Methods for preparing composite positive electrode active materials, composite positive electrode active materials and rechargeable lithium batteries
By mixing lithium iron phosphate-based compounds and lithium nickel-based composite oxides, composite positive electrode active materials in assembly form were prepared, which solved the problem of insufficient cycle life of lithium batteries under high voltage and high temperature, and achieved high energy density and excellent cycle life characteristics.
Patent Information
- Application Number
- CN202610662641.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-04-30
- Filing Date
- 2026-05-14
- Publication Date
- 2026-11-17
AI Technical Summary
In existing lithium batteries, lithium iron phosphate-based compounds suffer from deteriorated cycle life characteristics under high voltage, while lithium nickel-based composite oxides suffer from deteriorated storage characteristics at high temperatures, resulting in insufficient energy density and cycle life of lithium batteries.
A composite positive electrode active material with excellent structural stability was prepared by mixing lithium iron phosphate-based compounds and lithium nickel-based composite oxides and wet milling them.
It achieves high energy density, improved low-temperature discharge capacity, low-rate and high-rate cycle life characteristics, improved high-temperature storage characteristics, and low resistance, ensuring price competitiveness and high initial charge/discharge capacity.
Smart Images

Figure CN123105580A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a method for preparing composite positive electrode active materials, composite positive electrode active materials, and rechargeable lithium batteries. Background Technology
[0002] Portable information devices (such as cellular phones, laptops, or smartphones) or electric vehicles already use rechargeable lithium batteries with high energy density as their power source. Recently, research has been actively conducted to use rechargeable lithium batteries with high energy density as a power source or energy storage source for hybrid or electric vehicles.
[0003] Lithium cobalt-based oxides, such as lithium cobalt oxide (LiCoO2), lithium nickel-based composite oxides, such as lithium nickel cobalt manganese oxide (NCM) and lithium nickel cobalt aluminum oxide (NCA), and lithium iron phosphate (LiFe)-based compounds have been used as positive electrode active materials in rechargeable lithium batteries. Among these, due to the high prices of nickel (Ni) and cobalt (Co), low-cost lithium iron phosphate-based compounds using relatively inexpensive iron (Fe) as the main component are attracting attention.
[0004] Lithium iron phosphate-based compounds have an olivine structure, and therefore exhibit superior cycle life characteristics compared to other positive electrode active materials. However, when rechargeable lithium batteries employing lithium iron phosphate-based compounds are used at high voltages, the cycle life characteristics deteriorate, which limits the operating voltage of rechargeable lithium batteries.
[0005] To address this, lithium-nickel-based composite oxides can be mixed to achieve high energy density, high voltage operation, and high capacity, but the following problems exist: for rechargeable lithium batteries, high-temperature storage characteristics deteriorate. Summary of the Invention
[0006] This disclosure provides a method for preparing composite positive electrode active materials, the composite positive electrode active materials, and a rechargeable lithium battery. The composite positive electrode active materials ensure price competitiveness, exhibit high pellet (disc) density for rechargeable lithium batteries, provide high initial charge / discharge capacity and efficiency, provide improved average voltage levels, provide high low-temperature discharge capacity, and achieve excellent cycle life and high-rate cycle life, improved high-temperature storage characteristics, improved capacity per volume and energy density, and low resistivity.
[0007] A method for preparing a composite positive electrode active material according to some embodiments of the present disclosure may include: preparing a first positive electrode active material comprising a lithium iron phosphate-based compound and having primary particulate form; preparing a second positive electrode active material comprising a lithium nickel-based composite oxide and having primary particulate form; mixing the first positive electrode active material and the second positive electrode active material and wet milling them to prepare a first slurry; and adding the first slurry to a spray dryer and spray drying the first slurry to prepare a first dried product.
[0008] In some embodiments, the preparation of the first positive electrode active material may include: wet milling an iron phosphate-based precursor, a lithium raw material, and a carbon raw material mixed in a second solvent to prepare a second slurry; adding the wet-milled second slurry to a spray dryer and spray-drying the second slurry to prepare a second dried product; calcining the second dried product to prepare a second calcined product; and pulverizing the second calcined product.
[0009] In some embodiments, the second fired product may be in the form of secondary particles in which multiple primary particles can agglomerate.
[0010] In some embodiments, the pulverization of the second calcined product can be carried out at a pulverization speed greater than about 2000 rpm.
[0011] In some embodiments, the lithium iron phosphate-based compound may include a compound represented by Chemical Formula 1, a compound represented by Chemical Formula 2, or a combination thereof. Chemical Formula 1 is as follows:
[0012] Li a1 Fe (1-x1) M 1 x1 PO4,
[0013] Where 0.9 ≤ a1 ≤ 1.5 and 0 ≤ x1 ≤ 0.4. M 1 It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Chemical formula 2 is as follows:
[0014] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4,
[0015] Where 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, and x² + y² < 1. M 2It can be Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof.
[0016] In some embodiments, the lithium iron phosphate-based compound may include LiFePO4, LiMn 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4, LiMn 0.3 Fe 0.7 PO4 or combinations thereof.
[0017] In some embodiments, the average particle size of the primary particles of the first positive electrode active material may be greater than or equal to about 0.1 μm and less than about 2 μm.
[0018] In some embodiments, lithium-nickel-based composite oxides may be represented as follows:
[0019] Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 X b3 ,
[0020] Where 0.9 ≤ a³ ≤ 1.2, 0.3 ≤ x³ ≤ 1, 0 ≤ y³ ≤ 0.7, 0 ≤ z³ ≤ 0.7, 0.9 ≤ x³ + y³ + z³ ≤ 1.1, and 0 ≤ b³ ≤ 0.1. M 3 and M 4 Each of these can be independently Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. 3 and M 4 It can be different elements. X can be F, P, S or a combination thereof.
[0021] In some embodiments, the amount of nickel in the lithium nickel-based composite oxide may be from about 50 mol% to about 80 mol%, based on 100 mol% of the total metals other than lithium in the lithium nickel-based composite oxide.
[0022] In some embodiments, the average particle size of the primary particles of the second positive electrode active material can be from about 2 μm to about 8 μm.
[0023] In some embodiments, during the mixing and wet milling of the first positive electrode active material and the second positive electrode active material, the weight ratio of the first positive electrode active material and the second positive electrode active material may be from about 50:50 to about 99:1.
[0024] In some embodiments, adding a first slurry to a spray dryer and spray-drying the first slurry to prepare a first dried product may include spray-drying the first slurry at a temperature of about 150°C to about 400°C.
[0025] In some embodiments, the method for preparing the composite positive electrode active material may further include: after adding a first slurry to a spray dryer and spray-drying the first slurry to prepare a first dried product, calcining the first dried product to prepare a first calcined product.
[0026] In some embodiments, calcining the first dried product may include calcining the first dried product in a vacuum or in an inert gas at a temperature of about 300°C to about 1000°C.
[0027] According to some embodiments of this disclosure, the composite positive electrode active material is in particulate form, comprising: a first positive electrode active material comprising a lithium iron phosphate-based compound and having a plurality of primary particles, and a second positive electrode active material comprising a lithium nickel-based composite oxide and having a plurality of primary particles. The particulate form may include a plurality of primary particles of the first positive electrode active material and a plurality of primary particles of the second positive electrode active material. The porosity of the composite positive electrode active material may be less than or equal to about 25%. The aggregate density of the composite positive electrode active material may be greater than or equal to about 2.6 g / cc.
[0028] In some embodiments, the composite positive electrode active material is in the form of secondary particles, and the average particle size of the secondary particles of the composite positive electrode active material can be from about 3 μm to about 20 μm.
[0029] A rechargeable lithium battery according to some embodiments of this disclosure includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the composite positive electrode active material as described above.
[0030] The method for preparing composite positive electrode active materials according to some embodiments, the composite positive electrode active materials, and the rechargeable lithium battery can ensure price competitiveness, while providing high agglomerate density, high initial charge / discharge capacity and efficiency, improved average voltage level, high discharge capacity at low temperatures, excellent cycle life characteristics and high rate cycle life characteristics, improved high temperature storage characteristics, improved capacity per volume and energy density, and low resistance for rechargeable lithium batteries. Attached Figure Description
[0031] Figure 1 A schematic perspective view showing portions of a cylindrical rechargeable lithium battery according to some embodiments of the present disclosure.
[0032] Figure 2 A cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure is shown schematically.
[0033] Figure 3 and 4 Schematic exploded perspective views of pouch-type rechargeable lithium batteries according to some embodiments of the present disclosure.
[0034] Figure 5 and 6 Scanning electron microscope images of the cross-sections of the composite positive electrode active material of Example 2 at different magnifications. Detailed Implementation
[0035] Specific embodiments will be described in detail below so that those skilled in the art can readily implement them. However, this disclosure may be embodied in many different forms and is not to be construed as limited to the embodiments set forth herein.
[0036] The terminology used herein is for describing implementation methods and is not intended to limit the invention. Unless the context clearly specifies otherwise, singular expressions include plural expressions.
[0037] The term "combination" refers to a mixture, laminate, complex, copolymer, alloy, blend, or reaction product of the constituent elements.
[0038] Terms such as “comprising,” “including,” or “having” are intended to indicate the presence of features, quantities, steps, elements, or combinations thereof embodied, but those terms do not preclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.
[0039] In the accompanying drawings, for clarity, the thickness of layers, films, panels, or regions is exaggerated, and throughout the specification, the same reference numerals denote the same elements. It will be understood that when an element, such as a layer, film, region, or substrate, is referred to as being "on" another element, it may be directly on said other element, or there may be intermediate elements present. Conversely, when an element is referred to as being "directly on" another element, there are no intermediate elements present.
[0040] In addition, the term "layer" in this article includes not only the geometry formed on the entire surface when viewed from a plan view, but also the geometry formed on a portion of the surface.
[0041] The average particle size can be measured, for example, by a particle size analyzer or by transmission electron microscopy (TEM) or scanning electron microscopy (SEM) images. Alternatively, the average particle size value can be obtained by measuring using dynamic light scattering, performing data analysis, counting the number of particles in each size range, and calculating accordingly. In this disclosure, unless otherwise defined, the average particle size D... 50 This can mean the diameter of particles that have a cumulative volume of 50% in the particle size distribution, where the particles are considered (assumed) to be spherical. Unless otherwise defined, the average particle size is the value obtained by measuring the dimensions of approximately 20 randomly selected particles from scanning electron microscope (SEM) images and calculating the arithmetic mean of the dimensions of approximately 20 randomly selected particles, where the size of each particle is defined as the diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles.
[0042] The word "or" is not interpreted as exclusive; for example, "A or B" is interpreted as including A, B, or A+B.
[0043] The term "metal" is interpreted to include the concepts of common metals, transition metals, and metalloids (semi-metals). As used herein, the term "metalloid" refers to an element that has properties intermediate between those of metals and nonmetals. Examples of metalloids include, but are not limited to, boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb), and tellurium (Te).
[0044] As used herein, the term “vacuum” refers to a pressure in the range of 0.1 mbar to 10 mbar, as measured using a vacuum gauge in a processing chamber.
[0045] As used herein, the term "primary particle" refers to the smallest unit particle identified as an agglomeration (cluster) of individual particles when observed using a scanning electron microscope (SEM) of the positive electrode active material, where grain boundaries are not clearly distinguishable or are substantially (substantially) unobservable. Primary particles are the basic units constituting secondary particles formed by the aggregation of tens to hundreds of particles, and can exist individually or in a state where a small number (e.g., 20 or fewer) of primary particles are in contact with each other.
[0046] As used herein, the term "secondary particle" refers to an aggregate of primary particles of a given material, and may also be referred to as an assembly (assembly, collection) in this disclosure. Secondary particles have a structure in which primary particles are combined into individual particle forms (rather than a simple physical mixture) through interparticle contact and bonding. When observed using a scanning electron microscope (SEM), secondary particles can be identified as individual particle forms in which multiple primary particles are aggregated. Such secondary particles are distinguished from simple mixtures in which the corresponding particles are independently dispersed. Secondary particles can be formed by processes such as spray drying.
[0047] Method for preparing composite positive electrode active materials
[0048] A method for preparing a composite positive electrode active material according to some embodiments includes: preparing a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles; mixing the first positive electrode active material and a second positive electrode active material and wet milling them to prepare a first slurry, the second positive electrode active material comprising a lithium nickel-based composite oxide and in the form of primary particles; and adding the first slurry to a spray dryer and spray drying the first slurry to prepare a first dried product.
[0049] Lithium iron phosphate (LFP) compounds, exhibiting excellent structural stability, high heat resistance, and competitive pricing, are attracting attention. However, despite their superior cycle life characteristics, these characteristics deteriorate when used at high voltages, limiting their usable voltage.
[0050] High capacity has been attempted to be achieved using simple mixtures of lithium nickel-based composite oxides; however, while this allows for high energy density, high voltage operation, and high capacity, high-temperature storage characteristics can degrade.
[0051] In some implementations, lithium iron phosphate (LFP)-based compounds ensure price competitiveness, but these compounds can be prepared into assemblies (aggregates), pulverized, and separated into primary particles. Primary particles of LFP-based compounds and lithium nickel-based composite oxide particles in primary particle form can be wet-milled to prepare a slurry, which is then spray-dried to provide a composite positive electrode active material in assembly form. The composite positive electrode active material in assembly form enables high energy density, operation at high voltages, and operation at high capacities.
[0052] The assembly comprising lithium iron phosphate-based compounds and lithium nickel-based composite oxides offers all the advantages of mixing compared to simple hybrid forms, while simultaneously addressing the problems that occur in hybrid forms. More specifically, in the case of a composite positive electrode active material prepared according to a method for preparing a composite positive electrode active material according to some embodiments, the composite positive electrode active material has a particulate form comprising primary particles of lithium iron phosphate-based compounds and primary particles of lithium nickel-based composite oxides, specifically, a single secondary particle form in which the primary particles of lithium iron phosphate-based compounds and primary particles of lithium nickel-based composite oxides agglomerate, and more specifically, an assembly form, which improves low-temperature discharge capacity, low-rate and high-rate cycle life characteristics, and high-temperature storage characteristics for rechargeable lithium batteries.
[0053] In the following preparation method, terms using "first" and "second," other than the first positive electrode active material and the second positive electrode active material, are used to respectively identify (indicate) the process of preparing a composite positive electrode active material using the first positive electrode active material and the process of preparing the first positive electrode active material. For example, to identify terms commonly used in the process of preparing a composite positive electrode active material using both the first and second positive electrode active materials, and in the process of preparing the first positive electrode active material, such as slurry, the slurry formed in the process of preparing a composite positive electrode active material using both the first and second positive electrode active materials may be referred to as "first slurry," and the slurry in the process of preparing the first positive electrode active material may be referred to as "second slurry."
[0054] For convenience, following the order described in the claims, the process of preparing the composite positive electrode active material using the first positive electrode active material and the second positive electrode active material is referred to as "first," and the process of preparing the first positive electrode active material is referred to as "second." However, it should be understood that "first" and "second" do not indicate a specific order of occurrence.
[0055] Preparation of the first positive electrode active material
[0056] The above steps are a process for preparing (manufacturing) a first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles. The first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles can be prepared according to the methods described below, or a commercially available product can be obtained and used.
[0057] The preparation of a first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles may include: wet milling an iron iron phosphate-based precursor, a lithium raw material, and a carbon raw material mixed in a second solvent to prepare a second slurry; adding the wet-milled second slurry to a spray dryer and spray-drying the wet-milled second slurry to prepare a second dried product; calcining the second dried product to prepare a second calcined product; and pulverizing the second calcined product. By pulverizing the second calcined product, a first positive electrode active material comprising a lithium iron phosphate-based compound in the form of primary particles can be obtained. The steps for preparing the first positive electrode active material are described sequentially below.
[0058] First, a second slurry can be prepared by mixing an iron phosphate-based precursor, a lithium raw material, and a carbon raw material in a second solvent and then wet-milling the mixture. The preparation of the second slurry may include: mixing the iron phosphate-based precursor and the lithium raw material to prepare a raw material mixture; preparing the carbon raw material; and mixing the raw material mixture and the carbon raw material, adding the second solvent, and wet-milling to prepare the second slurry. The weight ratio of the raw material mixture to the carbon raw material is not particularly limited, but may be, for example, about 5:5 to about 99:1, about 6:4 to about 99:1, about 7:3 to about 99:1, about 8:2 to about 99:1, or about 9:1 to about 99:1.
[0059] Ferric phosphate precursors can be ferric phosphate precursors such as ferric phosphate (FePO4) and ferric phosphate (II) (Fe3(PO4)2), or they can be formed by adding phosphoric acid precursors such as phosphoric acid (H3PO4), ammonium dihydrogen phosphate (NH4H2PO4), diammonium hydrogen phosphate ((NH4)2HPO4), or trisodium phosphate (Na3PO4) to ferric raw materials such as ferric oxide (Fe2O3), ferric oxalate (FeC2O4), or ferric hydroxide (Fe(OH)3). Alternatively, ferric phosphate precursors can be manganese phosphate precursors formed by adding manganese raw materials such as manganese oxide, manganese carbonate, manganese sulfate, or manganese nitrate to ferric phosphate precursors. There are no limitations on the use of ferric phosphate precursors, as long as the ferric phosphate precursor is a known material used in solid-phase reactions.
[0060] Lithium raw materials may be, for example, Li2CO3, LiOH, their hydrates, or combinations thereof.
[0061] Carbon raw materials may include glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, poly(furfuryl alcohol), polyethylene glycol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, pitch resins, tar resins, or combinations thereof. For example, a mixture of glucose and polyethylene glycol may be used as a carbon raw material, and the mixing ratio by weight is not particularly limited, but may be, for example, about 10:90 to about 90:10, about 20:80 to about 80:20, about 30:70 to about 70:30, about 40:60 to about 60:40, or about 50:50.
[0062] Wet milling can be performed by adding a second solvent, which can be any one of ethylene glycol (EG), diethylene glycol (DEG), triethylene glycol (TEG), tetraethylene glycol (TetraEG), propylene glycol (PG), polyethylene glycol (PEG), polypropylene glycol (PPG), ethanol, water, and acetone.
[0063] Wet grinding can be performed using bead mills, ball mills, vibratory mills, or colloid mills. For example, in some embodiments, wet grinding can be performed using ball milling with zirconia balls, wherein the wet grinding can be performed by rotating the grinding vessel at a speed of about 50 rpm to about 2000 rpm for about 1 hour to about 10 hours.
[0064] In the preparation of the second slurry by wet milling, raw materials including Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof may be further added to the slurry. Raw materials including Al, Mg, Mn, Ti, V, or combinations thereof may be added. Raw materials including Al, Mg, Ti, V, or combinations thereof may be added as dopant elements, and based on the total metals other than lithium in the lithium iron phosphate-based compound of the first positive electrode active material, Al, Mg, Ti, V, or combinations thereof may be added in amounts of about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol%, or about 0.4 mol%. The Ti-containing raw material can be further added to the second slurry, and based on the total metals other than lithium in the first positive electrode active material, the amount of Ti added can be up to about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol%, or about 0.4 mol%. Therefore, the rate characteristics and cycle life characteristics of rechargeable lithium batteries can be improved.
[0065] Next, the wet-milled second slurry can be added to a spray dryer and spray-dried to produce a second dried product.
[0066] A second slurry, which has been wet-milled, can be injected into a spray dryer and sprayed to produce droplets (droplets) containing a uniform composition. The droplets can then be dried to produce a second dried product.
[0067] Spray dryers may include ultrasonic spray devices, single-fluid and dual-fluid air nozzle spray devices, ultrasonic nozzle spray devices, filter expansion droplet generators (FEAG), and disc droplet generators. Any known spray dryer may be used.
[0068] The amount of the second slurry added may vary depending on the spray dryer, but can be appropriately adjusted. For example, at a blower speed of about 50 Hz and an addition pressure of about 0.5 MPa, the addition rate of the second slurry may be less than or equal to about 1 kg / min, for example, less than or equal to about 1 kg / min, less than or equal to about 0.9 kg / min, less than or equal to about 0.8 kg / min, less than or equal to about 0.7 kg / min, less than or equal to about 0.6 kg / min, or less than or equal to about 0.5 kg / min and greater than or equal to about 0.01 kg / min, greater than or equal to about 0.05 kg / min, greater than or equal to about 0.1 kg / min, greater than or equal to about 0.15 kg / min, greater than or equal to about 0.2 kg / min, greater than or equal to about 0.3 kg / min, or greater than or equal to about 0.4 kg / min. The addition rate of the second slurry is a value converted based on the solids content (solids) and is defined as the amount of slurry supplied per minute (min) based on the mass of the solids content in the slurry. When the addition rate of the second slurry to the spray dryer meets the above range, secondary particles consisting of primary particles with uniform size can be manufactured, and the average size of the primary particles can be adjusted to be less than or equal to about 200 nm, and the size of the secondary particles can be controlled to make the size of the secondary particles uniform.
[0069] Spray drying can be carried out at a temperature greater than or equal to about 100°C, for example at about 150°C to about 400°C, about 150°C to about 300°C, about 200°C to about 300°C, or about 200°C to about 250°C to dry the components and evaporate the solvent.
[0070] Next, the second dried product can be fired to produce a second fired product.
[0071] In the preparation of the second calcined product, calcination can be carried out under vacuum or an inert gas and at a temperature of about 700°C to about 1000°C, for example about 725°C to about 900°C or about 750°C to about 800°C. The inert gas can be argon or nitrogen.
[0072] The second calcined product may include a lithium iron phosphate-based compound and may be in the form of secondary particles in which multiple primary particles are aggregated. The secondary particles may also be represented as assemblies. More specifically, the secondary particles of the second calcined product may have a spherical or ellipsoidal geometry because the primary particles are tightly aggregated together. The average particle size of the secondary particles may be, for example, about 3 μm to about 20 μm, about 5 μm to about 18 μm, or about 7 μm to about 15 μm. The average particle size of the secondary particles can be obtained by randomly selecting about 20 secondary particles from an electron microscope image of the second calcined product, measuring the size of each secondary particle, and calculating the arithmetic mean of the sizes of each secondary particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0073] The secondary particles of the second calcined product may include pores, and the porosity may be from about 10% to about 50%, for example from about 10% to about 40%, from about 10% to about 30%, or from about 10% to about 25%. The porosity may be, for example, the ratio of the area occupied by pores in the secondary particles to the cross-sectional area of the secondary particles, measured using an image analysis program such as ImageJ in a scanning electron microscope image of the cross-section of the secondary particles of the second calcined product. The cross-section of the secondary particles can be obtained by cutting the second calcined product using a focused ion beam (FIB). Images from a scanning electron microscope (SEM) can be acquired, for example, at a magnification of 5,000× to 50,000× under the same imaging conditions. Image analysis can be performed using a fixed threshold or a consistent threshold setting method equally applied to all samples. The porosity of the second fired product can be the average of the porosities measured for multiple second fired products, and can be obtained, for example, by measuring the porosity of at least 20 individual second fired products and calculating the average of the porosities of at least 20 individual second fired products.
[0074] The second calcined product may further include a carbon coating layer on the surface of the secondary particles, the surface of the primary particles constituting the secondary particles, or both. If the second calcined product is subsequently pulverized to prepare the first positive electrode active material of the primary particles, the carbon coating layer can improve the electrical conductivity of the first positive electrode active material and reduce the resistance of the positive electrode. The carbon coating layer can be formed by the above-described calcination process of the carbon raw materials.
[0075] Next, the second fired product can be crushed.
[0076] Crushing can be carried out using equipment such as a jet mill, ball mill, bead mill, or sand mill.
[0077] There are no particular limitations on the pulverization speed during the aforementioned pulverization process, as long as the second calcined product in the form of an assembly is separated into primary particles constituting the assembly, and the pulverization can be carried out at a pulverization speed exceeding approximately 2000 rpm, for example, approximately 3000 rpm to approximately 6000 rpm or approximately 4000 rpm to approximately 6000 rpm. The pulverization of the second calcined product can be carried out under conditions where the secondary particles can be pulverized and separated into multiple primary particles. If the pulverization speed is less than 2000 rpm, the secondary particles may not be pulverized and may remain in the form of an assembly. If the pulverization speed is greater than approximately 6000 rpm, the pulverized and separated primary particles may be damaged.
[0078] A first positive electrode active material comprising lithium iron phosphate-based compounds and in the form of primary particles can be prepared by pulverizing the second calcined product.
[0079] The active material of the first positive electrode includes lithium iron phosphate-based compounds.
[0080] Lithium iron phosphate-based compounds may include compounds represented by Chemical Formula 1, compounds represented by Chemical Formula 2, or combinations thereof. Chemical Formula 1 is as follows:
[0081] [Chemical Formula 1]
[0082] Li a1 Fe (1-x1) M 1 x1 PO4.
[0083] In chemical formula 1, 0.9 ≤ a1 ≤ 1.5, 0 ≤ x1 ≤ 0.4, and M 1 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a1 ≤ 1.5, for example, 0.90 ≤ a1 ≤ 1.2, or 0.95 ≤ a1 ≤ 1.1. Additionally, 0 ≤ x1 ≤ 0.4, 0 ≤ x1 ≤ 0.3, 0 ≤ x1 ≤ 0.2, 0 ≤ x1 ≤ 0.1, or 0 ≤ x1 ≤ 0.05.
[0084] Chemical formula 2 is as follows:
[0085] [Chemical Formula 2]
[0086] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4.
[0087] In chemical formula 2, 0.9 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² < 0.9, x² + y² < 1, and M 2 The elements are Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof. Furthermore, 0.90 ≤ a² ≤ 1.5, for example, 0.90 ≤ a² ≤ 1.2, or 0.95 ≤ a² ≤ 1.1. Additionally, 0.1 ≤ x² ≤ 0.9, 0.3 ≤ x² ≤ 0.9, or 0.4 ≤ x² ≤ 0.8 and 0 ≤ y² ≤ 0.4, 0 ≤ y² ≤ 0.3, 0 ≤ y² ≤ 0.2, 0 ≤ y² ≤ 0.1, or 0 ≤ y² ≤ 0.05.
[0088] Lithium iron phosphate-based compounds may include LiFePO4 and LiMn. 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4, LiMn 0.3 Fe 0.7 PO4 or combinations thereof.
[0089] Lithium iron phosphate-based compounds may include Al, Mg, Ti, V, or combinations thereof as doping elements, and may include Al, Mg, Ti, V, or combinations thereof in amounts of about 0.1 mol% to about 0.5 mol%, about 0.2 mol% to about 0.5 mol%, about 0.3 mol% to about 0.5 mol%, or about 0.4 mol% based on the total metals other than lithium, in which case the rate characteristics and cycle life characteristics of rechargeable lithium batteries may be improved.
[0090] Lithium iron phosphate-based compounds may include Ti, Al, or a combination thereof as doping elements, wherein the amount of Ti may be from about 0.1 mol% to about 0.5 mol% based on the total metals excluding lithium, and the amount of Al may be from about 0.1 mol% to about 0.5 mol%, from about 0.2 mol% to about 0.5 mol%, from about 0.3 mol% to about 0.5 mol%, or about 0.4 mol% based on the total metals excluding lithium. This can improve rate performance and cycle life characteristics for rechargeable lithium batteries.
[0091] M of chemical formula 1 1 And M of chemical formula 2 2The active material may include Al, Mg, Ti, V, or combinations thereof, which in this case can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. In Formulas 1 and 2, based on the total metals excluding lithium, Al, Mg, Ti, V, or combinations thereof may be included in amounts from about 0.1 mol% to about 0.5 mol%, from about 0.2 mol% to about 0.5 mol%, from about 0.3 mol% to about 0.5 mol% or about 0.4 mol%, and these amounts can improve the cycle life characteristics of the lithium iron phosphate-based positive electrode active material for rechargeable lithium batteries. For example, in Formula 1, 0.001≤x1≤0.005, 0.002≤x1≤0.005, 0.003≤x1≤0.005, or x1=0.004, and in Formula 2, 0.001≤x2≤0.005, 0.002≤x2≤0.005, 0.003≤x2≤0.005, or x2=0.004, in which case the cycle life characteristics of the lithium iron phosphate-based positive electrode active material can be improved for rechargeable lithium batteries.
[0092] The first positive electrode active material is in the form of primary particles, and the average particle size of the primary particles of the first positive electrode active material may be less than about 2 μm. The average particle size of the primary particles of the first positive electrode active material may be, for example, greater than or equal to about 0.1 μm and less than about 2 μm, about 0.1 μm to about 1.8 μm, about 0.1 μm to about 1.6 μm, about 0.1 μm to about 1.4 μm, about 0.1 μm to about 1.2 μm, about 0.1 μm to about 1 μm, about 0.1 μm to about 0.8 μm, about 0.2 μm to about 0.8 μm, about 0.3 μm to about 0.7 μm, or about 0.5 μm. The average particle size of the primary particles of the first positive electrode active material can be obtained by measuring the dimensions of approximately 20 primary particles of the first positive electrode active material in an electron microscope image of the surface or cross-section of the first positive electrode active material, and calculating the arithmetic mean of the dimensions of each particle, wherein the dimension of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. The average particle size of the primary particles of the first positive electrode active material can be smaller than the average particle size of the primary particles of the second positive electrode active material described below. That is, the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material within the secondary particles can be distinguished based on particle size.
[0093] According to some embodiments, the first positive electrode active material may have small and uniform primary particles. Therefore, the composite positive electrode active material including the first positive electrode active material has high charge / discharge capacity and excellent cycle life characteristics.
[0094] Furthermore, as measured by scanning electron microscopy (SEM) images of the cross-section of the composite positive electrode active material, the arithmetic mean size of the primary particles of the first positive electrode active material can be less than or equal to about 200 nm, about 50 nm to about 200 nm, or about 50 nm to about 150 nm, and the standard deviation of the arithmetic mean size can be less than or equal to about 100 nm, less than or equal to about 50 nm, less than or equal to about 30 nm, or less than or equal to about 15 nm, and can be greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 12 nm, or greater than or equal to about 13 nm. The arithmetic mean size and standard deviation of the primary particles of the first positive electrode active material can be obtained by measuring the size of about 20 random primary particles of the first positive electrode active material in SEM or TEM images of the surface or cross-section of the first positive electrode active material and calculating the arithmetic mean and the standard deviation of the arithmetic mean, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0095] The first positive electrode active material may further include a carbon coating layer on the surface of the primary particles. Since the specific details of the carbon coating layer can be described in the same manner as in the second calcined product, those details are omitted in this section.
[0096] Based on 100% by weight of the first positive electrode active material, a carbon coating layer may be included in amounts from about 0.1% by weight to about 3.9% by weight, for example, from about 0.5% by weight to about 3.9% by weight, from about 1% by weight to about 3.9% by weight, from about 1.5% by weight to about 3.9% by weight, or from about 1.7% by weight to about 3.9% by weight. The amount of carbon coating layer can be determined by completely burning the first positive electrode active material at a high temperature of about 1200°C to about 1400°C in an oxygen atmosphere to convert the carbon and sulfur in the first positive electrode active material into CO2 (or CO) and SO2, respectively.
[0097] Preparation of the second slurry
[0098] The preparation of the second slurry includes a process of mixing a first positive electrode active material and a second positive electrode active material, and wet milling the first and second positive electrode active materials. The second positive electrode active material comprises a lithium nickel-based composite oxide and is in the form of primary particles. The preparation of the second slurry may include: preparing a second positive electrode active material comprising a lithium nickel-based composite oxide and in the form of primary particles; and mixing the first and second positive electrode active materials and wet milling them to prepare the second slurry. Specific details regarding the first positive electrode active material may be the same as those described above, and therefore a description of the first positive electrode active material is omitted in this section.
[0099] The second positive electrode active material includes a lithium-nickel-based composite oxide.
[0100] The lithium-nickel-based composite oxide can be represented by the following Chemical Formula 3:
[0101] [Chemical Formula 3]
[0102] Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 X b3 .
[0103] In Chemical Formula 3, 0.9≤a3≤1.2, 0.3≤x3≤1, 0≤y3≤0.7, 0≤z3≤0.7, 0.9≤x3+y3+z3≤1.1, and 0≤b3≤0.1, M 3 and M 4 are each independently Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr, or a combination thereof, M 3 and M 4 are different elements, and X is F, P, S, or a combination thereof.
[0104] In Chemical Formula 3, 0.5≤x3≤0.8, 0.05≤y3≤0.35, and 0.15≤z3≤0.45; 0.5≤x3≤0.65, 0.05≤y3≤0.2, and 0.3≤z3≤0.45; or 0.55≤x3≤0.65, 0.05≤y3≤0.15, and 0.3≤z3≤0.4.
[0105] As a specific example, the lithium-nickel-based composite oxide may be represented by Chemical Formula 4 or Chemical Formula 5. Chemical Formula 4 is as follows:
[0106] [Chemical Formula 4]
[0107] Li a4 Ni x4 Co y4 M 5 z4 O 2-b4 X b4 .
[0108] In Chemical Formula 4, 0.9≤a4≤1.2, 0.3≤x4<1, 0<y4≤0.7, 0≤z4≤0.7, 0.9≤x4+y4+z4≤1.1, and 0≤b4≤0.1, M 5X is Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof, and X is F, P, S or combinations thereof.
[0109] In chemical formula 4, 0.5≤x4≤0.8, 0.05≤y4≤0.35, and 0.15≤z4≤0.45; 0.5≤x4≤0.65, 0.05≤y4≤0.2, and 0.3≤z4≤0.45; or 0.55≤x4≤0.65, 0.05≤y4≤0.15, and 0.3≤z4≤0.4.
[0110] Chemical formula 5 is as follows:
[0111] [Chemical Formula 5]
[0112] Li a5 Ni x5 Co y5 M 6 z5 M 7 w5 O 2-b5 X b5 .
[0113] In chemical formula 5, 0.9 ≤ a5 ≤ 1.2, 0.3 ≤ x5 ≤ 0.98, 0.01 ≤ y5 ≤ 0.69, 0.01 ≤ z5 ≤ 0.69, 0 ≤ w5 ≤ 0.68, 0.9 ≤ x5 + y5 + z5 + w5 ≤ 1.1, and 0 ≤ b5 ≤ 0.1, M 6 For Al, Mn, or a combination thereof, M 7 X is B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof, and X is F, P, S or a combination thereof.
[0114] In chemical formula 5, 0.5≤x5≤0.8, 0.05≤y5≤0.35, 0.15≤z5≤0.45, and 0≤w5≤0.3; 0.5≤x5≤0.65, 0.05≤y5≤0.2, 0.3≤z5≤0.45, and 0≤w5≤0.15; or 0.55≤x5≤0.65, 0.05≤y5≤0.15, 0.3≤z5≤0.4, and 0≤w5≤0.1.
[0115] Lithium-nickel-based composite oxides can be high-nickel-based positive electrode active materials. For example, in lithium-nickel-based composite oxides, based on 100 mol% of total metals excluding lithium, the amount of nickel can be greater than or equal to about 50 mol%, and can be, for example, about 50 mol% to about 100 mol%, about 50 mol% to about 99 mol%, about 50 mol% to about 90 mol%, about 50 mol% to about 85 mol%, about 50 mol% to about 80 mol%, about 50 mol% to about 75 mol%, about 50 mol% to about 70 mol%, about 50 mol% to about 65 mol%, or about 55 mol% to about 65 mol%. The composite positive electrode active material includes: a second positive electrode active material comprising a lithium-nickel-based composite oxide wherein the nickel content meets the above ranges, and a first positive electrode active material comprising a lithium iron phosphate-based compound, and can improve the capacity, efficiency, energy density, and cycle life characteristics of rechargeable lithium batteries.
[0116] The second positive electrode active material is in the form of primary particles, and the average particle size of the primary particles of the second positive electrode active material can be greater than or equal to about 2 μm. The average particle size of a single particle of the second positive electrode active material can be, for example, about 2 μm to about 8 μm, about 2 μm to about 5 μm, or about 2 μm to about 4 μm. The average particle size of the primary particles of the second positive electrode active material can be larger than the average particle size of the primary particles of the first positive electrode active material described above. The average particle size can be obtained by measuring the size of about 20 primary particles of the second positive electrode active material from a scanning electron microscope image (wherein, in the case of spherical particles, the diameter is measured, and in the case of non-spherical particles, the square root of the product of the major axis length and the minor axis length is measured), and then calculating the arithmetic mean of the sizes of the primary particles of the second positive electrode active material.
[0117] The second positive electrode active material can be manufactured by known methods or is a commercially available product. For example, the second positive electrode active material can be prepared by mixing a nickel-based precursor with a lithium source and then heat-treating it in an oxygen atmosphere to form a second positive electrode active material in the form of single particles.
[0118] Here, the term "single-particle form" can refer to a structure in which particles exist as independent phases in terms of morphology without aggregation, and can include structures that are substantially devoid of grain boundaries within the particles and consist of independently existing individual particles. A single particle can be represented as a monomeric structure, a non-aggregated structure, or a monolithic structure, and can be a single crystal.
[0119] Here, a single particle may correspond to a primary particle that constitutes a secondary particle in the composite positive electrode active material described below, and therefore, in this specification, a single particle may be used with the same meaning as a primary particle.
[0120] There are no particular limitations on the method of mixing the first positive electrode active material and the second positive electrode active material, and for example, a mixer can be used.
[0121] The weight ratio of the first positive electrode active material to the second positive electrode active material can be from about 50:50 to about 99:1, from about 55:45 to about 95:5, or from about 60:40 to about 9:1. If the weight ratio of the first and second positive electrode active materials meets the above ranges, high energy density, high voltage operation, and high capacity can be achieved while ensuring price competitiveness. However, when an excessive amount of the second positive electrode active material, which has a relatively large average particle size, is included, it is difficult to properly perform spray drying, and even if spray drying is performed, it is difficult to form an assembly as in some exemplary embodiments.
[0122] A first slurry can be prepared by adding a first solvent to the first and second positive electrode active materials during wet milling. The specific type of the first solvent may be the same as that of the second solvent described above, and therefore, a description of the specific type of the first solvent is omitted in this section. Wet milling can be performed by methods such as ultrasonic dispersion, stirred dispersion, using a homogenizer, using a high-shear mixer, using a jet mill, ball milling, or bead milling, and there are no particular limitations on the method of wet milling, as long as the method includes wet milling the first and second positive electrode active materials. For example, in some embodiments, wet milling can be performed using ball milling with zirconia balls, wherein wet milling can be performed by rotating the milling vessel at a speed of about 10 rpm to about 100 rpm for about 10 minutes to about 3 hours.
[0123] Preparation of the first dried product
[0124] The preparation of the first dried product includes adding a first slurry to a spray dryer and spray drying the first slurry.
[0125] A first slurry can be added to a spray dryer and sprayed to produce droplets comprising the desired uniform composition. The droplets can then be dried to prepare a first dried product. The solvent in the droplets evaporates, and the remaining solids can be dried in particulate form.
[0126] Spray dryers may include ultrasonic spray devices, single-fluid and dual-fluid air nozzle spray devices, ultrasonic nozzle spray devices, filtration expansion droplet generators (FEAG), and disc droplet generators. Any known spray dryer may be used.
[0127] The amount of the first slurry added may vary depending on the spray dryer, but can be adjusted appropriately. The addition rate of the first slurry may be less than or equal to about 1 kg / min, for example, less than or equal to about 1 kg / min, less than or equal to about 0.9 kg / min, less than or equal to about 0.8 kg / min, less than or equal to about 0.7 kg / min, less than or equal to about 0.6 kg / min, or less than or equal to about 0.5 kg / min and greater than or equal to about 0.01 kg / min, greater than or equal to about 0.05 kg / min, greater than or equal to about 0.1 kg / min, greater than or equal to about 0.15 kg / min, greater than or equal to about 0.2 kg / min, greater than or equal to about 0.3 kg / min, or greater than or equal to about 0.4 kg / min. The addition rate of the first slurry is a value converted based on the solids content (solids) and is defined as the amount of first slurry supplied per minute (min) based on the mass of the solids content in the first slurry. If the addition rate of the first slurry to the spray dryer meets the above range, the drying efficiency can be improved, powder with a narrow particle size distribution and a relatively uniform geometry can be formed, and clogging and contamination inside the dryer can be prevented.
[0128] Spray drying can be carried out at temperatures greater than or equal to about 100°C, for example about 150°C to about 400°C, about 150°C to about 300°C, or about 200°C to about 250°C to dry the components and evaporate the solvent.
[0129] The first dried product obtained according to the above steps may have a particulate form comprising primary particles of a first positive electrode active material and primary particles of a second positive electrode active material, and may have a secondary particle form in which the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material are aggregated, and the secondary particles may be represented as an assembly. The first dried product may correspond to or be the same as the composite positive electrode active material in this specification.
[0130] The method for preparing composite positive electrode active materials may further include: after adding a first slurry to a spray dryer and spray-drying the first slurry to prepare a first dried product, calcining the first dried product to prepare a first calcined product. The preparation of the first calcined product may be referred to as a first calcination step to distinguish the preparation of the first calcined product from spray drying and calcination of a second slurry. The composite positive electrode active material can be further strengthened by performing a first calcination step after spray drying, thereby further stabilizing the crystal structure of the composite positive electrode active material and significantly improving its electrochemical properties, mechanical strength, and cycle life stability.
[0131] The first firing step can be carried out under vacuum or an inert gas and at a temperature of about 300°C to about 1000°C, for example, about 300°C to about 500°C or about 350°C to about 450°C. The inert gas can be argon or nitrogen. If the above firing temperature meets the above range, the electrochemical properties, mechanical strength and cycle life stability of the composite positive electrode active material can be greatly improved.
[0132] The first positive electrode active material may be in particulate form comprising primary particles of the first positive electrode active material and primary particles of the second positive electrode active material, and may also be in the form of secondary particles or assemblies in which, for example, the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material are aggregated. The first calcined product may also correspond to the composite positive electrode active material in this specification, or may be the same as the composite positive electrode active material.
[0133] In the case of composite positive electrode active materials prepared according to the method for preparing composite positive electrode active materials according to some embodiments, the overall battery performance is improved compared with batteries formed by conventional simple mixing of positive electrode active materials, and the high-temperature storage characteristics are improved for rechargeable lithium batteries.
[0134] Composite positive electrode active material
[0135] According to some embodiments, a composite positive electrode active material includes: a first positive electrode active material comprising a lithium iron phosphate-based compound and in the form of primary particles; and a second positive electrode active material comprising a lithium nickel-based composite oxide and in the form of primary particles, wherein the composite positive electrode active material has a particulate form comprising a plurality of primary particles of the first positive electrode active material and a plurality of primary particles of the second positive electrode active material, the porosity of the composite positive electrode active material is less than or equal to about 25%, and the aggregate density of the composite positive electrode active material is greater than or equal to about 2.6 g / cc. The details of the first and second positive electrode active materials included in the composite positive electrode active material are the same as those described in the section concerning the method of preparing the composite positive electrode active material, and therefore the description of the first and second positive electrode active materials is omitted in that section.
[0136] The composite positive electrode active material can be in the form of secondary particles or assemblies, where primary particles of the first positive electrode active material and primary particles of the second positive electrode active material are aggregated. Primary particles of the first and second positive electrode active materials can be present within the composite positive electrode active material particles. The composite positive electrode active material particles are formed through the aggregation of primary particles of the first and second positive electrode active materials. This structure differs from a core-shell structure in which particles of the first positive electrode active material surround the surface of the core of the second positive electrode active material particles, thus having a shell structure. In this disclosure, the particulate form of the composite positive electrode active material can be referred to as a secondary particle form or an assembly form, and those described as secondary particle forms or assemblies should be understood to refer to composite positive electrode active material particles.
[0137] The composite positive electrode active material differs from the conventional form in which lithium iron phosphate-based compounds and lithium nickel-based composite oxides are mixed. When lithium iron phosphate-based compounds and lithium nickel-based composite oxides are conventionally mixed and used as positive electrode active materials, the following problem exists: after the electrode plate is formed, with repeated charging and discharging, high-temperature storage characteristics deteriorate due to the space (gap) generated between the particles of the lithium iron phosphate-based compound and the particles of the lithium nickel-based composite oxide. However, the composite positive electrode active material according to some embodiments solves the above-mentioned problem by having a particulate form, specifically a single secondary particle form by agglomerating primary particles of a first positive electrode active material and primary particles of a second positive electrode active material, more specifically an assembly form comprising: a first positive electrode active material in the form of primary particles of a lithium iron phosphate-based compound and a second positive electrode active material in the form of primary particles of a lithium nickel-based composite oxide.
[0138] The porosity of the composite positive electrode active material is less than or equal to about 25%, for example, about 10% to about 25%, about 10% to about 20%, about 10% to about 17%, about 12% to about 17%, or about 15% to about 17%. Porosity can refer to the ratio of the area occupied by pores in the cross-sectional area of the composite positive electrode active material particles. Porosity can be obtained, for example, by cutting the composite positive electrode active material particles with a focused ion beam (FIB) to obtain a cross-section, and measuring the ratio of the area occupied by pores in the cross-section of the composite positive electrode active material particles to the cross-sectional area of the composite positive electrode active material particles using an image analysis program such as ImageJ and a scanning electron microscope image of the cross-section. The cross-section of the secondary particles can be obtained by cutting the secondary particles with a focused ion beam (FIB). Images from a scanning electron microscope (SEM) can be acquired, for example, at a magnification of 5,000× to 50,000× under the same imaging conditions. Image analysis can be performed using a fixed threshold or a consistent threshold setting method equally applied to all samples. The porosity of the secondary particles can be the average of the porosities measured for multiple secondary particles, and can be obtained, for example, by measuring the porosity of at least 20 individual secondary particles and calculating the average porosity of the at least 20 individual secondary particles. If the porosity in the composite positive electrode active material particles meets the above range, during positive electrode compression, the primary particles can fill the spaces between the pores in the secondary particles, thereby improving the aggregate density or positive electrode density, and thus improving the capacity characteristics and energy density of the rechargeable lithium battery.
[0139] Furthermore, the agglomerate density of the composite positive electrode active material is greater than or equal to about 2.6 g / cc, for example, about 2.6 g / cc to about 3 g / cc, about 2.6 g / cc to about 2.8 g / cc, or about 2.6 g / cc to about 2.7 g / cc. The agglomerate density of the composite positive electrode active material can be measured as follows: 3 g of the composite positive electrode active material is placed in a mold, and the material is held in the mold at 25°C for 30 seconds. The thickness of the agglomerates is measured, and the agglomerate volume is calculated using the agglomerate thickness and the diameter of the mold. The mass of the composite positive electrode active material is then divided by the calculated volume. If the agglomerate density of the composite positive electrode active material meets the above range, powder characteristics can be improved, thereby improving capacity characteristics. If the porosity of the composite positive electrode active material particles meets the above range, during positive electrode compression, primary particles can further fill the pores in the secondary particles, and therefore, the agglomerate density of the composite positive electrode active material can be further improved as it is within the above range, and therefore, the energy density of the battery can be further increased.
[0140] The average particle size of the composite positive electrode active material particles can be, for example, about 3 μm to about 20 μm, about 6 μm to about 20 μm, about 6 μm to about 18 μm, about 8 μm to about 18 μm, about 10 μm to about 18 μm, or about 12 μm to about 18 μm. The average particle size of the composite positive electrode active material particles can be obtained, for example, by randomly selecting about 20 composite positive electrode active material particles from an electron microscope image of the composite positive electrode active material, measuring the size of each secondary particle, and calculating the arithmetic mean of the sizes of each secondary particle, wherein the size of each particle is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles.
[0141] The amounts of the first and second positive electrode active materials in the composite positive electrode active material can be appropriately controlled. Based on 100% by weight of the composite positive electrode active material, the first positive electrode active material may be included in an amount of about 50% to about 99% by weight, about 55% to about 95% by weight, or about 60% to about 90% by weight, and based on 100% by weight of the composite positive electrode active material, the second positive electrode active material may be included in an amount of about 1% to about 50% by weight, about 5% to about 45% by weight, or about 10% to about 40% by weight. If the first and second positive electrode active materials in the composite positive electrode active material are included to satisfy the above ranges, the battery can operate at high voltages, and for rechargeable lithium batteries, the overall battery performance (including initial charge / discharge capacity, efficiency, discharge capacity at low temperature (-20°C), and high-temperature storage characteristics) can be improved.
[0142] The composite positive electrode active material may further include a carbon coating layer on the particle surface of the composite positive electrode active material. The carbon coating layer can improve the electrical conductivity of the composite positive electrode active material and thereby reduce the resistance of the positive electrode comprising it.
[0143] The carbon coating layer may be the same as the carbon coating layer on the surface of the primary particles of the first positive electrode active material of the above-mentioned composite positive electrode active material, and therefore the description of the carbon coating layer is omitted in this section.
[0144] The number of primary particles of the second positive electrode active material in the composite positive electrode active material can be 10 or less, for example 9 or less, 8 or less, 7 or less, or 6 or less and 1 or more, 2 or more, or 3 or more. The number of primary particles of the second positive electrode active material in the composite positive electrode active material can be measured by imaging the cross-section or surface of the composite positive electrode active material using a scanning electron microscope. The first and second positive electrode active materials in the composite positive electrode active material can be distinguished by particle size, and the number of primary particles of the second positive electrode active material can be determined by counting the number of particles with a particle size greater than or equal to about 2 μm within a single composite positive electrode active material particle, where particle size refers to diameter in the case of spherical particles and the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles. Here, the number of primary particles of the second positive electrode active material can be the average number of primary particles of the second positive electrode active material in each of the multiple composite positive electrode active material particles.
[0145] The composite positive electrode active material can be prepared, for example, according to the method described above. The amount of composite positive electrode active material prepared according to the method described above can be used in equal quantities, and therefore, is omitted in this section.
[0146] Rechargeable lithium batteries
[0147] A rechargeable lithium battery according to some embodiments includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including the aforementioned composite positive electrode active material. A rechargeable lithium battery may include a positive electrode, a negative electrode, a separator between the positive and negative electrodes, and an electrolyte.
[0148] According to some embodiments, rechargeable lithium batteries can have generally improved battery performance by including the above-described positive electrode active material, and specifically, can provide improved low-temperature capacity and cycle life characteristics for rechargeable lithium batteries.
[0149] Rechargeable lithium batteries may have improved low-temperature capacity, such that the discharge capacity at low temperatures (e.g., about -20°C) is greater than or equal to about 105 mAh / g. The discharge capacity of a rechargeable lithium battery at low temperatures (-20°C) may be greater than or equal to about 106 mAh / g, greater than or equal to about 107 mAh / g, greater than or equal to about 108 mAh / g, greater than or equal to about 109 mAh / g, or greater than or equal to about 110 mAh / g and may be less than or equal to about 120 mAh / g. The low-temperature discharge capacity of the rechargeable lithium battery can be measured according to the methods described in the following evaluation examples.
[0150] Furthermore, when the high-temperature storage characteristics of a rechargeable lithium battery are evaluated by measuring its capacity retention after being placed at a high temperature (approximately 45°C) for 7 days, a high-temperature capacity retention rate of approximately 80% indicates that the high-temperature storage characteristics of the rechargeable lithium battery can be improved. The high-temperature capacity retention rate of a rechargeable lithium battery can be greater than or equal to approximately 81%, or greater than or equal to approximately 82% and less than or equal to approximately 100%, less than or equal to approximately 95%, or less than or equal to approximately 90%.
[0151] Depending on their geometry, rechargeable lithium batteries can be classified as cylindrical, prismatic, pouch-shaped, or coin-shaped. For example, Figure 1 This is a schematic diagram showing a cross-section of a cylindrical rechargeable lithium battery cut along a vertical axis according to some embodiments of the present disclosure and an electrode assembly 40 extending from the cylindrical rechargeable lithium battery. Figure 2 This is a cross-sectional view of a prismatic rechargeable lithium battery according to some embodiments of the present disclosure. Figure 3 and 4 Each of the following is a schematic exploded perspective view of a pouch-type rechargeable lithium battery according to some embodiments of the present disclosure. The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 between a positive electrode 10 and a negative electrode 20, and the electrode assembly 40 is housed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution (not shown).
[0152] The rechargeable lithium battery 100 may include a seal 60 of the sealed housing 50, such as Figure 1 As shown. Additionally, in Figure 2 The rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12, a negative electrode lead connector 21, and a negative electrode terminal 22. The rechargeable lithium battery 100 may include electrode connectors 70, which serve as electrical paths for conducting current generated in the electrode assembly 40 to the outside. The electrode connectors 70 may be as follows: Figure 4 The positive electrode terminal 71 and the negative electrode terminal 72 can be arranged in the same direction, or the positive electrode terminal 71 and the negative electrode terminal 72 can be arranged as follows: Figure 3 The same applies to the opposite direction.
[0153] The positive electrode, negative electrode, electrolyte, and separator that make up a rechargeable lithium battery will be described in sequence below.
[0154] positive electrode
[0155] The positive electrode includes a positive electrode current collector; and a positive electrode active material layer disposed on the positive electrode current collector and including the composite positive electrode active material prepared according to the method described above for preparing composite positive electrode active material. According to some embodiments, the positive electrode can improve overall battery performance by including the composite positive electrode active material prepared according to the method described above for preparing composite positive electrode active material, and specifically, for rechargeable lithium batteries, it can improve discharge capacity at low temperatures and high-temperature storage characteristics.
[0156] There are no particular restrictions on the positive electrode current collector, as long as it is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be an aluminum foil or stainless steel foil with a thickness of about 10 μm to about 15 μm.
[0157] The positive electrode active material layer includes the aforementioned composite positive electrode active material. Specific details of the composite positive electrode active material may be the same as those described above, and therefore a description of the composite positive electrode active material is omitted in this section.
[0158] The amount of composite positive electrode active material may be about 60% to about 99.9% by weight, about 70% to about 99.8% by weight, about 80% to about 99% by weight, or about 90% to about 98% by weight, based on a 100% by weight positive electrode active material layer.
[0159] The positive electrode active material layer may optionally further include a binder, a conductive material, or a combination thereof.
[0160] The binder can be used to ensure good adhesion between composite positive electrode active material particles and to ensure good adhesion of the composite positive electrode active material to the positive electrode current collector. Examples of binders may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide (polymers containing ethylene oxide), polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, nylon, but the binder is not limited to these.
[0161] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes undesirable chemical changes in the battery. Examples of conductive materials may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0162] In the positive electrode active material layer, based on 100% by weight of the positive electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the positive electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.
[0163] In addition to the components mentioned above, the positive electrode active material layer may further include other positive electrode active materials without prejudice to the purpose of this disclosure, or may further include irreversible positive electrode additives.
[0164] In addition to the aforementioned composite positive electrode active material, the positive electrode active material layer may further include a positive electrode active material having primary particle form and comprising the aforementioned lithium iron phosphate-based compound (hereinafter, "third positive electrode active material") and / or a positive electrode active material having primary particle form and comprising the aforementioned lithium nickel-based composite oxide (hereinafter, "fourth positive electrode active material"). Here, the third positive electrode active material and / or the fourth positive electrode active material may each be independently those of the first positive electrode active material and / or the second positive electrode active material included in the composite positive electrode active material, which exist in an unassembled and separated state. In this case, the average particle size of the primary particles of the third positive electrode active material may be the same as described above for the first positive electrode active material, and the average particle size of the primary particles of the fourth positive electrode active material may be the same as described above for the second positive electrode active material. Here, the third positive electrode active material and / or the fourth positive electrode active material exist in a non-aggregated, separated state, and do not agglomerate with the aforementioned composite positive electrode active material to form an assembled structure.
[0165] When the positive electrode active material layer further comprises a third positive electrode active material and / or a fourth positive electrode active material in addition to the composite positive electrode active material, the weight ratio of the composite positive electrode active material to the third positive electrode active material, the fourth positive electrode active material, or a combination thereof may be from about 1:9 to about 9:1. Positive electrode active materials comprising lithium iron phosphate-based compounds in the form of primary particles may further comprise the aforementioned carbon coating layer on the surface of the primary particles, and since the specific details of the carbon coating layer are as described above, those details are omitted in this section.
[0166] Irreversible positive electrode additives are compounds that act as sacrificial positive electrodes, compensating for the irreversible conversion of Li that no longer participates in the charging / discharging reaction by participating in the formation of an SEI (solid electrolyte interphase) film on the surface of the negative electrode during charging / discharging. Irreversible positive electrode additives are compounds that decompose during the formation process to provide Li and do not participate in subsequent charging / discharging processes. By adding such irreversible positive electrode additives, consumed lithium can be replenished, thereby compensating for lithium loss and improving the energy density, cycle life, and stability of rechargeable lithium batteries.
[0167] Irreversible positive electrode additives may include lithium iron-based oxides, lithium cobalt-based oxides, lithium nickel-based oxides, or combinations thereof.
[0168] The lithium iron-based oxide can be Li5FeO4, LiFeO2, LiFe5O8 or a combination thereof, and the use of Li5FeO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and thus greatly achieve the effect of an irreversible positive electrode additive.
[0169] The lithium cobalt-based oxide can be Li6CoO4, and the use of Li6CoO4 can provide a large amount of lithium during the formation process, which can greatly compensate for irreversible lithium, and thus greatly obtain the effect of an irreversible positive electrode additive.
[0170] The lithium nickel-based oxide can be Li2NiO2, and the use of Li2NiO2 can provide a large amount of lithium during the formation process, which can thus compensate for a large amount of irreversible lithium, and thus greatly achieve the effect of an irreversible positive electrode additive.
[0171] The average particle size D of the irreversible positive electrode additive 50 There are no particular limitations, but it can be, for example, about 0.5 μm to about 20 μm, about 0.5 μm to about 10 μm, about 0.5 μm to about 5 μm, or about 0.5 μm to about 3 μm.
[0172] negative electrode
[0173] The negative electrode for a rechargeable lithium battery includes a negative electrode current collector and a layer of negative electrode active material on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material and may optionally further include a binder, a conductive material, or a combination thereof.
[0174] There are no particular restrictions on the negative electrode current collector, as long as the negative electrode current collector is conductive and does not cause undesirable chemical changes in the rechargeable lithium battery, and can be a copper foil with a thickness of about 10 μm to about 15 μm.
[0175] Negative electrode active materials include materials capable of reversibly inserting / deintercalating lithium ions, lithium metal, lithium metal alloys, materials capable of doping and dedoping lithium, or transition metal oxides.
[0176] Materials capable of reversibly inserting / deintercalating lithium ions can be carbon-based negative electrode active materials, such as crystalline carbon, amorphous carbon, or combinations thereof. Crystalline carbon can be irregular, flake-like, spherical, or fibrous natural or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbonization products, or calcined coke.
[0177] As the alloy of lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.
[0178] The material capable of doping and dedoping lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. The Si-based negative electrode active material may be silicon, a silicon-carbon composite, SiO x (0<x≤2), a Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements [excluding Si], Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and may for example be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO₂, a Sn alloy, or a combination thereof.
[0179] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle diameter D of the silicon-carbon composite particles 50 may for example be about 0.5 μm to about 20 μm. According to some embodiments, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on the surfaces of the silicon particles. For example, it may include secondary particles (core) in which silicon primary particles are assembled (aggregated) and an amorphous carbon coating layer (shell) on the surfaces of the secondary particles. Amorphous carbon may also be present between the silicon primary particles, for example, the silicon primary particles may be coated with amorphous carbon. The secondary particles may be present dispersed in an amorphous carbon matrix.
[0180] The silicon-carbon composite may further include crystalline carbon. The silicon-carbon composite may include: a core including crystalline carbon and silicon particles, and an amorphous carbon coating layer on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may include soft carbon or hard carbon, a mesophase pitch carbonized product, or calcined coke.
[0181] When the silicon-carbon composite includes silicon and amorphous carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be about 10 wt% to about 50 wt%, and the amount of amorphous carbon may be about 50 wt% to about 90 wt%. In addition, when the composite includes silicon, amorphous carbon, and crystalline carbon, based on 100 wt% of the silicon-carbon composite, the amount of silicon may be about 10 wt% to about 70 wt%, the amount of crystalline carbon may be about 1 wt% to about 60 wt%, and the amount of amorphous carbon may be about 15 wt% to about 50 wt%.
[0182] In addition, the thickness of the amorphous carbon coating layer may be about 5 nm to about 100 nm. The average particle diameter D of silicon particles (primary particles) 50 may be about 10 nm to about 1 μm or about 10 nm to about 200 nm. In the present disclosure, when no definition is otherwise provided, the average particle diameter D 50 represents the particle diameter at a cumulative volume of about 50 vol% in the particle size distribution. The silicon particles may exist as elemental silicon, in the form of a silicon alloy, or in an oxidized form. The oxidized form of silicon may be represented as SiO x (0<x≤2). The atomic ratio of Si:O indicating the oxidation degree may be about 99:1 to about 33:67.
[0183] The Si-based negative electrode active material or Sn-based negative electrode active material may be mixed with the carbon-based negative electrode active material. When a mixture of the Si-based negative electrode active material or Sn-based negative electrode active material and the carbon-based negative electrode active material is used, the mixing ratio may be about 1:99 to about 90:10 by weight.
[0184] Based on 100 wt% of the negative electrode active material layer, the negative electrode active material may be included in an amount of about 90 wt% to about 99.8 wt% or about 94 wt% to about 99 wt%.
[0185] The binder serves to make the negative electrode active material particles adhere well to each other, and also to adhere the negative electrode active material to the negative electrode current collector. The binder may be a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.
[0186] The non-aqueous binder may include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or a combination thereof.
[0187] The aqueous binder may include styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.
[0188] When an aqueous binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity may be further included. As the cellulose-based compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. The alkali metal may be Na, K, or Li.
[0189] Dry adhesives can be polymeric materials that can be turned into fibers, and can be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.
[0190] Conductive materials are included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes undesirable chemical changes. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, or carbon nanotubes; metal-based materials including metal powders or fibers of copper, nickel, aluminum, or silver; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0191] Based on 100% by weight of the negative electrode active material layer, the amount of binder may be from about 0.1% by weight to about 5% by weight, and based on 100% by weight of the negative electrode active material layer, the amount of conductive material may be from about 0.1% by weight to about 5% by weight.
[0192] electrolytes
[0193] The electrolyte used in rechargeable lithium batteries is an electrolyte solution and includes a non-aqueous organic solvent and a lithium salt.
[0194] Non-aqueous organic solvents are used as media for transporting ions that participate in the electrochemical reactions of a battery. Non-aqueous organic solvents can be carbonate (carbonate-based) solvents, ester (ester-based) solvents, ether (ether-based) solvents, ketone (ketone-based) solvents, alcohol (alcohol-based) solvents, aprotic solvents, or combinations thereof.
[0195] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), or butyl carbonate (BC). Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, or caprolactone. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, or tetrahydrofuran. Ketone solvents may include cyclohexanone. Alcohol solvents may include ethanol or isopropanol, and aprotic solvents may include nitriles such as R-CN (where R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups); amides such as dimethylformamide; dioxolane such as 1,3-dioxolane or 1,4-dioxolane; or sulfolane.
[0196] Non-aqueous organic solvents can be used alone or in combination of two or more types, and when two or more types are used in combination, the mixing ratio can be appropriately adjusted depending on the expected battery performance, as is widely understood by those skilled in the art.
[0197] When using carbonate solvents, cyclic carbonates and chain carbonates can be mixed and used, and cyclic carbonates and chain carbonates can be mixed in a volume ratio of about 1:1 to about 1:9.
[0198] Non-aqueous organic solvents may further include aromatic hydrocarbon organic solvents. Carbonate solvents and aromatic hydrocarbon organic solvents may be mixed and used in a volume ratio of about 1:1 to about 30:1.
[0199] The electrolyte solution may further include vinylene carbonate, vinylene carbonate, or ethylene carbonate compounds to improve the cycle life of the rechargeable lithium battery.
[0200] Examples of ethylene carbonate compounds may include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.
[0201] Lithium salts dissolved in non-aqueous organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts may include at least one of the following: LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2 (where x and y are integers from 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).
[0202] The concentration of lithium salt can range from about 0.1 M to about 2.0 M. When the concentration of lithium salt is within this range, the electrolyte solution has suitable ionic conductivity and viscosity. Therefore, excellent performance can be achieved, and lithium ions can move efficiently.
[0203] diaphragm
[0204] Depending on the type of rechargeable lithium battery, a separator may be present between the positive and negative electrodes. The separator may be made of polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer membrane of two or more layers, and may be a hybrid multilayer membrane such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polypropylene three-layer separator, or a polypropylene / polypropylene / polypropylene three-layer separator.
[0205] The diaphragm may include a porous substrate and a coating on one or both surfaces of the porous substrate, comprising organic materials, inorganic materials, or combinations thereof.
[0206] The porous substrate may be a polymer film formed from any of the following polymers: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyacetal; polyamide; polyimide; polycarbonate; polyetherketone; polyaryletherketone; polyetherimide; polyamideimide; polybenzimidazole; polyethersulfone; polyphenylene ether; cyclic olefin copolymer; polyphenylene sulfide; polyethylene naphthalate; polytetrafluoroethylene (e.g., Teflon). ® (TEFLON ® Porous substrates may include glass fibers, or composite films comprising polymers and glass fibers.
[0207] The porous substrate may have a thickness of about 1 μm to about 40 μm, for example, about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm.
[0208] Organic materials may include (meth)acrylic acid copolymers, which include a first structural unit and a second structural unit derived from (meth)acrylamide, wherein the second structural unit includes at least one structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.
[0209] Inorganic materials may include the following inorganic particles: Al₂O₃, SiO₂, TiO₂, SnO₂, CeO₂, MgO, NiO, CaO, Ga₂O₃, ZnO, ZrO₂, Y₂O₃, SrTiO₃, BaTiO₃, Mg(OH)₂, boehmite, and combinations thereof, but inorganic materials are not limited to these. The average particle size D of the inorganic particles... 50 It can be about 1 nm to about 2000 nm, for example about 100 nm to about 1000 nm or about 100 nm to about 700 nm.
[0210] Organic and inorganic materials can be mixed in a coating, or coatings containing organic materials and coatings containing inorganic materials can be stacked.
[0211] The coating thickness can be from about 0.5 μm to about 20 μm, for example from about 1 μm to about 10 μm or from about 1 μm to about 5 μm.
[0212] In the following sections, embodiments and comparative examples of the present invention are described. However, the embodiments described below are merely some implementations of the present invention, and the present invention is not limited to the embodiments described below.
[0213] Example 1
[0214] (1) Preparation of composite positive electrode active material
[0215] (Preparation of the active material for the first positive electrode)
[0216] Mn, as a phosphate-based precursor 0.6 Fe 0.4 PO4 and Li2CO3, as a lithium raw material, were mixed at a molar ratio of 2:1 to prepare a raw material mixture. Additionally, a carbon raw material was prepared by mixing glucose and polyethylene glycol at a weight ratio of 5:5. 90 wt% of the raw material mixture and 10 wt% of the carbon raw material were mixed to form a combined mixture, and distilled water, as a second solvent, was added to the combined mixture to wet-mill the mixture into a second slurry. Wet milling was performed using a ball mill. Specifically, approximately 90 wt% of the raw material mixture and approximately 10 wt% of the carbon source material were introduced into a milling vessel with a capacity of approximately 5 L along with approximately 3 kg of zirconia balls and approximately 2 kg of water, and wet milling was performed by rotating the vessel at approximately 100 rpm for approximately 3 hours. During wet milling, TiO2, as a titanium-based raw material, was added, and the amount was adjusted such that Ti accounted for 0.4 mol%, based on the total metals other than lithium in the final lithium iron phosphate-based compound.
[0217] A second slurry, wet-milled, is fed into a spray dryer (Büchi Mini SprayDryer B-290) at 0.5 kg / min and then spray-dried at 200°C to obtain a second dried product. This second dried product is then calcined at 750°C for 8 hours to obtain a second calcined product, which is then pulverized into primary particles using an air-jet mill at 6000 rpm to obtain a first positive electrode active material. The second calcined product (which comprises a lithium iron phosphate-based compound in the form of secondary particles (or assemblies) where multiple primary particles agglomerate) is pulverized into a first positive electrode active material where the multiple primary particles do not agglomerate but are instead separated. The first positive electrode active material has Li(Mn) 0.6 Fe 0.4 ) 0.996 Ti 0.004The PO4 composition is in the form of primary particles with an average particle size of 0.5 μm. A carbon coating layer was confirmed to have formed on the surface of each primary particle.
[0218] (Preparation of the active material for the second positive electrode)
[0219] Ni 0.6 Co 0.1 Mn 0.3 (OH)₂ and LiOH were mixed in a 1:1 molar ratio and subjected to a first heat treatment at 850°C for 15 hours in an oxygen atmosphere to prepare LiNi particles with an average particle size of 3 μm. 0.6 Co 0.1 Mn 0.3 The composition of O2 is a lithium nickel-based composite oxide.
[0220] Subsequently, the lithium-nickel-based composite oxide and tungsten oxide (WO3) in single-particle form were introduced into a Henschel mixer and mixed for 30 minutes to prepare a mixture. At this point, the tungsten content derived from tungsten oxide was adjusted to 0.25 mol%, based on 100 mol% of all metals except lithium in the final second positive electrode active material.
[0221] The mixture is then subjected to a second heat treatment to obtain the second positive electrode active material. The heat treatment is performed by a heating step, increasing the temperature from 25°C to 400°C at a rate of 6.25°C / min, followed by a holding step at 400°C for 5 hours. The second positive electrode active material has LiNi 0.5985 Co 0.09975 Mn 0.29925 W 0.0025 The O2 composition is in the form of single particles with an average particle size of approximately 3 μm. The single particles of the second positive electrode active material correspond to the primary particles that constitute the secondary particles in the composite positive electrode active material described below, and are used herein with the same meaning as primary particles.
[0222] (Preparation of composite positive electrode active material)
[0223] The first positive electrode active material and the second positive electrode active material were mixed at a weight ratio of 9:1 for 30 minutes at 15 rpm using a mixer (L5M-A), and water was added as the first solvent for wet milling to prepare a first slurry. The first slurry was added to a spray dryer (Büchi Mini Spray Dryer B-290) at a rate of 0.5 kg / min and then spray dried at 200°C to obtain a first dried product. Wet milling was performed using a ball mill. Specifically, about 3 kg of zirconia balls, about 2 kg of water, and about 2 kg of a mixture of the first and second positive electrode active materials mixed at a weight ratio of 9:1 were introduced into a milling vessel with a capacity of about 5 L, and the vessel was rotated at a speed of about 50 rpm for about 1 hour. The first dried product was a composite positive electrode active material in the form of secondary particles in which the primary particles of the first positive electrode active material and the primary particles of the second positive electrode active material agglomerated.
[0224] (2) Manufacturing of the positive electrode
[0225] A composite positive electrode active material was prepared by mixing polyvinylidene fluoride as a binder and carbon nanotubes as a conductive material at a weight ratio of 96:2:2 (positive electrode active material: binder: conductive material). This composition was dispersed in N-methylpyrrolidone solvent to prepare a positive electrode active material slurry, which was then coated onto a 15 μm thick Al foil, dried, and compressed to fabricate the positive electrode.
[0226] (3) Manufacturing of rechargeable lithium battery cells
[0227] A negative electrode active material slurry was prepared by dispersing 97.5% by weight graphite as the negative electrode active material, 1.5% by weight carboxymethyl cellulose and 1% by weight styrene-butadiene rubber as binders in distilled water. This slurry was coated onto a 10 μm thick Cu foil, then dried and compressed to fabricate the negative electrode.
[0228] An electrode assembly was fabricated by placing a 10 μm thick polyethylene separator between the positive and negative electrodes. This assembly was then inserted into a housing, and an electrolyte was injected into the housing to fabricate a rechargeable lithium-ion battery cell (a pouch cell at the 100 mAh level). The electrolyte was prepared by mixing EC (ethylene carbonate): EMC (ethyl methyl carbonate): DMC (dimethyl carbonate) at a volume ratio of 2:4:4 and dissolving 1.15 M LiPF6 in the mixed solvent.
[0229] Example 2
[0230] The composite positive electrode active material, the positive electrode, and the rechargeable lithium battery cell were manufactured in essentially the same manner as in Example 1, except that: in part “(1) Preparation of composite positive electrode active material” of Example 1, after the first slurry was fed into a spray dryer and spray-dried to obtain a first dried product, the first dried product was additionally calcined at 400°C for 8 hours under a nitrogen atmosphere to obtain a first calcined product, which was used as the composite positive electrode active material in place of the first dried product of Example 1 in “(2) Manufacturing of positive electrode”.
[0231] Comparative Example 1
[0232] The composite positive electrode active material, positive electrode, and rechargeable lithium battery cell were manufactured in essentially the same manner as in Example 1, except that: a lithium iron phosphate-based compound in the form of secondary particles with an average particle size of 10 μm, wherein the primary particles therein agglomerate, are used instead of the first positive electrode active material obtained during the preparation of the second slurry in part “(1) Preparation of Composite Positive Electrode Active Material” of Example 1. In other words, compared with Example 1, which obtained a lithium iron phosphate-based compound in the form of primary particles and then wet-milled it together with the second positive electrode active material, Comparative Example 1 differs from Example 1 in that: a lithium iron phosphate-based compound in the form of secondary particles, wherein the primary particles are agglomerated, is wet-milled together with the second positive electrode active material.
[0233] The lithium iron phosphate-based compound was prepared in essentially the same manner as the first positive electrode active material of Example 1, in the form of secondary particles with an average particle size of 10 μm, except that: in the preparation process of the second slurry of Example 1, the wet grinding time was changed from 3 hours to 6 hours and the grinding speed was changed from 6000 rpm to 1500 rpm.
[0234] Comparative Example 2
[0235] The positive electrode and rechargeable lithium battery cell were manufactured in essentially the same manner as in Example 1, except that the first positive electrode active material obtained in part “(1) Preparation of composite positive electrode active material” and the prepared second positive electrode active material were simply mixed at 15 rpm for 30 minutes at a weight ratio of 9:1 to prepare the positive electrode active material in part “(2) Manufacturing of positive electrode” of Example 1.
[0236] Evaluation Example 1: Evaluation of Composite Positive Electrode Active Materials
[0237] (1) Porosity evaluation
[0238] The porosity of the composite positive electrode active materials prepared in Examples 1 and 2 and Comparative Example 1 was measured and is shown in Table 1. Using the ImageJ image analysis program, the ratio of the area occupied by pores to the cross-sectional area of the secondary particles in the cross-section of the secondary particles was measured from scanning electron microscope images of the cross-section of the secondary particles, and this ratio is expressed as porosity in Table 1.
[0239] (2) Particle analysis
[0240] The composite positive electrode active material prepared in Example 2 was analyzed by taking cross-sectional scanning electron microscope images. Figure 5 and 6 Scanning electron microscope images of the cross-sections of the composite positive electrode active material of Example 2 at different magnifications.
[0241] Within a single composite positive electrode active material particle, black indicates internal pores, and gray indicates the first and second positive electrode active materials. Among those marked in gray, the second positive electrode active material refers to particles with a particle size greater than or equal to about 2 μm, while the first positive electrode active material refers to the remaining particles with a particle size less than about 2 μm. Particle size is defined as diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles.
[0242] refer to Figure 5 and 6 A composite positive electrode active material particle shows that multiple first positive electrode active material particles and multiple second positive electrode active material particles agglomerate with each other to form an assembly.
[0243] Similar to Example 2, cross-sectional scanning electron microscope images of the composite positive electrode active materials prepared in Example 1 and Comparative Example 1 were taken, and the average particle size of the secondary particles, the arithmetic mean size of the primary particles of the first positive electrode active material, the standard deviation of the arithmetic mean size of those primary particles, and the average particle size of the primary particles of the second positive electrode active material were measured. The results are shown in Table 1.
[0244] The average particle size of the secondary particles was obtained as follows: approximately 20 secondary particles were randomly selected from the scanning electron microscope images of each composite positive electrode active material, the size of each secondary particle was measured, and the arithmetic mean of the sizes of each secondary particle was calculated. The size of each secondary particle was defined as the diameter in the case of spherical particles, and as the square root of the product of the major and minor axes in the case of non-spherical particles. The average particle size of the primary particles of the first and second positive electrode active materials was also obtained as follows: approximately 20 primary particles of the first and second positive electrode active materials were randomly selected from the scanning electron microscope images of each composite positive electrode active material, respectively. The size of each primary particle was measured, and the arithmetic mean of the sizes of each primary particle was calculated. The size of each primary particle was defined as the diameter in the case of spherical particles, and as the square root of the product of the major and minor axes in the case of non-spherical particles. In this case, within the composite positive electrode active material, as described above, particles with a particle size of less than about 2 μm are considered primary particles of the first positive electrode active material and their particle size is measured to obtain an arithmetic mean, while particles with a particle size greater than or equal to about 2 μm are considered primary particles of the second positive electrode active material and their particle size is measured to obtain an arithmetic mean.
[0245] The arithmetic mean size and standard deviation of the first positive electrode active material were obtained by measuring the size of any 20 primary particles of the first positive electrode active material from a scanning electron microscope image of the cross-section of the composite positive electrode active material (wherein the particle size is defined as the diameter in the case of spherical particles, and as the square root of the product of the major axis length and the minor axis length in the case of non-spherical particles), and calculating the arithmetic mean and the standard deviation of the arithmetic mean.
[0246] The number of primary particles of the second positive electrode active material in the composite positive electrode active material was determined by counting the number of particles with a size greater than or equal to about 2 μm in a scanning electron microscope image of the cross-section of the composite positive electrode active material. The particle size was defined as the diameter in the case of spherical particles and as the square root of the product of the major and minor axes in the case of non-spherical particles. Here, the number of primary particles is the average number of primary particles of the second positive electrode active material in multiple composite positive electrode active material particles.
[0247] Meanwhile, unlike Examples 1 and 2 and Comparative Example 1, Comparative Example 2 (in which the first positive electrode active material and the second positive electrode active material are simply mixed, rather than the mixture being spray-dried into a dried product and calcined into an assembly) has the first positive electrode active material and the second positive electrode active material in a dispersed state, and therefore, there is no evaluation of Comparative Example 2 in Table 1.
[0248] Table 1:
[0249]
[0250] Referring to Table 1, the composite positive electrode active materials of Examples 1 and 2 have a first positive electrode active material exhibiting relatively small and uniform primary particles, which, together with the primary particles of the second positive electrode active material, form an assembly. Meanwhile, in Comparative Example 1, the first positive electrode material is not obtained by pulverizing the calcined product to obtain primary particles, but rather by the calcined product itself, i.e., in the form of an assembly. Although Comparative Example 1 is manufactured in an assembly form as in Examples 1 and 2, it exhibits relatively high porosity and is relatively non-uniform due to the large standard deviation in the primary particles of the first positive electrode active material.
[0251] Evaluation Example 2: Particle Density Evaluation
[0252] The agglomerate density of the (composite) positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2 was determined as follows: 3 g of the (composite) positive electrode active material was placed in a mold, and the (composite) positive electrode active material was held in the mold at 25°C for 30 seconds. The thickness of the agglomerate was measured, and the agglomerate volume was calculated using the agglomerate thickness and the diameter of the mold. The mass of the (composite) positive electrode active material was then divided by the calculated volume.
[0253] Evaluation Example 3: Evaluation of Battery Performance
[0254] The battery performance of the rechargeable lithium battery cells of Examples 1 and 2 and Comparative Examples 1 and 2 was evaluated at an evaluation voltage of 4.45 V.
[0255] (1) Evaluation of initial charge / discharge capacity and efficiency
[0256] The rechargeable lithium-ion battery cells of Examples 1 and 2, as well as Comparative Examples 1 and 2, were charged at 25°C at a rate of 0.2 C to the evaluation voltage and discharged at a rate of 0.2 C to a cutoff voltage of 3.0 V to measure the initial charge / discharge capacity, which was used to calculate the initial efficiency according to Equation 1. The results are shown in Table 2.
[0257] Equation 1 is as follows:
[0258] [Equation 1]
[0259] Initial efficiency [%] = [Discharge capacity in the first cycle / Charge capacity in the first cycle] × 100
[0260] (2) Average voltage
[0261] The average voltage of the rechargeable lithium battery cells of Examples 1 and 2 and Comparative Examples 1 and 2 was measured at 50% SOC (State of Charge) during the initial discharge period, and the results are shown in Table 2.
[0262] (3) Low-temperature capacity evaluation
[0263] The rechargeable lithium-ion battery cells of Examples 1 and 2, as well as Comparative Examples 1 and 2, were fully charged to the evaluation voltage at a rate of 0.2 C, and then discharged to 3.0 V at a rate of 0.2 C in an atmosphere set to -20°C to measure the low-temperature discharge capacity. The results are shown in Table 2.
[0264] (4) Cyclic life characteristic evaluation
[0265] After initial charging and discharging, the rechargeable lithium battery cells of Examples 1 and 2 and Comparative Examples 1 and 2 were repeatedly charged at a rate of 1 C to the evaluation voltage, and then discharged at a rate of 1 C to a cutoff voltage of 3.0 V 50 times or more to calculate the ratio of the discharge capacity of the 50th cycle to the initial discharge capacity according to Equation 2, and the results are shown in Table 2.
[0266] Equation 2 is as follows:
[0267] [Equation 2]
[0268] Cycle lifetime [%] = [Discharge capacity at 50th cycle / Discharge capacity at 1st cycle] × 100
[0269] (5) Evaluation of high temperature storage characteristics
[0270] The rechargeable lithium-ion battery cells of Examples 1 and 2, as well as Comparative Examples 1 and 2, were charged at a rate of 0.2 C to 98% SOC and then placed in a high-temperature room at 45°C for 7 days to calculate the capacity retention rate. The results are shown in Table 2.
[0271] (6) Capacity evaluation per volume
[0272] The capacity per volume of the rechargeable lithium-ion battery cells of Examples 1 and 2 and Comparative Examples 1 and 2 were evaluated, and the results are shown in Table 2. Specifically, the capacity per volume was obtained by multiplying the density by the capacity.
[0273] Table 2:
[0274]
[0275] Referring to Table 2, in contrast to Comparative Examples 1 and 2, Examples 1 and 2 (which use dried products obtained by: [a] wet milling of a first positive electrode active material in the form of primary particles and a second positive electrode active material in the form of primary particles to prepare a slurry, and [b] drying the slurry, and [c] additionally calcining the dried product) exhibit excellent agglomerate density, average voltage, low-temperature discharge capacity, 1 C cycle life, high-temperature capacity retention, and capacity per volume. In particular, the rechargeable lithium-ion battery cells of Examples 1 and 2 exhibit significantly superior low-temperature discharge capacity and high-temperature capacity retention (compared to those of the Comparative Examples), confirming that the interconnectivity between particles ensures the continuous formation of conductive paths, resulting in smooth movement of electrons and lithium ions, and thus excellent discharge characteristics in low-temperature environments. Meanwhile, the positive electrode active material of Comparative Example 1 has an assembly form similar to that of Example 1, but exhibits a non-uniform assembly form, thus leading to uneven distribution of electrochemical reactions within the electrode and obstacles in the lithium-ion transport path, resulting in deterioration of low-temperature discharge performance. Furthermore, in the positive electrode active material of Comparative Example 2, the first positive electrode active material and the second positive electrode active material are simply mixed, and therefore, there is no sufficient electrochemical reaction between the two types of particles. This leads to the isolation of each particle, and thus the overall battery performance deteriorates due to the physical connection problem between the two types of particles, resulting in a significant deterioration of the high-temperature storage characteristics.
[0276] While the invention has been described with respect to some embodiments as described above, this disclosure is not limited to the embodiments described above. Rather, this disclosure covers various modifications and equivalent arrangements of the embodiments described above.
[0277] <Description of representative figure labels>
[0278] 100: Rechargeable lithium battery; 10: Positive electrode
[0279] 11: Positive electrode lead connector 12: Positive electrode terminal
[0280] 20: Negative electrode 21: Negative electrode lead connector
[0281] 22: Negative electrode terminal; 30: Diaphragm
[0282] 40: Electrode assembly; 50: Housing
[0283] 60: Seal 70: Electrode terminal
[0284] 71: Positive electrode connector; 72: Negative electrode connector
Claims
1. A method for preparing a composite positive electrode active material, the method comprising: Prepare a first positive electrode active material comprising a lithium iron phosphate-based compound and having primary particulate form; Prepare a second positive electrode active material comprising a lithium-nickel-based composite oxide and having primary particle form; The first positive electrode active material and the second positive electrode active material are mixed and wet-milled to prepare a first slurry; as well as The first slurry is added to a spray dryer and the first slurry is spray-dried to prepare a first dried product.
2. The method according to claim 1, wherein preparing the first positive electrode active material comprises: The iron phosphate-based precursor, lithium raw material and carbon raw material mixed in the second solvent are wet-milled to prepare the second slurry; A second slurry, which has been wet-milled, is added to a spray dryer and the second slurry is spray-dried to prepare a second dried product; The second dried product is calcined to prepare a second calcined product; as well as The second fired product is pulverized.
3. The method according to claim 2, wherein the second calcined product is in the form of secondary particles formed by the agglomeration of multiple primary particles.
4. The method according to claim 2, wherein in the pulverization of the second calcined product, the pulverization is carried out at a pulverization speed greater than 2000 rpm.
5. The method according to claim 1, wherein the lithium iron phosphate-based compound comprises a compound represented by chemical formula 1, a compound represented by chemical formula 2, or a combination thereof: [Chemical Formula 1] Li a1 Fe (1-x1) M 1 x1 PO4, Where 0.9≤a1≤1.5, 0≤x1≤0.4, and M 1 It is Al, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or combinations thereof. [Chemical Formula 2] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4, Where 0.9≤a²≤1.5, 0.1≤x²≤0.9, 0≤y²<0.9, x²+y²<1, and M 2 It is Al, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Sr, Ti, V, W, Y, Zn, Zr or a combination thereof.
6. The method according to claim 1, wherein the lithium iron phosphate-based compound comprises LiFePO4, LiMn 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4, LiMn 0.3 Fe 0.7 PO4 or combinations thereof.
7. The method according to claim 1, wherein the average particle size of the primary particles of the first positive electrode active material is greater than or equal to 0.1 μm and less than 2 μm.
8. The method according to claim 1, wherein the lithium-nickel-based composite oxide is represented by the following: Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 X b3 , Where 0.9≤a³≤1.2, 0.3≤x³≤1, 0≤y³≤0.7, 0≤z³≤0.7, 0.9≤x³+y³+z³≤1.1, and 0≤b³≤0.1, M 3 and M 4 Each of the following elements independently is Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, Zr, or combinations thereof, M 3 and M 4 Let X be distinct elements, and let X be F, P, S or a combination thereof.
9. The method of claim 1, wherein the amount of nickel in the lithium nickel-based composite oxide is from 50 mol% to 80 mol% based on 100 mol% of the total metals other than lithium in the lithium nickel-based composite oxide.
10. The method according to claim 1, wherein the average particle size of the primary particles of the second positive electrode active material is 2 μm to 8 μm.
11. The method according to claim 1, wherein in the mixing and wet milling of the first positive electrode active material and the second positive electrode active material, the weight ratio of the first positive electrode active material and the second positive electrode active material is from 50:50 to 99:
1.
12. The method of claim 1, wherein adding the first slurry to the spray dryer and spray drying the first slurry to prepare the first dried product comprises spray drying the first slurry at a temperature of 150°C to 400°C.
13. The method of claim 1, further comprising, after adding the first slurry to a spray dryer and spray-drying the first slurry to prepare the first dried product, calcining the first dried product to prepare the first calcined product.
14. The method of claim 13, wherein calcining the first dried product comprises calcining the first dried product in a vacuum or in an inert gas at a temperature of 300°C to 1000°C.
15. A composite positive electrode active material, having a particulate form, said composite positive electrode active material comprising: The first positive electrode active material includes lithium iron phosphate-based compounds and has the form of multiple primary particles; and The second positive electrode active material includes lithium-nickel-based composite oxides and is in the form of multiple primary particles. The composite positive electrode active material is in particulate form, which includes multiple primary particles of the first positive electrode active material and multiple primary particles of the second positive electrode active material. The porosity of the composite positive electrode active material is less than or equal to 25%, and The aggregate density of the composite positive electrode active material is greater than or equal to 2.6 g / cc.
16. The composite positive electrode active material according to claim 15, wherein the particle form of the composite positive electrode active material is a secondary particle form, and the average particle size of the secondary particles of the composite positive electrode active material is 3 μm to 20 μm.
17. A rechargeable lithium battery, comprising: Positive electrode; negative electrode; and Electrolytes, The positive electrode includes: Positive electrode current collector; and A positive electrode active material layer is disposed on the positive electrode current collector and includes the composite positive electrode active material according to claim 15 or 16.