A bulk doping and interface modification synergistic modification of lithium manganese iron phosphate cathode material, its preparation method and application
By synergistic modification through Mg2+ bulk doping and zirconium-containing interface modification, the structural stability and interfacial side reaction problems of lithium manganese iron phosphate cathode materials were solved, realizing the preparation of high-performance lithium manganese iron phosphate cathode materials and improving the electrochemical performance of the materials.
Patent Information
- Application Number
- CN202611500687.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium manganese iron phosphate cathode materials suffer from insufficient intrinsic structural stability, severe side reactions at the particle/electrolyte interface, and a reduced proportion of active material due to reliance on higher carbon content to improve electron transport.
A synergistic strategy combining Mg2+ bulk doping with zirconium-containing nano-interface modification and carbon coating was adopted. The precursor of manganese iron magnesium oxalate was mixed with lithium phosphorus source, zirconium source and carbon source by ball milling and then subjected to a one-time two-stage solid-state heat treatment to form a lithium iron phosphate cathode material with Mg bulk doping, zirconium-containing interface modification and carbon coating.
The material's discharge capacity and cycle retention were significantly improved at lower carbon content, Li+ transport kinetics were improved, interfacial charge transfer resistance was reduced, the process flow was simplified, and the overall performance of the material was improved.
Smart Images

Figure CN123105590A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery cathode material technology, and more specifically relates to a lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification, its preparation method and application. Background Technology
[0002] Lithium iron phosphate (LiFePO4, LFP) has been widely commercialized in electric vehicles and large-scale energy storage due to its excellent safety, long cycle life, and low cost. However, its operating voltage is relatively low (approximately 3.4V vs. Li / Li). + Theoretically limited energy density makes it difficult to meet the demands of next-generation high-energy-density batteries. By replacing some of the Fe in LFP with Mn, olivine-type lithium manganese iron phosphate (LiMn) can be constructed. x Fe 1-x PO4, LMFP), can introduce Mn 2+ / Mn 3+ Redox pairs (operating voltage approximately 4.1V) can increase the operating voltage and theoretical specific energy of materials.
[0003] Despite the aforementioned advantages, the commercialization of LMFP still faces three core technological challenges: (1) The intrinsic electronic conductivity is extremely low, much lower than that of ternary materials. It is severely polarized at medium and high rates, resulting in insufficient capacity utilization.
[0004] (2) Jahn-Teller distortion and manganese dissolution. Mn generated during charging. 3+ (d) 4 High spin, t 2g 3 e g 1 This induces Jahn-Teller distortion, causing localized distortion of the MnO6 octahedron, leading to lattice stress accumulation and gradual structural degradation; simultaneously, Mn... 3+ via disproportionation reaction (2Mn) 3+ →Mn 2+ +Mn 4+ Mn generated 2+ It is easily dissolved and migrated to the negative electrode, damaging the SEI film and causing loss of active material and active lithium, thus leading to rapid capacity decay.
[0005] (3) Severe side reactions occur at the particle surface and electrolyte interface, resulting in insufficient interfacial stability. In the olivine structure, Li... + The main migration occurs along the
[010] direction, and the diffusion channels are inherently narrow. At the same time, the particle surface is prone to side reactions with the electrolyte during charge-discharge cycles, resulting in a continuous increase in interfacial impedance. Both of these factors together limit the performance of the material's rate capability and cycle stability.
[0006] To address the above problems, existing research mainly focuses on modification through the following approaches: (1) Carbon coating: The formation of a conductive carbon layer on the particle surface by pyrolysis of organic carbon source can effectively improve electronic conductivity and is currently the most mature commercial modification method. Carbon coating can improve electronic conductivity and may affect the contact state between the material surface and the electrolyte, but it is still difficult to meet the requirements of both the main structure and interface stability by relying solely on carbon coating. Some existing processes use a higher amount of carbon source to improve electronic conductivity, but an excessively high proportion of inactive carbon will reduce the proportion of active main body per unit mass and may affect the compaction and processing performance of the material. Therefore, if the conductivity and structural stability can be improved from the intrinsic level of the material through bulk doping and interface modification, it is expected to achieve a balance of comprehensive performance at a lower carbon content.
[0007] (2) Single-site bulk doping: using Mg 2+ 、Nb 5+ Ti 4+ V 3+ Substituting lattice sites with isovalent or equivalent ions can improve material properties at the intrinsic structural level. Among these, Mg... 2+ Mg can be used as a host crystalline phase doping element to regulate the local lattice environment, which is beneficial to improving the structural stability of materials during cycling. The degree of improvement in material performance by single Mg doping is related to composition, structure, and interface state, and still needs to be combined with interface regulation.
[0008] (3) Surface oxide modification: Coating the surface of cathode particles with inert nano-coatings such as Al2O3, TiO2, and ZrO2 can form a physical isolation layer between the particles and the electrolyte, thereby suppressing side reactions and improving interface stability and reducing interface impedance. However, this type of surface modification mainly acts on the outer interface structure of the particles and has a limited impact on the stability of the intrinsic crystal structure of the material. It may not be able to simultaneously and fully improve the stability of the main structure and the interface. Moreover, most existing surface modification schemes are independent processes, lacking synergistic design with bulk doping and carbon coating, and the process flow is relatively cumbersome.
[0009] Therefore, how to solve the problems of insufficient intrinsic structural stability of existing lithium manganese iron phosphate cathode materials, serious side reactions at the particle / electrolyte interface, and the reduced proportion of active materials caused by relying on higher carbon content to improve electron transport has become an urgent problem to be solved in this field. Summary of the Invention
[0010] The purpose of this invention is to provide a bulk doping and interface modification synergistic modification of lithium manganese iron phosphate cathode material, its preparation method, and its application. Specifically, it uses Mg... 2+ High-performance lithium manganese iron phosphate (LiMn) prepared by a synergistic strategy of bulk doping combined with zirconium-containing nano-interface modification and carbon coating x Fe1-x PO4 (LMFP) cathode materials are proposed to address the problems existing in the aforementioned technologies.
[0011] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of this invention is to provide a method for preparing a lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification, comprising the following steps: The manganese iron magnesium oxalate precursor, lithium phosphorus source, zirconium source and carbon source were ball-milled and mixed, and then dried to obtain a mixed precursor powder. The mixed precursor powder was subjected to a one-time two-stage solid-state heat treatment under an inert atmosphere. After cooling, the bulk doping and interface modification synergistically modified lithium manganese iron phosphate cathode material was obtained.
[0012] Furthermore, the preparation steps of the manganese iron magnesium oxalate precursor include: Using manganese salt, ferrous salt, and magnesium salt as reactants, and ascorbic acid as a reducing agent, a co-precipitation reaction was carried out with sodium oxalate under an inert atmosphere. After the reaction was completed, the mixture was aged to obtain the manganese iron magnesium oxalate precursor.
[0013] In the magnesium manganese oxalate precursor prepared by this invention, Mg is introduced into the magnesium manganese oxalate precursor through co-precipitation.
[0014] Optionally, the manganese salt includes manganese sulfate and / or manganese chloride.
[0015] Optionally, the ferrous salt includes ferrous sulfate and / or ferrous chloride.
[0016] Optionally, the magnesium salt includes magnesium sulfate and / or magnesium chloride.
[0017] Optionally, the molar ratio of Mn, Fe and Mg in the reactants is x(1-y):(1-x)(1-y):y, where 0.5≤x≤0.6 and 0.005≤y≤0.020.
[0018] Preferably, Mg accounts for 0.8 mol% to 1.2 mol% of the total molar amount of Mn, Fe and Mg in the reactants.
[0019] Optionally, the amount of the reducing agent is 1 mol% to 5 mol% of the total metal ions in the reactants.
[0020] Optionally, the sodium oxalate is introduced in solution form at a concentration of 0.1~1.0 mol / L (preferably 0.5 mol / L).
[0021] Optionally, the molar ratio of the oxalate molar amount in the sodium oxalate to the total molar amount of metal ions in the manganese, ferrous, and magnesium salts is 1:1.
[0022] Optionally, the reaction temperature in the coprecipitation reaction is 25~50℃, the stirring speed before the addition of sodium oxalate is 30~80 rpm, and the stirring speed after the addition of sodium oxalate is 20~60 rpm.
[0023] Optionally, the aging time is 2 to 6 hours.
[0024] Furthermore, the lithium phosphorus source includes LiH2PO4, or a combination of Li2CO3 and NH4H2PO4, or a combination of LiOH and NH4H2PO4.
[0025] Furthermore, the zirconium source includes at least one of ZrOCl2·8H2O, ZrO(NO3)2·nH2O, and Zr(CH3COO)4.
[0026] Furthermore, the carbon source includes at least one of glucose, sucrose, and citric acid.
[0027] Furthermore, the total molar amount of Mn, Fe and Mg in the manganese iron magnesium oxalate precursor is denoted as M, the molar amount of Li in the lithium source is (1.03~1.06):1 (preferably (1.04~1.05):1); the molar amount of Zr in the zirconium source is 0.1mol%~1.0mol% of M (preferably 0.25mol%~0.50mol%).
[0028] Furthermore, the amount of carbon source added is controlled with the carbon content of the lithium manganese iron phosphate cathode material being 1.5 wt.% to 2.5 wt.% (preferably 1.8 wt.% to 2.2 wt.%).
[0029] Furthermore, the ball milling mixing is a wet ball milling with the following parameters: ball milling speed 400~600 rpm (preferably 500~600 rpm), ball milling time 4~8 h (preferably 6~8 h), ball-to-material mass ratio of (8~12):1, and ethanol as the dispersion medium.
[0030] Furthermore, the drying temperature is 70~90℃.
[0031] Furthermore, the inert atmosphere is argon or nitrogen, and the gas flow rate is 80~120 mL / min.
[0032] Furthermore, the program parameters for the one-time two-stage solid-state heat treatment are as follows: in the first stage, the temperature is increased to 380~430℃ (preferably 390~420℃) at a rate of 3~5℃ / min (preferably 4℃ / min) and held for 3~5h (preferably 3~4h); in the second stage, the temperature is increased to 700~800℃ (preferably 720~780℃) at a rate of 3~5℃ / min (preferably 4℃ / min) and held for 8~12h (preferably 8~10h).
[0033] The second technical solution of the present invention provides a lithium manganese iron phosphate cathode material with synergistic modification by bulk doping and interface modification, wherein the lithium manganese iron phosphate cathode material with synergistic modification by bulk doping and interface modification is prepared by the above preparation method.
[0034] The lithium manganese iron phosphate cathode material provided by the present invention is a lithium manganese iron phosphate cathode material having Mg bulk doping, zirconium-containing modified regions and carbon coating layers.
[0035] The third technical solution of the present invention provides an application of the above-mentioned bulk doping and interface modification synergistic modified lithium manganese iron phosphate cathode material in lithium-ion power batteries or energy storage batteries.
[0036] The fourth technical solution of the present invention provides an electrode, wherein the active component of the electrode includes the above-mentioned bulk doping and interface modification synergistically modified lithium manganese iron phosphate cathode material.
[0037] Fifth technical solution of the present invention: A lithium-ion battery is provided, wherein the lithium-ion battery uses the above-mentioned electrode as the positive electrode.
[0038] The sixth technical solution of the present invention: provides an energy storage device, wherein the energy storage device uses the above-mentioned electrode as the positive electrode.
[0039] The present invention discloses the following technical effects: This invention introduces Mg, Mn, and Fe into the precursor simultaneously during the oxalate co-precipitation stage, allowing Mg to enter the olivine-type main crystal phase and form bulk doping during subsequent high-temperature reactions. This facilitates the control of the local lattice environment and improves structural stability during cycling. Simultaneously, a zirconium source is introduced during the wet mixing stage, and a zirconium-containing modified region is formed on the surface or interface of the main particles through a single-charge, two-stage heat treatment, effectively reducing interfacial charge transfer resistance and improving the cycling stability of the material. Mg bulk doping and zirconium-containing interfacial modification achieve functional division and synergy at different spatial scales, resulting in a significant reduction in the Warburg coefficient of the jointly modified sample and Li... + Transport kinetics were significantly improved. Even with low carbon content, Mg / Zr synergistic modification achieved excellent discharge capacity and cycle retention. Further increasing the carbon source dosage did not produce additional performance gains, indicating a good synergistic fit between bulk doping, interface modification, and carbon coating. Furthermore, both Mg and Zr sources are inexpensive and readily available commercial salts. Bulk doping, interface modification, and carbon coating were synergistically completed in a single-stage, continuous two-stage solid-state heat treatment process, eliminating the need for additional surface coating steps. This simplified process has the potential for further scale-up preparation. Attached Figure Description
[0040] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a schematic diagram of the process flow for preparing lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification according to the present invention.
[0041] Figure 2 The XRD patterns of the cathode materials prepared in Example 2, Comparative Example 1, and Comparative Example 2 are shown.
[0042] Figure 3 The images show the TEM and mapping diagrams of the bulk doping and interface modification synergistic modified lithium manganese iron phosphate cathode material prepared in Example 2, where (a) and (b) are TEM images, and (c) to (i) are mapping diagrams.
[0043] Figure 4 This is a comparison graph of the electrochemical performance of the cathode materials of Comparative Example 1, Comparative Example 2, Comparative Example 5, and Example 2. The graph includes charge-discharge curves and cycle performance curves after 200 cycles at 28°C and 1C.
[0044] Figure 5 The electrochemical EIS spectra (left) and equivalent circuit fitting results (right) of the cathode materials of Comparative Example 1, Comparative Example 2 and Example 2 are shown.
[0045] Figure 6 The above are XPS spectra of the cathode material prepared in Example 2, where (a) is the full XPS spectrum and (b) is the high-resolution spectrum of Zr 3d. Detailed Implementation
[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0047] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0048] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0049] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0050] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0051] Unless otherwise specified, all raw materials and reagents involved in the specific embodiments of this invention are commercially available products.
[0052] Unless otherwise specified, room temperature and normal temperature in the specific embodiments of this invention refer to 20-30℃.
[0053] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0054] In some specific embodiments, the present invention provides a method for preparing carbon-coated lithium manganese iron phosphate cathode material by synergistic modification of Mg bulk doping and zirconium-containing interface, the steps of which include: Preparation of S1, the precursor of coprecipitated manganese iron magnesium oxalate: Manganese, ferrous, and magnesium salts were dissolved in deionized water in a molar ratio of Mn:Fe:Mg = x(1-y):(1-x)(1-y):y, where 0.5 ≤ x ≤ 0.6 and 0.005 ≤ y ≤ 0.020. Ascorbic acid, accounting for 1%–5% of the total molar amount of Mn, Fe, and Mg metal ions, was added as a reducing agent. Under an inert atmosphere, a coprecipitation reaction was carried out with sodium oxalate solution (concentration 0.1–1.0 mol / L, molar amount of oxalate to total metal ions 1:1). After the reaction, the mixture was aged for 2–6 hours. After solid-liquid separation, washing with water, and drying, a Mg-coprecipitated manganese-iron-magnesium oxalate precursor was obtained (no zirconium source was added during the coprecipitation stage). S2. Raw material mixing and wet ball milling: The manganese iron magnesium oxalate precursor obtained in step S1 is mixed with a lithium phosphorus source (LiH2PO4), a zirconium source (ZrOCl2·8H2O), and a carbon source (glucose). The total molar amount of Mn, Fe, and Mg is denoted as M, and the molar ratio of LiH2PO4 to M is (1.03~1.06):1. The amount of Zr added is 0.1%~1.0% of the total molar amount of M. The carbon source forms a carbon coating layer during the subsequent heat treatment process, and the amount added is controlled to achieve a carbon content of 1.5 wt.%~2.5 wt.% in the lithium manganese iron magnesium phosphate cathode material. Wet ball milling was performed using anhydrous ethanol as the dispersion medium at a speed of 400-600 rpm for 4-8 h, with a ball-to-material mass ratio of (8-12):1. The slurry after ball milling was dried at 70-90℃ to obtain mixed precursor powder. S3. One-time two-stage inert atmosphere solid-state heat treatment: The mixed precursor powder obtained in step S2 is placed in an inert atmosphere and heated to 380-430℃ at 3-5℃ / min and held for 3-5h to decompose oxalate and pre-carbonize carbon source. Then, without discharging, adding raw materials, or remixing, the temperature is increased to 700-800℃ at 3-5℃ / min and held for 8-12h to form olivine-type lithium manganese iron phosphate main crystal phase. At the same time, Mg introduced into the precursor by co-precipitation enters the main crystal phase to form bulk phase doping, and zirconium species form zirconium-containing modified regions on the surface or interface of the main particles. Glucose is pyrolyzed and carbonized to form a carbon coating layer. After heat treatment, the material is cooled in the furnace to obtain a lithium iron phosphate cathode material with a composite structure of Mg bulk doping, zirconium-containing interface modification, and carbon coating.
[0055] The lithium manganese iron phosphate cathode material prepared by the present invention includes a Mg-containing olivine-type lithium manganese iron phosphate host crystal phase, a Zr-containing modified region located on the surface or interface region of the host particles, and a carbon coating layer; wherein, Mg exists in the olivine-type host crystal phase, the Zr-containing modified region is at least partially located between the host particles and the carbon coating layer, and the local thickness of the carbon coating layer is 2~5 nm.
[0056] The Zr-modified region involved in this invention refers to a modified region containing zirconium located on the surface or interface of lithium manganese iron phosphate particles. The oxygen-zirconium stoichiometry is not predetermined, nor is it required to form a continuous film covering the entire particle surface. Its spatial location is determined by the correspondence between electron microscopy morphology and elemental distribution.
[0057] In the preparation method, firstly, a manganese-iron-magnesium oxalate coprecipitation precursor is prepared by oxalic acid coprecipitation. The manganese salt, ferrous salt and magnesium salt are dissolved in a predetermined molar ratio and coprecipitated with sodium oxalate under the protection of ascorbic acid and an inert atmosphere. This allows Mg to be introduced into the precursor along with Mn and Fe during the coprecipitation process.
[0058] Subsequently, the obtained co-precipitated precursor of manganese iron magnesium oxalate was mixed with lithium phosphorus source, zirconium source and carbon source in a certain proportion and ball-milled. Then, it was subjected to a two-stage heat treatment in an inert atmosphere. No material was discharged, no raw materials were added or remixed between the two heat treatment stages, and no additional surface coating treatment was performed. The first stage heat treatment decomposed oxalate and pre-carbonized glucose. The second stage heat treatment formed the main crystal phase of olivine-type lithium manganese iron phosphate and promoted the Mg introduced by co-precipitation to enter the main crystal phase to form bulk doping. At the same time, zirconium-containing modified regions were formed on the surface or interface of the main particles, and glucose was pyrolyzed and carbonized to form a carbon coating layer.
[0059] Unlike methods that directly add Mg source for high-temperature diffusion doping during the solid-phase batching stage, this invention first introduces Mg, Mn, and Fe simultaneously during the oxalate precursor co-precipitation stage, allowing Mg to be introduced during the precursor preparation stage and then enter the olivine-type lithium manganese iron phosphate main crystal phase to form bulk doping during the subsequent high-temperature solid-phase reaction, thereby improving the structural stability of the main crystal lattice.
[0060] Meanwhile, zirconium source and glucose carbon source are introduced in the subsequent wet ball milling mixing stage. Through a two-stage inert atmosphere heat treatment completed in one charge, zirconium-containing modified regions are formed on the surface or interface of the main particles, and a carbon coating layer is formed, thereby obtaining a composite modified material with Mg bulk doping, zirconium-containing modified regions and carbon coating layer.
[0061] Through the above steps, the Mg bulk doping mainly plays the role of lattice stabilization, the zirconium-containing interface modification region mainly plays the role of interface protection and interface impedance regulation, and the carbon coating layer mainly plays the role of electronic conductivity network construction. Functional division and synergy are achieved at different spatial scales, thereby taking into account the discharge capacity, rate performance and cycle stability of the material under the condition of low carbon content.
[0062] Example 1 The preparation steps of lithium manganese iron phosphate cathode material with synergistic modification of bulk doping and interface modification include: Preparation of S1, the precursor of coprecipitated manganese iron magnesium oxalate: According to the molar ratio of Mn:Fe:Mg = 49.5:49.5:1, MnSO4·H2O, FeSO4·7H2O, and MgSO4·7H2O were weighed and dissolved together in deionized water, wherein Mg accounted for 1.0 mol% of the total molar amount of Mn, Fe, and Mg. Ascorbic acid, accounting for 3 mol% of the total molar amount of Mn, Fe, and Mg metal ions, was added as a reducing agent, and a mixed metal salt solution with a total metal ion concentration of 1.0 mol / L was prepared under nitrogen protection.
[0063] Subsequently, a 0.5 mol / L Na₂C₂O₄ aqueous solution was added to the above mixed metal salt solution at a rate of 25 mL / min, so that Mn 2+ Fe 2+ and Mg 2+ A coprecipitation reaction was carried out simultaneously with oxalate (the molar ratio of oxalate in sodium oxalate to the total molar amount of metal ions in the manganese, ferrous, and magnesium salts was 1:1). The reaction temperature was 25℃, the stirring speed was 50 r / min, and stirring continued for 30 min after the addition was completed, followed by aging for 4 h. The resulting precipitate was filtered, washed three times with deionized water, and vacuum dried at 80℃ for 12 h to obtain the Mg-coprecipitated manganese-iron-magnesium oxalate precursor (theoretical equivalent molar mass is approximately 179.13 g / mol).
[0064] S2. Raw material mixing and wet ball milling: 1.498 g of the magnesium manganese iron oxalate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4), 0.0067 g of zirconium source (ZrOCl2·8H2O) and 0.17 g of carbon source (glucose). The mixture was wet-milled using stainless steel grinding balls with anhydrous ethanol as the dispersion medium at a speed of 500 rpm for 6 h. The ball-to-material mass ratio was 10:1. The slurry after ball milling was dried at 80℃ for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder. In this step, based on the theoretical composition of the precursor, the total molar amount of Mn, Fe, and Mg is approximately 8.36 mmol, the molar ratio of LiH2PO4 to M is approximately 1.05:1, and the molar amount of added Zr is approximately 0.25% of M. The amount of glucose added is 0.17 g, and the design target for the final residual carbon content is 2 wt.%, with the actual residual carbon content determined by measurement.
[0065] S3. One-time two-stage inert atmosphere solid-state heat treatment: The mixed precursor powder obtained in step S2 was placed in an inert atmosphere (argon, flow rate 100 mL / min), heated to 400℃ at 4℃ / min and held for 4 h; then heated to 750℃ at 4℃ / min and held for 10 h.
[0066] After heat treatment, the material was cooled in the furnace to obtain a lithium iron phosphate cathode material with synergistic modification of bulk doping and interface modification (1.0 mol% Mg + 0.25 mol% Zr synergistic modification), denoted as S2.
[0067] Example 2 The preparation steps of lithium manganese iron phosphate cathode material with synergistic modification of bulk doping and interface modification include: S1, Same as Example 1.
[0068] S2. Raw material mixing and wet ball milling: 1.498 g of the magnesium manganese iron oxalate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4), 0.0135 g of zirconium source (ZrOCl2·8H2O) and 0.17 g of carbon source (glucose). The mixture was wet-milled using stainless steel grinding balls with anhydrous ethanol as the dispersion medium at a speed of 500 rpm for 6 h. The ball-to-material mass ratio was 10:1. The slurry after ball milling was dried at 80℃ for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder. In this step, based on the theoretical composition of the precursor, the total molar amount of Mn, Fe, and Mg is approximately 8.36 mmol, the molar ratio of LiH2PO4 to M is approximately 1.05:1, and the molar amount of added Zr is approximately 0.50% of M. The amount of glucose added is 0.17 g, and the designed target for the final residual carbon content is 2 wt.%, with the actual residual carbon content determined by measurement. S3. One-time two-stage inert atmosphere solid-state heat treatment: The mixed precursor powder obtained in step S2 was placed in an inert atmosphere (argon, flow rate 100 mL / min), heated to 400℃ at 4℃ / min and held for 4 h; then heated to 750℃ at 4℃ / min and held for 10 h.
[0069] After heat treatment, the material was cooled in the furnace to obtain a lithium iron phosphate cathode material with synergistic modification of bulk doping and interface modification (1.0 mol% Mg + 0.50 mol% Zr synergistic modification), denoted as S3.
[0070] Example 3 The proposed method for preparing lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification is as follows: Preparation of S1, the precursor of coprecipitated manganese iron magnesium oxalate: According to the molar ratio of Mn∶Fe∶Mg=49.75∶49.75∶0.50, MnSO4·H2O, FeSO4·7H2O, and MgSO4·7H2O were weighed and dissolved together in deionized water, wherein Mg accounted for 0.50% of the total molar amount of Mn, Fe, and Mg. The remaining co-precipitation, aging, washing, and drying conditions were the same as in Example 1. Based on the above feed ratio and the theoretical composition of oxalate dihydrate, the theoretical equivalent molar mass of the precursor was approximately 179.28 g / mol.
[0071] S2. Raw material mixing and wet ball milling: 1.499 g of the magnesium manganese iron oxalate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4), 0.0135 g of zirconium source (ZrOCl2·8H2O) and 0.17 g of carbon source (glucose). The mixture was wet-milled with stainless steel grinding balls using anhydrous ethanol as the dispersion medium at a speed of 500 rpm for 6 h, with a ball-to-material mass ratio of 10:1. The slurry after ball milling was dried at 80 ℃ for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder.
[0072] In this step, the total molar amount of Mn, Fe and Mg is denoted as M, the molar ratio of LiH2PO4 to M is approximately 1.05:1, and the amount of Zr added is approximately 0.50% of M.
[0073] S3. One-time two-stage inert atmosphere solid-state heat treatment: Similar to Example 2, no material is discharged, no raw materials are added, and no remixing occurs between the two heat treatment stages. The material is cooled with the furnace after the heat treatment is completed.
[0074] The prepared lithium manganese iron phosphate cathode material sample is designated as S4, in which the feed ratios of Mg and added Zr are 0.50% and 0.50% of the total molar amounts of Mn, Fe and Mg, respectively.
[0075] Example 4 The proposed method for preparing lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification is as follows: Preparation of S1, the precursor of coprecipitated manganese iron magnesium oxalate: According to the molar ratio of Mn:Fe:Mg = 58.80:39.20:2.00, MnSO4·H2O, FeSO4·7H2O, and MgSO4·7H2O were weighed and dissolved together in deionized water, wherein Mg accounted for 2.00% of the total molar amount of Mn, Fe, and Mg. The remaining co-precipitation, aging, washing, and drying conditions were the same as in Example 1. Based on the above feed ratio and the theoretical composition of oxalate dihydrate, the theoretical equivalent molar mass of the precursor was approximately 178.73 g / mol.
[0076] S2. Raw material mixing and wet ball milling: 1.494 g of the manganese iron magnesium oxalate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4), 0.0135 g of zirconium source (ZrOCl2·8H2O) and 0.17 g of carbon source (glucose). The mixture was wet-milled with stainless steel grinding balls using anhydrous ethanol as the dispersion medium at a speed of 500 rpm for 6 h, with a ball-to-material mass ratio of 10:1. The slurry after ball milling was dried at 80 ℃ for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder.
[0077] In this step, the total molar amount of Mn, Fe and Mg is denoted as M, the molar ratio of LiH2PO4 to M is approximately 1.05:1, and the amount of Zr added is approximately 0.50% of M.
[0078] S3. One-time two-stage inert atmosphere solid-state heat treatment: Similar to Example 2, no material is discharged, no raw materials are added, and no remixing occurs between the two heat treatment stages. The material is cooled with the furnace after the heat treatment is completed.
[0079] The prepared lithium manganese iron phosphate cathode material sample is designated as S5, in which the feed ratios of Mg and added Zr are 2.00% and 0.50% of the total molar amounts of Mn, Fe and Mg, respectively.
[0080] Comparative Example 1 The preparation steps of lithium manganese iron phosphate cathode material include: S1. Preparation of undoped manganese oxalate-iron coprecipitate precursor: According to the molar ratio of Mn: Fe = 50:50, MnSO4·H2O and FeSO4·7H2O were weighed and dissolved in deionized water. Ascorbic acid, accounting for 3 mol% of the total molar amount of Mn and Fe metal ions, was added as a reducing agent, and a mixed metal salt solution with a total metal ion concentration of 1.0 mol / L was prepared under nitrogen protection.
[0081] Prepare a separate 0.5 mol / L Na₂C₂O₄ aqueous solution and add it according to a 1:1 molar ratio of oxalate to Mn and Fe. Under nitrogen protection, add the Na₂C₂O₄ solution to the above mixed metal salt solution at a rate of 25 mL / min, so that Mn... 2+ and Fe 2+ A coprecipitation reaction was carried out with oxalate. The reaction temperature was controlled at 25℃, the stirring speed was 50 r / min, and stirring was continued for 30 min after the addition was completed, followed by aging for 4 h. The resulting precipitate was separated by vacuum filtration, washed three times with deionized water, and then dried under vacuum at 80℃ for 12 h to obtain the undoped manganese iron oxalate coprecipitate precursor (theoretical equivalent molar mass is approximately 179.44 g / mol).
[0082] S2. Raw material mixing and wet ball milling: 1.500 g of the undoped manganese iron oxalate coprecipitate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4) and 0.17 g of carbon source (glucose). Anhydrous ethanol was used as the dispersion medium, and the mixture was wet-milled using stainless steel grinding balls at a speed of 500 rpm for 6 h with a ball-to-material mass ratio of 10:1. The slurry after ball milling was dried at 80℃ for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder.
[0083] S3. One-time two-stage inert atmosphere solid-state heat treatment: The mixed precursor powder obtained in step S2 was placed in an inert atmosphere (argon, flow rate 100 mL / min), heated to 400℃ at 4℃ / min and held for 4 h; then heated to 750℃ at 4℃ / min and held for 10 h.
[0084] After heat treatment, the material is cooled in the furnace to obtain lithium manganese iron phosphate cathode material, denoted as S0.
[0085] This comparative example was used to prepare LMFP / C materials without Mg bulk doping and zirconium-containing interface modification, serving as a performance comparison benchmark.
[0086] Comparative Example 2 The preparation steps of lithium manganese iron phosphate cathode material include: S1, Same as Example 1.
[0087] S2. Raw material mixing and wet ball milling: 1.498 g of the magnesium manganese iron oxalate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4) and 0.17 g of carbon source (glucose). The mixture was wet-milled using stainless steel grinding balls with anhydrous ethanol as the dispersion medium at a speed of 500 rpm for 6 h at a ball milling ratio of 10:1. The slurry after ball milling was dried at 80 °C for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder. S3. One-time two-stage inert atmosphere solid-state heat treatment: The mixed precursor powder obtained in step S2 was placed in an inert atmosphere (argon, flow rate 100 mL / min), heated to 400℃ at 4℃ / min and held for 4 h; then heated to 750℃ at 4℃ / min and held for 10 h.
[0088] After heat treatment, the material is cooled in the furnace to obtain lithium manganese iron phosphate cathode material, denoted as S1.
[0089] This comparative example is used to examine the individual effect of Mg bulk doping formed after the introduction of Mg in the oxalic acid coprecipitation stage on the performance of LMFP materials. No zirconium source is added in the mixing stage.
[0090] Comparative Example 3 The difference from Example 2 is that the amount of ZrOCl2·8H2O added is 0.0405g, that is, the amount of Zr added is increased to 1.50 mol of the total molar amount of Mn, Fe and Mg.
[0091] This comparative example is used to examine the effect of excessive Zr addition on the overall performance of the material.
[0092] Comparative Example 4 The difference compared to Example 2 is that the amount of glucose added is 0.44 g.
[0093] In this comparative example, only the amount of glucose was increased to examine the effect of increasing the amount of carbon source on the material properties.
[0094] Comparative Example 5 The preparation steps of lithium manganese iron phosphate cathode material include: S1, same as Comparative Example 1.
[0095] S2. Raw material mixing and wet ball milling: 1.500 g of the undoped manganese iron oxalate coprecipitate precursor obtained in step S1 was mixed with 0.912 g of lithium phosphorus source (LiH2PO4), 0.0135 g of zirconium source (ZrOCl2·8H2O) and 0.17 g of carbon source (glucose). Anhydrous ethanol was used as the dispersion medium, and the mixture was wet-milled using stainless steel grinding balls at a speed of 500 rpm for 6 h with a ball-to-material mass ratio of 10:1. The slurry after ball milling was dried at 80℃ for 8 h, then ground and passed through a 500-mesh sieve to obtain the mixed precursor powder.
[0096] S3. One-time two-stage inert atmosphere solid-state heat treatment: The mixed precursor powder obtained in step S2 was placed in an inert atmosphere (argon, flow rate 100 mL / min), heated to 400℃ at 4℃ / min and held for 4 h; then heated to 750℃ at 4℃ / min and held for 10 h.
[0097] After heat treatment, the material is cooled in the furnace to obtain lithium manganese iron phosphate cathode material.
[0098] This comparative example is used to examine the individual effect of zirconium-containing interface modification on material properties without Mg bulk doping.
[0099] Test case Figure 1 This is a schematic diagram of the process flow for preparing lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification according to the present invention.
[0100] Figure 2The figures show the XRD patterns of the cathode materials prepared in Example 2, Comparative Example 1, and Comparative Example 2. As can be seen from the figures, the main diffraction peaks of the three samples can all be attributed to the olivine-type lithium manganese iron phosphate main crystal phase. The positions of the main diffraction peaks are generally consistent, indicating that after introducing Mg and performing zirconium-containing interface modification, the material still maintains the olivine-type main crystal structure and the main crystal phase type has not been changed.
[0101] Figure 3 The images show TEM and mapping images of the bulk doping and interface modification synergistically modified lithium manganese iron phosphate cathode material prepared in Example 2, where (a) and (b) are TEM images, and (c) to (i) are mapping images. As can be seen from the images, HRTEM observation shows that there is an interface region of about 1-3 nm on the local surface of the S3 particles, without clear lattice fringes, and a coating region of about 2-5 nm can be observed on its outer side; the elemental distribution results show that Zr is enriched on the particle surface or at the interface.
[0102] Electrochemical testing methods: The obtained cathode material, Super P, and PVDF were mixed at a mass ratio of 8:1:1, slurried with NMP, and coated onto aluminum foil. The resulting cathode sheet was dried, pressed, and cut to size, with a material loading of 2 mg·cm³. -2 .
[0103] A battery was assembled and tested using a lithium sheet as the counter electrode, a Celgard separator, and an electrolyte containing LiPF6.
[0104] Using the Blue Electric system, constant current charge-discharge tests were conducted at 28 °C within the range of 2.5–4.5 V, with 1C = 170 mA·g. -1 Charge-discharge curves were tested at 0.2C, followed by 200 cycles at 1C. Specific capacity was calculated based on the mass of the composite cathode material, excluding additional conductive agents, binders, and current collectors; capacity retention was the ratio of the discharge specific capacity at the 200th cycle to that at the first 1C cycle.
[0105] Figure 4 The figure shows a comparison of the electrochemical performance of the cathode materials in Comparative Examples 1, 2, 5, and 2. As can be seen from the figure, under conditions of 28 °C and 1C, the initial discharge specific capacity of Example 2, which is jointly modified with Mg and zirconium-containing interface modification, is 152.0 mAh·g. -1 The capacity retention rate after 200 cycles was 94.5%, which was higher than that of the unmodified Comparative Example 1 (80.7%), the Comparative Example 2 (87.3%) with only Mg introduced, and the Comparative Example 5 (85.9%) with only zirconium source added. This indicates that the combined modification has good capacity utilization and cycling stability under the measured conditions.
[0106] EIS testing methods: Using the Chenhua electrochemical workstation, under the same pretreatment, state of charge, and temperature conditions, the EIS of each sample was tested in potential-controlled mode. The AC perturbation amplitude was 10 mV, and the frequency range was 10 mV. 5 ~10 -2 Hz. Using ZView and Figure 5 The equivalent circuit shown is fitted with the charge transfer resistance Rct, and Z′ is fitted with ω in the commonly applicable low-frequency linear range. -1 / 2 The relationship (ω=2πf) is used to compare the diffusion-related impedances by slope.
[0107] Figure 5 The left image shows the electrochemical EIS spectra (left panel) and the equivalent circuit fitting results (right panel) of the cathode materials of Comparative Example 1, Comparative Example 2, and Example 2. As can be seen from the figures, the EIS fitting results indicate that the charge transfer resistance R of the samples in Comparative Example 1, Comparative Example 2, and Example 2 is... ct The Ω values are approximately 35.05 Ω, 30.91 Ω, and 15.85 Ω, respectively. Compared to Comparative Example 1 and Comparative Example 2, the R value of Example 2 is... ct The reductions of approximately 54.8% and 48.7% respectively indicate that the combined modification of Mg bulk doping and zirconium-containing interface is beneficial for reducing interfacial charge transfer resistance. Further analysis of Z′ and ω in the low-frequency region... -1 / 2 Linear fitting was performed, and the Z′ versus ω values of the samples from Comparative Example 1, Comparative Example 2, and Example 2 were compared. -1 / 2 The fitting slopes were approximately 59.83, 57.21, and 37.50, respectively. The Warburg coefficient of Example 2 was reduced by approximately 37.3% and 34.5% compared to Comparative Example 1 and Comparative Example 2, respectively. Under the same conditions of SOC, temperature, and fitting range, this can serve as supplementary evidence for its lower diffusion-related impedance.
[0108] Figure 6 The figures show the XPS spectra of the cathode material prepared in Example 2, where (a) is the full XPS spectrum and (b) is the high-resolution Zr 3d spectrum. As can be seen from the figures, the material obtained in Example 2 was characterized using X-ray photoelectron spectroscopy, and binding energy correction was performed using the C 1s peak as a reference. Figure 6 As shown in (a), the corresponding characteristic signals of Fe 2p, Mn 2p, O 1s, C 1s, Zr3d, P 2p, and Li 1s can be observed in the XPS full spectrum. Figure 6 As shown in (b), the high-resolution spectrum of Zr 3d exhibits spin-orbit splitting double peaks at approximately 182.3 eV and 184.7 eV, which are attributed to Zr 3d, respectively. 5 / 2 and Zr 3d 3 / 2 The peak spacing is approximately 2.4 eV, similar to Zr. 4+ The chemical states match. (Combination) Figure 3The Zr enrichment results shown above support the existence of zirconium-containing modified regions at the surface or interface of material particles, and the detected zirconium chemical state is consistent with that of Zr. 4+ Consistent.
[0109] The main electrochemical properties of the cathode materials prepared in the examples and comparative examples were tested and compared, and the results are shown in Table 1.
[0110] 0.2C capacity: at a rate of 0.2C, i.e., 34 mA·g -1 The specific current was used to discharge the charged test battery at a constant current to 2.5 V, and the discharge capacity was recorded. The discharge capacity was divided by the mass of the composite cathode material prepared in the cathode sheet to obtain the 0.2C discharge specific capacity, expressed in mAh·g. -1 .
[0111] Median voltage: Based on the 0.2C discharge curve described above, the voltage corresponding to when the cumulative discharge capacity reaches 50% of the total discharge capacity is read as the median discharge voltage, in V. When the 50% capacity position is located between two adjacent sampling points, linear interpolation is used to determine the corresponding voltage. Initial capacity at 1C: 170 mA·g at 1C rate -1 Cyclic testing was conducted at a specific current. The discharge capacity of the first cycle in the 1C cycle test was divided by the mass of the composite cathode material prepared in the cathode sheet to obtain the initial 1C discharge specific capacity, in mAh·g. -1 If there were separate activation or rate testing previously, their cycles will not be counted in this stage of the cycle count. 200-cycle retention rate: Within the above temperature and voltage range, a 200-cycle test is performed at a 1C rate. The ratio of the discharge specific capacity of the 200th cycle to the discharge specific capacity of the first cycle of the 1C cycle test is taken as the 200-cycle capacity retention rate, which is calculated by the following formula: Capacity retention rate = (Discharge specific capacity of the 200th cycle ÷ Initial discharge specific capacity of the 1C cycle) × 100%.
[0112] Table 1. Electrochemical performance of Examples 1, 2 and Comparative Examples 1-5 As can be seen from the data in Table 1: The test results for Comparative Example 1 are as follows: 0.2C discharge specific capacity 148.2 mAh·g -1 The median voltage is 3.92 V, and the initial discharge specific capacity at 1C is 125.9 mAh·g. -1 The discharge specific capacity after 200 cycles at 28℃ and 1C is 101.6 mAh·g. -1 The capacity retention rate was 80.7%.
[0113] The sample in Comparative Example 2 had a 0.2C discharge specific capacity of 155.4 mAh·g. -1 The median voltage is 3.94 V, and the initial discharge specific capacity at 1C is 144.1 mAh·g. -1 The discharge specific capacity after 200 cycles at 28℃ and 1C is 125.8 mAh·g. -1 The capacity retention rate was 87.3%. Compared with Comparative Example 1, Comparative Example 2 showed an increase of 18.2 mAh·g in 1C discharge capacity. -1 The capacity retention rate increased by 6.6 percentage points after 200 cycles, indicating that the introduction of Mg in the oxalic acid co-precipitation stage and subsequent sintering to form bulk doping is beneficial to improving the capacity utilization and cycling performance of the material.
[0114] This indicates that under the above test conditions, the introduction of Mg is beneficial to improving the capacity utilization and cycle stability of the material.
[0115] The sample in Example 1 had a 0.2C discharge specific capacity of 160.8 mAh·g. -1 The median voltage is 3.96V, and the 1C discharge specific capacity is 149.3mAh·g. -1 The capacity retention rate was 92.6% after 200 cycles at 28℃ and 1C. Compared with Comparative Example 2 modified with Mg alone, the capacity retention rate was further increased by 5.3 percentage points after the introduction of 0.25 mol% Zr, indicating that zirconium-containing interface modification has a significant effect on improving the cycling stability of the material.
[0116] The sample in Example 2 had a 0.2C discharge specific capacity of 163.1 mAh·g. -1 The median voltage is 3.97 V, and the initial discharge specific capacity at 1C is 152.0 mAh·g. -1 After 200 cycles at 28℃ and 1C, the discharge specific capacity still reaches 143.6 mAh·g. -1 The capacity retention rate was 94.5%.
[0117] The sample in Comparative Example 3 had a 0.2C discharge specific capacity of 154.6 mAh·g. -1 The median voltage is 3.94V, and the 1C discharge specific capacity is 140.2mAh·g. -1 The capacity retention rate was 89.1% after 200 cycles at 28℃ and 1C. Compared with Example 2, when the Zr addition amount was increased to 1.50 mol%, the discharge capacity and cycle stability of the material decreased, indicating that excessive Zr interface modification is not conducive to the overall performance of the material.
[0118] In Comparative Example 4, increasing the glucose feed amount from 0.17 g to 0.44 g did not further improve the discharge capacity and cycle retention rate of the material, indicating that further increasing the carbon source feed amount does not bring corresponding electrochemical performance gains.
[0119] The sample in Comparative Example 5 had a discharge specific capacity of 156.7 mAh·g at 0.2C. -1 The median voltage is 3.93 V, and the initial discharge specific capacity at 1C is 134.1 mAh·g. -1 The discharge specific capacity after 200 cycles at 28℃ and 1C is 115.2 mAh·g. -1 The capacity retention rate was 85.9%. Compared with Comparative Example 1, zirconium-containing interface modification alone can improve the discharge capacity and cycle stability of the material, but its cycle stability is lower than that of the sample in Example 2 with synergistic modification of Mg bulk doping and zirconium-containing interface modification.
[0120] Overall, the initial 1C capacity of Example 2 was 152.0 mAh·g. -1 After 200 cycles, the concentration is 143.6 mAh·g. -1 The retention rate was approximately 94.5%; it demonstrated good capacity utilization and cycle retention among the listed samples.
[0121] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0122] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification, characterized in that the steps include: include: Using manganese salt, ferrous salt and magnesium salt as reactants, and ascorbic acid as a reducing agent, a co-precipitation reaction was carried out with sodium oxalate under an inert atmosphere. After the reaction was completed, the mixture was aged to obtain the manganese iron magnesium oxalate precursor. The manganese iron magnesium oxalate precursor, lithium phosphorus source, zirconium source and carbon source were ball-milled and mixed, and then dried to obtain a mixed precursor powder. The mixed precursor powder was subjected to a one-time two-stage solid-state heat treatment under an inert atmosphere. After cooling, the bulk doping and interface modification synergistically modified lithium manganese iron phosphate cathode material was obtained.
2. The preparation method according to claim 1, characterized in that, The manganese salt includes manganese sulfate and / or manganese chloride; And / or, the ferrous salt comprises ferrous sulfate and / or ferrous chloride; And / or, the magnesium salt includes magnesium sulfate and / or magnesium chloride; And / or, the molar ratio of Mn, Fe and Mg in the reactants is x(1-y):(1-x)(1-y):y, where 0.5≤x≤0.6 and 0.005≤y≤0.020; And / or, the amount of the reducing agent is 1 mol% to 5 mol% of the total metal ions in the reactants. And / or, the sodium oxalate is introduced in solution form at a concentration of 0.1~1.0 mol / L; And / or, the molar ratio of the oxalate molar amount in the sodium oxalate to the total molar amount of metal ions in the manganese salt, ferrous salt and magnesium salt is 1:1; And / or, the reaction temperature in the coprecipitation reaction is 25~50℃; And / or, the aging time is 2 to 6 hours.
3. The preparation method according to claim 1, characterized in that, The lithium phosphorus source includes LiH2PO4, or a combination of Li2CO3 and NH4H2PO4, or a combination of LiOH and NH4H2PO4. And / or, the zirconium source includes at least one of ZrOCl2·8H2O, ZrO(NO3)2·nH2O, and Zr(CH3COO)4; And / or, the carbon source includes at least one of glucose, sucrose and citric acid; And / or, the total molar amount of Mn, Fe and Mg in the manganese iron magnesium oxalate precursor is denoted as M, the molar amount of Li in the lithium source is (1.03~1.06):1 to M, and the molar amount of Zr in the zirconium source is 0.1mol%~1.0mol% of M. And / or, the amount of carbon source added is controlled with the carbon content of the lithium manganese iron phosphate cathode material being 1.5 wt.% to 2.5 wt.%.
4. The preparation method according to claim 1, characterized in that, The ball milling process is a wet ball milling process with the following parameters: ball milling speed 400~600 rpm, ball milling time 4~8 h, ball-to-material mass ratio (8~12):1, and ethanol as the dispersion medium. And / or, the drying temperature is 70~90℃; And / or, the inert atmosphere is argon or nitrogen, and the gas flow rate is 80~120mL / min.
5. The preparation method according to claim 1, characterized in that, The procedure parameters for the one-time two-stage solid-state heat treatment are as follows: in the first stage, the temperature is increased to 380-430℃ at a rate of 3-5℃ / min and held for 3-5 hours; in the second stage, the temperature is increased to 700-800℃ at a rate of 3-5℃ / min and held for 8-12 hours.
6. A lithium manganese iron phosphate cathode material synergistically modified by bulk doping and interface modification, characterized in that, The bulk doping and interface modification synergistically modified lithium manganese iron phosphate cathode material is prepared by the preparation method described in any one of claims 1-5.
7. The application of the lithium manganese iron phosphate cathode material with synergistic bulk doping and interface modification as described in claim 6 in lithium-ion power batteries or energy storage batteries.
8. An electrode, characterized in that, The active component of the electrode includes the lithium manganese iron phosphate cathode material synergistically modified by bulk doping and interface modification as described in claim 6.
9. A lithium-ion battery, characterized in that, The lithium-ion battery uses the electrode described in claim 8 as the positive electrode.
10. An energy storage device, characterized in that, The energy storage device uses the electrode described in claim 8 as the positive electrode.