A starch-based closed-cell hard carbon material with graphene oxide-induced pulsed Joule heat sealing, its preparation method and application
By using graphene oxide-induced pulsed Joule heat sealing technology, the problems of structural collapse and high open pore ratio in starch-based hard carbon materials during carbonization were solved, achieving efficient formation of closed pore structures and improving the sodium storage performance of sodium-ion battery anodes.
Patent Information
- Application Number
- CN202611271664.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing starch-based hard carbon materials are prone to foaming during carbonization, with a high proportion of open pores and difficulty in directional formation of closed-pore structures, resulting in low initial coulombic efficiency.
The pulsed Joule thermal sealing technology induced by graphene oxide achieves continuous control of precursor structure evolution and pore structure through the two-dimensional confinement effect of graphene oxide, cross-linking induction of oxygen-containing functional groups, low-temperature pre-carbonized conductive network, and pulsed Joule thermal rapid electrothermal conversion coupling.
A sodium storage structure with disordered carbon layers, short-range graphite microcrystals, and internal nanopores was formed, which improved the proportion of closed pores and the contribution of sodium storage at low potential plateau, thereby enhancing the plateau capacity and first coulombic efficiency of the sodium-ion battery anode.
Smart Images

Figure CN123105599A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery electrode materials technology, and in particular to a method for preparing a graphene oxide / starch-based hard carbon material and its application in the negative electrode of a sodium-ion battery. Background Technology
[0002] Sodium-ion batteries, due to the abundance and low cost of sodium resources, have shown great application potential in large-scale energy storage. Hard carbon materials, with their low cost, structural stability, large interlayer spacing suitable for sodium-ion storage, and abundant defect sites, have become one of the most promising anode materials for sodium-ion batteries. The sodium storage performance of hard carbon is closely related to its microstructure, with its capacity mainly originating from the high-potential slope region (>0.1 V vs Na). + / Na) and low potential plateau region (<0.1 V vs Na) + Existing research indicates that slope capacity is primarily influenced by defect concentration, while plateau capacity is mainly determined by closed-cell structure or interlayer spacing. Therefore, controlling the defect and pore structures of hard carbon materials is crucial for improving their reversible capacity and first coulombic efficiency.
[0003] Starch, as a widely available, renewable, and low-cost biomass precursor, has a naturally spherical structure and is an important raw material for the preparation of hard carbon. However, starch is prone to foaming during direct high-temperature carbonization, leading to structural collapse, excessive specific surface area, and incomplete formation of closed-cell structures, resulting in irreversible capacity loss and a low plateau capacity.
[0004] In existing technologies, starch structure is typically regulated by esterification crosslinking with crosslinking agents (such as maleic anhydride) or by external pore-forming methods. For example, Zheng Z. et al. (Advanced Energy Materials, 2024, 14(3):2303064) reported a method to improve sodium storage performance by crosslinking starch with maleic anhydride followed by CO2 pore-forming and high-temperature pore-closing treatment. Although the above methods improve material properties to some extent, they require additional chemical crosslinking agents or activation / pore-forming steps, making the process complex. Furthermore, the crosslinking, pore-forming, and structure regulation processes are independent of each other, making it difficult to achieve synergistic regulation of the microstructure of hard carbon.
[0005] Therefore, it is necessary to develop a simple and efficient method for preparing hard carbon materials that requires low amounts of additives and can regulate the evolution of precursor structure before carbonization. Summary of the Invention
[0006] To address the problems of easy foaming, high open pore ratio, difficulty in directional formation of closed pore structures, and low initial coulombic efficiency in existing starch-based hard carbon materials during carbonization, this invention provides a starch-based closed-pore hard carbon material with graphene oxide-induced pulsed Joule heating for pore sealing and its preparation method. This method couples the two-dimensional confinement effect of graphene oxide, the cross-linking induction effect of oxygen-containing functional groups, the conductive network after low-temperature pre-carbonization, and the rapid electrothermal conversion effect of pulsed Joule heating into the same process route, achieving continuous control over the evolution of the precursor structure and the formation of the pore structure. To achieve the above objectives, this invention adopts the following technical solution: A method for preparing a starch-based closed-cell hard carbon material with graphene oxide-induced pulsed Joule heat sealing includes the following steps: starch gelatinization and graphene oxide compounding, drying and shaping, compaction or roll forming orientation, oxygen-containing atmosphere pre-oxidation, inert atmosphere low-temperature pre-carbonization, and pulsed Joule heat rapid carbonization sealing.
[0007] Preferably, the starch is one or more of soluble starch, corn starch, and potato starch.
[0008] Preferably, the concentration of the graphene oxide dispersion is 0.5-5 mg / mL, and the mass ratio of starch to graphene oxide is 80:1-300:1.
[0009] Preferably, the drying process is freeze drying.
[0010] Preferably, the compaction, hot pressing, or roller pressing process is performed at a pressure of 30–120 MPa for a time of 3–15 min.
[0011] Preferably, the pre-oxidation treatment is performed at a temperature of 200 °C-300 °C for 6 hours.
[0012] Preferably, the temperature for the low-temperature pre-carbonization is 500-800℃. The heating rate is 1-10℃ / min; the holding time is 0.5-3 h.
[0013] Preferably, the inert atmosphere includes at least one of nitrogen, helium, argon, neon, and xenon.
[0014] Preferably, the conditions for the pulsed Joule heat treatment are: heating to 1200-2000 ℃ within 0.5-60 s; pulse treatment number 1-10 times; single pulse duration 1-30 s; and interval between two adjacent pulses 10-120 s.
[0015] This invention also provides a starch-based closed-cell hard carbon material prepared by the above-described preparation method. The starch-based closed-cell hard carbon material has a sodium storage structure composed of disordered carbon layers, short-range graphite microcrystals, and internal nanopores, with a BET specific surface area of 0.5-20 m² / g and a (002) interlayer spacing d.002 The wavelength ranges from 0.360 to 0.400 nm, and the tap density ranges from 0.60 to 1.20 g / cm³.
[0016] The present invention also provides the application of the starch-based closed-cell hard carbon material in the anode of sodium-ion batteries.
[0017] Beneficial effects: (1) The present invention upgrades graphene oxide from a traditional single conductive additive or structural modifier to a multi-stage functional medium, making it a two-dimensional coating and confinement medium in the composite stage, a cross-linking induction medium in the pre-oxidation stage, a conductive network precursor in the low-temperature pre-carbonization stage, and an electrothermal conversion framework in the pulse Joule heating stage, forming a continuous structural regulation chain.
[0018] (2) The present invention induces the orientation and arrangement of graphene oxide sheets by compaction or rolling, and combines pre-oxidation to solidify the starch structure in advance, which can effectively inhibit the softening, foaming, pore connection and skeleton collapse of starch in subsequent high temperature treatment.
[0019] (3) The present invention uses pulsed Joule heating for rapid carbonization and sealing, which is different from the slow heating carbonization of conventional tube furnaces. The instantaneous thermal shock of Joule heating can cause the outer layer of the carbon skeleton to shrink rapidly, induce the closure of open pores and retain the internal nanopore cavity, thereby increasing the closed pore ratio and the contribution of low potential plateau to sodium storage.
[0020] (4) This invention does not require the introduction of additional highly corrosive activators or a large amount of chemical crosslinking agents. The process is simple, the raw materials are widely available, the cost is low, and it has the potential for large-scale preparation.
[0021] (5) The obtained starch-based closed-cell hard carbon material has a low open pore content, a suitable (002) crystal plane interlayer spacing and a high tap density, which can be used to prepare sodium-ion battery anodes, which is beneficial to improve plateau capacity, first coulombic efficiency and cycle stability. Attached Figure Description
[0022] Figure 1 This is a scanning electron microscope image of the graphene oxide / starch-based hard carbon material prepared in Example 1 of the present invention. Detailed Implementation
[0023] The technical solution of the present invention will be further described below with reference to the embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention. Unless otherwise stated, the reagents and materials used in the embodiments can be obtained through conventional commercial means, and the test methods used are all conventional methods in the art.
[0024] Example 1 (1) Weigh 5 g of soluble starch and add it to deionized water. Stir at 85 °C for 1 h to allow the starch to gelatinize and swell, and obtain starch gelatinized liquid. Add graphene oxide dispersion at a starch to graphene oxide mass ratio of 150:1. After ultrasonic dispersion for 30 min, continue stirring for 2 h to allow graphene oxide sheets to adsorb and coat the surface of starch particles, and obtain graphene oxide / starch composite slurry.
[0025] (2) The composite slurry obtained in step (1) is freeze-dried to obtain a graphene oxide / starch composite precursor with a two-dimensional confined structure.
[0026] (3) The composite precursor was placed in a mold and compacted under 50 MPa pressure for 10 min to obtain the orientation confinement precursor, and then pre-oxidized in air atmosphere at 220℃ for 6 h.
[0027] (4) The cross-linked confinement precursor was placed in a tube furnace and heated to 650 °C at 5 °C / min under an argon atmosphere and held for 1 h to obtain a pre-carbonized intermediate.
[0028] (5) The pre-carbonized intermediate is sandwiched between graphite electrodes and subjected to pulse Joule heat treatment in an argon atmosphere to rapidly heat it to 1600 °C. The number of pulses is 3, the duration of a single pulse is 10 s, and the interval between two adjacent pulses is 60 s. After cooling, starch-based closed-cell hard carbon material is obtained.
[0029] Example 2 Starch-based closed-cell hard carbon materials were prepared according to the method of Example 1, except that: in step (1), the mass ratio of starch to graphene oxide was 100:1; in step (5), the pulse Joule heat treatment temperature was about 1500 ℃, the number of pulses was 2, and the duration of a single pulse was 15 s.
[0030] Example 3 Starch-based closed-cell hard carbon materials were prepared according to the method of Example 1, except that: in step (1), the mass ratio of starch to graphene oxide was 200:1; in step (5), the pulse Joule heat treatment temperature was about 1700 ℃, the number of pulses was 3, and the duration of a single pulse was 8 s.
[0031] Comparative Example 1 Without adding graphene oxide and without pulsed Joule heat treatment, 5 g of soluble starch was dried, compacted, and pre-oxidized, then heated to 1500 °C at 5 °C / min and held for 2 h under an argon atmosphere to obtain starch-based hard carbon material.
[0032] Comparative Example 2 The starch gelatinization, graphene oxide composite, freeze-drying, compaction, and pre-oxidation were carried out according to the method of Example 1, except that low-temperature pre-carbonization and pulse Joule heat treatment were not performed. Instead, the temperature was increased to 1500 ℃ at 5 ℃ / min and held for 2 h in an argon atmosphere to obtain a conventional tube furnace carbonized sample.
[0033] Comparative Example 3 The starch gelatinization, graphene oxide compounding, drying, and low-temperature pre-carbonization were carried out according to the method of Example 1, except that no compaction or rolling treatment was performed, and no pre-oxidation was performed; instead, pulse Joule heat treatment was performed directly.
[0034] Test Example 1 The graphene oxide / starch-based hard carbon materials prepared in Comparative Examples 1-3 and Examples 1-3 were mixed with sodium carboxymethyl cellulose at a mass ratio of 95:5 to form a slurry. The slurry was uniformly coated onto a copper current collector foil and dried in an oven at 60 °C for 2 h. The slurry was then cut into circular electrodes with a diameter of 8 mm. After drying the electrodes in a vacuum oven at 120 °C for 10 h, the mass of the active material was weighed and transferred to a glove box. Using sodium metal as the counter electrode and 1 M NaClO4 dissolved in ethylene carbonate and diethyl carbonate solution as the electrolyte, CR2025 coin cells were assembled.
[0035] The assembled CR2025 button cells were subjected to charge-discharge performance tests under the following conditions: current density set to 0.1 C (1 C = 300 mA g). -1 The discharge voltage is 0.001 V, and the charging voltage is 3 V.
[0036] Table 1. Electrochemical and structural performance of graphene oxide / starch-based hard carbon materials in Examples 1-3 (Comparative) As shown in Table 1, compared with the comparative example, the graphene oxide / starch-based closed-cell hard carbon material prepared in the embodiments of the present invention has higher reversible specific capacity and plateau capacity, higher initial coulombic efficiency and higher tap density. At the same time, the BET specific surface area is significantly reduced and the closed-cell specific surface area is significantly increased. This indicates that the synergistic treatment of graphene oxide confinement, pre-oxidation curing, low-temperature pre-carbonization conductive network construction and pulsed Joule heating rapid sealing is beneficial to the formation of closed-cell structure and the improvement of sodium storage performance.
Claims
1. A method for preparing a starch-based closed-cell hard carbon material with graphene oxide-induced pulsed Joule heat sealing, characterized in that, Includes the following steps: (1) Add starch to water and gelatinize at 60-95 °C for 0.5-3 h, then add graphene oxide dispersion and mix to obtain graphene oxide / starch composite slurry, wherein the mass ratio of starch to graphene oxide is 80:1-300:1; (2) After the composite slurry obtained in step (1) is freeze-dried, spray-dried or vacuum-dried, it is compacted, hot-pressed or roller-pressed to obtain an orientation-confined precursor. (3) The orientation-confined precursor obtained in step (2) is pre-oxidized in an oxygen-containing atmosphere to cause starch to undergo dehydration condensation and cross-linking curing, thereby obtaining a cross-linked confined precursor. (4) The cross-linked confinement precursor obtained in step (3) is heated to 500-800 °C under an inert atmosphere for 0.5-3 h to pre-carbonize the graphene oxide in situ to form a conductive carbon network, thereby obtaining a pre-carbonized intermediate. (5) The pre-carbonized intermediate obtained in step (4) is subjected to pulse Joule heat treatment, which raises the temperature to 1200-2000 ℃ within 0.5-60 s, inducing the open pores to shrink and form a closed pore structure, thereby obtaining graphene oxide / starch-based closed pore hard carbon material.
2. The preparation method according to claim 1, characterized in that: The starch is selected from one or more of soluble starch, corn starch, potato starch, wheat starch, and cassava starch; the concentration of the graphene oxide dispersion is 0.5-5 mg / mL.
3. The preparation method according to claim 1, characterized in that: In step (2), the pressure of the compaction, hot pressing or roller pressing is 10-200 MPa and the time is 1-30 min.
4. The preparation method according to claim 1, characterized in that: In step (5), the pulse Joule heat treatment is carried out in a vacuum, nitrogen, argon or helium atmosphere, with 1-10 pulses, a single pulse duration of 1-30 s, and an interval of 10-120 s between two adjacent pulses.
5. A starch-based closed-cell hard carbon material prepared by the preparation method according to any one of claims 1-4, characterized in that: The starch-based closed-cell hard carbon material has a sodium storage structure composed of disordered carbon layers, short-range graphite microcrystals, and internal nanopores.
6. The starch-based closed-cell hard carbon material as described in claim 5, characterized in that: The starch-based closed-cell hard carbon material has a BET specific surface area of 0.5-20 m² / g and a closed-cell specific surface area of 500-2000 m² / g. (002) Interlayer spacing d 002 The wavelength range is 0.360-0.400 nm; the tap density is 0.60-1.20 g / cm³.
7. A sodium-ion battery negative electrode, characterized in that: The sodium-ion battery negative electrode comprises the starch-based closed-cell hard carbon material as described in any one of claims 5-6.
8. A sodium-ion battery, characterized in that: The sodium-ion battery comprises the sodium-ion battery negative electrode as described in claim 7.