Method for preparing high-pressure recycled lithium iron phosphate materials using waste lithium iron phosphate powder

By employing a gradient oxidation reaction mechanism and a graded mixing secondary sintering method, the problem of improving the compaction density and electrochemical performance of recycled waste lithium iron phosphate materials was solved, resulting in the preparation of high-compact, high-performance lithium iron phosphate materials suitable for high-end power and energy storage batteries.

CN123105591APending Publication Date: 2026-11-17WUHAN RIKOMAY NEW ENERGY CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202611618622.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare high-compact lithium iron phosphate cathode materials that meet the requirements of high-end power and energy storage batteries through the regeneration of waste lithium iron phosphate. The problems include the single phase structure of the precursor in the material repair and regeneration stage, the serious homogenization of particle morphology, and the lack of an adjustable gradation control window in the particle size range, which makes it difficult to improve the compaction density.

Method used

By employing a gradient oxidation reaction mechanism, precursors with different phase compositions and morphological characteristics are prepared through peroxidation and non-peroxidation reaction pathways, respectively. Combined with graded mixing and secondary sintering, a regenerated lithium iron phosphate material with tightly packed particles of different sizes and uniform grain size distribution is formed.

Benefits of technology

It significantly improves the compaction density and electrochemical performance of regenerated lithium iron phosphate, with a compaction density of 2.60–2.66 g/cm3, a powder resistivity reduction of 44–88%, and excellent electrochemical performance, with a discharge capacity of 158–164 mAh/g at 0.1C rate and a specific capacity of 419–428 mAh/cm3.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105591A_ABST
    Figure CN123105591A_ABST
Patent Text Reader

Abstract

This invention relates to the field of waste lithium iron phosphate material recycling technology, specifically to a method for preparing high-compact regenerated lithium iron phosphate material using waste lithium iron phosphate powder. The method includes: pretreatment of waste lithium iron phosphate powder, preparation of a dual-path precursor, graded mixing and secondary gradient sintering, and finally, air-jet pulverization of the sintered regenerated lithium iron phosphate to obtain the final product. This method prepares precursors with different phase compositions and morphological characteristics by controlling the peroxidation and non-peroxidation reaction pathways, and utilizes their particle gradation effect to prepare high-compact density regenerated lithium iron phosphate material. The compaction density of the obtained material is 2.60–2.70 g / cm³. 3 The powder resistivity is 3.5–10.2Ω, the 0.1C rate discharge capacity is 158–164 mAh / g, and the specific capacity is 419–428 mAh / cm³. 3 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of waste lithium iron phosphate recycling technology, specifically involving a method for preparing high-density regenerated lithium iron phosphate materials using waste lithium iron phosphate powder. The method is based on the gradient oxidation reaction mechanism of waste lithium iron phosphate, and by controlling the peroxidation and non-peroxidation reaction pathways, precursors with different phase compositions and morphological characteristics are prepared respectively. The high-density regenerated lithium iron phosphate cathode materials are prepared by utilizing their particle size distribution effect, which can be directly applied to high-end power batteries and energy storage batteries. Background Technology

[0002] Lithium iron phosphate (LiFePO4, LFP) is the mainstream cathode material for power batteries and energy storage batteries. Its high safety, long cycle life, and low cost have led to a continuous increase in market demand. With the first batch of power batteries entering their retirement period, the recycling and reuse of spent lithium iron phosphate has become a key area of ​​research and development in the industry.

[0003] Existing recycling technologies for waste lithium iron phosphate mainly fall into two categories: one is the hydrometallurgical route, which involves leaching valuable elements through acid or alkali leaching and then resynthesizing the precursor. Although this process produces high-purity products, it is lengthy, generates large amounts of wastewater, and is not economically viable. The other is the direct repair route, which restores the electrochemical activity of failed lithium iron phosphate through methods such as lithium replenishment and reduction roasting. This route is shorter and cheaper, but the compaction density of the recycled materials is generally low, making it difficult to meet the design requirements of high-compact batteries.

[0004] Chinese invention patent application CN 115092903 A discloses a method for preparing high-compact-density lithium iron phosphate. This method improves the primary particle crystallinity and tap density of the cathode material by using a low-surface-area iron phosphate precursor and adding a co-solvent, thereby improving the material's kinetic properties and increasing the compaction density of lithium iron phosphate. This method is mainly applicable to the process of preparing lithium iron phosphate from iron phosphate, but not to the regeneration of retired lithium iron phosphate. Chinese invention patent application CN114497479 A discloses a high-compact-density, high-performance lithium iron phosphate cathode material and its preparation method. This method uses large-particle iron phosphate and small-particle iron phosphate with additives, and prepares high-compact-density lithium iron phosphate through a two-calcination process. This method belongs to the iron phosphate-to-lithium iron phosphate process and is not applicable to the regeneration of retired lithium iron phosphate. Chinese invention patent application CN106450547 A discloses a method for recovering iron phosphate and lithium carbonate from lithium iron phosphate waste. This method uses oxidative roasting and acid washing to prepare iron phosphate and lithium carbonate. This method has a relatively long process, generates waste acid, and is not environmentally friendly. Chinese invention patent application CN120364760 A discloses an oxide intermediate and its application. The oxide intermediate prepared by this method has a uniform particle morphology, and the preparation of high-pressure, high-pressure lithium iron phosphate requires the addition of small-particle iron sources. Chinese invention patent application CN121180969 A discloses a low-temperature resistant, high-pressure, high-pressure lithium iron phosphate cathode material, its preparation method, and a battery. This method uses multiple phosphorus and iron sources in combination to prepare lithium iron phosphate, resulting in complex process control, complex ingredient formulation, low tolerance for errors, and poor consistency in product realization. Chinese invention patent application CN121493919 A ​​discloses a method for preparing ultra-high-pressure, high-pressure lithium iron phosphate materials and its application, using two iron-phosphorus ratio iron phosphates with high and low iron-phosphorus ratios and a double-calcination process to prepare lithium iron phosphate. This method is mainly applicable to the preparation of lithium iron phosphate from iron phosphate and is not suitable for the regeneration of retired lithium iron phosphate. Chinese invention patent application CN121672455... Chinese invention patent application A discloses a method for preparing high-pressure lithium iron phosphate. This method uses the ferrous oxalate method and the iron phosphate method to prepare lithium iron phosphate with different physicochemical properties. After mixing, secondary grinding and secondary sintering, nanoscale particle size distribution and carbon coating optimization are achieved. This scheme is suitable for new lithium iron phosphate materials, but not for direct repair and regeneration. Chinese invention patent application CN 121839529A discloses a lithium iron phosphate cathode material based on two-step sintering and gradient carbon coating and its preparation method. This method first prepares lithium iron phosphate, performs a first reduction sintering under carbon source-free conditions, and then performs a second carbon coating to construct three types of carbon-coated lithium iron phosphate. This method has the risk of uneven mixing leading to abnormal slurry mixing at the end.PCT patent application No. WO 2021114747 A1 (Chinese patent application No. CN 113036253 A) discloses a method for selective oxidation-reduction regeneration of waste lithium iron phosphate, the regenerated lithium iron phosphate, and lithium-ion batteries. This method uses multiple gases to selectively oxidize waste lithium iron phosphate and then regenerates it to produce lithium iron phosphate. However, the intermediate oxides produced by this method are relatively homogeneous and cannot produce particle size distribution. Therefore, the overall performance of the regenerated lithium iron phosphate is relatively poor, failing to meet the requirements of power batteries and high-end energy storage.

[0005] In summary, most existing production processes involving high-density lithium iron phosphate (LFP) use virgin raw materials. The process of repairing and regenerating waste LFP to prepare high-density LFP has significant technical bottlenecks: the precursor phase structure obtained in the material repair and regeneration stage is simple, the particle morphology of the product is highly homogeneous, and there is a lack of controllable gradation control windows in the particle size range. Ultimately, it is difficult to improve the compaction density of LFP powder prepared by regeneration and repair, and it is impossible to produce high-density LFP cathode materials that meet the requirements of high-end power and energy storage batteries. Summary of the Invention

[0006] The purpose of this invention is to address the problem in existing technologies where the compaction density of regenerated lithium iron phosphate powder is difficult to improve, making it impossible to produce high-compact lithium iron phosphate cathode materials that meet the requirements of high-end power and energy storage batteries. This invention provides a method for preparing high-compact regenerated lithium iron phosphate materials using waste lithium iron phosphate powder. This method is based on a gradient oxidation reaction mechanism for preparing regenerated lithium iron phosphate materials. It utilizes the characteristic reaction equations of waste lithium iron phosphate under peroxidation and non-peroxidation conditions to directionally prepare precursors with different phase compositions and morphologies. Through graded mixing and secondary sintering regeneration, regenerated lithium iron phosphate cathode materials with high compaction density and excellent electrochemical performance are obtained.

[0007] The present invention discloses a method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder, comprising the following steps: (1) Pretreatment of waste lithium iron phosphate powder The molar ratio of Li, Fe, and P and the residual carbon content in waste lithium iron phosphate powder were determined. Based on the ratio of Li:Fe:P = 1.02 to 1.08:1:1 in the target recycled lithium iron phosphate material, the lithium source was calculated and supplemented. If necessary, the iron and phosphorus sources were supplemented to obtain pretreated black powder. (2) Preparation of peroxide precursor - driving reaction pathway (I) The pretreated black powder and carbon source were mixed and calcined in an atmosphere with an oxygen volume fraction of 20-100% at 450-650℃ to obtain a peroxide precursor containing characteristic products Li3PO4 phase, FePO4 phase and Fe2O3 phase. (3) Preparation of non-peroxide precursors - driving reaction pathway (II) The pretreated black powder was mixed with a carbon source and calcined at 300-500°C in an atmosphere with an oxygen volume fraction of 10-20% to obtain a non-peroxide precursor containing the characteristic products Li3Fe2(PO4)3 phase and Fe2O3 phase. (4) Graded mixing and secondary gradient sintering The peroxide precursor and the non-peroxide precursor are mixed at a mass ratio of 20-45:55-80, with the sum of their masses being 100. After adding carbon source and dopant modifier, water is added to form a slurry, which is then spray-granulated. Under an inert atmosphere, the mixture is calcined in two stages at 450-550℃ and 680-760℃. By utilizing the different nucleation temperatures of different materials, the staged calcination forms a sintered body of regenerated lithium iron phosphate with tightly packed particles of different sizes and a uniform grain size distribution. The resulting material is then pulverized by airflow to obtain high-pressure compacted regenerated lithium iron phosphate material.

[0008] Further, the regenerated lithium iron phosphate sintered body obtained in step (4) is naturally cooled to room temperature and subjected to air jet milling to control the product particle size D50 to 1.0-1.5μm, thus obtaining high-pressure compacted regenerated lithium iron phosphate material.

[0009] The compaction density of the high-compaction regenerated lithium iron phosphate material prepared by the above method is 2.60–2.66 g / cm³. 3 The powder resistivity is 3.5–10.2Ω, the discharge capacity at 0.1C rate is 158–164 mAh / g, and the specific capacity is 419–428 mAh / cm³. 3 .

[0010] Further, the specific process parameters for preparing the peroxide precursor in step (2) above are as follows: pretreated black powder and carbon source are mixed at a mass ratio of 100:1 to 3, deionized water is added to adjust the slurry to a solid content of 30 to 45%, and the slurry with a particle size D50 of 300 to 600 nm is obtained by grinding. The obtained slurry is spray-dried in an atmosphere with an oxygen volume fraction of 20 to 100%, and the dried powder is calcined in an atmosphere with an oxygen volume fraction of 20 to 100% at 450 to 650°C for 4 to 7 hours and then air-jet pulverized to obtain the peroxide precursor.

[0011] Further, the specific process parameters for the preparation of the non-peroxide precursor in step (3) above are as follows: pretreated black powder and carbon source are mixed at a mass ratio of 100:10-20, deionized water is added to adjust the slurry to a solid content of 40-55%, and the slurry with a particle size D50 of 300-600 nm is obtained by grinding. The obtained slurry is spray-dried in an atmosphere with an oxygen volume fraction of 10-20%, and the dried powder is placed in an atmosphere with an oxygen volume fraction of 10-20% and calcined at 300-500℃ for 2-4 hours before being air-jet pulverized to obtain the non-peroxide precursor.

[0012] Further, the specific process parameters for the graded mixing described in step (4) above are as follows: the peroxide precursor and the non-peroxide precursor are mixed at a mass ratio of 20-45:55-80, and the sum of their masses is 100 to obtain a mixture. At the same time, carbon source is added at 1-10% of the total mass of the mixture, and dopant modifier is added at 0.1-1.5% of the total mass of the mixture. Deionized water is added to the mixture after adding carbon source and dopant modifier to adjust the slurry to a solid content of 35-45%. The mixture is then ground to obtain a slurry with a particle size D50 of 0.3-0.6 μm. The obtained slurry is then spray-dried in an air atmosphere to obtain spherical particles with a D50 of 20-30 μm.

[0013] Furthermore, the specific process parameters for the secondary gradient sintering described in step (4) above are as follows: the spherical particles obtained by spray granulation are placed in an inert atmosphere furnace and calcined using a segmented heating program: First stage: Heat to 450-550℃ at a heating rate of 2-4℃ / min and hold for 1-2 hours; This stage promotes the initial solid-phase reaction of Li3PO4 and FePO4 in the peroxidation precursor and Li3Fe2(PO4)3 in the non-peroxidation precursor, while the carbon source begins to pyrolyze to form a reducing carbon coating layer. The second stage involves further heating at a rate of 1–3 °C / min to 680–760 °C, holding at this temperature for 6–10 hours to form a sintered body of regenerated lithium iron phosphate with tightly packed particles and uniform grain size distribution. This stage is where the key regeneration reaction occurs. From the peroxide precursor Li3PO4 + FePO4 + C → LiFePO4 + CO↑; Li3Fe2(PO4)3 + Fe2O3 + C → LiFePO4 + CO↑, derived from a non-peroxide precursor; The two reaction equations above are only used to illustrate the direction of formation of the main product. In the actual reaction, reduction is provided by an additional carbon source, which in this process will reduce Fe. 3+ Reduced to Fe 2+ The conversion of Li3Fe2(PO4)3 to LiFePO4 is completed; the high reactivity of the small particle surface promotes the diffusion bonding of the large particle edge, forming a regenerated lithium iron phosphate sintered body with tightly packed particles of different sizes and uniform grain size distribution.

[0014] The process parameters for spray drying in the preparation of the above-mentioned peroxide precursor are: inlet air temperature of 180-240℃, outlet air temperature of 90-110℃, and atomizer operating frequency of 35-45Hz.

[0015] The process parameters for spray drying in the preparation of the above-mentioned non-peroxide precursor are: inlet air temperature of 190-250℃, outlet air temperature of 95-120℃, and atomizer operating frequency of 35-45Hz.

[0016] The process parameters for spray drying in the above-mentioned graded mixing process are: inlet air temperature of 190-250℃, outlet air temperature of 95-120℃, and atomizer operating frequency of 35-45Hz.

[0017] The process parameters for airflow pulverization in this invention are as follows: pulverization pressure is controlled at 0.2–0.3 MPa, grading frequency is 35–40 Hz, and pulverized particle size D50 is 1.0–1.5 μm.

[0018] Furthermore, the reaction equation for the peroxide precursor-driven reaction pathway (I) described in this invention is as follows: 12LiFePO4+6LiOH+3O2→6Li3PO4+6FePO4+3Fe2O3+3H2O(I); The above reaction formula is only used to illustrate the direction of the formation of the main oxidation products. The actual batching shall be carried out according to the Li:Fe:P ratio described in step (1), and the product ratio shall be based on the actual measurement in Table 2.

[0019] The characteristic products of the peroxide precursor described in this invention contain Li3PO4, FePO4, and Fe2O3 phases. The mass percentages of each component in the characteristic products of the peroxide precursor are: Li3PO4: 17-21%, FePO4: 45-52%, Fe2O3: 23-28%, with the remainder being other phases, totaling 1-15% (the other phases are due to the iron-phosphorus-lithium ratio not meeting the 1:1:1 ratio; during the solid-state sintering reaction, some excess elements react directly to generate small amounts of other iron-phosphorus-lithium compounds). The particle morphology is dense blocky or spherical, with a BET specific surface area of ​​3-8 m². 2 / g, with an average particle size D50 of 1.0–1.5 μm. Li3PO4 acts as the lithium-ion conductor phase, while FePO4 and Fe2O3 act as iron-rich phases; the coexistence of these three phases is a characteristic feature of the peroxide precursor. The O2 required during the reaction is maintained by an oxygen-enriched atmosphere or by increasing the gas inlet flow rate, calcination time, and sintering temperature, thus ensuring the presence of Fe in LiFePO4. 2+ Completely oxidized to Fe 3+ Finally, a three-phase mixture of Li3PO4, FePO4 and Fe2O3 was obtained.

[0020] Furthermore, the reaction equation for the non-peroxidation precursor-driven reaction pathway (II) described in this invention is as follows: LiFePO4+5FePO4+5LiOH +1 / 4O2→2Li3Fe2(PO4)3+Fe2O3+5 / 2H2O (II); The FePO4 in the above reaction formula (II) comes from waste lithium iron phosphate powder and is not an external raw material; Similarly, the above reaction formula is only used to illustrate the direction of the formation of the main oxidation products. The actual ingredients are prepared according to the Li:Fe:P ratio described in step (1), and the product ratio is based on the actual measurement in Table 2.

[0021] The characteristic products of the non-peroxidized precursor described in this invention contain both Li3Fe2(PO4)3 and Fe2O3 phases. The mass percentages of each component in the characteristic products of the non-peroxidized precursor are as follows: Li3Fe2(PO4)3: 65-76%, Fe2O3: 15-20%, and incompletely converted LiFePO4: 2-10%, with the remainder being other phases. The total amount of other phases is ≤10% (the other phases are due to the iron-phosphorus-lithium ratio not meeting the 1:1:1 ratio; during the solid-state sintering reaction, some excess elements react directly to generate small amounts of other iron-phosphorus-lithium compounds). The particle morphology is a loose and porous structure with a BET specific surface area of ​​15-30 m². 2 / g, with an average particle size D50 of 1.0–1.5 μm. Li3Fe2(PO4)3 belongs to the NASICON structure, exhibiting good structural stability and lithium-ion conductivity, and together with Fe2O3, forms a dense precursor framework. During the reaction, an excess carbon source is required. The gas inlet volume, sintering time, and calcination temperature are controlled during calcination to reduce excessive oxidation of LiFePO4, ultimately yielding a mixed phase of Li3Fe2(PO4)3, LiFePO4, and Fe2O3.

[0022] The waste lithium iron phosphate powder mentioned in this invention is obtained by crushing and separating the positive electrode sheets of waste lithium iron phosphate batteries with a capacity retention rate of 60-85%, then heat-treating them at 80-120°C for 0.5-1h to remove the electrolyte, and then sieving to remove aluminum foil and separator fragments.

[0023] The lithium source described in this invention is selected from one or more of lithium carbonate, lithium hydroxide, and lithium oxalate. Of course, the choice of lithium source in this invention is not limited to the above-mentioned substances; other products of the same type can be used as substitutes, as long as they conform to the principles of this invention.

[0024] The carbon source used in this invention is selected from one or more of glucose, sucrose, starch, polyethylene glycol, graphene, and acetylene black. However, the choice of carbon source in this invention is not limited to the above-mentioned options.

[0025] The doping modifier described in this invention is a metal doping modifier and / or a non-metal doping modifier. The metal doping modifier is one or more of titanium dioxide, niobium pentoxide, ammonium metavanadate, magnesium oxide, and zirconium dioxide; the non-metal doping modifier is one or more of melamine, urea, and polyaniline. Of course, the choice of doping modifier in this invention is not limited to the above-mentioned substances; other products of the same type can be used as substitutes, as long as they meet the inventive purpose of this invention.

[0026] In this invention, the roasting described in steps (2) and (3) is carried out in a rotary kiln.

[0027] In this invention, the equipment used for the secondary gradient sintering in step (4) is a tube furnace or a box furnace, and the inert atmosphere is nitrogen or argon. For large-scale industrial production, a roller kiln can be used, and the inert atmosphere is nitrogen or argon, preferably nitrogen.

[0028] Preferably, the grinding described in this invention is performed using a sand mill.

[0029] Application of high-pressure recycled lithium iron phosphate materials in the cathode of lithium-ion power batteries or energy storage batteries.

[0030] The compacted regenerated lithium iron phosphate material has a particle size D50 of 1.0–1.5 μm and a compaction density of 2.60–2.66 g / cm³. 3 The powder resistivity is 3.5–10.2Ω, the 0.1C rate discharge capacity is 158–164 mAh / g, and the specific capacity is 419–428 mAh / cm³. 3 .

[0031] The application is as the positive electrode active material of square aluminum-cased battery cells or energy storage battery cells.

[0032] The method of this invention was developed by the inventors based on in-depth research on the characteristics of waste lithium iron phosphate powder and high-density lithium iron phosphate materials. By controlling the degree of oxidation of waste lithium iron phosphate, the inventors induced two different reaction pathways—the peroxidation pathway and the non-peroxidation pathway—to generate intermediate product phase combinations and particle morphology characteristics with significant differences. Using these as precursors, the inventors designed the gradation and obtained high-density regenerated lithium iron phosphate materials after secondary repair and sintering. Different oxidation pathways produce different precursors. In an inert atmosphere, FePO4 begins to form lithium iron phosphate at around 510°C, Fe2O3 begins to nucleate and form lithium iron phosphate at around 630°C, and Li3Fe2(PO)3 undergoes a lattice transformation at 650°C to form lithium iron phosphate. The nucleation and growth temperatures required for different precursors vary significantly. Under the same sintering conditions, precursors with lower nucleation temperatures (FePO4) grow more easily and act as a supporting framework in high-compaction systems. Furthermore, the dense structure of the precursor can increase the true density of the material and effectively improve powder compaction. Precursors with higher nucleation temperatures (Li3Fe2(PO)3) can provide better filling in high-compaction systems, and this loose and porous structure is conducive to electrolyte wetting, which is beneficial to improving the rate performance of the material. Precursors with intermediate nucleation temperatures (Fe2O3) can fill the gaps between large and small particles in high-compaction systems, reducing voids and ultimately forming a particle size distribution of large, medium, and small, enabling direct repair and regeneration of high-compaction lithium iron phosphate materials.

[0033] Compared with the prior art, the present invention has the following beneficial effects: (1) Significantly improved compaction density: Based on the multi-phase mixing obtained through two characteristic reaction pathways, the compaction density of recycled materials can reach 2.60–2.66 g / cm³. 3 Compared to using only a single non-peroxide precursor (Comparative Example 1, 2.41 g / cm³), 3 ) and using only a single peroxide precursor (Comparative Example 2, 2.35 g / cm) 3 All of these parameters show significant improvement; the powder resistivity ranges from 3.5 to 10.2 Ω, which is approximately 44% to 88% lower than that of conventionally repaired regenerated lithium iron phosphate materials.

[0034] (2) Excellent electrochemical performance: The Li3PO4 component in the peroxide precursor forms a lithium-ion conduction network after secondary sintering, while the Li3Fe2(PO4)3 in the non-peroxide precursor has a NASICON-type structure. Its three-dimensional lithium-ion transport channels form a transition interface between LiFePO4 grains during sintering, which is beneficial to reducing interface impedance and improving rate performance. Its difference from conventional olivine-type LiFePO4 is that the NASICON-type structure is formed by the strong PO4 between octahedrons and tetrahedrons. A three-dimensional rigid framework is constructed using covalent bonds. The octahedrons and tetrahedrons, connected by strong PO covalent bonds, form this rigid framework, enabling reversible insertion / extraction closer to theoretical values. This effectively improves the rate performance of olivine-type LiFePO4. The resulting recycled lithium iron phosphate material, when assembled into a battery, exhibits a discharge capacity of 158–164 mAh / g at 0.1C, a first-time battery efficiency of 98–99.15% at 0.1C, a discharge capacity of 144–152 mAh / g at 1C, and a specific capacity of 419–428 mAh / cm³. 3 .

[0035] (3) The reaction path is clear and controllable: Based on reaction equations (I) and (II), a clear correspondence between the degree of oxidation and the product phase is established, the operation window is clear, and the process reproducibility is high.

[0036] (4) Strong adaptability of raw materials: It is suitable for waste lithium iron phosphate with different failure levels (capacity retention rate of 60-85%). By adjusting the ratio of the molar amount of lithium source added to the molar amount of P in waste LFP powder, i.e. 0.15≤n(Li added) / n(P)≤0.5, the degree of peroxidation / non-peroxidation reaction and the product ratio can be flexibly controlled.

[0037] (5) Environmentally friendly: The entire process has no aqueous phase acid leaching step and no waste acid or wastewater discharge. Attached Figure Description

[0038] Figure 1 This is a schematic flowchart of the method for preparing high-pressure recycled lithium iron phosphate according to the present invention; Figure 2 The curves showing the relationship between 0.1C discharge voltage and DOD for Examples 1-6 and Comparative Examples 1-2 are shown. Figure 3 SEM image of high-pressure recycled lithium iron phosphate prepared in Example 2; Figure 4 The image shows a high-pressure recycled lithium iron phosphate SEM image prepared in Example 3. Detailed Implementation

[0039] The following description, in conjunction with the technical solution of this invention, provides a clearer and more complete explanation of the relevant content. It should be noted that the embodiments described herein are only a part of the implementation methods of this invention, and not all of them. Other implementation methods obtained by those skilled in the art based on the embodiments of this invention without creative effort should also fall within the protection scope of this invention. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions in the art or according to the manufacturer's recommendations; the raw materials and reagents used, unless otherwise specified, are considered to be readily available through commercial channels such as the conventional market.

[0040] The present invention discloses a method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder, comprising: pretreatment of waste lithium iron phosphate powder and replenishment of lithium to a Li:Fe:P ratio of 1.02–1.08:1:1; calcination at 450–650°C with an oxygen volume fraction of 20–100% to obtain a peroxide precursor; calcination at 300–500°C with an oxygen volume fraction of 10–20% to obtain a non-peroxide precursor; mixing the two at a ratio of 20–45:55–80 and replenishing with a carbon source and dopant, followed by spray granulation; calcination in an inert atmosphere at two stages at 450–550°C and 680–760°C, followed by air jet milling of the calcined product to control the product particle size D50 to be 1.0–1.5 μm, thereby obtaining the high-pressure recycled lithium iron phosphate material.

[0041] Specifically, a method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to various embodiments of the present invention includes the following steps: (1) Pretreatment of waste lithium iron phosphate powder The molar ratio of Li, Fe, and P and the residual carbon content in waste lithium iron phosphate powder were determined. Based on the ratio of Li:Fe:P = 1.02 to 1.08:1:1 in the target recycled lithium iron phosphate material, the lithium source was calculated and supplemented. If necessary, the iron and phosphorus sources were supplemented to obtain pretreated black powder. (2) Preparation of peroxide precursor - driving reaction pathway (I) Pretreated black powder and carbon source are mixed at a mass ratio of 100:1 to 3, and deionized water is added to adjust the slurry to a solid content of 30 to 45%. The slurry is then ground to obtain a particle size D50 of 300 to 600 nm. The obtained slurry is spray-dried in an atmosphere with an oxygen volume fraction of 20 to 100%. The dried powder is then calcined in an atmosphere with an oxygen volume fraction of 20 to 100% at 450 to 650 °C for 4 to 7 hours and then air-jet pulverized to obtain the peroxide precursor. (3) Preparation of non-peroxide precursors - driving reaction pathway (II) Pretreated black powder and carbon source are mixed at a mass ratio of 100:10-20, and deionized water is added to adjust the slurry to a solid content of 40-55%. The slurry is then ground to obtain a particle size D50 of 300-600 nm. The obtained slurry is spray-dried in an atmosphere with an oxygen volume fraction of 10-20%. The dried powder is then calcined in an atmosphere with an oxygen volume fraction of 10-20% at 300-500℃ for 2-4 hours and then air-jet pulverized to obtain a non-peroxide precursor. (4) Graded mixing and secondary gradient sintering Graded mixing: The peroxide precursor and the non-peroxide precursor are mixed at a mass ratio of 20-45:55-80, and the sum of their masses is 100 to obtain a mixture. At the same time, 1-10% of the total mass of the mixture is added with carbon source and 0.1-1.5% of the total mass of the mixture with dopant modifier. Deionized water is added to the mixture with added carbon source and dopant modifier to adjust the slurry to a solid content of 35-45%. The mixture is then ground to obtain a slurry with a particle size D50 of 0.3-0.6 μm. The obtained slurry is spray-dried in an air atmosphere to obtain spherical particles with a D50 of 20-30 μm. Secondary gradient sintering: The resulting spherical particles are placed in an inert atmosphere furnace and calcined using a segmented heating program. First stage: Heat to 450-550℃ at a heating rate of 2-4℃ / min, and hold for 1-2 hours; The second stage involves continuing to heat the material at a rate of 1–3 °C / min to 680–760 °C and holding it at that temperature for 6–10 hours to form a sintered body of regenerated lithium iron phosphate with tightly packed particles of varying sizes and a uniform grain size distribution. Furthermore, the obtained recycled lithium iron phosphate sintered body is naturally cooled to room temperature, subjected to air jet milling, and the product particle size D50 is controlled to be 1.0-1.5μm. Iron is removed (by electromagnetism, controlling magnetic matter ≤1ppm), and packaged to finally obtain high-pressure compacted recycled lithium iron phosphate material.

[0042] Furthermore, the parameters for spray drying described in step (2) above are: an inlet air temperature of 180-240°C, an outlet air temperature of 90-110°C, and an atomizer operating frequency of 35-45Hz.

[0043] Furthermore, the parameters for spray drying in step (3) above are: inlet air temperature of 190-250°C, outlet air temperature of 95-120°C, and atomizer operating frequency of 35-45Hz.

[0044] Furthermore, the parameters for spray drying in step (4) above are: inlet air temperature of 190-250°C, outlet air temperature of 95-120°C, and atomizer operating frequency of 35-45Hz.

[0045] Furthermore, in each embodiment of the present invention, the process parameters for airflow pulverization of the recycled lithium iron phosphate sintered body in steps (2) and (3) are as follows: the pulverization pressure is controlled at 0.2 to 0.3 MPa, the grading frequency is 35 to 40 Hz, and the pulverized particle size D50 is 1.0 to 1.5 μm.

[0046] The waste lithium iron phosphate powder described in the various embodiments of the present invention is obtained by crushing and separating the positive electrode sheets of waste lithium iron phosphate batteries with a capacity retention rate of 60-85%, heat-treating them at 80-120°C for 0.5-1h to remove the electrolyte, and then sieving to remove aluminum foil and separator fragments.

[0047] The lithium source described in the various embodiments of the present invention is selected from one or more of lithium carbonate, lithium hydroxide, and lithium oxalate; of course, the selection of lithium source in the present invention is not limited to the above substances, and other products of the same type can also be used instead, as long as they conform to the principle of the present invention.

[0048] The carbon source described in the various embodiments of the present invention is selected from one or more of glucose, sucrose, starch, polyethylene glycol, graphene, and acetylene black. However, the selection of the carbon source in the present invention is not limited to the above-mentioned selections.

[0049] In the various embodiments of this invention, the doping modifier is a metal doping modifier and / or a non-metal doping modifier. The metal doping modifier is one or more of titanium dioxide, niobium pentoxide, ammonium metavanadate, magnesium oxide, and zirconium dioxide; the non-metal doping modifier is one or more of melamine, urea, and polyaniline. Of course, the choice of doping modifier in this invention is not limited to the above-mentioned substances; other products of the same type can be used instead, as long as they meet the inventive purpose of this invention.

[0050] The roasting described in steps (2) and (3) of the various embodiments of the present invention is carried out in a rotary kiln.

[0051] In each embodiment of the present invention, the equipment used for secondary gradient sintering in step (4) is a tube furnace or a box furnace. In industrial production, the equipment used can be a roller kiln. The inert atmosphere is nitrogen or argon. In the following embodiments, the equipment used for secondary gradient sintering is a tube furnace, and the inert atmosphere is nitrogen atmosphere.

[0052] The grinding described in the various embodiments of the present invention is performed using a sand mill.

[0053] The following section selects waste lithium iron phosphate battery cathode sheets with different capacity retention rates and uses the method of this invention to prepare high-density regenerated lithium iron phosphate cathode materials.

[0054] Table 1 below is a list of detailed process parameters for the preparation of peroxidized and non-peroxidized precursors in various embodiments and comparative examples of the present invention; Table 2 below shows the content of characteristic products in the peroxidized and non-peroxidized precursors in various embodiments of the present invention; Table 3 below is a detailed list of process parameters for the precursor particle size distribution and secondary calcination process in various embodiments and comparative examples of the present invention. Table 4 below lists the performance parameters of the recycled lithium iron phosphate materials prepared in various embodiments and comparative examples of the present invention.

[0055] Table 1. List of detailed process parameters for the preparation of peroxidized and non-peroxidized precursors in various embodiments and comparative examples of the present invention. Note: The Li:Fe:P value after lithium replenishment cannot be a fixed value due to uneven mixing in actual production.

[0056] Table 2. Content of characteristic products in peroxidation precursors and non-peroxidation precursors in various embodiments of the present invention. Table 3. Detailed process parameters for precursor particle size distribution and secondary calcination in various embodiments and comparative examples of the present invention. Table 4. Performance parameters of the recycled lithium iron phosphate materials prepared in various embodiments and comparative examples of the present invention. Note: The button batteries used to test the performance of the recycled lithium iron phosphate materials in Table 4 above were prepared by the following methods: (1) Slurry preparation: according to the mass ratio of active material: conductive agent: binder = 9:0.5:0.5, add solvent and stir to make a uniform slurry; (2) Coating and primary drying: coat the slurry uniformly on the surface of the current collector positive electrode aluminum foil, and vacuum dry at 80°C for 6 hours to remove the solvent; (3) Rolling and punching: compact the dried electrode sheet by rolling at 10 MPa and punching it into a circular electrode sheet with a diameter of 14 mm; (4) Secondary vacuum drying: vacuum dry the punched electrode sheet at 100°C for 12 hours to completely remove moisture and residual solvent; (5) Component pretreatment: the metal shell, spring sheet and gasket are ultrasonically cleaned with anhydrous ethanol and then dried; the electrolyte is dehydrated to a water content of <10ppm. Positive electrode pre-assembly: In a glove box (H2O<0.1 ppm, O2<0.1 ppm), the positive electrode shell, positive electrode sheet, and separator are stacked in sequence, 50 μL of electrolyte is added for wetting, and the mixture is left to stand for 15 minutes; (6) Negative electrode pre-assembly: The negative electrode shell, spring sheet, gasket, and lithium sheet are stacked in sequence. Mold sealing: The negative electrode assembly is flipped and fastened onto the positive electrode assembly, and 1.0 ton pressure is applied for sealing; (7) Standing and testing: After standing at room temperature for 4 hours to stabilize the open circuit voltage, electrochemical performance testing is performed.

[0057] In this experiment, the powder resistance and powder compaction density were tested using the Yuaneng PRCD-2100 equipment. The main steps were as follows: (1) Preparatory work: the instrument was preheated for 30 minutes, and the gold-plated four probes and Φ13mm mold were cleaned; the lithium iron phosphate powder was dried and cooled, and 1.0000g of sample was weighed; (2) Sample loading: the lower pressure head was placed into the mold, the powder was poured in, the level was tapped lightly, the upper pressure head with probes was installed, and the pressure station was placed; (3) Software parameter setting: the four probe mode was selected; the pressure was set to 20MPa, the pressure increase rate was 0.5MPa / s, the pressure holding time was 30s, and the sample weight was entered; (4) Automatic detection: the test was started, the equipment was pressurized and held, the thickness and resistance were automatically collected, the compaction density and powder resistivity were calculated and the curve was generated; (5) Post-processing: the pressure head was reset, the compact was removed from the mold; the mold and probes were thoroughly cleaned; the test was performed in parallel 3 times and the test data was exported. The values ​​in Table 4 above are the arithmetic mean of three parallel tests, and the range of compacted density is no greater than 0.02 g / cm³. 3 The relative deviation of powder resistance is no greater than 5.

[0058] As can be seen from Tables 3 and 4 above, the high-compact density regenerated lithium iron phosphate material prepared by the method of this invention has a particle size D50 ranging from 1.0 to 1.5 μm and a compaction density ranging from 2.60 to 2.66 g / cm³. 3 The powder resistivity ranges from 3.5 to 10.2 Ω, the 0.1C discharge capacity is 158 to 164 mAh / g, the initial battery efficiency at 0.1C is 98 to 99.15%, the 1C discharge capacity is 144 to 152 mAh / g, and the specific capacity is 419 to 428 mAh / cm³. 3 .

[0059] In practical applications, size is the main factor restricting the energy of power batteries. Under the same volume, specific capacity is an important indicator for measuring the quality of a material. As shown in Table 4, the specific capacity of the regenerated lithium iron phosphate prepared in Examples 1-6 is greater than that of Comparative Examples 1-2. Compared with the regenerated lithium iron phosphate prepared by peroxidation alone (Comparative Example 2) and the regenerated lithium iron phosphate prepared by non-peroxidation (Comparative Example 1), the sintering method of peroxidation and non-peroxidation mixture (Examples 1-6 of this invention) can better achieve particle size distribution. Small particles provide capacity, while large particles provide a skeleton function. Under the combined effect of large and small particles, the specific capacity can be improved better. The resistivity of the regenerated lithium iron phosphate powder obtained in Examples 1-6 is 3.5-10.2Ω, which is much lower than that of the comparative examples of 18.3Ω and 30.2Ω. This is because the regenerated lithium iron phosphate material obtained in Examples 1-6 of this invention has a more dense spatial packing. Under the same pressure, the more densely packed the material, the lower the powder resistivity.

[0060] Figure 2 shows the 0.1 C discharge voltage-DOD curves of the battery cells assembled from the recycled lithium iron phosphate materials of Examples 1-6 and Comparative Examples 1-2. Compared with Comparative Examples 1 and 2, Examples 1-6 have a longer discharge voltage plateau. This proves that the preparation scheme of mixing and grading peroxide precursors and non-peroxide precursors can ensure higher discharge capacity while improving the compaction density of lithium iron phosphate.

[0061] Under the same depth of discharge (DOD) conditions, the difference between the charging plateau voltage and the discharging plateau voltage represents the overall polarization of the cell. The larger the difference, the worse the cell's kinetic performance. Comparing the two sets of comparative examples reveals that when preparing high-density lithium iron phosphate using a single precursor, material polarization increases significantly, and rate performance shows a marked decline. However, the mixed gradation process of peroxide-non-peroxide precursors can effectively reduce cell polarization and optimize material kinetic characteristics. This conclusion can also be corroborated by the 1C discharge specific capacity test results.

[0062] Figure 3 and Figure 4 The figures show the electron microscopy morphology of Examples 2 and 3 of this invention. As can be seen from the figures, the main body of the material consists of spherical and near-spherical lithium iron phosphate particles. The particles have regular morphology and form a large, medium, and small particle size distribution. Filamentous conductive materials are distributed on the particle surface and between particles, and the conductive components are uniformly attached between the particles, forming a continuous conductive path, which is beneficial for improving the overall conductivity of the powder. In contrast, the main body of the recycled lithium iron phosphate materials obtained in Comparative Examples 1 and 2 consists of spherical and near-spherical particles. The particles have regular morphology and a relatively concentrated particle size, without a significant large, medium, and small particle size distribution. This relatively concentrated particle size is not conducive to forming a high-compaction product, ultimately resulting in a lower specific capacity. Note: Figure 3 , Figure 4 The information bar at the bottom edge contains the imaging parameters automatically generated by the electron microscope equipment.

[0063] The above description is merely an embodiment of the present invention and is not intended to limit the scope of protection of the present invention. For those skilled in the art, the present invention can have various modifications and variations. All modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder, characterized in that, Includes the following steps: (1) Pretreatment of waste lithium iron phosphate powder The molar ratio of Li, Fe, and P and the residual carbon content in waste lithium iron phosphate powder were determined. Based on the ratio of Li:Fe:P = 1.02 to 1.08:1:1 in the target recycled lithium iron phosphate material, the lithium source was calculated and supplemented to obtain pretreated black powder. (2) Preparation of peroxide precursor - driving reaction pathway (I) The pretreated black powder and carbon source were mixed and calcined at 450–650°C in an atmosphere with an oxygen volume fraction of 20–100% to obtain a peroxide precursor. The peroxide precursor contained characteristic products with the following mass percentage contents: Li3PO4: 17–21%, FePO4: 45–52%, Fe2O3: 23–28%, and the balance being other phases, with a total amount of other phases of 1–15%. (3) Preparation of non-peroxide precursors - driving reaction pathway (II) The pretreated black powder was mixed with a carbon source and calcined at 300–500°C in an atmosphere with an oxygen volume fraction of 10–20% to obtain a non-peroxidized precursor; the non-peroxidized precursor contained characteristic products in the following mass percentages: Li3Fe2(PO4)3: 65-76%, Fe2O3: 15-20%, and incompletely converted LiFePO4: 2-10%, with the balance being other phases, the total amount of other phases ≤10%; (4) Graded mixing and secondary gradient sintering The peroxide precursor and the non-peroxide precursor are mixed at a mass ratio of 20-45:55-80, with the sum of their masses being 100. After adding carbon source and dopant modifier, water is added to form a slurry, which is then spray-granulated. Under an inert atmosphere, the mixture is calcined in two stages at 450-550℃ and 680-760℃, followed by air jet pulverization to obtain high-pressure compaction regenerated lithium iron phosphate material.

2. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: After the sintered recycled lithium iron phosphate obtained in step (4) is naturally cooled to room temperature, it is subjected to air jet milling to control the product particle size D50 to be 1.0 to 1.5 μm, thus obtaining high-pressure compacted recycled lithium iron phosphate material.

3. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The specific process for preparing the peroxide precursor in step (2) is as follows: pretreated black powder and carbon source are mixed at a mass ratio of 100:1 to 3, deionized water is added to adjust the slurry to a solid content of 30 to 45%, and the slurry with a particle size D50 of 300 to 600 nm is obtained by grinding. The obtained slurry is spray-dried in an atmosphere with an oxygen volume fraction of 20 to 100%, and the dried powder is calcined in an atmosphere with an oxygen volume fraction of 20 to 100% at 450 to 650°C for 4 to 7 hours and then air-jet pulverized to obtain the peroxide precursor.

4. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The specific process for preparing the non-peroxide precursor in step (3) is as follows: pretreated black powder and carbon source are mixed at a mass ratio of 100:10-20, deionized water is added to adjust the slurry to a solid content of 40-55%, and the slurry with a particle size D50 of 300-600 nm is obtained by grinding. The obtained slurry is spray-dried in an atmosphere with an oxygen volume fraction of 10-20%, and the dried powder is placed in an atmosphere with an oxygen volume fraction of 10-20% and calcined at 300-500℃ for 2-4 hours before air jet pulverization to obtain the non-peroxide precursor.

5. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The specific process of graded mixing in step (4) is as follows: the peroxide precursor and the non-peroxide precursor are mixed at a mass ratio of 20-45:55-80, and the sum of their masses is 100 to obtain a mixture. At the same time, carbon source is added at 1-10% of the total mass of the mixture, and dopant modifier is added at 0.1-1.5% of the total mass of the mixture. Deionized water is added to the mixture with added carbon source and dopant modifier to adjust the slurry to a solid content of 35-45%. The mixture is then ground to obtain a slurry with a particle size D50 of 0.3-0.6 μm. The obtained slurry is then spray-dried in an air atmosphere to obtain spherical particles with a D50 of 20-30 μm.

6. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The specific process of the secondary gradient sintering in step (4) is as follows: the spherical particles obtained by spray granulation are placed in an inert atmosphere furnace and calcined using a segmented heating program: First stage: Heat to 450-550℃ at a heating rate of 2-4℃ / min, and hold for 1-2 hours; The second stage involves continuing to heat the material at a rate of 1–3 °C / min to 680–760 °C and holding it at that temperature for 6–10 hours to form a sintered body of regenerated lithium iron phosphate with tightly packed particles of varying sizes and a uniform grain size distribution.

7. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The reaction equation for the preparation of the peroxide precursor-driven reaction pathway (I) is as follows: 12LiFePO4+6LiOH+3O2→6Li3PO4+6FePO4+3Fe2O3+3H2O (I).

8. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The peroxide precursor has a dense, massive or spherical morphology and a BET specific surface area of ​​3–8 m². 2 / g, with an average particle size D50 of 1.0–1.5 μm.

9. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The reaction equation for the preparation of the non-peroxidized precursor-driven reaction pathway (II) is as follows: LiFePO4+5FePO4+5LiOH +1 / 4O2→2Li3Fe2(PO4)3+Fe2O3+5 / 2H2O (II).

10. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The non-peroxide precursor has a loose and porous particle morphology with a BET specific surface area of ​​15–30 m². 2 / g, with an average particle size D50 of 1.0–1.5 μm.

11. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The waste lithium iron phosphate powder is obtained by crushing and separating the positive electrode sheets of waste lithium iron phosphate batteries with a capacity retention rate of 60-85%, then heat-treating them at 80-120°C for 0.5-1h to remove the electrolyte, and then sieving to remove aluminum foil and separator fragments.

12. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The lithium source is selected from one or more of lithium carbonate, lithium hydroxide, and lithium oxalate.

13. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The carbon source is selected from one or more of glucose, sucrose, starch, polyethylene glycol, graphene, and acetylene black.

14. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The doping modifier is a metal doping modifier and / or a non-metal doping modifier. The metal doping modifier is one or more of titanium dioxide, niobium pentoxide, ammonium metavanadate, magnesium oxide, and zirconium dioxide. The non-metal doping modifier is one or more of melamine, urea, and polyaniline.

15. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 3, characterized in that: The process parameters for spray drying are: inlet air temperature of 180-240℃, outlet air temperature of 90-110℃, and atomizer operating frequency of 35-45Hz.

16. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 4, characterized in that: The process parameters for spray drying are: inlet air temperature of 190-250℃, outlet air temperature of 95-120℃, and atomizer operating frequency of 35-45Hz.

17. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 5, characterized in that: The process parameters for spray drying are: inlet air temperature of 190-250℃, outlet air temperature of 95-120℃, and atomizer operating frequency of 35-45Hz.

18. The method for preparing high-pressure recycled lithium iron phosphate material from waste lithium iron phosphate powder according to claim 1, 2, 3, or 4, characterized in that: The process parameters for the airflow pulverization are as follows: the pulverization pressure is controlled at 0.2 to 0.3 MPa, the grading frequency is 35 to 40 Hz, and the pulverized particle size D50 is 1.0 to 1.5 μm.

19. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The roasting described in steps (2) and (3) is carried out in a rotary kiln.

20. The method for preparing high-pressure recycled lithium iron phosphate material using waste lithium iron phosphate powder according to claim 1, characterized in that: The equipment used for the secondary gradient sintering is a tube furnace or a box furnace, and the inert atmosphere is nitrogen or argon.

21. The application of high-pressure recycled lithium iron phosphate material in the positive electrode of lithium-ion power batteries or energy storage batteries, characterized in that: The high-pressure recycled lithium iron phosphate material is prepared by the method according to any one of claims 1-20.

22. The application of the high-pressure recycled lithium iron phosphate material according to claim 21 in the positive electrode of lithium-ion power batteries or energy storage batteries, characterized in that: The application is as the positive electrode active material of square aluminum-cased battery cells or energy storage battery cells.

Citation Information

Patent Citations

  • Method for recycling iron phosphate and lithium carbonate from lithium iron phosphate waste

    CN106450547A

  • Selective oxidation-reduction regeneration method of waste lithium iron phosphate, regenerated lithium iron phosphate and lithium ion battery

    CN113036253A

  • High-compaction high-performance lithium iron phosphate positive electrode material and preparation method thereof

    CN114497479A

  • Preparation method of lithium iron phosphate with high compaction density

    CN115092903A

  • Oxidation intermediate and application thereof

    CN120364760A