A method for in-situ co-formation of bicrystalline graded lithium manganese iron phosphate cathode material by single precursor dual-temperature induced co-existence
The method of forming bicrystalline nucleus-graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by single precursor at dual temperature solves the problems of uneven particle size distribution and high-temperature sintering in existing lithium manganese iron phosphate cathode materials, and achieves high pressure compaction and long cycle stability, making it suitable for large-scale production.
Patent Information
- Application Number
- CN202611619013.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing processes for preparing lithium manganese iron phosphate cathode materials suffer from problems such as uneven particle size distribution, poor material stability, low production efficiency, and high cost. In particular, impurity phases are easily generated during high-temperature sintering, leading to battery performance degradation.
A method for forming bicrystalline graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor at two temperatures is adopted. Through multi-stage calcination under an inert atmosphere and precise control of different temperature platforms, a symbiotic structure of large and ultrafine grains is formed, avoiding the drawbacks of high-temperature sintering.
It significantly improves the compaction density of the material and the volumetric energy density of the battery, enhances the fast-charging performance at higher rates, reduces the energy consumption of the preparation process, and enhances the phase purity and cycle stability of the material, making it suitable for large-scale production.
Smart Images

Figure CN123105592A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to methods for preparing cathode materials for lithium-ion batteries, and more particularly to a method for in-situ co-formation of bicrystalline graded lithium manganese iron phosphate cathode materials by dual-temperature induction of a single precursor. Background Technology
[0002] Lithium manganese iron phosphate (LMFP) combines high theoretical specific capacity, high operating voltage, low cost, and good safety performance, making it one of the core cathode materials for next-generation high-energy-density lithium-ion batteries. In industrial applications, material compaction density, phase purity, and cycle stability are key indicators restricting its electrochemical performance and mass production. To improve the material's packing density and rate performance, the industry commonly employs particle gradation technology to optimize the structure of LMFP.
[0003] Existing gradation modification technologies employ a dual-system independent preparation process, which involves separately preparing large-particle-size and small-particle-size precursor powders. These powders are then mechanically and physically mixed after separate milling, spraying, and sintering to obtain a composite material with varying particle sizes. This type of process essentially involves external powder composite formation rather than intrinsic particle structure control. The large and small particles are merely physically bonded, resulting in a break in the continuity of the interfacial carbon coating layer. This allows the electrolyte to easily penetrate and erode along the interface, inducing particle delamination and accelerated manganese ion dissolution during cycling, leading to poor structural stability. Furthermore, the sintering thermodynamic windows of the two powders differ, making it difficult to guarantee crystallization consistency. This results in high particle packing porosity and limited improvement in compaction density. In addition, the dual-slurry independent preparation process requires significant equipment investment, involves complex procedures, makes batch consistency difficult to control, and leads to high mass production costs.
[0004] Traditional high-temperature solid-state sintering and conventional segmented sintering processes rely on random homogeneous nucleation of free metal ions and phosphate ions. This process has a high nucleation barrier and a long induction period, requiring prolonged high-temperature holding to complete the crystal phase transformation. This method has two major drawbacks: first, the high activation energy of homogeneous nucleation and slow crystallization rate result in a long overall sintering cycle, high energy consumption, and low production efficiency; second, under the high-temperature, long-term sintering environment, free phosphate ions in the system are prone to deep thermal decomposition, generating low-valent phosphorus active intermediates. These intermediates react with free manganese and iron ions in the system, continuously generating MnP, FeP metal phosphides, and Mn2P2O7 pyrophosphate impurities. Furthermore, these impurities are irreversible defect phases that continuously catalyze electrolyte decomposition, disrupt electrode interface stability, and accelerate the dissolution of active metals, ultimately leading to rapid capacity decay and poor cycle stability of the battery. Summary of the Invention
[0005] Purpose of the invention: The technical problem to be solved by the present invention is to address the drawbacks of the traditional physical mixing and gradation method, and to provide a preparation process for lithium manganese iron phosphate cathode material, so as to achieve in-situ symbiotic formation of dual-nucleus graded lithium manganese iron phosphate cathode material to improve compaction, while avoiding the drawbacks of high-temperature sintering during the preparation process.
[0006] Technical solution: The present invention provides a method for in-situ co-formation of bicrystalline graded lithium manganese iron phosphate cathode material by dual-temperature induction using a single precursor, comprising the following steps:
[0007] (1) Manganese iron phosphate is mixed with manganese source, iron source, phosphorus source, lithium source and carbon source, and water, and then milled to form a slurry. The slurry is spray-dried to obtain spherical composite precursor powder. The total number of moles of manganese and iron provided by the manganese iron phosphate accounts for 40-60% of the total number of moles of manganese and iron in the theoretical lithium manganese iron phosphate cathode material.
[0008] (2) The composite precursor powder is placed in an inert atmosphere and calcined for 25-50 min at a first isothermal platform at 490-530℃, then calcined for 60-125 min at a second isothermal platform at 590-640℃, and finally calcined for 3-5 h at a third isothermal platform at 660-690℃ to obtain a dual-core graded lithium manganese iron phosphate cathode material.
[0009] Furthermore, in step (1) of this method, the manganese source is selected from at least one of manganese tetroxide, manganese carbonate or manganese oxalate, the iron source is selected from at least one of anhydrous ferric phosphate, ferrous carbonate, ferrous oxalate or iron tetroxide, and the phosphorus source is selected from at least one of anhydrous ferric phosphate, ammonium dihydrogen phosphate, ammonium monohydrogen phosphate or diammonium hydrogen phosphate.
[0010] Furthermore, the molar ratio of Mn to Fe in the lithium manganese iron phosphate cathode material prepared by this method is (5-7):(3-5), (Mn+Fe):P=1:(1.01~1.05), Li:(Mn+Fe)=(1.03~1.08):1; the molar ratio of Mn to Fe in the lithium manganese iron phosphate is (5-7):(3-5).
[0011] Furthermore, in step (1) of the method, the lithium source is selected from at least one of lithium carbonate, lithium oxalate, or lithium oxide.
[0012] Furthermore, in step (1) of this method, the carbon source is selected from at least one of sucrose, citric acid, glucose or polyethylene glycol, and its added mass is 10-15% of the total mass of manganese iron phosphate, manganese source, iron source, phosphorus source and lithium source.
[0013] Furthermore, in step (1) of this method, the solid content in the slurry is 40 wt%~55 wt%.
[0014] Furthermore, in step (1) of this method, the final particle size D50 of the sand mill is 0.3~0.8μm.
[0015] Furthermore, in step (1) of this method, the inlet air temperature of the spray dryer is 180-220 ℃ and the outlet air temperature is 80-110 ℃.
[0016] Furthermore, the method is characterized in that, in step (2), the heating rate of the first isothermal platform is 5~10℃ / min, and the heating rates of the second and third isothermal platforms are both 5~8℃ / min.
[0017] Beneficial effects: Compared with the prior art, the significant advantages of the present invention are:
[0018] (1) The lithium manganese iron phosphate cathode material prepared by this method has a dual-scale grain structure, and the compaction density of the finished product is stable at ≥2.50 g / cm³. 3 It significantly improves the volumetric energy density of the battery, has high compaction performance, and also takes into account high-rate fast charging performance;
[0019] (2) This method can significantly reduce the activation energy of secondary nucleation, shorten the nucleation induction period and sintering cycle, significantly reduce the overall energy consumption of preparation, greatly improve production efficiency, and is suitable for large-scale industrial mass production.
[0020] (3) The method can effectively avoid the formation of impurities such as MnP, FeP metal phosphides and Mn2P2O7 pyrophosphate during the preparation process, greatly improve the purity of the material phase, effectively inhibit the catalytic decomposition of electrolyte and the dissolution of manganese ions, and the capacity retention rate after 1000 cycles is significantly better than the existing process, and the long-term cycle stability is greatly optimized. Attached Figure Description
[0021] Figure 1 Here is a SEM image of the lithium iron phosphate cathode material from Example 1;
[0022] Figure 2 Here is a SEM image of the lithium iron phosphate cathode material from Example 2;
[0023] Figure 3 Here is a SEM image of the lithium iron phosphate cathode material in Comparative Example 1-1;
[0024] Figure 4 SEM images of lithium iron phosphate cathode materials in Comparative Examples 1-2;
[0025] Figure 5 SEM images of lithium iron phosphate cathode materials in Comparative Examples 1-3;
[0026] Figure 6 Here is a SEM image of the lithium iron phosphate cathode material in Comparative Example 2;
[0027] Figure 7 SEM image of lithium manganese iron phosphate cathode material in Comparative Example 3;
[0028] Figure 8 The image shows the SEM image of the lithium iron phosphate cathode material in Comparative Example 4. Detailed Implementation
[0029] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be noted that all raw materials used in the present invention are commercially available. The single precursor described in the present invention is ferromanganese phosphate, and the ferromanganese phosphate used in the following embodiments and comparative examples is Mn6Fe4PO4.
[0030] Example 1
[0031] The method for forming a dual-nucleus graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor at two temperatures in Example 1 includes the following steps:
[0032] (1) Based on the fact that the final Mn:Fe molar ratio of lithium manganese iron phosphate cathode material is 6:4 and the total number of manganese and iron moles provided by ferromanganese phosphate accounts for 50% of the total number of manganese and iron moles in the theoretical lithium manganese iron phosphate cathode material, the addition amounts of spherical ferromanganese phosphate, manganese tetroxide and anhydrous ferric phosphate are determined respectively.
[0033] (2) Weigh ammonium dihydrogen phosphate (for phosphorus supplementation) according to the ratio of (Mn+Fe):P = 1:1.03 in the lithium manganese iron phosphate cathode material, weigh lithium carbonate according to the ratio of Li:(Mn+Fe) = 1.05:1 in the system, and weigh sucrose according to the content of 12% of the total mass of manganese iron phosphate, manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate and lithium carbonate.
[0034] (3) Mix manganese iron phosphate, manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate, lithium carbonate, sucrose and water, and grind them together to form a homogeneous slurry with a solid content of 48 wt% and D50=0.8 μm. Spray dry the slurry at an inlet air temperature of 200℃ and an outlet air temperature of 90℃ to obtain spherical composite precursor powder.
[0035] (4) The composite precursor powder was placed in an inert atmosphere and calcined for 35 min at a first isothermal platform at 510℃ (heating rate of 8℃ / min), then calcined for 90 min at a second isothermal platform at 610℃ (heating rate of 8℃ / min), and finally calcined for 4 h at a third isothermal platform at 675℃ (heating rate of 8℃ / min) to obtain lithium manganese iron phosphate cathode material.
[0036] Example 2
[0037] Example 2 is basically the same as Example 1, except for the amount of spherical manganese ferric phosphate, manganese tetroxide, and anhydrous ferric phosphate added, as follows:
[0038] (1) Based on the fact that the final Mn:Fe molar ratio of lithium manganese iron phosphate cathode material is 6:4 and the total number of manganese and iron moles provided by ferromanganese phosphate accounts for 60% of the total number of manganese and iron moles in the theoretical lithium manganese iron phosphate cathode material, the addition amounts of spherical ferromanganese phosphate, manganese tetroxide and anhydrous ferric phosphate are determined respectively.
[0039] Comparative Example 1-1
[0040] The preparation method of the lithium manganese iron phosphate cathode material in Comparative Example 1-1 uses ferromanganese phosphate and lithium carbonate as raw materials for sintering, removes manganese tetroxide and anhydrous iron phosphate from the binary nucleation system, and adopts a conventional two-stage sintering process. The specific steps are as follows:
[0041] (1) According to the final Mn:Fe molar ratio of lithium manganese iron phosphate cathode material being 6:4, spherical manganese iron phosphate is weighed. At this time, the Mn:Fe molar ratio of spherical manganese iron phosphate is 6:4.
[0042] (2) Weigh ammonium dihydrogen phosphate (for phosphorus supplementation) according to the ratio of (Mn+Fe):P = 1:1.03 in the lithium manganese iron phosphate cathode material, weigh lithium carbonate according to the ratio of Li:(Mn+Fe) = 1.05:1 in the system, and weigh sucrose according to the content of 12% of the total mass of manganese iron phosphate, ammonium dihydrogen phosphate and lithium carbonate.
[0043] (3) Mix manganese iron phosphate, ammonium dihydrogen phosphate, lithium carbonate, sucrose and water, and grind them together to form a homogeneous slurry with a solid content of 48wt% and D50=0.8 μm. Spray dry the slurry at an inlet air temperature of 200℃ and an outlet air temperature of 90℃ to obtain spherical composite precursor powder.
[0044] (4) The composite precursor powder was placed in an inert atmosphere and calcined for 125 min at a second isothermal platform at 610℃ (heating rate of 8℃ / min), and finally calcined for 4 h at a third isothermal platform at 675℃ (heating rate of 8℃ / min) to obtain lithium manganese iron phosphate cathode material.
[0045] Comparative Examples 1-2
[0046] The comparative example 1-2 describes a method for preparing lithium manganese iron phosphate cathode materials using conventional quaternary raw materials through stepwise sintering. The specific steps are as follows:
[0047] (1) Weigh out manganese tetroxide and anhydrous iron phosphate according to the molar ratio of Mn:Fe of lithium manganese iron phosphate cathode material as 6:4;
[0048] (2) Weigh ammonium dihydrogen phosphate according to the ratio of (Mn+Fe):P = 1:1.03 in the lithium manganese iron phosphate cathode material, weigh lithium carbonate according to the ratio of Li:(Mn+Fe) = 1.05:1 in the system, and weigh sucrose according to the content of 12% of the total mass of manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate and lithium carbonate.
[0049] (3) Manganese tetroxide, anhydrous ferric phosphate, ammonium dihydrogen phosphate, lithium carbonate, sucrose and water are mixed and ground in an integrated sand mill to prepare a homogeneous slurry with a solid content of 48 wt% and D50=0.8 μm; the slurry is spray-dried at an inlet air temperature of 200℃ and an outlet air temperature of 90℃ to obtain spherical composite precursor powder.
[0050] (4) The composite precursor powder was placed in an inert atmosphere and calcined for 35 min at a first isothermal platform at 510℃ (heating rate of 8℃ / min), then calcined for 90 min at a second isothermal platform at 610℃ (heating rate of 8℃ / min), and finally calcined for 4 h at a third isothermal platform at 675℃ (heating rate of 8℃ / min) to obtain lithium manganese iron phosphate cathode material.
[0051] Comparative Examples 1-3
[0052] Comparative Examples 1-3 are basically the same as Example 1, except that they use a conventional two-stage sintering process. The specific steps are as follows:
[0053] (1) Based on the fact that the final Mn:Fe molar ratio of lithium manganese iron phosphate cathode material is 6:4 and the total number of manganese and iron moles provided by ferromanganese phosphate accounts for 50% of the total number of manganese and iron moles in the theoretical lithium manganese iron phosphate cathode material, the addition amounts of spherical ferromanganese phosphate, manganese tetroxide and anhydrous ferric phosphate are determined respectively.
[0054] (2) Weigh ammonium dihydrogen phosphate (for phosphorus supplementation) according to the ratio of (Mn+Fe):P = 1:1.03 in the lithium manganese iron phosphate cathode material, weigh lithium carbonate according to the ratio of Li:(Mn+Fe) = 1.05:1 in the system, and weigh sucrose according to the content of 12% of the total mass of manganese iron phosphate, manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate and lithium carbonate.
[0055] (3) Mix manganese iron phosphate, manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate, lithium carbonate, sucrose and water, and grind them together to form a homogeneous slurry with a solid content of 48 wt% and D50=0.8 μm. Spray dry the slurry at an inlet air temperature of 200℃ and an outlet air temperature of 90℃ to obtain spherical composite precursor powder.
[0056] (4) The composite precursor powder was placed in an inert atmosphere and calcined for 125 min at a second isothermal platform at 610℃ (heating rate of 8℃ / min), and finally calcined for 4 h at a third isothermal platform at 675℃ (heating rate of 8℃ / min) to obtain lithium manganese iron phosphate cathode material.
[0057] Comparative Example 2
[0058] Comparative Example 2 is basically the same as Example 2, except that it uses a conventional two-stage sintering process. The specific steps are as follows:
[0059] (1) Based on the fact that the final Mn:Fe molar ratio of lithium manganese iron phosphate cathode material is 6:4 and the total number of manganese and iron moles provided by ferromanganese phosphate accounts for 60% of the total number of manganese and iron moles in the theoretical lithium manganese iron phosphate cathode material, the addition amounts of spherical ferromanganese phosphate, manganese tetroxide and anhydrous ferric phosphate are determined respectively.
[0060] (2) Weigh ammonium dihydrogen phosphate (for phosphorus supplementation) according to the ratio of (Mn+Fe):P = 1:1.03 in the lithium manganese iron phosphate cathode material, weigh lithium carbonate according to the ratio of Li:(Mn+Fe) = 1.05:1 in the system, and weigh sucrose according to the content of 12% of the total mass of manganese iron phosphate, manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate and lithium carbonate.
[0061] (3) Mix manganese iron phosphate, manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate, lithium carbonate, sucrose and water, and grind them together to form a homogeneous slurry with a solid content of 48 wt% and D50=0.8 μm. Spray dry the slurry at an inlet air temperature of 200℃ and an outlet air temperature of 90℃ to obtain spherical composite precursor powder.
[0062] (4) The composite precursor powder was placed in an inert atmosphere and calcined for 125 min at a second isothermal platform at 610℃ (heating rate of 8℃ / min), and finally calcined for 4 h at a third isothermal platform at 675℃ (heating rate of 8℃ / min) to obtain lithium manganese iron phosphate cathode material.
[0063] Comparative Example 3
[0064] The comparative example is basically the same as Example 1, except that the total number of moles of manganese and iron provided by ferromanganese phosphate accounts for 30% of the total number of moles of manganese and iron in the theoretical lithium manganese iron phosphate cathode material.
[0065] Comparative Example 4
[0066] The comparative example is basically the same as Example 1, except that the total number of moles of manganese and iron provided by ferromanganese phosphate accounts for 70% of the total number of moles of manganese and iron in the theoretical lithium manganese iron phosphate cathode material.
[0067] Performance testing
[0068] The compaction density of lithium manganese iron phosphate cathode material was tested according to GBT30835-2014 using a PRCD1100 powder compaction testing device; the results are shown in Table 1.
[0069] The lithium manganese iron phosphate cathode materials obtained in the above examples and comparative examples were used to prepare coin cells and their electrochemical performance was evaluated using the following method: Lithium manganese iron phosphate cathode material, Super P (conductive carbon black), and PVDF were uniformly mixed in an NMP solution at a ratio of 90:5:5 to obtain a mixed slurry. The slurry was applied to bright aluminum foil by hand and then dried at 100°C. After the NMP had completely evaporated, the electrode sheet was cut into electrode sheets with a diameter of 13 mm. The electrode sheets were then dried overnight at 105°C in a vacuum oven. After weighing the electrode sheets, they were quickly transferred to a glove box. Lithium metal was used as the counter electrode, Celgard 2400 was used as the separator, and the electrolyte was 1 mol / L. The assembled battery was prepared by dissolving LiPF6 in a mixed solvent of EC / DMC / EMC (volume ratio 1:1:1). Electrochemical performance was tested using the Xinwei testing system, employing constant current-constant voltage charging (CC-CV) and constant current discharging (DC) methods to analyze the charge and discharge behavior of the coin cell. The test voltage range was 2.0-4.35V.
[0070] Table 1. Cathode Material Performance Data
[0071]
[0072] As can be seen from the data in Examples 1 and 2 of Table 1, the compacted density of lithium manganese iron phosphate powder prepared by the process of the present invention can reach 2.53-2.55 g / cm³. 3 It exhibits a high reversible specific capacity of 142 mAh / g at 1C and 153 mAh / g at 0.1C, with a capacity retention rate of 92.1% after 1000 cycles, demonstrating excellent electrochemical cycling stability.
[0073] Meanwhile, the structure of the cathode materials prepared in Examples 1-2 of this invention was characterized, and the results obtained are as follows: Figure 1-2 As shown. From this Figure 1-2It is known that the lithium manganese iron phosphate systems in Examples 1 and 2 exhibit two types of controllable-scale primary grains. Measurements show that the large grain size ranges from 200 to 400 nm, while the ultrafine filled grain size ranges from 30 to 80 nm. The ultrafine grains are uniformly and discretely embedded in the intergranular gaps of the large grains, without regional agglomeration of ultrafine grains or continuous large pores formed by the accumulation of large grains, achieving an intrinsically graded filling structure for single particles. Furthermore, the lithium manganese iron phosphate grains in Examples 1 and 2 have rounded and regular contours, smooth and dense crystal surfaces, and a continuous and complete integrated carbon coating layer without cracks or peeling defects. The large and small grains coexist through sequential crystallization within the same precursor microsphere, with high fusion at the two-phase interface and no obvious phase separation boundaries caused by physical mixing. In addition, it can also be achieved through... Figure 1 and Figure 2 The microstructure shows that there are no flocculent or dot-like phosphide impurity crystals or agglomerates throughout the entire area, the grain size distribution range is narrow, and there are no abnormally large grains or nano-impurity flocs.
[0074] The performance data for Comparative Example 1-1 are shown in Table 1, and the morphology is as follows: Figure 3 As shown, there are numerous interconnected open pores between the grains, resulting in loose powder packing and microscopic packing, with a compaction density of only 2.42 g / cm³. 3 The single large-grain structure results in a long lithium-ion diffusion path and inherent shortcomings in rate electrochemical performance.
[0075] The performance data of Comparative Examples 1-2 are shown in Table 1, and their morphologies are as follows: Figure 4 As shown, in Comparative Examples 1-2, the process did not include manganese iron phosphate. Using manganese tetroxide, anhydrous iron phosphate, ammonium dihydrogen phosphate, and lithium carbonate as raw materials, the final prepared lithium manganese iron phosphate cathode material had a compaction density of only 2.24 g / cm³. 3 The capacity retention rate after 1000 cycles was only 81.5%, and Figure 4 The medium-sized and irregular grains exhibit severe agglomeration of smaller particles. Small particle size results in a large specific surface area, numerous reactive sites, and a large contact area with the electrolyte, making them prone to side reactions, exacerbating Mn dissolution, and leading to poor cycle performance.
[0076] The performance data of comparative examples 1-3 are shown in Table 1, and their morphologies are as follows: Figure 5 As shown, although Comparative Examples 1-3 fully configured the dual-system nucleation materials, the first isothermal platform for the 490-530 ℃ low-temperature seed preparation was omitted, and instead... Figure 5 It can be seen that the grains are significantly adhered, the packing density is greatly reduced, and the compacted density is only 2.36 g / cm³. 3 .
[0077] The performance data of Comparative Example 2 are shown in Table 1, and the morphology is as follows: Figure 6As shown, Comparative Example 2 also fully configured the dual-system nucleation raw materials, but the first isothermal platform for the 490-530 ℃ low-temperature seed preparation was omitted, and instead... Figure 6 It can be seen that the grains are significantly aggregated, the packing density is greatly reduced, and the compacted density is only 2.34 g / cm³. 3 .
[0078] The performance data of Comparative Example 3 are shown in Table 1, and the morphology is as follows: Figure 7 As shown, Comparative Example 3 also features a complete dual-system nucleation material configuration, but the total molar number of manganese and iron provided by ferromanganese phosphate accounts for 30% of the total molar number of manganese and iron in the theoretical lithium manganese iron phosphate cathode material. Figure 7 It can be seen that as the proportion of small particles increases and the proportion of large particles decreases, the gradation effect weakens, the compaction density decreases, and the circulation performance deteriorates.
[0079] The performance data of Comparative Example 4 are shown in Table 1, and the morphology is as follows: Figure 8 As shown, Comparative Example 4 also has a complete dual-system nucleation material configuration, but the total molar number of manganese and iron provided by ferromanganese phosphate accounts for 70% of the total molar number of manganese and iron in the theoretical lithium manganese iron phosphate cathode material. Figure 8 It can be seen that as the proportion of large particles increases and the proportion of small particles decreases, the gradation effect weakens, the compaction density decreases, the proportion of large particles increases, the lithium-ion transport path becomes longer, and the electrical performance deteriorates.
[0080] Based on the above structural and performance analysis, the further analysis of the mechanism is that the present invention combines ferromanganese phosphate, which has the same olivine structure as lithium manganese iron phosphate cathode material, with manganese source, lithium source, iron source, phosphorus source and carbon source, and adopts a sintering temperature gradient formed by a first isothermal platform of low temperature 490-530℃, a second isothermal platform of 590-640℃ and a third high temperature isothermal platform of 660-690℃. In this way, during the sintering process, ferromanganese phosphate and lithium source are pre-formed as the main body for large-size grain nucleation and induced crystal nuclei. Manganese tetroxide, anhydrous ferric phosphate and lithium source react to form the main body for ultrafine grain nucleation. Ammonium dihydrogen phosphate precisely replenishes the phosphorus element in the fine grain system. Combined with the dual-temperature time-series differentiated crystallization technology, namely the low temperature first isothermal platform and the high temperature second isothermal platform, the present invention realizes the in-situ generation of dual-scale grain symbiotic structure inside a single precursor microsphere.
[0081] Specifically, the first constant temperature platform insulation zone at low temperature is the low-temperature in-situ seed crystal pre-preparation stage. This temperature is strictly below the activation threshold of the fine-grained system. This temperature range is the exclusive homogeneous epitaxial nucleation window for the large-grained system, thus only completing the seed crystal pre-preparation. That is, the reaction of manganese iron phosphate with lithium, which has the same olivine structure as the lithium manganese iron phosphate cathode material, precipitates olivine seeds in-situ inside the precursor, forming a continuous and stable seed crystal framework, without the precipitation of ultrafine grains generated by the reaction of manganese source, lithium source, iron source, and phosphorus source, thus achieving precise isolation of the crystallization sequence.
[0082] The high-temperature second isothermal platform's holding zone features a dedicated high-temperature reaction window that triggers ultrafine grain heterogeneous nucleation and growth at the interstitial sites of the large-grain framework. Specifically, manganese tetroxide, anhydrous iron phosphate, and lithium carbonate react to generate ultrafine grains that fill the spaces between the grain framework. Simultaneously, the seed crystal framework continues to grow, ultimately forming a primary dense gradation structure of "large-grain framework + ultrafine grain interstitial filling" within the intact single particle. Furthermore, the pre-formed olivine seed crystal has a high lattice matching degree with the target product, lithium manganese iron phosphate, which can transform high-barrier homogeneous nucleation into low-barrier heterogeneous nucleation, significantly reducing the activation energy for secondary fine-grain nucleation, greatly shortening the nucleation induction period and overall sintering holding time, effectively reducing preparation energy consumption and improving production efficiency. Simultaneously, the seed crystal pre-formed in situ in the first isothermal platform zone possesses excellent ion adsorption and immobilization capabilities, rapidly capturing free Mn within the system. 2+ Fe 3+ PO4 3- Plasma promotes the orderly reconstruction of the olivine phase by free ions on the seed crystal surface, significantly reducing the concentration of free ions in the system. It inhibits the deep thermal decomposition of phosphate from the source of the reaction, eliminates the formation of low-valent phosphorus intermediates, completely avoids the precipitation of MnP, FeP metal phosphides and pyrophosphate impurities, and greatly improves the phase purity and electrochemical stability of the material.
[0083] This mechanism is also directly confirmed by the microstructure of the lithium manganese iron phosphate cathode material in Example 1, which demonstrates a dual mechanism: the olivine seed crystals pre-fabricated on the first heating platform serve as low-barrier nucleation sites, allowing ions to be oriented and orderly reconstructed on the seed crystal surface, resulting in uniform and controllable grain growth and eliminating the size polarization caused by random homogeneous nucleation in seedless systems. The mutual filling of dual-scale grains significantly reduces the powder packing porosity, corresponding to a powder compaction density of 2.53 g / cm³. 3 This is the optimal sample in this group.
[0084] In contrast, the Comparative Example 1-1 system did not introduce fine-crystal nucleation precursors such as Mn3O4, anhydrous FePO4, and ammonium dihydrogen phosphate, relying solely on a single homogeneous epitaxial nucleation pathway, thus failing to construct a dual-scale in-situ symbiotic structure. The Comparative Example 1-2 process lacked a low-temperature olivine seed preparation step, relying entirely on random homogeneous nucleation by free ions at high potential barriers. This resulted in a long nucleation induction period, requiring prolonged high-temperature holding. Under high-temperature conditions, free phosphate ions underwent deep thermal decomposition to generate low-valent phosphorus reactive intermediates, which reacted with transition metal ions to precipitate phosphide impurities. Ion diffusion lacked directional constraint, leading to disordered grain growth, agglomeration, and high powder porosity. Although Comparative Examples 1-3 were equipped with complete dual-system nucleation materials, the first isothermal platform of the 490-530 ℃ low-temperature seed crystal pre-preparation was cancelled, and there were no pre-prepared heterogeneous nucleation sites for olivine. The fine-grained components underwent high-barrier homogeneous nucleation, and the grain growth sequence was disordered. Some grains were excessively Oswald ripened and coarsened, and the ultrafine grains agglomerated irregularly, failing to uniformly fill the gaps between large grains. Local voids and local fine-grained agglomerates coexisted.
[0085] In summary, this invention constructs two nucleation systems with different thermodynamic properties within a single-particle system through precise design of precursor components, and achieves separation of crystallization time by relying on precise dual-temperature control.
[0086] In addition to the above embodiments, it should be noted that the process and parameter conditions defined by the present invention can achieve the technical effects claimed above, and therefore no further experimental verification is required.
Claims
1. A method for preparing a double-crystal core-sized lithium manganese iron phosphate cathode material by single precursor double-temperature induced in-situ symbiotic formation, characterized in that, Includes the following steps: (1) Manganese iron phosphate is mixed with manganese source, iron source, phosphorus source, lithium source and carbon source, and water, and then milled to form a slurry. The slurry is spray-dried to obtain spherical composite precursor powder. The total number of moles of manganese and iron provided by the manganese iron phosphate accounts for 40-60% of the total number of moles of manganese and iron in the theoretically generated lithium manganese iron phosphate cathode material. (2) The composite precursor powder is placed in an inert atmosphere and calcined for 25-50 min at a first isothermal platform at 490-530℃, then calcined for 60-125 min at a second isothermal platform at 590-640℃, and finally calcined for 3-5 h at a third isothermal platform at 660-690℃ to obtain a dual-core graded lithium manganese iron phosphate cathode material.
2. The method for in-situ symbiotic formation of double crystal nucleus graded lithium iron manganese phosphate cathode material by single precursor double temperature induction according to claim 1, characterized in that, The manganese source is selected from at least one of manganese tetroxide, manganese carbonate, or manganese oxalate; the iron source is selected from at least one of anhydrous ferric phosphate, ferrous carbonate, ferrous oxalate, or ferric tetroxide; and the phosphorus source is selected from at least one of anhydrous ferric phosphate, ammonium dihydrogen phosphate, ammonium monohydrogen phosphate, or diammonium hydrogen phosphate.
3. The method for in-situ symbiotic formation of double crystal nucleus graded lithium iron manganese phosphate cathode material by single precursor double temperature induction according to claim 1, characterized in that, The molar ratio of Mn to Fe in the lithium manganese iron phosphate cathode material is (5-7):(3-5), the molar ratio of (Mn+Fe):P is 1:(1.01~1.05), and the molar ratio of Li:(Mn+Fe) is (1.03~1.08):1; the molar ratio of Mn to Fe in the lithium manganese iron phosphate is (5-7):(3-5).
4. The method for forming a double crystal nucleus graded lithium iron manganese phosphate cathode material by single precursor and double temperature induced in-situ symbiosis according to claim 1, characterized in that, In step (1), the lithium source is selected from at least one of lithium carbonate, lithium oxalate or lithium oxide.
5. The method for forming a dual-nucleus graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor under dual-temperature conditions according to claim 1, characterized in that, In step (1), the carbon source is selected from at least one of sucrose, citric acid, glucose or polyethylene glycol, and its added mass is 10-15% of the total mass of manganese iron phosphate, manganese source, iron source, phosphorus source and lithium source.
6. The method for forming a dual-nucleus graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor under dual-temperature conditions according to claim 1, characterized in that, In step (1), the solid content in the slurry is 40 wt%~55 wt%.
7. The method for forming a dual-nucleus graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor under dual-temperature conditions according to claim 1, characterized in that, In step (1), the final particle size D50 of the sand mill is 0.3~0.8 μm.
8. The method for forming a dual-nucleus graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor under dual-temperature conditions according to claim 1, characterized in that, In step (1), the inlet air temperature of the spray dryer is 180-220 ℃ and the outlet air temperature is 80-110 ℃.
9. The method for forming a dual-nucleus graded lithium manganese iron phosphate cathode material by in-situ symbiosis induced by a single precursor under dual-temperature conditions according to claim 1, characterized in that, In step (2), the heating rate of the first isothermal platform is 5~10 ℃ / min, and the heating rates of the second and third isothermal platforms are both 5~8 ℃ / min.