A method for regenerating waste lithium iron phosphate materials and the regenerated lithium iron phosphate materials
By combining ball milling and low-temperature calcination with hydrothermal treatment, carbon impurities in waste lithium iron phosphate materials are effectively removed, solving the performance degradation problem caused by high-temperature calcination and realizing the preparation of highly efficient recycled lithium iron phosphate materials.
Patent Information
- Application Number
- CN202611206114.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
In existing waste lithium iron phosphate material recycling technologies, high-temperature calcination to remove carbon impurities leads to a decline in material performance, and it is difficult to effectively control lithium-ion diffusion channels and lattice repair under high-temperature conditions.
Ammonium persulfate and polyols are used as activators. Oxygen-containing functional groups and structural defects are generated through ball milling. Then, the mixture is calcined at low temperature in an oxygen atmosphere. Combined with hydrothermal treatment and low-temperature calcination under an inert atmosphere, carbon impurities are effectively removed and lithium ions are added.
While reducing energy consumption, the electrochemical performance of the recycled lithium iron phosphate material was improved, the residual carbon content was reduced, the lithium-ion diffusion channels were enhanced, and the high reactivity and electrochemical performance of the material were ensured.
Smart Images

Figure CN123105583A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of lithium iron phosphate material regeneration, specifically to a method for regenerating waste lithium iron phosphate material and the regenerated lithium iron phosphate material. Background Technology
[0002] In existing waste lithium iron phosphate material recycling technologies, the waste lithium iron phosphate material is usually ball-milled and then directly subjected to hydrothermal lithium replenishment, followed by high-temperature (≥700℃) calcination under an inert atmosphere.
[0003] Waste lithium iron phosphate materials contain some carbon material impurities, such as conductive carbon skeletons and binders. In order to remove these carbon material impurities, the calcination temperature needs to be maintained at a high level. If the calcination temperature is lowered, the residual carbon content in the recycled lithium iron phosphate material will be high, which will affect the electrochemical performance of the recycled lithium iron phosphate material. Summary of the Invention
[0004] The first aspect of this application provides a method for regenerating waste lithium iron phosphate materials, comprising the following steps: Obtain waste lithium iron phosphate materials; Waste lithium iron phosphate material is mixed with an activator and ball-milled to obtain activated lithium iron phosphate material; wherein the activator includes ammonium persulfate and polyol; The activated lithium iron phosphate material was calcined at a first temperature in an oxygen-rich atmosphere to obtain the calcined lithium iron phosphate material. The calcined lithium iron phosphate material was mixed with a lithium replenishing agent to obtain a mixture. The mixture was then subjected to hydrothermal treatment under an inert atmosphere to obtain a precursor. The precursor is calcined at a second temperature under an inert atmosphere to obtain recycled lithium iron phosphate material; wherein the second temperature is 350℃~450℃.
[0005] In some optional embodiments of the first aspect of this application, the polyol is selected from at least one of ethylene glycol, 1,2-propanediol, 1,3-propanediol and glycerol.
[0006] In some optional embodiments of the first aspect of this application, the polyol is selected from ethylene glycol.
[0007] In some optional embodiments of the first aspect of this application, the mass ratio of ammonium persulfate to polyol ranges from 1:(1~3).
[0008] In some optional embodiments of the first aspect of this application, the mass of the activator is 5% to 15% of the mass of the waste lithium iron phosphate material.
[0009] In some optional embodiments of the first aspect of this application, mixing waste lithium iron phosphate material with an activator and then ball milling it includes: Waste lithium iron phosphate material is mixed with an activator and ball-milled at 300 rpm to 400 rpm for 2 to 4 hours.
[0010] In some optional embodiments of the first aspect of this application, the activated lithium iron phosphate material is calcined at a first temperature in an oxygen-containing atmosphere to obtain the calcined lithium iron phosphate material, comprising: The activated lithium iron phosphate material was calcined for 1 to 2 hours at an oxygen concentration of 6% to 10% and a first temperature of 300°C to 400°C, and then naturally cooled to room temperature to obtain the calcined lithium iron phosphate material.
[0011] In some optional embodiments of the first aspect of this application, the lithium replenishing agent includes a lithium source and a carbon source; The calcined lithium iron phosphate material was mixed with a lithium supplementer to obtain a mixture. The amount of lithium source added was controlled so that the molar ratio of Fe to Li in the mixture was 1:(1~1.05), and the amount of carbon source added was 10%~30% of the mass of the calcined lithium iron phosphate material. The mixture is subjected to hydrothermal treatment under an inert atmosphere to obtain a precursor, including: subjecting the mixture to hydrothermal treatment at 200℃~300℃ for 1h~2h under an inert atmosphere, and then naturally cooling to room temperature after the hydrothermal treatment to obtain lithium iron phosphate material after lithium supplementation. The lithium iron phosphate material after lithium supplementation was vacuum dried at 50℃~100℃ for 6h~8h to obtain the precursor.
[0012] In some optional embodiments of the first aspect of this application, the precursor is calcined at a second temperature under an inert atmosphere to obtain a recycled lithium iron phosphate material, comprising: Under an inert atmosphere, the temperature is increased to 350℃~450℃ at a heating rate of 5℃ / min~10℃ / min, and the precursor is calcined for 2h~3h. After cooling to room temperature, recycled lithium iron phosphate material is obtained.
[0013] In some optional embodiments of the first aspect of this application, after obtaining the calcined lithium iron phosphate material and before mixing the calcined lithium iron phosphate material with the lithium replenishing agent, the method further includes: The calcined lithium iron phosphate material was washed with water and dried.
[0014] Secondly, a recycled lithium iron phosphate material is provided, which is prepared by the above-mentioned method for recycling waste lithium iron phosphate material.
[0015] Beneficial effects: In the recycling method for waste lithium iron phosphate material provided in the first aspect of this application, the waste lithium iron phosphate material is mixed with an activator and ball-milled to activate the waste lithium iron phosphate material. During the ball milling process, a large number of oxygen-containing functional groups and structural defects are generated on the surface of carbon impurities (conductive carbon skeleton, binder residue) in the waste lithium iron phosphate material, and the carbon impurities are transformed into easily removable forms. At the same time, the surface of the lithium iron phosphate particles also generates lattice distortion and vacancy defects due to mechanical force, providing a fast channel for subsequent lithium ion diffusion. The activated lithium iron phosphate material is then calcined at a first temperature with oxygen to obtain calcined lithium iron phosphate material with a clean surface and high reactivity. The abundant defect sites (such as oxygen vacancies and step dislocations) on the surface of the calcined lithium iron phosphate material reduce the activation energy of lithium ion migration, providing a fast channel for lithium ion diffusion. At the same time, the oxygen-containing functional groups on the surface enhance hydrophilicity, promote the mass transfer efficiency of the lithium source at the interface during hydrothermal processes, so that the inert calcination temperature can be reduced to 350℃~450℃ to complete the lattice repair, thereby avoiding Fe 2+ High-performance regeneration is achieved under the premise of oxidative instability. Attached Figure Description
[0016] Figure 1 This is a method flowchart of one embodiment of this application. Detailed Implementation
[0017] The present application will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only for explaining the present application and are not intended to limit the present application.
[0018] In one embodiment, such as Figure 1 As shown, a method for regenerating waste lithium iron phosphate materials is provided, including the following steps: Step 1: Obtain waste lithium iron phosphate materials; Step 2: Mix the waste lithium iron phosphate material with the activator and ball mill it to obtain activated lithium iron phosphate material; wherein, the activator includes ammonium persulfate and polyol; Step 3: In an oxygen-rich atmosphere, the activated lithium iron phosphate material is calcined at a first temperature to obtain the calcined lithium iron phosphate material. Step 4: Mix the calcined lithium iron phosphate material with a lithium replenishing agent to obtain a mixture. Perform hydrothermal treatment on the mixture under an inert atmosphere to obtain a precursor. Step 5: Under an inert atmosphere, the precursor is calcined at a second temperature to obtain recycled lithium iron phosphate material; wherein the second temperature is 350℃~450℃.
[0019] In the above scheme, waste lithium iron phosphate material is mixed with an activator and ball-milled, resulting in the formation of numerous oxygen-containing functional groups and structural defects on the surface of the waste lithium iron phosphate material. Carbon impurities in the waste lithium iron phosphate material are transformed into easily removable forms. The activated lithium iron phosphate material is then calcined at a first temperature with oxygen to obtain a clean surface and highly reactive calcined lithium iron phosphate material. The abundant defect sites on the surface of the calcined lithium iron phosphate material provide a rapid channel for lithium-ion diffusion, allowing for effective lithium-ion replenishment and lattice structure repair at only 350℃~450℃ under an inert atmosphere, thereby avoiding Fe... 2+ High-performance regeneration is achieved under the premise of oxidative instability.
[0020] The waste lithium iron phosphate material in this embodiment includes carbon material impurities such as conductive carbon skeleton and binder residue. The waste lithium iron phosphate material originates from waste lithium iron phosphate battery cathode materials. The specific steps for obtaining the waste lithium iron phosphate material are as follows: Waste lithium iron phosphate battery cathode material is initially crushed, then deeply crushed using an air jet mill, and sieved through a screen to obtain powder. The powder is then mixed with a 0.1 mol / L to 0.5 mol / L dilute NaOH solution at a mass ratio of 1:(2 to 5), stirred at room temperature for 2 to 4 hours, and centrifuged to remove aluminum from the powder, thus obtaining waste lithium iron phosphate material.
[0021] In some optional embodiments of this application, the polyol is selected from at least one of ethylene glycol, 1,2-propanediol, 1,3-propanediol, and glycerol. Ethylene glycol, 1,2-propanediol, 1,3-propanediol, and glycerol can serve as liquid media and dispersants, providing hydroxyl sites to participate in free radical oxidation reactions.
[0022] In some optional embodiments of this application, the polyol is selected from ethylene glycol. Ethylene glycol exhibits better performance in terms of reaction tunability, liquid-phase stability (boiling point 197°C), and avoidance of introducing foreign metal cation impurities.
[0023] The following description uses ammonium persulfate and ethylene glycol as activators to further illustrate this example.
[0024] Waste lithium iron phosphate materials contain carbon material impurities such as conductive carbon skeletons and binder residues. These carbon material impurities can cause the structure to peel off and break due to the ball milling shear force during the ball milling process, resulting in a large number of defects and active sites (such as dangling bonds and edge carbon atoms).
[0025] On the other hand, ammonium persulfate is a strong oxidizing agent. The peroxy bond (-OO-) in the ammonium persulfate molecule is relatively weak and easily breaks when subjected to external energy (such as heat, mechanical force, or free radical initiation), generating sulfate free radicals (SO42-), which have strong oxidizing properties. -The ball milling process generates intense impacts, shearing, and friction from the high-speed moving grinding balls, converting mechanical energy into the chemical energy of the reaction system. The instantaneous temperature at the impact point of the grinding balls triggers the thermal decomposition of ammonium persulfate, with local pressures reaching GPa levels, forcing ammonium persulfate or its decomposition products into the interlayers or defects of the carbon material. Simultaneously, ball milling achieves molecular-level uniform contact in the solid-liquid-solid multiphase system, overcoming the diffusion limitations inherent in traditional liquid-phase oxidation.
[0026] Ethylene glycol serves as a liquid medium and dispersant, ensuring uniform contact between ammonium persulfate and the carbon materials in the waste lithium iron phosphate material. The hydroxyl groups (-OH) of ethylene glycol can be attacked by free radicals, generating ethylene glycol free radicals. These free radicals can further react with the carbon materials or ammonium persulfate, propagating and maintaining the free radical chain reaction. Ethylene glycol has a high boiling point (197℃), allowing it to remain liquid under the localized high temperatures generated by ball milling, thus stabilizing the reaction environment.
[0027] More specifically, during the ball milling process, the mechanical energy of the ball milling directly acts on the ammonium persulfate molecules, causing the peroxy bonds in the ammonium persulfate molecules to break: S2O8 2- 2SO4 - Simultaneously, localized high temperatures further promote thermal decomposition: S2O8 2- 2SO4 - ·
[0028] Sulfate radicals oxidize ethylene glycol to produce ethylene glycol radicals and hydrogen sulfate ions: HOCH2CH2OH + SO42- - ·→HOCH2CH2O - ·+HSO4 - Ethylene glycol has high free radical reactivity and can continue to react with ammonium persulfate, forming a free radical cycle and continuously generating oxidizing active substances (SO4). - ·、·OH).
[0029] The generated free radicals (SO4) - Under the uniform mixing conditions provided by ball milling, · and ·OH directly attack the defects and edge sites of carbon materials, forming carbon-oxygen free radicals, which in turn introduce oxygen-containing functional groups (such as -COOH, -OH, C=O).
[0030] Ball milling can be carried out at a relatively low overall temperature for the following reasons: the activation energy of the free radical oxidation pathway is low, eliminating the need for high-temperature thermal activation; the reaction preferentially occurs at local defects in carbon materials, where the reaction barrier is lower; and the involvement of ethylene glycol modulates the oxidation intensity, preventing damage to the carbon framework caused by excessive oxidation.
[0031] Oxidation introduces oxygen-containing functional groups on the surface and edges of the carbon layer, increasing interlayer spacing and reducing interlayer forces. The shearing force of ball milling simultaneously strips away the carbon layer, exposing the interior of the carbon material for continued reaction. This results in the formation of numerous oxygen-containing functional groups and structural defects on the surface of carbon impurities, transforming carbon impurities in waste lithium iron phosphate materials into easily removable forms.
[0032] This proposal uses ammonium persulfate and ethylene glycol to lower the oxidation temperature of carbon materials. Therefore, under the condition of 300℃~400℃, not only are binders and conductive agents effectively removed, but the carbon content of the material is also reduced, and the subsequent regeneration calcination temperature is reduced to 350℃~450℃, thereby reducing energy consumption and process costs.
[0033] Ethylene glycol and ammonium persulfate have a synergistic activating effect. Ethylene glycol not only acts as a dispersion medium, but its hydroxyl groups also participate in regulating the oxidation reaction pathway: under the mechanical force of ball milling or localized thermal energy, ammonium persulfate decomposes to produce sulfate free radicals (SO42-). - Ethylene glycol can generate ethylene glycol radicals through dehydrogenation, thus constructing a continuous free radical chain reaction. This mechanism transforms the originally violent direct oxidation of ammonium persulfate into indirect, mild, and controllable free radical oxidation, effectively avoiding excessive oxidation of the lithium iron phosphate matrix (Fe). 2+ It destroys carbon impurities while precisely achieving low-temperature removal of carbon impurities.
[0034] In some optional embodiments of this application, the mass ratio of ammonium persulfate to polyol ranges from 1:(1~3).
[0035] In the above scheme, the mass ratio of ammonium persulfate to polyol is in the range of 1:(1~3). This ratio ensures sufficient oxidation activity to effectively activate carbon impurities, while avoiding excessive ammonium persulfate leading to Fe. 2+ Oxidation or excessive polyols can lead to increased residual carbon. Furthermore, the mass ratio of ammonium persulfate to polyol should be 1:2, at which point the carbon removal rate and material structure achieve the optimal balance.
[0036] The activator is uniformly coated on the surface of the material during ball milling. The active oxygen released by the thermal decomposition of ammonium persulfate reduces the oxidation temperature of the carbon material.
[0037] In some optional embodiments of this application, the mass of the activator is 5% to 15% of the mass of the waste lithium iron phosphate material.
[0038] In the above scheme, the mass of the activator is positively correlated with the carbon impurity content in the waste lithium iron phosphate material; the higher the carbon content, the greater the required activator dosage. Setting the mass of the activator to 5%~15% of the mass of the waste lithium iron phosphate material, within this range, can achieve sufficient activation of the carbon layer and avoid excessive ammonium persulfate leading to sulfur residue.
[0039] In some optional embodiments of this application, mixing waste lithium iron phosphate material with an activator and then ball milling it includes: Waste lithium iron phosphate material is mixed with an activator and ball-milled at 300 rpm to 400 rpm for 2 to 4 hours.
[0040] With this setup, ball milling at 300 rpm to 400 rpm for 2 to 4 hours improves the surface activity and specific surface area of waste lithium iron phosphate materials, reduces the activation energy required for carbon oxidation, lowers the carbon oxidation temperature, and achieves low-temperature calcination treatment. This effectively avoids damage to the structure of lithium iron phosphate materials under high-temperature conditions and ensures the integrity of the lithium iron phosphate crystal structure.
[0041] In some optional embodiments of this application, the activated lithium iron phosphate material is calcined at a first temperature in an oxygen-containing atmosphere to obtain the calcined lithium iron phosphate material, which includes: The activated lithium iron phosphate material was calcined for 1 to 2 hours at an oxygen concentration of 6% to 10% and a first temperature of 300°C to 400°C, and then naturally cooled to room temperature to obtain the calcined lithium iron phosphate material.
[0042] This setup, with calcination occurring in an oxygen concentration of 6%–10%, provides sufficient oxidant to remove carbon impurities while preventing excessive oxidation that could lead to Fe degradation. 2+ To Fe 3+ The conversion effectively improved carbon removal efficiency.
[0043] In some optional embodiments of this application, the lithium supplement includes a lithium source and a carbon source; The calcined lithium iron phosphate material was mixed with a lithium supplementer to obtain a mixture. The amount of lithium source added was controlled so that the molar ratio of Fe to Li in the mixture was 1:(1~1.05), and the amount of carbon source added was 10%~30% of the mass of the calcined lithium iron phosphate material. The mixture is subjected to hydrothermal treatment under an inert atmosphere to obtain a precursor, including: subjecting the mixture to hydrothermal treatment at 200℃~300℃ for 1h~2h under an inert atmosphere, and then naturally cooling to room temperature after the hydrothermal treatment to obtain lithium iron phosphate material after lithium supplementation. The lithium iron phosphate material after lithium supplementation was vacuum dried at 50℃~100℃ for 6h~8h to obtain the precursor.
[0044] In this embodiment, the lithium source is selected from commonly used lithium sources such as lithium acetate, and the carbon source is selected from at least one of citric acid and glucose. The lithium source replenishes the lithium missing in the crystal lattice; the carbon sources such as citric acid and glucose create a reducing atmosphere and suppress Fe. 2+ Oxidation and modification of the conductive carbon layer on the particle surface.
[0045] In some optional embodiments of this application, the precursor is calcined at a second temperature under an inert atmosphere to obtain recycled lithium iron phosphate material, comprising: Under an inert atmosphere, the temperature is increased to 350℃~450℃ at a heating rate of 5℃ / min~10℃ / min, and the precursor is calcined for 2h~3h. After cooling to room temperature, recycled lithium iron phosphate material is obtained.
[0046] In some optional embodiments of this application, after obtaining the calcined lithium iron phosphate material and before mixing the calcined lithium iron phosphate material with the lithium replenishing agent, the method further includes: The calcined lithium iron phosphate material was washed with water and dried.
[0047] In this embodiment, the washing and drying process specifically includes: washing the calcined lithium iron phosphate material with deionized water 2 to 3 times, stirring for 10 to 30 minutes each time, filtering after washing and drying at 70 to 90 degrees Celsius for 3 to 5 hours to remove residual soluble sulfur-containing impurities on the material surface and improve the purity of the powder.
[0048] In another embodiment, a recycled lithium iron phosphate material is provided, which is prepared by the above-described method for recycling waste lithium iron phosphate material.
[0049] The present application is further illustrated below with reference to embodiments and comparative examples. Unless otherwise specified, the raw materials, reagents, materials and equipment used in this application are all commercially available products conventionally used in the art.
[0050]
Example 1
[0051] S2. Mix the waste lithium iron phosphate material with the activator and ball mill it at a speed of 350 rpm for 3 hours to obtain activated lithium iron phosphate material. The mass of the activator is 10% of the mass of the waste lithium iron phosphate material, and the mass ratio of ammonium persulfate to ethylene glycol in the activator is 1:2.
[0052] S3. The activated lithium iron phosphate material is calcined under conditions of 8% oxygen concentration and 350°C for 2 hours, and then naturally cooled to room temperature to obtain the calcined lithium iron phosphate material.
[0053] S4. The calcined lithium iron phosphate material is mixed with lithium acetate and glucose to obtain a mixture. The amount of lithium acetate added is controlled so that the molar ratio of Fe to Li in the mixture is 1:1.05. The amount of glucose added is 20% of the mass of the calcined lithium iron phosphate material. The mixture is subjected to hydrothermal treatment under a nitrogen atmosphere. The microwave-assisted hydrothermal temperature is controlled at 250°C for 1.5 hours. After natural cooling to room temperature, the lithium-added lithium iron phosphate material is obtained. The lithium-added lithium iron phosphate material is vacuum dried at 60°C for 6 hours to obtain the precursor.
[0054] S5. Place the precursor into a crucible and heat it to a second temperature of 400°C at a heating rate of 6°C / min under a nitrogen atmosphere. Hold the temperature for 2 hours and cool to room temperature to obtain the recycled lithium iron phosphate material.
[0055]
Example 2
[0056]
Example 3
[0057]
Example 4
[0058]
Example 5
[0059]
Example 6
[0060]
Example 7
[0061]
Example 8
[0062]
Example 9
[0063] Comparative Example 1 The difference between this comparative example and Example 1 is that no activator is used in S2, while the other steps are the same. The specific steps of S2 are as follows: S2. The waste lithium iron phosphate material is ball-milled at a speed of 350 rpm for 3 hours to obtain activated lithium iron phosphate material.
[0064] Comparative Example 2 The difference between this comparative example and Example 1 is that no activator is used in S2, the first temperature is different in S3, and the second temperature is different in S5; the remaining steps are the same. The specific steps of S2, S3, and S5 are as follows: S2. The waste lithium iron phosphate material is ball-milled at a speed of 350 rpm for 3 hours to obtain activated lithium iron phosphate material.
[0065] S3. The activated lithium iron phosphate material is calcined under conditions of 8% oxygen concentration and 600℃ for 2 hours and then naturally cooled to room temperature to obtain the calcined lithium iron phosphate material.
[0066] S5. Place the precursor into a crucible and heat it to a second temperature of 800°C at a heating rate of 6°C / min under a nitrogen atmosphere. Hold the temperature for 2 hours and cool to room temperature to obtain the recycled lithium iron phosphate material.
[0067] Comparative Example 3 The difference between this comparative example and Example 1 is that the type of activator is different in S2, while the other steps are the same. The specific steps of S2 are as follows: S2. Mix the waste lithium iron phosphate material with the activator ammonium persulfate, and ball mill it at a speed of 350 rpm for 3 hours to obtain activated lithium iron phosphate material; wherein the mass of the activator ammonium persulfate is 10% of the mass of the waste lithium iron phosphate material.
[0068] Comparative Example 4 The difference between this comparative example and Example 1 is that the type of activator is different in S2, while the other steps are the same. The specific steps of S2 are as follows: S2. Mix the waste lithium iron phosphate material with the activator ethylene glycol, and ball mill it at a speed of 350 rpm for 3 hours to obtain activated lithium iron phosphate material; wherein, the mass of the activator ethylene glycol is 10% of the mass of the waste lithium iron phosphate material.
[0069] [Performance Testing] Table 1 summarizes some of the conditional parameters of each embodiment and comparative example.
[0070] Table 1 Summary of Condition Parameters for Each Embodiment and Comparative Example
[0071] The performance of the recycled lithium iron phosphate materials obtained in each embodiment and comparative example was tested, and the test results are shown in Table 2. The test methods are as follows: Test method for residual carbon content: A high-frequency infrared carbon-sulfur analyzer (according to GB / T 3524-2018) is used. 0.15g of sample is weighed and burned in a high-frequency induction furnace with oxygen to completely convert the carbon elements in the sample into carbon dioxide. The CO2 content is then measured and converted into residual carbon rate.
[0072] Fe 3+ The method for determining the content of iron and ferrous iron was as follows: The o-phenanthroline spectrophotometric method was used. 0.2 g of sample was leached with hydrochloric acid, and after adjusting the volume, the total iron and ferrous iron content were measured separately. The Fe content was calculated by difference. 3+ Percentage of total iron by mass.
[0073] The method for testing the discharge specific capacity is as follows: CR2032 coin cells (lithium foil counter electrode, 1M LiPF6EC / DMC=1:1 electrolyte) are made from recycled lithium iron phosphate material. The cells are charged and discharged at a constant current rate of 0.1C at 25℃, with a voltage range of 2.5V to 3.65V. The first discharge specific capacity is recorded.
[0074] Table 2
[0075] As shown in Table 2, the initial discharge specific capacity of Examples 1 to 9 is 144 mAh / g to 154 mAh / g, while the initial discharge specific capacity of Comparative Examples 1 to 4 is 125 mAh / g to 136 mAh / g. The initial discharge specific capacity of each example is higher than that of the comparative examples.
[0076] Regarding the residual carbon content, the residual carbon content of Examples 1 to 9 ranged from 0.24% to 0.79%, which was lower than that of Comparative Examples 1, 3, and 4. As for Comparative Example 2, the first temperature was 600°C and the second temperature was 800°C. Although this reduced the residual carbon content of the recycled lithium iron phosphate material to some extent, the Fe content in Comparative Example 2 was significantly lower. 3+ The content is as high as 16.5%, which leads to a decrease in the specific capacity of the first discharge.
[0077] In Fe 3+ Regarding the content, Fe in Examples 1 to 9 3+ The content is 3.0%~5.1%, which is lower than that of comparative examples 1 to 3.
[0078] Comparative Example 3 used only ammonium persulfate. Compared to Example 1, Comparative Example 3 showed excessive oxidation, leading to Fe... 2+The high degree of oxidation and high residual carbon content lead to a decrease in the first discharge specific capacity of the regenerated lithium iron phosphate material.
[0079] Comparative Example 4 used only ethylene glycol. Compared to Example 1, Comparative Example 4 had insufficient carbon removal, higher residual carbon, and higher Fe content. 2+ The high degree of oxidation leads to a decrease in the initial discharge specific capacity of the regenerated lithium iron phosphate material.
[0080] It should be noted that, in this document, "comprising," "including," or any other variation thereof is intended to cover non-exclusive inclusion, such that a process, method, or article that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, or article.
[0081] The various embodiments in this specification are described in a related manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.
[0082] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the principles of this application should be included within the scope of protection of this application.
Claims
1. A method for regenerating waste lithium iron phosphate materials, characterized in that, Includes the following steps: Obtain waste lithium iron phosphate materials; The waste lithium iron phosphate material is mixed with an activator and ball-milled to obtain activated lithium iron phosphate material; wherein the activator includes ammonium persulfate and polyol; The activated lithium iron phosphate material is calcined at a first temperature in an oxygen-rich atmosphere to obtain calcined lithium iron phosphate material. The calcined lithium iron phosphate material is mixed with a lithium replenishing agent to obtain a mixture, and the mixture is subjected to hydrothermal treatment under an inert atmosphere to obtain a precursor. The precursor is calcined at a second temperature under an inert atmosphere to obtain recycled lithium iron phosphate material; wherein the second temperature is 350℃~450℃.
2. The method for regenerating waste lithium iron phosphate materials as described in claim 1, characterized in that, The polyol is selected from at least one of ethylene glycol, 1,2-propanediol, 1,3-propanediol and glycerol; Preferably, the polyol is selected from ethylene glycol.
3. The method for regenerating waste lithium iron phosphate materials as described in claim 1 or 2, characterized in that, The mass ratio of ammonium persulfate to the polyol is in the range of 1:(1~3).
4. The method for regenerating waste lithium iron phosphate materials as described in claim 3, characterized in that, The mass of the activator is 5% to 15% of the mass of the waste lithium iron phosphate material.
5. The method for regenerating waste lithium iron phosphate materials as described in claim 1, characterized in that, The step of mixing the waste lithium iron phosphate material with an activator and then ball milling it includes: The waste lithium iron phosphate material is mixed with the activator and ball-milled at a speed of 300 rpm to 400 rpm for 2 to 4 hours.
6. The method for regenerating waste lithium iron phosphate materials as described in claim 1, characterized in that, The activated lithium iron phosphate material is calcined in an oxygen-rich atmosphere at a first temperature to obtain calcined lithium iron phosphate material comprising: The activated lithium iron phosphate material is calcined for 1-2 hours at an oxygen concentration of 6%-10% and a first temperature of 300-400℃, and then naturally cooled to room temperature to obtain the calcined lithium iron phosphate material.
7. The method for regenerating waste lithium iron phosphate materials as described in claim 1, characterized in that, The lithium supplement agent includes a lithium source and a carbon source; The calcined lithium iron phosphate material is mixed with a lithium supplementer to obtain a mixture in which the amount of lithium source added is controlled such that the molar ratio of Fe to Li in the mixture is 1:(1~1.05), and the amount of carbon source added is 10%~30% of the mass of the calcined lithium iron phosphate material. The step of subjecting the mixture to hydrothermal treatment under an inert atmosphere to obtain the precursor includes: The mixture was subjected to hydrothermal treatment at 200℃~300℃ for 1h~2h under an inert atmosphere, and then naturally cooled to room temperature after the hydrothermal treatment to obtain lithium iron phosphate material after lithium replenishment. The lithium iron phosphate material after lithium supplementation is vacuum dried at 50℃~100℃ for 6h~8h to obtain the precursor.
8. The method for regenerating waste lithium iron phosphate materials as described in claim 1, characterized in that, The precursor is calcined at a second temperature under an inert atmosphere to obtain recycled lithium iron phosphate material, comprising: Under an inert atmosphere, the temperature is increased to 350℃~450℃ at a heating rate of 5℃ / min~10℃ / min, and the precursor is calcined for 2h~3h and then cooled to room temperature to obtain the recycled lithium iron phosphate material.
9. The method for regenerating waste lithium iron phosphate materials as described in claim 1, characterized in that, After obtaining the calcined lithium iron phosphate material, and before mixing the calcined lithium iron phosphate material with the lithium replenishing agent, the method further includes: The calcined lithium iron phosphate material is washed with water and dried.
10. A recycled lithium iron phosphate material, characterized in that, It is prepared by the waste lithium iron phosphate material regeneration method according to any one of claims 1 to 9.