Preparation method and application of a low-expansion, high-power silicon-carbon composite anode material

By doping boron and lithium into MOF materials and depositing solid electrolyte and amorphous carbon on the surface of silicon-carbon composite materials, the problems of poor conductivity and large expansion of existing silicon-carbon composite materials are solved, realizing high-power and low-expansion silicon-carbon composite materials and improving the performance of lithium-ion batteries.

CN123105598APending Publication Date: 2026-11-17HUIYANG (GUIZHOU) NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611194493.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicon-carbon composite materials suffer from poor electronic conductivity and poor binding force of dopants, resulting in limited improvement in power performance. Furthermore, porous carbon has small pore volume, low compressive strength, and large expansion, which affects cycle performance.

Method used

Using MOF materials as the matrix, boron and lithium are doped into porous carbon by vapor deposition to form a bridging structure, depositing nano-silicon and heteroatoms, and depositing solid electrolyte and amorphous carbon on the outer layer to improve the electronic and ionic conductivity of the material. A bilayer structure is formed by atomic vapor deposition to confine the core expansion.

Benefits of technology

The material's electronic conductivity and lithium-ion diffusion rate were improved, while the powder resistivity and expansion rate were reduced, resulting in improved initial efficiency and cycle performance. The specific surface area and lithium-ion diffusion coefficient of the material were significantly increased.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105598A_ABST
    Figure CN123105598A_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery materials technology, specifically to a method for preparing and applying a low-expansion, high-power silicon-carbon composite anode material. Using MOF material as a matrix, borane gas, metal gas, and peroxide crosslinking agent gas are sequentially introduced under negative pressure. Nano-silicon is then deposited in the pores via silane pyrolysis, and finally, inorganic lithium salt and carbon source gas are deposited on its surface using ALD technology. The resulting material incorporates boron to reduce bulk defects and improve structural stability; metal doping enhances the electronic conductivity; and the crosslinking gas further improves structural stability. The outer layer is coated with lithium salt and amorphous carbon to enhance both ionic and electronic conductivity. When applied to lithium-ion batteries, the resulting material exhibits low expansion and high power performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery materials technology, specifically to a method for preparing and applying a low-expansion, high-power silicon-carbon composite anode material. Background Technology

[0002] The current novel silicon-carbon materials are mainly composed of porous carbon and nano-silicon deposited in the pores. The difference in electronic conductivity causes deviations in the power performance of these materials.

[0003] Although some researchers have improved the electronic conductivity of porous carbon by doping it with metals or non-metals, the volatilization of dopant elements during high-temperature carbonization has resulted in limited doping effectiveness. This is because the doping of materials is carried out under different temperature and other conditions, leading to poor doping uniformity and weak bonding between the dopant and the host element, thus limiting the improvement in power performance. Furthermore, porous carbon prepared using current resin-based or biomass-based materials suffers from small pore volume and low compressive strength, resulting in significant material expansion and reduced cycle performance.

[0004] Therefore, to address the shortcomings of the existing technologies, our research team has developed a low-expansion, high-power silicon-carbon composite anode material preparation process. Summary of the Invention

[0005] To address the aforementioned deficiencies in the existing technology, the purpose of this invention is to provide a method for preparing and applying low-expansion, high-power silicon-carbon composite anode materials.

[0006] One objective of this invention is to provide a method for preparing a low-expansion, high-power silicon-carbon composite anode material, comprising the following steps: Step S1: Transfer the MOF material to a fluidized bed as a matrix, evacuate to ≤10Pa, heat to 600-800℃, introduce borane gas for 30-300min, then heat to 1000-1500℃, introduce lithium source gas for 30-300min, finally cool to 300-600℃, introduce peroxide crosslinking agent gas for 10-60min, and allow to cool naturally to room temperature to obtain a porous carbon precursor material. The ratio of MOF material:borane gas:lithium source gas:peroxide crosslinking gas = 10g:0.3-30L:0.3-30L:0.1-6L. Step S2: Transfer the porous carbon precursor material to a fluidized bed, introduce inert gas to purge the air from the tube, heat to 600-700℃, and simultaneously introduce silane gas and heteroatom mixed gas at a flow rate of 100-500 SCCM for 30-300 min to obtain silicon-carbon precursor material. The ratio of porous carbon precursor to heteroatom mixed gas is 200 g: 3-150 L, and the volume ratio of silane gas to heteroatom gas in the heteroatom mixed gas is 10:1-5. Step S3: Transfer the silicon-carbon precursor material into a vacuum chamber as a substrate, use the solid electrolyte as a target, and deposit the solid electrolyte on the surface of the silicon-carbon precursor material by atomic vapor deposition to obtain a solid electrolyte-coated porous silicon-carbon composite. Step S4: The solid electrolyte-coated porous silicon-carbon composite is transferred to a tube furnace by atomic vapor deposition. The air inside the tube is vented, and the furnace is heated to 800-1100°C. A carbon source mixed gas is introduced for 60-600 min, and the furnace is cooled to room temperature under an inert atmosphere to obtain the silicon-carbon composite material. The ratio of solid electrolyte-coated porous silicon-carbon composite to carbon source mixed gas is 100 g to 0.6-30 L, and the volume ratio of carbon source gas to nitrogen in the carbon source mixed gas is 10:1-3.

[0007] Further, in step S1, the MOF material is one of ZIF-8, MOF-808, ZIF-67, MOF-818, MOF-74, MOF-545, and MIL-101(Cr); the borane gas is one of diborane, triphenylborane, triethoxyborane, trimethoxyborane, and dimethylamineborane, which are generated by sublimation upon heating; the lithium source gas is lithium hydride, which is generated by sublimation upon heating; and the peroxide crosslinking agent gas is one of peracetic acid, peroxyethyl ether, peroxybenzoic acid, and benzoyl peroxide, which are generated by sublimation upon heating.

[0008] Furthermore, in step S1, the flow rates of borane gas, lithium source gas, and peroxide crosslinking agent gas are 10-100 SCCM.

[0009] Furthermore, in step S2, the silicon source is one of silane, silane, dichlorosilane, or trichlorosilane; the heteroatom gas is one of hydrogen sulfide, ammonia, phosphine, or dinitrogen tetrahydride.

[0010] Furthermore, the solid electrolyte in step S3 is... , , , , , , One of them, the , 0 < x ≤ 1, the , 0 < x < 2, 0 < y < 3.

[0011] Furthermore, the atomic vapor deposition method specifically includes: The solid electrolyte material was deposited as a target for 1 second, purged with nitrogen for 60 seconds, introduced with an oxygen source for 5 seconds, purged with nitrogen for 5 seconds, introduced with water for 0.05 seconds, and purged with nitrogen for 50 seconds. Repeat the above steps 10-100 times.

[0012] Atomic vapor deposition (AVD) involves the decomposition of multiple elements under the same conditions, which can be uniformly and densely deposited on a substrate. It features process controllability, good uniformity, and the formation of compounds between deposited elements, thereby improving the structural stability of the material. It also has the advantages of a high ion diffusion coefficient.

[0013] Furthermore, in step S4, the carbon source is one of ethylene, acetylene, methane, ethane, propane, and cyclohexane.

[0014] Furthermore, in step S4, the flow rate of the carbon source mixed gas is 10-50 SCCM.

[0015] Another objective of this invention is to provide an application of a low-expansion, high-power silicon-carbon composite anode material, which is used in lithium-ion batteries.

[0016] The beneficial effects of this invention are: 1. The method of the present invention uses MOF material as a matrix and deposits boron and lithium elements in its large pores by vapor deposition to improve the electronic and ionic conductivity of the material. The resistivity of the powder is less than 1 Ω·cm. Furthermore, a crosslinking agent is used to form a bridging structure between carbon atoms and between carbon atoms and heteroatoms, thereby improving the strength of the pores.

[0017] 2. The specific surface area of ​​the material prepared by the method of this invention is 2.34-3.77. Nano-silicon and heteroatoms are co-deposited in a porous carbon precursor. The nano-silicon enhances the specific capacity of the core, while the heteroatoms improve the electronic conductivity of the core. Furthermore, the heteroatoms fill the spaces between the nano-silicon nanoparticles, reducing porosity and improving lithium-ion diffusion rate and electronic conductivity, thus enhancing initial efficiency. The lithium-ion diffusion coefficient ranges from 4.21 to 9.88. , The efficiency of the button cell was improved to 95% for the first time in testing.

[0018] 3. Solid electrolyte and amorphous carbon are deposited sequentially on the outer layer to improve the ion diffusion coefficient and electronic conductivity of the material. At the same time, the double-layer structure of the material restricts the expansion of the core nano-silicon during charging and discharging, thereby improving cycle performance. The full-charge expansion of the coin cell is as low as 65.3%, and the cycle performance of the pouch cell is improved to 93.15%. Attached Figure Description

[0019] Figure 1 The image shown is a SME diagram of the silicon-carbon material prepared in Example 1 of this invention. Detailed Implementation

[0020] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention.

[0021] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0022] Example 1

[0023] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of ZIF-8 material to a fluidized bed as the matrix, evacuate to 1Pa, then heat to 700℃, and introduce diborane gas at a flow rate of 50SCCM for 150min. Then heat to 1200℃ and introduce lithium hydride gas at a flow rate of 50SCCM for 150min. Finally, cool down to 450℃ and introduce peracetic acid gas at a flow rate of 50SCCM for 30min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce nitrogen inert gas to purge the air from the tube. Then, raise the temperature to 650℃ and simultaneously introduce a mixture of silane gas and hydrogen sulfide gas (volume ratio: silane gas: hydrogen sulfide gas = 10:3) at a flow rate of 300 SCCM for 150 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit the material as a target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 50 times from step ① to deposit the silicon-carbon precursor material on its surface. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was vented and the furnace was heated to 900°C. Ethylene mixed gas (volume ratio, ethylene gas: nitrogen = 10:2) was introduced at a flow rate of 30 SCCM for 300 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0024] Example 2

[0025] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of MOF-808 material to a fluidized bed as the matrix, evacuate to 1Pa, then heat to 600℃, and introduce triphenylborane gas at a flow rate of 10SCCM for 300min. Then heat to 1000℃ and introduce lithium hydride gas at a flow rate of 10SCCM for 300min. Finally, cool down to 300℃ and introduce peroxyethyl ether gas at a flow rate of 10SCCM for 60min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce nitrogen inert gas to purge the air in the tube. Then, raise the temperature to 600℃ and simultaneously introduce a mixture of silane gas and ammonia gas (volume ratio, silane gas: ammonia gas = 10:1) at a flow rate of 100 SCCM for 300 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit the material as a target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 10 times from step ① to deposit the silicon-carbon precursor material on its surface. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was vented and the furnace was heated to 800°C. Acetylene mixed gas (volume ratio: acetylene:nitrogen = 10:1) was introduced at a flow rate of 10 SCCM for 600 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0026] Example 3

[0027] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of ZIF-67 material to a fluidized bed as the matrix, evacuate to 1Pa, then heat to 800℃, and introduce triethoxyborane gas at a flow rate of 100SCCM for 30min. Then heat to 1500℃ and introduce lithium hydride gas at a flow rate of 100SCCM for 30min. Finally, cool down to 600℃ and introduce benzoyl peroxide gas at a flow rate of 100SCCM for 10min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce an inert gas to purge the air from the tube. Then, raise the temperature to 680℃ and simultaneously introduce a mixture of trichlorosilane gas and dinitrogen tetrahydride gas (volume ratio: trichlorosilane gas: dinitrogen tetrahydride gas = 10:5) at a flow rate of 450 SCCM for 100 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit material as target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen source for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 60 times from step ① to deposit on the surface of its silicon-carbon precursor material. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was purged and the furnace was heated to 1000°C. Ethane mixed gas (volume ratio: ethane:nitrogen = 10:3) was introduced at a flow rate of 50 SCCM for 60 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0028] Example 4

[0029] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of MOF-818 material to a fluidized bed as the matrix, evacuate to 1.5Pa, then heat to 700℃, and introduce trimethoxyborane gas at a flow rate of 90SCCM for 90min. Then heat to 1400℃ and introduce lithium hydride gas at a flow rate of 90SCCM for 30min. Finally, cool down to 500℃ and introduce peroxybenzoic acid gas at a flow rate of 90SCCM for 20min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce an inert gas to purge the air from the tube. Then, raise the temperature to 700℃ and simultaneously introduce a mixture of dichlorosilane gas and phosphine gas (volume ratio: dichlorosilane gas: phosphine gas = 10:5) at a flow rate of 500 SCCM for 30 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit the material as a target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 100 times from step ① to deposit the silicon-carbon precursor material on its surface. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was vented and the furnace was heated to 1100°C. A methane mixed gas (volume ratio: methane:nitrogen = 10:3) was introduced at a flow rate of 50 SCCM for 60 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0030] Example 5

[0031] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of MOF-74 material to a fluidized bed as the matrix, evacuate to 2Pa, then heat to 750℃, and introduce dimethylamine borane gas at a flow rate of 140SCCM for 90min. Then heat to 1400℃ and introduce lithium hydride gas at a flow rate of 150SCCM for 30min. Finally, cool down to 500℃ and introduce peroxybenzoic acid gas at a flow rate of 160SCCM for 20min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce an inert gas to purge the air from the tube. Then, raise the temperature to 680℃ and simultaneously introduce a mixture of dichlorosilane gas and phosphine gas (volume ratio: dichlorosilane gas: phosphine gas = 10:5) at a flow rate of 400 SCCM for 30 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit the material as a target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 100 times from step ① to deposit the silicon-carbon precursor material on its surface. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was vented and the furnace was heated to 1100°C. A mixture of propane gas (volume ratio: propane: nitrogen = 10:3) was introduced at a flow rate of 40 SCCM for 500 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0032] Example 6

[0033] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of MOF-545 material to a fluidized bed as the matrix, evacuate to 10Pa, then heat to 750℃, and introduce dimethylamine borane gas at a flow rate of 260SCCM for 200min. Then heat to 1400℃ and introduce lithium hydride gas at a flow rate of 260SCCM for 200min. Finally, cool down to 500℃ and introduce peroxybenzoic acid gas at a flow rate of 260SCCM for 40min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce an inert gas to purge the air from the tube. Then, raise the temperature to 620℃ and simultaneously introduce a mixture of silane gas and phosphine gas (volume ratio: silane gas: phosphine gas = 10: 5) at a flow rate of 200 SCCM for 30 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit the material as a target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 70 times from step ① to deposit the silicon-carbon precursor material on its surface. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was vented and the furnace was heated to 900°C. A cyclohexane mixed gas (volume ratio of cyclohexane gas to nitrogen gas = 10:3) was introduced at a flow rate of 30 SCCM for 400 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0034] Example 7

[0035] A method for preparing a low-expansion, high-power silicon-carbon composite anode material includes the following steps: Step S1: Transfer 10g of MIL-101(Cr) material to a fluidized bed as the matrix, evacuate to 5Pa, then heat to 650℃, and introduce triphenylborane gas at a flow rate of 150SCCM for 200min. Then heat to 1200℃ and introduce lithium hydride gas at a flow rate of 150SCCM for 150min. Finally, cool down to 400℃ and introduce peracetic acid gas at a flow rate of 150SCCM for 30min. Then allow it to cool naturally to room temperature to obtain a porous carbon precursor material. Step S2: Transfer 200g of porous carbon precursor material to a fluidized bed. First, introduce an inert gas to purge the air from the tube. Then, raise the temperature to 630℃ and simultaneously introduce a mixture of silane gas and ammonia gas (volume ratio: silane gas: ammonia gas = 10:5) at a flow rate of 250 SCCM for 30 min to obtain silicon-carbon precursor material. Step S3: The silicon-carbon precursor material is transferred into the vacuum chamber and used as a substrate by atomic vapor deposition (ALD). As a target material, follow these steps: ① ① Deposit the material as a target for 1 second; ② Purge with nitrogen for 60 seconds; ③ Introduce oxygen for 5 seconds; ④ Purge with nitrogen for 5 seconds; ⑤ Introduce water for 0.05 seconds; ⑥ Purge with nitrogen for 50 seconds; ⑦ Cycle 70 times from step ① to deposit the silicon-carbon precursor material on its surface. A solid electrolyte-coated porous silicon-carbon composite was obtained; Step S4: 100g of solid electrolyte-coated porous silicon-carbon composite was transferred to a tube furnace by atomic vapor deposition. The air inside the tube was vented and the furnace was heated to 850°C. Acetylene mixed gas (volume ratio: acetylene:nitrogen = 10:3) was introduced at a flow rate of 40 SCCM for 450 min. Then, the furnace was cooled to room temperature under a nitrogen inert atmosphere to obtain the silicon-carbon composite material.

[0036] To further verify the effectiveness of the present invention, the inventors conducted a series of verification experiments, some of which are excerpted below.

[0037] Comparative Example 1 Unlike Example 1, ZIF was used to replace the porous carbon precursor material in step S1, i.e., no doping was performed; otherwise, it was the same as Example 1.

[0038] Comparative Example 2 Unlike Example 1, no solid electrolyte is deposited on its surface, i.e., step S3 is omitted; otherwise, it is the same as Example 1.

[0039] Comparative Example 3 Unlike Example 1, amorphous carbon is not deposited on its surface, i.e., step S4 is not performed; otherwise, it is the same as Example 1.

[0040] The above embodiments and comparative examples were tested.

[0041] 1. SEM testing The silicon-carbon composite anode material prepared in Example 1 was tested by scanning electron microscopy (SEM). Figure 1 The image shows a SEM image of the silicon-carbon composite material prepared in Example 1. As can be seen from the image, the material exhibits a spherical structure with a uniform size distribution and a particle size between 5 and 10 μm.

[0042] 2. Physicochemical property testing The specific surface area of ​​the silicon-carbon composite materials obtained in Examples 1-3 and Comparative Examples 1-3 was tested according to the methods in the national standard GB / T 38823-2020 "Silicon-Carbon". The powder resistivity of each silicon-carbon composite material was tested using a four-probe tester. The gas production of each silicon-carbon composite material was also tested (100g of powder was added to deionized water and left to stand at 45°C for 48 hours before testing the gas production). The lithium-ion diffusion coefficient of the material was tested by GITT (galvanostatic titration). In the GITT test, the material was first left to stand for 10 minutes, then discharged at 0.1C, 0.05C, and 0.01C rates to 5mV, then discharged at 0.01mA for 30 seconds to 5mV, then left to stand for 30 seconds, then charged at 0.1C rate to 2V, and finally left to stand for 10 minutes. The test results are shown in Table 1 below.

[0043] 3. Button cell battery test The silicon-carbon composite materials obtained in Examples 1-3 and Comparative Examples 1-3 were used as the active materials for the negative electrode sheets of the batteries to prepare coin cells; the specific preparation process of each coin cell is as follows: Preparation of battery negative electrode sheets: Binder, conductive agent and solvent were added to the silicon-carbon composite materials (as active materials of battery negative electrode sheets) corresponding to Examples 1-3 and Comparative Examples 1-3, respectively, and stirred to form a slurry. The slurry was coated on copper foil, and after drying and rolling, the battery negative electrode sheets were obtained. Among them, LA132 binder was used as binder, SP (conductive carbon black) was used as conductive agent, and NMP was used as solvent. The ratio was: silicon-carbon composite material: SP: LA132: NMP = 95g: 1g: 4g: 220mL. Fabrication of coin cells: Electrolyte is used Solution, in which, The concentration of the active ingredient was 1 mol / L, and the solvent used was a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) with a weight ratio of 1:1. A lithium metal sheet was used as the counter electrode, and a polypropylene (PP) membrane was used as the separator. The simulated battery was assembled in an argon-filled glove box. The electrochemical performance was tested on a Wuhan Landian CT2001A battery tester under the following conditions: charge / discharge voltage range of 0.005V to 2.0V, charge / discharge rate of 0.1C. The initial discharge specific capacity and initial efficiency were calculated, and the charge DCR (50% SOC) of the coin cell was also tested. The physicochemical properties and coin cell test results are shown in Table 1 below.

[0044] ; As shown in Table 1 above, the coin cells made using the silicon-carbon composite materials provided in Examples 1-3 of this application are significantly better than those of Comparative Examples 1-2 in terms of first discharge specific capacity, first discharge efficiency, and powder resistivity. This is because the MOF in the materials of the examples has a large-pore porous structure, which reduces expansion. Furthermore, the core doping with heteroatoms and lithium reduces defects and improves electronic conductivity, thereby improving rate capability and first discharge efficiency. At the same time, the solid electrolyte and amorphous carbon encapsulated in the shell improve the lithium-ion diffusion rate and electronic conductivity, thereby reducing DCR.

[0045] 4. Soft-pack battery test The silicon-carbon composite materials obtained in Examples 1-3 and Comparative Examples 1-3 were each doped with 90% artificial graphite as negative electrode materials (i.e., negative electrode sheets), using ternary materials. A 5Ah pouch cell was assembled using positive electrode material, electrolyte, and separator; the separator for the pouch cell is Celegard 2400, and the electrolyte is... Solution, in which The solvent for the solution is a mixture of EC and DEC in a volume ratio of 1:1. The concentration was 1.1 mol / L; the following performance tests were performed on each pouch cell: (1) Cyclic performance: The charge / discharge rate is 1C / 1C, the voltage range is 2.5V~4.2V, and the battery's 500-cycle performance is tested at a temperature of 25±3℃.

[0046] (2) HPPC (Hybrid Power Pulse Capability Characteristic) test: The charging DCR (DC resistance) was tested at different SOCs (10%, 30%, 50%, 70%, 90%) using 3C charging / 4C discharging rates respectively.

[0047] The test results are shown in Table 2.

[0048] ; As shown in Table 2, the pouch lithium-ion batteries prepared using the silicon-carbon composite materials obtained in each embodiment exhibit better cycle performance than those in the comparative examples, and their charge DCR is lower at different SOCs. This is because the silicon-carbon composite materials obtained in each embodiment have lower full-charge expansion and higher specific surface area, which improves the material's cycle performance; simultaneously, the silicon-carbon composite materials obtained in each embodiment have lower powder resistivity, which helps improve the material's fast-charging performance.

[0049] In summary, the method for preparing silicon-carbon composite materials provided by this invention improves the electronic and ionic conductivity of MOF porous carbon materials by doping them with heteroatoms and lithium, reducing defects and enhancing power performance. Furthermore, by coating the core surface with a solid electrolyte and an amorphous carbon bilayer structure, the expansion of the core is constrained, thus improving cycle performance. The resulting silicon-carbon material exhibits excellent power performance, low expansion, and good cycle performance.

[0050] Although the present invention has been described in detail above with general descriptions, specific embodiments, and experiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing a silicon-carbon composite anode material, characterized in that, Includes the following steps: Step S1: Transfer the MOF material to a fluidized bed as a matrix, evacuate to ≤10Pa, heat to 600-800℃, introduce borane gas for 30-300min, then heat to 1000-1500℃, introduce lithium source gas for 30-300min, finally cool to 300-600℃, introduce peroxide crosslinking agent gas for 10-60min, and allow to cool naturally to room temperature to obtain a porous carbon precursor material. The ratio of MOF material:borane gas:lithium source gas:peroxide crosslinking gas = 10g:0.3-30L:0.3-30L:0.1-6L. Step S2: Transfer the porous carbon precursor material to a fluidized bed, introduce inert gas to purge the air from the tube, heat to 600-700℃, and introduce silane gas and heteroatom mixed gas at a flow rate of 100-500 SCCM for 30-300 min to obtain silicon-carbon precursor material. The ratio of porous carbon precursor to heteroatom mixed gas is 200 g: 3-150 L, and the volume ratio of silane gas to heteroatom gas in the heteroatom mixed gas is 10:1-5. Step S3: Transfer the silicon-carbon precursor material into a vacuum chamber as a substrate, use the solid electrolyte as a target, and deposit the solid electrolyte on the surface of the silicon-carbon precursor material by atomic vapor deposition to obtain a solid electrolyte-coated porous silicon-carbon composite. Step S4: The solid electrolyte-coated porous silicon-carbon composite is transferred to a tube furnace by atomic vapor deposition. The air inside the tube is vented, and the furnace is heated to 800-1100°C. A carbon source mixed gas is introduced at a flow rate of 10-50 SCCM for 60-600 min. The furnace is then cooled to room temperature under an inert atmosphere to obtain the silicon-carbon composite material. The ratio of solid electrolyte-coated porous silicon-carbon composite to carbon source mixed gas is 100 g to 0.6-30 L, and the volume ratio of carbon source gas to nitrogen in the carbon source mixed gas is 10:1-3.

2. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, The MOF material in step S1 is one of ZIF-8, MOF-808, ZIF-67, MOF-818, MOF-74, MOF-545, and MIL-101(Cr).

3. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, The borane gas is one of the following: diborane, triphenylborane, triethoxyborane, trimethoxyborane, and dimethylamineborane, which are generated by sublimation upon heating; the lithium source gas is lithium hydride, which is generated by sublimation upon heating; and the peroxide crosslinking agent gas is one of peracetic acid, peroxyethyl ether, peroxybenzoic acid, and benzoyl peroxide, which are generated by sublimation upon heating.

4. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, In step S1, the flow rates of borane gas, lithium source gas, and peroxide crosslinking agent gas are 10-100 SCCM.

5. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, In step S2, the silicon source is one of silane, silane, dichlorosilane, or trichlorosilane; the heteroatom gas is one of hydrogen sulfide, ammonia, phosphine, or dinitrogen tetrahydrogen.

6. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, The solid electrolyte in step S3 is , , , , , , One of them, the , 0 < x ≤ 1, the , 0 < x < 2, 0 < y < 3.

7. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, The atomic vapor deposition method is specifically as follows: The solid electrolyte material was deposited as a target for 1 second, purged with nitrogen for 60 seconds, introduced with an oxygen source for 5 seconds, purged with nitrogen for 5 seconds, introduced with water for 0.05 seconds, and purged with nitrogen for 50 seconds. Repeat the above steps 10-100 times.

8. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, In step S4, the carbon source is one of ethylene, acetylene, methane, ethane, propane, and cyclohexane.

9. The method for preparing the silicon-carbon composite anode material according to claim 1, characterized in that, In step S4, the flow rate of the carbon source mixed gas is 10-50 SCCM.