite slurry to prepare a hydroxyapatite microparticle suspension, but the suspension contains a large amount of inorganic salts. These inorganic salts originate from byproducts generated during the reaction of the calcium and phosphorus source solutions and from additional inorganic acid and alkali neutralization reactants. The large amount of inorganic salts can corrode equipment during spray drying, shortening its lifespan. In addition, the concentration of hydroxyapatite in the suspension is 10 g / L. The low solid content will increase the energy consumption of spray drying, resulting in poor process economy.

[0006] Chinese invention patent document CN104741067A discloses a method for preparing a carbon hydroxyapatite-carbon aerosol composite material. The method involves dissolving water-soluble carbohydrates, water-soluble polymers, and soluble calcium salts in water, adding a phosphate solution, and reacting at 140-300℃ for 3-17 hours. After washing, drying, and calcination, the composite material is obtained. This process involves the reaction of polyhydroxy aldehydes or ketones in the carbohydrates with carboxyl polymers in the water-soluble polymers at high temperatures to form a cross-linked network structure, ultimately forming a carbon-containing composite material after high-temperature calcination. In this process, the carbohydrates primarily provide a carbon source, while the water-soluble polymers not only provide a carbon source but also act as a linker, facilitating the formation of the aerosol network and preventing the structural collapse of the carbon-containing composite material. (See the appendix of this patent document.) Figure 2 It can be seen that the composite material prepared by this method basically does not contain hydroxyapatite phase, and the composite material is mainly composed of carbon-containing aerogel. This patented method cannot achieve the continuous preparation of high-purity, high specific surface area, and wide pore size range of hydroxyapatite. Summary of the Invention

[0007] To address the technical problems existing in the prior art, this invention provides a method for continuous preparation of flower-like hydroxyapatite materials, as well as the products and applications thereof. This method can solve the problem that it is difficult to adjust hydroxyapatite materials to a flower-like morphology, and can also achieve continuous large-scale production of high-purity, high-specific-surface-area, and wide-pore-range flower-like hydroxyapatite. At the same time, it can also effectively solve the problems of long reaction time, high environmental pollution, and high energy consumption in traditional hydroxyapatite preparation processes, as well as the problem that hydroxyapatite prepared by traditional processes has poor adsorption performance for dye-containing wastewater.

[0008] To solve the above technical problems, the technical solution adopted by the present invention is as follows: A method for continuous preparation of flower-like hydroxyapatite materials includes the following steps: Step S01: After mixing calcium acetate, aspartic acid, and deionized water, ammonia water is added to adjust the pH to 10.9-11.1 to obtain a calcium-containing solution; the concentration of calcium acetate in the calcium-containing solution is 1-1.5 mol / L; the molar amount of aspartic acid added to the calcium-containing solution is 0.3-1.5% of the molar amount of calcium acetate. Step S02: After mixing ammonium phosphate with deionized water, add ammonia to adjust the pH to 10.1-10.5, and then add sugar to adjust the viscosity to 30-40 cP to obtain a phosphorus-containing solution. Step S03: Simultaneously and continuously introduce the calcium-containing solution and the phosphorus-containing solution into the dynamic tubular reactor for stirring and reaction to continuously obtain a reaction slurry; after solid-liquid separation, wet-based flower-shaped hydroxyapatite is obtained; Step S04: After mixing wet-based flower-shaped hydroxyapatite with deionized water, spray dry to obtain flower-shaped hydroxyapatite material.

[0009] Preferably, in step S01, the concentration of ammonia is 25-28 wt%. In step S02, the ammonium phosphate salt is triammonium phosphate or diammonium hydrogen phosphate; the sugar is glucose or sucrose; and the concentration of ammonia water is 25-28 wt%.

[0010] Preferably, in step S03, the molar concentration ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution is 1.67-1.70:1.

[0011] Preferably, in step S03, the flow rate of the calcium-containing solution introduced into the dynamic tubular reactor is controlled to be 0.01-0.015 L / min, and the flow rate of the phosphorus-containing solution introduced into the dynamic tubular reactor is 0.01-0.015 L / min; and the volume ratio of the phosphorus-containing solution to the calcium-containing solution introduced into the dynamic tubular reactor per unit time is 0.95-1.05:1.

[0012] Preferably, in step S03, the residence time of the calcium-containing solution and the phosphorus-containing solution in the dynamic tubular reactor is 50-75 min; The temperature of the stirred reaction is 40-80℃, and the stirring speed is 100-300 r / min.

[0013] Preferably, in step S04, the ratio of the absolute dry weight of wet-based flower-shaped hydroxyapatite to the weight of deionized water is 1:5-10.

[0014] Preferably, in step S04, the spray drying conditions are: feed rate of 15-30 mL / min, inlet air temperature of 170-190℃, and outlet air temperature of 90-100℃. The nozzle diameter of the spray dryer is 0.75-2mm.

[0015] A flower-like hydroxyapatite material was prepared using the aforementioned method.

[0016] An application of the aforementioned flower-like hydroxyapatite material includes the following steps: adding the flower-like hydroxyapatite material to dye-containing wastewater, performing adsorption treatment at room temperature, separating the solid and liquid, and recovering the adsorbed flower-like hydroxyapatite material.

[0017] Preferably, the dye concentration in the dye-containing wastewater is 100-300 mg / L; The mass-to-volume ratio of flower-shaped hydroxyapatite material to dye-containing wastewater is 0.4-1.2 g: 1000 mL. Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The continuous preparation method of flower-like hydroxyapatite material of the present invention uses a high-concentration calcium source solution and ammonium phosphate solution to carry out a low-temperature solvothermal reaction in a dynamic tubular reactor, followed by spray drying to obtain flower-like hydroxyapatite material; the entire preparation time does not exceed 3 hours, which is much shorter than the preparation time of hydroxyapatite by traditional methods, and can realize the continuous large-scale preparation of flower-like hydroxyapatite material. At the same time, the process is simple to operate, does not require the use of organic solvents or surfactants in the synthesis process, and the raw materials and products in the reaction process are non-toxic, which is a green and environmentally friendly process and is more suitable for large-scale industrial production.

[0018] (2) In the continuous preparation process of the flower-like hydroxyapatite material of the present invention, the surface charge (Zeta) electronegativity of the material is adjusted by controlling the amount of aspartic acid added. Aspartic acid reduces the electronegativity of the material, which helps the material to attract each other, aggregate and grow, and helps to form a flower-like morphology. However, too much aspartic acid will lead to an increase in the electronegativity of the Zeta sites of the material, resulting in an increase in the material's repulsive force and inhibiting the formation of the flower-like morphology. At the same time, aspartic acid and sugars are both environmentally friendly green substances that are harmless to the environment and human body.

[0019] (3) In the continuous preparation of flower-like hydroxyapatite material of the present invention, the sugar substances used can adjust the viscosity of the solution and stabilize the viscosity of the solution at 30-40 cP. The viscous effect of the sugar binds the movement of microspheres, restricts the disordered dispersion of particles, guides the microspheres to be oriented and stacked in an orderly manner, and has a synergistic effect with aspartic acid to jointly promote the formation of flower-like morphology of hydroxyapatite.

[0020] (4) In the continuous preparation of flower-like hydroxyapatite material of the present invention, ammonia water can not only adjust the pH of calcium-containing solution and phosphorus-containing solution, but also neutralize the hydrogen ions released by the calcium-phosphorus reaction in real time, stabilize the alkaline environment of the system, continuously promote the forward progress of HAP synthesis reaction, inhibit the generation of acidic calcium hydrogen phosphate impurity phase, and facilitate the generation of pure phase product.

[0021] (5) In the continuous preparation of flower-like hydroxyapatite material of the present invention, the dynamic tubular reactor used allows for continuous flow reaction of solutions with high viscosity or containing solid particles. This is because the reactor is equipped with a rotatable dynamic stirring / turbulence component, which, together with a large-diameter flow channel, can continuously generate turbulent and shear flow, destroy the laminar boundary layer of high-viscosity fluids, prevent the sedimentation of solid particles, maintain continuous overall plug flow, and enable calcium-containing solutions and phosphorus-containing solutions to have good interfacial contact reaction, greatly improving mass transfer and heat transfer efficiency. Compared with the traditional batch reactor, the reaction rate can be greatly improved. However, microchannel reactors are limited by narrow pipe diameters, and when the viscosity of the solution is high or solid particles are present, pipe blockage will occur, resulting in poor practicality.

[0022] (6) In the continuous preparation process of the flower-like hydroxyapatite material of the present invention, the spray drying technology used can basically decompose and remove the by-product ammonium acetate salt adsorbed during the in-situ growth of the flower-like hydroxyapatite material at high temperature, thereby improving the purity of the flower-like hydroxyapatite material (purity can reach 99.02-99.28%), which belongs to the level of high-purity hydroxyapatite material. At the same time, compared with high-temperature calcination technology, the spray drying technology helps to maintain the high surface area of ​​the material. This is because hydroxyapatite will grow secondary during high-temperature calcination. Although it can improve the crystallinity of the material, it will significantly reduce the specific surface area of ​​the material, thereby affecting its adsorption performance for dyes in wastewater. That is, high-temperature calcination is not conducive to improving the specific surface area and adsorption effect of the material. In addition, during the in-situ growth of the flower-like hydroxyapatite material, sugars and aspartic acid will be adsorbed on the surface, and they will not decompose during the spray drying process. A large number of polar hydrophilic groups such as amino, carboxyl, and hydroxyl groups are left on the surface of the material, which greatly improves the hydrophilicity of the flower-like hydroxyapatite and lays the foundation for the material to have excellent pollutant adsorption performance.

[0023] (7) The flower-like hydroxyapatite material prepared by the present invention is composed of microspheres and has a specific surface area of ​​240.82-259.79 m². 2 With a water contact angle ranging from 54.1 to 71.2°, this material exhibits a 140.32-159.25% increase in specific surface area and a 20.54-39.62% increase in hydrophilicity compared to flower-shaped hydroxyapatite materials prepared by traditional intermittent calcination methods. Furthermore, its adsorption rate in dye-containing wastewater with a concentration of 100-300 mg / L reaches 99.02-99.63%, representing a 10.08-10.64% improvement over flower-shaped hydroxyapatite materials prepared by traditional methods under the same testing conditions. This makes it an excellent adsorbent for treating dye-containing wastewater and possesses broad prospects for industrial application. Attached Figure Description

[0024] Figure 1 The image shows a scanning electron microscope (SEM) image of the flower-like hydroxyapatite material prepared in Example 1.

[0025] Figure 2 The X-ray diffraction (XRD) patterns of the hydroxyapatite materials prepared in Examples 1-4, Comparative Examples 1-2, and Comparative Examples 7-9 are shown.

[0026] Figure 3 The figures show nitrogen adsorption-desorption (N2-BET) test results of the hydroxyapatite materials prepared in Example 1 and Comparative Example 8.

[0027] Figure 4 The water contact angle test diagrams are for the hydroxyapatite materials prepared in Example 1 and Comparative Example 8; where (a) represents Example 1 and (b) represents Comparative Example 8.

[0028] Figure 5 Transmission electron microscopy (TEM) images of the hydroxyapatite materials prepared for comparative examples 3-6; where (a) represents comparative example 3, (b) represents comparative example 4, (c) represents comparative example 5, and (d) represents comparative example 6.

[0029] Figure 6 The surface charge (Zeta) test diagrams of the reaction slurry obtained in step (3) of Examples 1-4, Comparative Examples 3 and 4 are shown. Detailed Implementation

[0030] To provide a clearer understanding of the technical features, objectives, and effects of this invention, specific embodiments are now described. It should be noted that the following detailed descriptions are exemplary and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0031] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments of the present invention. As used herein, "first," "second," etc., are used to distinguish similar objects and are not used to describe a particular order or sequence. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0032] This invention provides a method for the continuous preparation of flower-like hydroxyapatite materials, comprising the following steps: Step S01: After mixing calcium acetate, aspartic acid, and deionized water, ammonia water is added to adjust the pH to 10.9-11.1 to obtain a calcium-containing solution; the concentration of calcium acetate in the calcium-containing solution is 1-1.5 mol / L; the molar amount of aspartic acid added to the calcium-containing solution is 0.3-1.5% of the molar amount of calcium acetate. Step S02: After mixing ammonium phosphate with deionized water, add ammonia to adjust the pH to 10.1-10.5, and then add sugar to adjust the viscosity to 30-40 cP to obtain a phosphorus-containing solution. Step S03: Simultaneously and continuously introduce the calcium-containing solution and the phosphorus-containing solution into the dynamic tubular reactor for stirring and reaction to continuously obtain a reaction slurry; after solid-liquid separation, wet-based flower-shaped hydroxyapatite is obtained; Step S04: After mixing wet-based flower-shaped hydroxyapatite with deionized water, spray dry to obtain flower-shaped hydroxyapatite material.

[0033] In this embodiment of the invention, a low-temperature solvothermal reaction is carried out in a dynamic tubular reactor using a high-concentration calcium source solution and an ammonium phosphate solution, followed by spray drying, which effectively realizes the continuous large-scale preparation of flower-like hydroxyapatite materials. In this process, high-concentration calcium source solutions and ammonium phosphate solutions can effectively enhance the driving force of chemical reactions, accelerate crystal nucleation and growth rates, and meet the needs of continuous preparation. At the same time, the aspartic acid used can regulate the electronegativity of the surface charge (Zeta) of the material, which helps the material attract each other, aggregate and grow, and promotes the formation of flower-like morphology. In addition, the solution viscosity regulated by sugars relies on the thickening effect of sugars to bind the movement of microspheres, restrict the disordered dispersion of particles, guide the directional stacking and orderly assembly of microspheres, and has a synergistic effect with aspartic acid to jointly promote the formation of flower-like morphology of hydroxyapatite. Furthermore, the ammonia water used can not only adjust the pH of calcium-containing and phosphorus-containing solutions, but also neutralize the hydrogen ions released by the calcium-phosphorus reaction in real time, stabilize the alkaline environment of the system, continuously promote the forward progress of HAP synthesis reaction, inhibit the formation of acidic calcium hydrogen phosphate impurity phase, and facilitate the production of pure phase products.

[0034] Furthermore, in the dynamic tubular reaction process, the dynamic tubular reactor allows for continuous flow reactions of solutions with high viscosity or containing solid particles. This is because the reactor is equipped with a rotatable dynamic stirring / turbulence-disrupting component, combined with a large-diameter flow channel, which continuously generates turbulent and shear flow, disrupting the laminar boundary layer of high-viscosity fluids, preventing solid particle sedimentation, and maintaining continuous overall plug flow transport. After the dynamic tubular reaction, the accompanying spray drying technology can essentially decompose the by-product ammonium acetate salts adsorbed during the in-situ growth of the flower-like hydroxyapatite material at high temperatures, improving the purity of the flower-like hydroxyapatite material. In addition, during the in-situ growth of the flower-like hydroxyapatite material, sugars and aspartic acid are adsorbed on the surface, and these do not decompose during the spray drying process. The material surface retains a large number of polar hydrophilic groups such as amino, carboxyl, and hydroxyl groups, significantly improving the hydrophilicity of the flower-like hydroxyapatite and laying the foundation for the material to have excellent pollutant adsorption performance.

[0035] Preferably, in step S01, the concentration of ammonia is 25-28 wt%.

[0036] Preferably, in step S02, the ammonium phosphate salt is triammonium phosphate or diammonium hydrogen phosphate; the sugar is glucose or sucrose; and the concentration of ammonia water is 25-28 wt%.

[0037] Preferably, in step S03, the molar concentration ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution is 1.67-1.70:1.

[0038] Preferably, in step S03, the flow rate of the calcium-containing solution introduced into the dynamic tubular reactor is controlled to be 0.01-0.015 L / min; the flow rate of the phosphorus-containing solution introduced into the dynamic tubular reactor is 0.01-0.015 L / min; and the volume ratio of the phosphorus-containing solution to the calcium-containing solution introduced into the dynamic tubular reactor per unit time is 0.95-1.05:1 (more preferably 1:1).

[0039] Preferably, in step S03, the residence time of the calcium-containing solution and the phosphorus-containing solution in the dynamic tubular reactor is 50-75 min; the temperature of the stirring reaction is 40-80℃; and the stirring speed of the stirring reaction is 100-300 r / min.

[0040] Preferably, in step S04, the ratio of the oven-dry weight of wet-based flower-shaped hydroxyapatite to the weight of deionized water is 1:5-10; the spray drying conditions are: feed rate of 15-30 mL / min, inlet air temperature of 170-190℃, outlet air temperature of 90-100℃; and the nozzle diameter of the spray dryer is 0.75-2 mm.

[0041] The present invention also provides flower-shaped hydroxyapatite prepared by the aforementioned method.

[0042] This invention also provides the application of the aforementioned flower-like hydroxyapatite in the adsorption treatment of dye-containing wastewater, including the following steps: Flower-shaped hydroxyapatite was added to dye-containing wastewater, and after stirring at room temperature, the solids were separated and collected to recover the adsorbed flower-shaped hydroxyapatite. The dye concentration in the adsorbed wastewater was analyzed using an ultraviolet spectrophotometer.

[0043] Preferably, the dye concentration in the dye-containing wastewater is 100-300 mg / L; the mass-to-volume ratio of the flower-shaped hydroxyapatite material to the dye-containing wastewater is 0.4-1.2 g: 1000 mL.

[0044] Preferably, the stirring time at room temperature is 0.3-1h (more preferably 0.3-0.5h).

[0045] To enable those skilled in the art to more clearly understand the technical solution of the present invention, the present invention will be further described below with reference to some specific embodiments. Unless otherwise specified, the experimental methods used in each embodiment are conventional methods; unless otherwise specified, the reagents and materials used in each embodiment are commercially available products.

[0046] In subsequent embodiments of the present invention, the viscometer used consists of a stirring system, a sensing system, and a display system. The viscometer model is DV2TLVTJ0, brand is AMETEK Brookfield, stirring speed is 0.1-200 rpm, viscosity range is 0-320000000 cP, and operating temperature is 0-40℃.

[0047] The dynamic tubular reactor used consists of a feeding system, a sensing system, a temperature control system, a pressure control system, a stirring system, and a display system. The model of the dynamic tubular reactor is VTRWSS0014 / VTRWHS0014 (horizontal), manufactured by Shandong Weijing Chemical Technology Co., Ltd., with a temperature range of -20 to 200℃, a pressure of 0-2MPa, a liquid holdup of 1.5L, a stirring speed of 0-300r / min, and a voltage of 380V / 50HZ.

[0048] The spray dryer used consists of a feeding system, a temperature control system, a fan, a separation system, a control system, nozzles, a sensing system, and a collection device. The spray dryer model is DC-1500 experimental spray dryer, manufactured by Shanghai Dacheng Experimental Equipment Co., Ltd., with inlet air temperature of 30-260℃, outlet air temperature of 30-130℃, maximum feed rate of 0-2000mL / h, nozzle diameter of 0.75-2mm, and voltage of 220V.

[0049] Example 1 This invention provides a method for the continuous preparation of flower-like hydroxyapatite materials, the specific steps of which are as follows: (1) Mix 1.25 mol calcium acetate, 0.0075 mol aspartic acid and 955 mL deionized water, then add 45 mL 27 wt% ammonia water and adjust the pH to 11.05 to obtain a calcium-containing solution. (2) According to the molar ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution of 1.69:1, the corresponding molar amount of diammonium hydrogen phosphate (about 0.74 mol) is mixed with 905 mL of deionized water, then 95 mL of 27 wt% ammonia water is added to adjust the pH to 10.29, and then glucose is added to adjust the viscosity. When the viscosity of the solution is measured by the viscometer to be 35 cP, the addition of glucose is stopped to obtain the phosphorus-containing solution. (3) Calcium-containing solution and phosphorus-containing solution are simultaneously fed into dynamic tubular reactor through the feeding system of dynamic tubular reactor for solvothermal reaction. The flow rate of calcium-containing solution and phosphorus-containing solution is controlled at 0.0125 L / min, the residence time of material in dynamic tubular reactor is 60 min, the reaction temperature is 60℃, and the stirring speed is 200 r / min to obtain reaction slurry. The reaction slurry is filtered to obtain wet-based flower-shaped hydroxyapatite. (4) Take 100g of dry wet-based flower-shaped hydroxyapatite and mix it with 700g of deionized water. Then, feed it into the spray dryer through the feeding system of the spray dryer. Control the feeding speed to 20mL / min, the inlet air temperature to 180℃, and the outlet air temperature to 95℃. Spray dry the flower-shaped hydroxyapatite through the 1.5mm nozzle of the spray dryer.

[0050] This embodiment also provides flower-shaped hydroxyapatite prepared using the aforementioned method.

[0051] Example 2 This invention provides a method for the continuous preparation of flower-like hydroxyapatite materials, the specific steps of which are as follows: (1) Mix 1.0 mol calcium acetate, 0.005 mol aspartic acid and 972 mL deionized water, then add 28 mL 27 wt% ammonia water and adjust the pH to 10.94 to obtain a calcium-containing solution; (2) According to the molar ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution of 1.68:1, the corresponding molar amount of diammonium hydrogen phosphate (about 0.60 mol) is mixed with 920 mL of deionized water, then 80 mL of 27 wt% ammonia water is added to adjust the pH to 10.10, and then glucose is added to adjust the viscosity. When the viscosity of the solution is measured by the viscometer to be 30 cP, the addition of glucose is stopped to obtain the phosphorus-containing solution. (3) Calcium-containing solution and phosphorus-containing solution are simultaneously fed into dynamic tubular reactor through the feeding system of dynamic tubular reactor for solvothermal reaction. The flow rate of calcium-containing solution and phosphorus-containing solution is controlled to be 0.01 L / min, the residence time of material in dynamic tubular reactor is 75 min, the reaction temperature is 40℃, and the stirring speed is 100 r / min to obtain reaction slurry. The reaction slurry is filtered to obtain wet-based flower-shaped hydroxyapatite. (4) Take 100g of dry wet-based flower-shaped hydroxyapatite and 500g of deionized water, mix them, and feed them into the spray dryer through the feeding system of the spray dryer. Control the feeding speed to 15mL / min, the inlet air temperature to 170℃, and the outlet air temperature to 90℃. Spray dry through the 0.75mm nozzle of the spray dryer to obtain flower-shaped hydroxyapatite.

[0052] This embodiment also provides flower-shaped hydroxyapatite prepared using the aforementioned method.

[0053] Example 3 This invention provides a method for the continuous preparation of flower-like hydroxyapatite materials, the specific steps of which are as follows: (1) Mix 1.5 mol calcium acetate, 0.0225 mol aspartic acid and 936 mL deionized water, then add 64 mL 27 wt% ammonia water and adjust the pH to 11.10 to obtain a calcium-containing solution; (2) According to the molar ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution of 1.70:1, mix the corresponding molar amount of diammonium hydrogen phosphate (about 0.88 mol) with 888 mL of deionized water, then add 112 mL of 27 wt% ammonia water, adjust the pH to 10.47, and then add glucose to adjust the viscosity. When the viscosity of the solution is measured by the viscometer to be 40 cP, stop adding glucose to obtain the phosphorus-containing solution. (3) Calcium-containing solution and phosphorus-containing solution are simultaneously fed into dynamic tubular reactor through the feeding system of dynamic tubular reactor for solvothermal reaction. The flow rate of calcium-containing solution and phosphorus-containing solution is controlled at 0.015 L / min, the residence time of material in dynamic tubular reactor is 50 min, the reaction temperature is 80℃, and the stirring speed is 300 r / min to obtain reaction slurry. The reaction slurry is filtered to obtain wet-based flower-shaped hydroxyapatite. (4) Take 100g of dry wet-based flower-shaped hydroxyapatite and mix it with 1000g of deionized water. Then, feed it into the spray dryer through the feeding system of the spray dryer. Control the feeding speed to be 25mL / min, the air inlet temperature to be 190℃, and the air outlet temperature to be 100℃. Spray dry through the 2.0mm nozzle of the spray dryer to obtain flower-shaped hydroxyapatite.

[0054] This embodiment also provides flower-shaped hydroxyapatite prepared using the aforementioned method.

[0055] Example 4 The continuous preparation method of flower-like hydroxyapatite material in Example 4 is the same as that in Example 1, except that the ammonium phosphate salt used in step (2) is different. Triammonium phosphate is used in Example 4. Other steps and process parameters are the same as in Example 1.

[0056] Comparative Example 1 Comparative Example 1 adopts the technical solution of Example 1, except that the amount of calcium acetate in the calcium-containing solution in step (1) is different, changing the amount of calcium acetate added from 1.25 mol in Example 1 to 0.5 mol; at the same time, in step (2), the amount of diammonium hydrogen phosphate added is changed accordingly based on the molar ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution being 1.69:1. Other steps and process parameters are the same as in Example 1.

[0057] Comparative Example 2 Comparative Example 2 adopts the technical solution of Example 1, except that in step (1), ammonia is not used to adjust the pH, and deionized water is used to make up for the volume lost due to the omission of ammonia. Other steps and process parameters are the same as in Example 1.

[0058] Comparative Example 3 Comparative Example 3 uses the technical solution of Example 1, except that the addition of aspartic acid is omitted in step (1). Other steps and process parameters are the same as in Example 1.

[0059] Comparative Example 4 Comparative Example 4 uses the technical solution of Example 1, except that the amount of aspartic acid added in step (1) is changed from 0.0075 mol in Example 1 to 0.0375 mol. Other steps and process parameters are the same as in Example 1.

[0060] Comparative Example 5 Comparative Example 5 uses the technical solution of Example 1, except that the addition of glucose is omitted in step (2). Other steps and process parameters are the same as in Example 1.

[0061] Comparative Example 6 Comparative Example 6 uses the technical solution of Example 1, except that glucose is used in step (2) to adjust the viscosity to 10 cP. Other steps and process parameters are the same as in Example 1.

[0062] Comparative Example 7 Comparative Example 7 uses the technical solution of Example 1, except that the residence time of the calcium-containing solution and the phosphorus-containing solution in the dynamic tubular reactor is changed from 60 min to 45 min. Other steps and process parameters are the same as in Example 1.

[0063] Comparative Example 8 Comparative Example 8 adopts the technical solution of Example 1, the difference being that the drying method in step (4) is different, replacing spray drying with tube furnace treatment; the specific operation steps are as follows: After the wet-based flower-shaped hydroxyapatite was vacuum dried at 100℃ for 10h, 10g of the dry-based flower-shaped hydroxyapatite was placed in a tube furnace, and the heating rate was controlled at 5℃ / min. The temperature was raised from room temperature to 500℃ and calcined for 2h to obtain flower-shaped hydroxyapatite.

[0064] All other steps and process parameters are the same as in Example 1.

[0065] Comparative Example 9 Comparative Example 9 adopts the technical solution of Example 1, except that the method of adjusting pH in steps (1) and (2) is different. The original method of adjusting the pH of the solution with ammonia water is replaced with adjusting the pH of the solution with solid sodium hydroxide. The specific operation steps are as follows: (1) Mix 1.25 mol calcium acetate, 0.0075 mol aspartic acid and 1000 mL deionized water, then add solid sodium hydroxide and adjust the pH to 11.05 to obtain a calcium-containing solution; (2) According to the molar ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution of 1.69:1, the corresponding molar amount of diammonium hydrogen phosphate (about 0.74 mol) is mixed with 1000 mL of deionized water, then solid sodium hydroxide is added to adjust the pH to 10.29, and then glucose is added to adjust the viscosity. When the viscosity of the solution is measured by the viscometer to be 35 cP, the addition of glucose is stopped to obtain the phosphorus-containing solution.

[0066] All other steps and process parameters are the same as in Example 1.

[0067] Comparative Example 10 Comparative Example 10 adopts the technical solution of Example 1, except that the calcium source used in step (1) is different. In Comparative Example 10, calcium acetate is replaced with calcium chloride. Other steps and process parameters are the same as those in Example 1.

[0068] Comparative Example 11 Comparative Example 11 adopts the technical solution of Example 1, except that the nozzle diameter of the spray dryer in step (4) is different. In Comparative Example 11, the nozzle diameter is changed from 1.5 mm to 0.5 mm. Other steps and process parameters are the same as those in Example 1.

[0069] During the preparation of Comparative Example 11, it was found that when the nozzle diameter was reduced from 1.5 mm to 0.5 mm, the material could not be effectively atomized. Analysis revealed that this was because the nozzle diameter of the spray dryer was too small, causing material particles to clog the nozzle during atomization, thus preventing atomization. Therefore, it is necessary to select an appropriate nozzle diameter for the preparation of flower-shaped hydroxyapatite; otherwise, the drying efficiency will be affected.

[0070] Application Example 1 200 mg of Reactive Red W-2BR dye was mixed with 1 L of deionized water to simulate dye-containing wastewater. Then, 0.8 g of the hydroxyapatite material prepared in Examples 1-4 and Comparative Examples 1-9 were added to 1 L of dye-containing wastewater, stirred at room temperature for 0.4 h, and then centrifuged to obtain the adsorbed hydroxyapatite material and the adsorbed dye-containing wastewater. The dye concentration in the adsorbed dye-containing wastewater was analyzed using a UV spectrophotometer, and the adsorption rate was calculated. The specific results are shown in Table 1.

[0071] The adsorption rate is calculated using the formula: X = (C0 - C1) / C0 × 100%, where X is the adsorption rate (%), C0 is the concentration of the dye-containing wastewater before hydroxyapatite adsorption (mg / L), and C1 is the concentration of the dye-containing wastewater after hydroxyapatite adsorption (mg / L).

[0072] Furthermore, the specific surface area and water contact angle of the hydroxyapatite materials prepared in Examples 1-4 and Comparative Example 8 were determined by nitrogen adsorption-desorption (N2-BET) tests; and the purity of the hydroxyapatite materials prepared in Examples 1-4 and Comparative Example 10 was tested. The specific results are shown in Table 1.

[0073] The purity test method is as follows: Take 1g of hydroxyapatite, add 10mL of aqua regia (37% hydrochloric acid: concentrated nitric acid volume ratio of 3:1) and dissolve completely, then dilute to 100mL with deionized water, and analyze the Ca content using inductively coupled plasma mass spectrometry (ICP). 2+ The formula for calculating concentration and purity is: W=C Ca,实际 / C Ca,理论 ×100%, C Ca,理论 Ca after complete dissolution of hydroxyapatite material 2+ Theoretical concentration, mg / L; C Ca,实际 The Ca2+ of hydroxyapatite material dissolved in aqua regia 2+ Concentration, mg / L.

[0074] Table 1. Summary of test results for hydroxyapatite materials in each embodiment and comparative example.

[0075] As shown in Table 1, the adsorption test results of dye-containing wastewater indicate that the flower-like hydroxyapatite materials in Examples 1-4 exhibited an adsorption rate of 99.02-99.52% for dyes in the wastewater, which is significantly higher than that of the hydroxyapatite material prepared by the intermittent conventional calcination process in Comparative Example 8 (adsorption rate 89.95%). Compared to Comparative Example 8, the adsorption performance of each example for dyes in the wastewater was improved by 10.08-10.64%, indicating that high-temperature calcination in a tubular furnace affects the adsorption effect of hydroxyapatite materials on dyes in wastewater.

[0076] As shown in Table 1, the specific surface area of ​​the flower-like hydroxyapatite materials in Examples 1-4 is 240.82-259.79 m². 2 / g, far exceeding the hydroxyapatite material (specific surface area 100.21m²) prepared by the intermittent conventional calcination process in Comparative Example 8. 2 / g); compared to Comparative Example 8, the specific surface area of ​​the flower-like hydroxyapatite in each embodiment increased by 140.32-159.25%, indicating that in the continuous preparation process of the present invention, high-temperature calcination in a tube furnace will reduce the specific surface area of ​​the flower-like hydroxyapatite, thereby affecting its adsorption performance for dyes in wastewater.

[0077] As shown in Table 1, the water contact angles of the flower-like hydroxyapatite in Examples 1-4 ranged from 54.1° to 71.2°, indicating significantly higher hydrophilicity compared to the hydroxyapatite material prepared by the intermittent conventional calcination process in Comparative Example 8 (water contact angle 89.6°). Compared to Comparative Example 8, the hydrophilicity of the flower-like hydroxyapatite in each example increased by 20.54%-39.62%. This suggests that during the prolonged high-temperature calcination in the tubular furnace, aspartic acid and sugars continuously decompose, leading to a decrease in the hydrophilicity of the flower-like hydroxyapatite. In contrast, the spray drying process largely avoids the decomposition of aspartic acid and sugars. Therefore, aspartic acid and sugars not only induce the formation of flower-like morphology but also enhance the hydrophilicity of the flower-like hydroxyapatite. This is because aspartic acid and sugars contain a large number of hydrophilic polar groups such as hydroxyl, carboxyl, and amino groups, which contribute to improved hydrophilicity.

[0078] As shown in Table 1, the purity of the hydroxyapatite materials prepared in Examples 1-4 and Comparative Example 10 is 99.02-99.28% and 97.82%, respectively (high-purity HAP is defined as ≥99% purity). This indicates that the type of calcium salt in the calcium-containing solution affects the purity of the hydroxyapatite material. Analysis reveals that this is because calcium acetate combines with ammonium ions in ammonium phosphate during the preparation process to form ammonium acetate, which decomposes rapidly during spray drying. In contrast, the calcium chloride used in Comparative Example 10 combines with ammonium ions in ammonium phosphate to form ammonium chloride, which does not decompose significantly during spray drying, thus reducing purity. Therefore, in conjunction with the continuous preparation process of this invention, selecting a suitable calcium salt has a significant impact on the purity of the flower-like hydroxyapatite.

[0079] Table 1 compares Examples 1-4 with Comparative Example 1, and in conjunction with... Figure 2 It can be seen that the concentration of calcium acetate in a calcium-containing solution affects the reaction rate; that is, a high concentration of calcium ions is beneficial to promoting the reaction rate and obtaining pure-phase hydroxyapatite.

[0080] Table 1 compares Examples 1-4 with Comparative Example 2, and in conjunction with... Figure 2It is evident that a pure-phase HAP cannot be obtained without adjusting the pH of the calcium-containing solution. This is because the reaction between calcium ions in the calcium-containing solution and phosphate ions in the phosphorus-containing solution produces hydrogen ions. Without adjusting the pH of the calcium-containing solution, it is difficult to provide an alkaline growth environment for the flower-like hydroxyapatite material, resulting in a mixed phase of HAP and dicalcium phosphate. Therefore, adjusting the pH of the calcium-containing solution is crucial and key to obtaining a pure-phase HAP; otherwise, a dicalcium phosphate impurity phase will be obtained.

[0081] Table 1 compares Examples 1-4 with Comparative Examples 3-4, and in conjunction with... Figure 1 and Figure 5 It is known that both the absence of aspartic acid and the excessive addition of aspartic acid will result in hydroxyapatite materials with a microsphere morphology. This is because aspartic acid has the function of regulating surface charge. An appropriate amount of aspartic acid is conducive to the mutual attraction and agglomeration of hydroxyapatite with a microsphere morphology, which will then assemble into a flower-like morphology. Under the same conditions, the flower-like morphology is more conducive to the adsorption of dye-containing wastewater.

[0082] Table 1 compares Examples 1-4 with Comparative Examples 5-6, and in conjunction with... Figure 5 It is known that hydroxyapatite materials with microsphere morphology can be obtained by adding no glucose or adding a small amount of glucose. This is because glucose has the function of regulating the viscosity of the solution. An appropriate amount of glucose can stably control the viscosity of the solution at 30-40 cP, which can limit the disordered dispersion of particles and guide the microspheres to be oriented and orderly assembled, thus helping to form a flower-like morphology. Under the same conditions, the flower-like morphology of hydroxyapatite is more conducive to the adsorption of dye-containing wastewater.

[0083] Table 1 compares Examples 1-4 with Comparative Example 7, and in conjunction with... Figure 2 It can be seen that when the residence time of the material in the dynamic tubular reactor is shortened (Comparative Example 7), the product obtained is a mixed phase of hydroxyapatite and dicalcium phosphate, meaning that the residence time affects the pure phase of HAP. Therefore, the residence time of the material in the dynamic tubular reactor must be controlled to obtain pure phase HAP.

[0084] Table 1 compares Examples 1-4 with Comparative Example 8, and in conjunction with... Figure 2 and Figure 3 as well as Figure 4 It is known that high-temperature calcination in a tubular furnace reduces the specific surface area and hydrophilicity of the material, thereby affecting its adsorption performance for dyes in wastewater. This is because HAP undergoes secondary growth during high-temperature calcination, which, while increasing the crystallinity of hydroxyapatite, reduces the specific surface area. Simultaneously, aspartic acid and sugars also decompose significantly during high-temperature calcination, further reducing the material's hydrophilicity.

[0085] Table 1 compares Examples 1-4 with Comparative Example 9, and in conjunction with... Figure 2It is known that when sodium hydroxide is used instead of ammonia to adjust the pH of calcium-containing and phosphorus-containing solutions, the resulting material is not a pure-phase HAP. This is because ammonia can construct a buffer system, providing a sufficient backup alkali source during the in-situ preparation of HAP, and continuously neutralizing the H+ ions generated during the synthesis of HAP from calcium-containing solutions and phosphate ions from phosphorus-containing solutions. + The reaction provides a stable alkaline environment throughout, preventing the formation of calcium hydrogen phosphate impurities in acidic conditions. Sodium hydroxide, however, has no buffering capacity because calcium ions in calcium-containing solutions and phosphate ions in phosphorus-containing solutions continuously generate H+ during HAP synthesis. + When OH - After consumption, the pH of the system drops significantly, creating an acidic local environment. The final product is a mixed phase containing dicalcium phosphate and HAP, and pure HAP cannot be obtained. Therefore, selecting a suitable pH adjuster is crucial for the preparation of HAP.

[0086] As shown in Table 1, comparing Examples 1-4 with Comparative Example 10, the type of calcium salt in the calcium-containing solution affects the purity of the material. This is because, in the continuous preparation process of this invention, calcium acetate combines with ammonium ions in ammonium phosphate to form ammonium acetate, which decomposes rapidly during spray drying; while calcium chloride combines with ammonium ions in ammonium phosphate to form ammonium chloride, which does not decompose significantly during spray drying. Therefore, under the continuous preparation process conditions of this invention, selecting a suitable calcium salt has a significant impact on the purity of the flower-like hydroxyapatite material.

[0087] Figure 1 The image shows a scanning electron microscope (SEM) image of the flower-like hydroxyapatite prepared in Example 1. As can be seen from the image, the flower-like morphology of this hydroxyapatite is assembled from microspheres.

[0088] Figure 2 The figures show the X-ray diffraction (XRD) patterns of the hydroxyapatite materials prepared in Examples 1-4, Comparative Examples 1-2, and Comparative Examples 7-9. As can be seen from the figures, Examples 1-4 and Comparative Example 8 are pure-phase HAP, conforming to the hydroxyapatite card (PDF#72-1243), while Comparative Examples 1-2 and Comparative Example 9 contain impurities of calcium hydrogen phosphate (PDF#72-1240), indicating they are mixtures of HAP and calcium hydrogen phosphate. This suggests that a high concentration of calcium ions promotes the reaction rate and is beneficial for obtaining pure-phase HAP; therefore, the amount of calcium acetate added to the calcium-containing solution should be appropriately selected (Comparative Example 1). The pH of the calcium-containing solution and the pH adjuster affect the preparation of pure-phase HAP; pH adjustment and the pH-adjusting reagent are very important (Comparative Examples 2 and 9). The residence time in the dynamic tubular reactor affects pure-phase HAP; the reaction time of the reaction system should be appropriately controlled (Comparative Example 7). High-temperature calcination promotes secondary growth of HAP and increases the crystallinity of the material, but reduces the specific surface area (Comparative Example 8).

[0089] Figure 3 The figures show nitrogen adsorption-desorption (N2-BET) tests of the hydroxyapatite materials prepared in Example 1 and Comparative Example 8. The test procedure was as follows: 0.2 g of the sample was placed on a nitrogen total adsorption analyzer (Guoyi Quantum V-Sorb 2800P), and firstly, vacuum desorption was performed at 120 °C for 6 h. Then, the desorbed mass was weighed, and finally, nitrogen adsorption-desorption was performed at 77 K. As can be seen from the figures, the specific surface areas of Example 1 and Comparative Example 8 were 259.79 m² / s². 2 / g, 100.21m 2 / g, high-temperature calcination will reduce the specific surface area of ​​the material, thereby affecting the adsorption performance of the material.

[0090] Figure 4 The water contact angle test results are shown for the hydroxyapatite materials prepared in Example 1 and Comparative Example 8; Note: Figure 4 In the middle (a), it is represented as Example 1. Figure 4 (b) represents Comparative Example 8. The testing procedure of this method is as follows: 0.2g of the sample to be tested is compressed into a tablet using a tablet press, and then placed on a water contact angle tester (Guangdong Beidou CA500S) to test the water contact angle of the sample. As can be seen from the figure, the left and right water contact angles of Example 1 are 57.9° and 57.3°, respectively, with an average water contact angle of 57.6°; the left and right water contact angles of Comparative Example 8 are 89.4° and 89.8°, respectively, with an average water contact angle of 89.6°. That is, high-temperature calcination reduces the hydrophilicity of the material, thereby affecting the adsorption performance of the material on dyes in wastewater.

[0091] Figure 5 Transmission electron microscopy (TEM) images of the hydroxyapatite materials prepared in comparative examples 3-6; Figure 5 (a) represents Comparative Example 3. Figure 5 (b) represents Comparative Example 4. Figure 5 (c) represents Comparative Example 5. Figure 5 (d) represents Comparative Example 6. As shown in the figure, the hydroxyapatite materials prepared under the conditions of no aspartic acid (Comparative Example 3), excess aspartic acid (Comparative Example 4), no glucose (Comparative Example 5), and a small amount of glucose (Comparative Example 6) did not produce flower-like morphology, and their morphology remained microspheres. This indicates that aspartic acid and glucose have a synergistic effect in inducing flower-like morphology, but the amount of aspartic acid and glucose added must be controlled.

[0092] Figure 6The figures show the surface charge (Zeta) test results of the reaction slurries obtained in step (3) of Examples 1-4, Comparative Examples 3 and 4. As can be seen from the figures, aspartic acid reduces the surface charge. In particular, neither the addition of no aspartic acid (Comparative Example 3) nor the addition of excess aspartic acid (Comparative Example 4) induces the formation of flower-like morphology in the hydroxyapatite material. This is because insufficient aspartic acid results in insufficient attraction, making it difficult for spherical particles to assemble into a flower-like morphology, while excessive aspartic acid leads to mutual repulsion and inhibition of assembly. Therefore, an appropriate amount of aspartic acid synergistically induces the formation of flower-like morphology in hydroxyapatite with sugars.

[0093] Application Example 2 100 mg of Reactive Red W-2BR dye was mixed with 1 L of deionized water to simulate dye-containing wastewater. Then, 0.4 g of the flower-shaped hydroxyapatite from Example 1 was added to 1 L of dye-containing wastewater. After stirring at room temperature for 0.3 h, the mixture was centrifuged to obtain the adsorbed hydroxyapatite material and the adsorbed dye-containing wastewater. The dye concentration in the adsorbed dye-containing wastewater was analyzed using a UV spectrophotometer, and the adsorption rate was calculated. The test results showed that the adsorption rate for the dye-containing wastewater was 99.63%.

[0094] Application Example 3 300 mg of reactive bright red W-2BR dye was mixed with 1 L of deionized water to simulate dye-containing wastewater. Then, 1.2 g of the flower-shaped hydroxyapatite from Example 1 was added to 1 L of dye-containing wastewater. After stirring at room temperature for 0.5 h, the mixture was centrifuged to obtain the adsorbed hydroxyapatite material and the adsorbed dye-containing wastewater. The dye concentration in the adsorbed dye-containing wastewater was analyzed using a UV spectrophotometer, and the adsorption rate was calculated. The test results showed that the adsorption rate for the dye-containing wastewater was 99.47%.

[0095] As can be seen from Application Examples 1-3, the flower-like hydroxyapatite of the present invention can achieve an adsorption rate of 99.02-99.63% in dye-containing wastewater with a concentration of 100-300 mg / L, indicating that the material has good dye adsorption capacity.

[0096] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for continuous preparation of flower-like hydroxyapatite material, characterized in that, Includes the following steps: Step S01: After mixing calcium acetate, aspartic acid, and deionized water, ammonia water is added to adjust the pH to 10.9-11.1 to obtain a calcium-containing solution; the concentration of calcium acetate in the calcium-containing solution is 1-1.5 mol / L; the molar amount of aspartic acid added to the calcium-containing solution is 0.3-1.5% of the molar amount of calcium acetate. Step S02: After mixing ammonium phosphate with deionized water, add ammonia to adjust the pH to 10.1-10.5, and then add sugar to adjust the viscosity to 30-40 cP to obtain a phosphorus-containing solution. Step S03: Simultaneously and continuously introduce the calcium-containing solution and the phosphorus-containing solution into the dynamic tubular reactor for stirring and reaction to continuously obtain a reaction slurry; after solid-liquid separation, wet-based flower-shaped hydroxyapatite is obtained; Step S04: After mixing wet-based flower-shaped hydroxyapatite with deionized water, spray dry to obtain flower-shaped hydroxyapatite material.

2. The method for continuous preparation of flower-like hydroxyapatite material according to claim 1, characterized in that, In step S01, the concentration of ammonia water is 25-28 wt%. In step S02, the ammonium phosphate salt is triammonium phosphate or diammonium hydrogen phosphate; the sugar is glucose or sucrose; and the concentration of ammonia water is 25-28 wt%.

3. The method for continuous preparation of flower-like hydroxyapatite material according to claim 1, characterized in that, In step S03, the molar concentration ratio of calcium acetate in the calcium-containing solution to ammonium phosphate in the phosphorus-containing solution is 1.67-1.70:

1.

4. The method for continuous preparation of flower-like hydroxyapatite material according to claim 1, characterized in that, In step S03, the flow rate of the calcium-containing solution introduced into the dynamic tubular reactor is controlled to be 0.01-0.015 L / min, and the flow rate of the phosphorus-containing solution introduced into the dynamic tubular reactor is controlled to be 0.01-0.015 L / min; and the volume ratio of the phosphorus-containing solution to the calcium-containing solution introduced into the dynamic tubular reactor per unit time is 0.95-1.05:

1.

5. The method for continuous preparation of flower-like hydroxyapatite material according to claim 1, characterized in that, In step S03, the residence time of the calcium-containing solution and the phosphorus-containing solution in the dynamic tubular reactor is 50-75 min. The temperature of the stirred reaction is 40-80℃, and the stirring speed is 100-300 r / min.

6. The method for continuous preparation of flower-like hydroxyapatite material according to claim 1, characterized in that, In step S04, the ratio of the absolute dry weight of wet-based flower-shaped hydroxyapatite to the weight of deionized water is 1:5-10.

7. The method for continuous preparation of flower-like hydroxyapatite material according to claim 1, characterized in that, In step S04, the conditions for spray drying are: feed rate of 15-30 mL / min, inlet air temperature of 170-190℃, and outlet air temperature of 90-100℃. The nozzle diameter of the spray dryer is 0.75-2mm.

8. A flower-like hydroxyapatite material, characterized in that, It is prepared by the method described in any one of claims 1-7.

9. An application of the flower-like hydroxyapatite material as described in claim 8, characterized in that, Includes the following steps: Flower-shaped hydroxyapatite material was added to dye-containing wastewater, and after adsorption treatment at room temperature, solid-liquid separation was performed to recover the adsorbed flower-shaped hydroxyapatite material.

10. The application of the flower-like hydroxyapatite material according to claim 9, characterized in that, The dye concentration in the dye-containing wastewater is 100-300 mg / L; The mass-to-volume ratio of flower-shaped hydroxyapatite material to dye-containing wastewater is 0.4-1.2 g: 1000 mL.

Citation Information

Patent Citations

  • Method of preparing hydroxyapatite with three-dimensional nanoflower structure

    CN102556993A

  • Preparation method of carbonate hydroxylapatite-carbon aerosol composite material

    CN104741067A

  • Hydroxyapatite microspheres with low crystallinity and preparation method thereof

    CN120270970A