A silicon-carbon composite anode material based on silane pyrolysis and gradient chemical vapor deposition and its preparation method

By directionally depositing nano-silicon particles on and inside carbon nanotubes and coating them with a conductive carbon outer layer, the problems of uniform silicon deposition and volume expansion buffering in silicon-carbon composite materials were solved, and a highly efficient three-dimensional conductive network was constructed, which improved the cycle stability and rate performance of lithium-ion batteries.

CN123105602APending Publication Date: 2026-11-17XI AN JIAOTONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611312452.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing silicon-carbon composite materials, the porous carbon matrix has tortuous pores, point contact conductivity, and rigidity that makes it brittle and difficult to deposit silicon uniformly, buffer volume expansion, and build a uniform and rapid three-dimensional conductive network, leading to the failure of silicon-carbon anode materials during cycling.

Method used

A method combining silane pyrolysis and gradient chemical vapor deposition was used to directionally deposit nano-silicon particles on the surface and inside of carbon nanotubes. Then, an outer layer of conductive carbon was coated with acetylene gas to construct a three-dimensional conductive network and a mechanical buffer layer, forming a gradient interface layer between the three-dimensional framework of carbon nanotubes and the outer layer of conductive carbon.

Benefits of technology

Uniform deposition of silicon on a carbon nanotube framework and directional control of grain size were achieved, constructing an efficient electron/ion conduction channel, which significantly improved the cycle stability and rate performance of silicon-carbon anode materials, making them suitable for high-energy-density lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105602A_ABST
    Figure CN123105602A_ABST
Patent Text Reader

Abstract

This invention discloses a silicon-carbon composite anode material and its preparation method based on silane pyrolysis and gradient chemical vapor deposition, belonging to the field of lithium-ion battery material technology. The method involves placing carbon nanotubes in a vapor deposition reactor, simultaneously introducing silane gas and chain hydrocarbon gas, and heating. The active carbon radicals generated by the pyrolysis of the chain hydrocarbons form heterogeneous nucleation sites on the surface of the carbon nanotubes, inducing silicon atoms to be directionally deposited on and inside the carbon nanotubes to form nano-silicon particles. Subsequently, acetylene is introduced and heated for pyrolysis, coating the carbon nanotubes and silicon particles with a conductive carbon outer layer. This material, supported by a three-dimensional framework of carbon nanotubes, together with the conductive carbon outer layer, constructs a three-dimensional conductive network and a gradient interface layer that is rigid inside and flexible outside, suppressing the aggregation of silicon particles and buffering the volume expansion of silicon. The silicon-carbon composite anode material of this invention exhibits excellent cycle stability and rate performance, making it suitable for high-energy-density lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery material technology, and relates to a silicon-carbon composite anode material based on silane pyrolysis and gradient chemical vapor deposition and its preparation method. Background Technology

[0002] Silicon-based materials are considered important candidates for next-generation lithium-ion battery anode materials due to their extremely high theoretical specific capacity (approximately 4200 mAh / g). However, pure silicon anodes undergo massive volume expansion (over 300%) during charge and discharge, leading to pulverization of the active material, repeated rupture and regeneration of the solid electrolyte interface film, and rapid capacity decay. Furthermore, silicon's inherent poor conductivity limits its practical applications.

[0003] To overcome the aforementioned shortcomings, silicon-carbon composite materials have emerged. Combining silicon with carbon materials allows the mechanical buffering effect of the carbon matrix to absorb volume expansion stress, while the excellent conductivity of carbon enhances the overall electrochemical performance of the electrode. Currently, chemical vapor deposition (CVD) is one of the mainstream processes for preparing silicon-carbon anodes, typically using silane (SiH4) as the silicon source to deposit silicon within or on the surface of a porous carbon framework.

[0004] However, existing CVD silicon-carbon processes have significant limitations when simply introducing silane gas: during silane pyrolysis, silicon atoms readily undergo homogeneous nucleation, forming free silicon particles rather than uniformly deposited on the carbon matrix surface, leading to uneven silicon distribution and severe agglomeration. Simultaneously, silicon grain size is difficult to control precisely, easily growing too large, and generating enormous stress due to volume expansion during cycling, accelerating electrode failure. Furthermore, existing silicon-carbon materials use porous carbon as the carbon matrix. The porous carbon matrix has tortuous pores, point contact conductivity, and is rigid and fragile, which is detrimental to uniform silicon deposition, volume expansion buffering, and the construction of a uniform and rapid three-dimensional conductive network, thus limiting further improvements in the overall performance of silicon-carbon anodes. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a silicon-carbon composite anode material and preparation method based on silane pyrolysis and gradient chemical vapor deposition, so as to solve the problems of tortuous pores, point contact conductivity, rigidity and fragility of porous carbon matrix in the prior art, which are not conducive to uniform silicon deposition, volume expansion buffering and construction of uniform and rapid three-dimensional conductive network.

[0006] To achieve the above objectives, the present invention employs the following technical solution: This invention discloses a method for preparing silicon-carbon composite anode materials based on silane pyrolysis and gradient chemical vapor deposition, comprising the following steps: S1, carbon nanotubes are placed in a vapor deposition reactor, and silane gas and chain hydrocarbon gas are introduced and heated at the same time, so that the active carbon free radicals generated by the cracking of the chain hydrocarbons form heterogeneous nucleation sites on the surface of carbon nanotubes, inducing silicon atoms to be directionally deposited on the surface and inside of carbon nanotubes as nano-silicon particles, forming carbon nanotubes with silicon nanoparticles attached to the surface. S2, acetylene gas is introduced into the vapor deposition reactor and heated to decompose it, thereby coating the carbon nanotubes and silicon particles with a conductive carbon outer layer to obtain a silicon-carbon composite anode material.

[0007] A further improvement of the present invention is that: Preferably, in S1, the vapor deposition reactor includes any one of a fluidized bed, a rotary kiln, a vibrating bed, and a fixed bed.

[0008] Preferably, in S1, the chain hydrocarbon gas is any one of methane, acetylene, ethylene, ethane, propylene, and propane.

[0009] Preferably, in step S1, after the carbon nanotubes are placed in the vapor deposition reactor, nitrogen gas is introduced to purge the air.

[0010] Preferably, in S1, the diameter of the carbon nanotube is 10nm~50nm.

[0011] Preferably, in S1, the volume ratio of the silane gas to the chain hydrocarbon gas is 1:1, and the flow rates of both the silane gas and the chain hydrocarbon gas are 0.5 L / min.

[0012] Preferably, in S1, the silane pyrolysis heating temperature is 400℃~650℃, and the heating time is 30 min~120 min.

[0013] Preferably, in S2, the acetylene cracking heating temperature is 600℃~900℃, and the heating time is 30 min~90 min.

[0014] A silicon-carbon composite anode material prepared by any one of the above methods, comprising: Three-dimensional framework of carbon nanotubes; Nanoscale silicon particles deposited on the surface and inside of carbon nanotubes, the silicon particles being formed by the high-temperature pyrolysis of silane; A conductive carbon outer layer coating the surface of carbon nanotubes and silicon particles; The carbon nanotube three-dimensional framework and the conductive carbon outer layer together construct a three-dimensional conductive network.

[0015] Preferably, the particle size of the inner silicon particle is 10 nm to 50 nm; the thickness of the outer conductive carbon layer is 5 nm to 20 nm, and the electronic conductivity is ≥33 mS / cm.

[0016] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a method for preparing a silicon-carbon composite anode material. The method includes: placing carbon nanotubes in a vapor deposition reactor (fluidized bed, rotary kiln, vibrating bed, or fixed bed); simultaneously introducing silane gas and one of the chain hydrocarbon gases (methane, acetylene, ethylene, ethane, propylene, or propane) into the reactor; heating to decompose the silane, resulting in silicon vapor deposition inside the carbon nanotubes; and then introducing acetylene gas for further heating and decomposition, yielding a three-dimensional conductive silicon-carbon composite anode material with uniform silicon deposition. The material, from the inside out, consists of a three-dimensional conductive carbon framework of carbon nanotubes, nano-silicon particles anchored to the surface and interior of the carbon nanotubes, and amorphous carbon coating the surfaces of the carbon nanotubes and nano-silicon particles. This invention, by constructing a gradient interface layer, achieves synergistic electron / ion conduction, mechanical buffering with an inner rigidity and outer flexibility, and interface self-healing, significantly improving the cycle stability and rate performance of the silicon-carbon anode material, making it suitable for high-energy-density lithium-ion batteries.

[0017] This method employs a process route combining vapor deposition with multi-component gas synergistic control. The entire process is carried out in a vapor deposition reactor, eliminating the need for high-pressure equipment. Through precise control of gas ratios and deposition timing, uniform deposition of silicon on a carbon nanotube framework and directional control of grain size can be achieved. The process is simple and easily scaled up. After placing the carbon nanotubes in the vapor deposition reactor, this invention innovatively introduces silane gas and chain hydrocarbon gas simultaneously. Under heating conditions, silane decomposes and deposits silicon in the vapor phase inside and on the surface of the carbon nanotubes. During this process, the active carbon radicals generated by the decomposition of chain hydrocarbons act as "inducers." These radicals preferentially adsorb onto the surface of the carbon nanotubes, forming numerous heterogeneous nucleation sites and capturing silicon atoms in the gas phase. This forces silicon atoms to undergo heterogeneous nucleation and growth on the carbon nanotube surface, rather than free homogeneous nucleation in the gas phase. This mechanism fundamentally inhibits the aggregation and uncontrolled growth of silicon particles, achieving nanoscale, highly dispersed, and directional anchoring of silicon on the carbon nanotube framework. Subsequently, the introduction of silane and chain hydrocarbon gases was stopped, and acetylene gas was introduced and heated for cracking, forming an amorphous carbon coating layer in situ on the surface of the carbon nanotubes with deposited silicon nanoparticles. This coating layer not only acts as a physical buffer to alleviate the volume expansion of silicon during charging and discharging, but also constructs a highly efficient electron / ion dual continuous transport channel through the synergistic effect of the three-dimensional conductive network of carbon nanotubes and the external carbon layer. The above-mentioned multi-gas stepwise deposition strategy, by combining the inhibitory effect of chain hydrocarbon gas on silicon growth with the in-situ encapsulation of silicon by acetylene, achieves simultaneous improvement in the fine structure control of silicon and interface stability, ensuring that the composite material maintains its structural integrity during repeated cycling.

[0018] This invention also discloses a silicon-carbon composite anode material, which uses a three-dimensional carbon nanotube framework as the supporting matrix. The inner layer consists of nano-silicon particles formed by the high-temperature pyrolysis of silane, uniformly deposited on the surface of the carbon nanotubes; the outer layer is a conductive carbon coating layer formed by the high-temperature pyrolysis of acetylene, tightly encapsulating the carbon nanotubes and silicon particles. The three-dimensional carbon nanotube framework and the conductive carbon outer layer together construct a highly efficient three-dimensional conductive network, ensuring rapid electron transport between active particles and between particles and the current collector. The mechanical buffering effect of the carbon coating layer effectively suppresses the volume expansion of silicon during charge and discharge, preventing active material shedding and interface delamination. The inner nano-silicon layer provides a high capacity contribution, while the outer conductive carbon layer and the carbon nanotube framework synergistically form a continuous electronic pathway, significantly reducing the charge transfer impedance of the electrode and improving the rate performance and cycle stability of the battery. Using the silicon-carbon material modified by this invention, the electrode expansion rate can be significantly reduced while maintaining a high initial coulombic efficiency and capacity retention. Attached Figure Description

[0019] Figure 1 Here is a SEM image of the silicon-carbon composite material of the present invention; Figure 2 TEM images showing the uniformity of deposited silicon particles in the examples and comparative examples; Figure 3 The graph shows a performance test comparison between the examples and the comparative examples. Detailed Implementation

[0020] The present invention will now be described in further detail with reference to the accompanying drawings: To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0021] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if 60 is listed for a specific parameter... 120 and 80 The range of 110 is understood to be 60. 110 and 80 The range of 120 is also expected. Furthermore, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4, and 5 are listed, then the following ranges are all expected: 1 3.1 4.1 5.2 3, 2 4 and 2 5. In this application, unless otherwise stated, the numerical range "a" "b" represents a shortened representation of any combination of real numbers from a to b, where both a and b are real numbers. For example, the numerical range "0"... "5" indicates that all "0"s have been listed in this article. All real numbers between "5" and "0". "5" is simply an abbreviation for these numerical combinations. In addition, when a parameter is expressed as an integer greater than or equal to 2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0022] In the description of this application, it should be noted that, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," and "outer," etc., indicating orientation or positional relationships, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. Furthermore, the terms "first," "second," and "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance. "Vertical" is not vertical in the strict sense, but within the allowable tolerance range. "Parallel" is not parallel in the strict sense, but within the allowable tolerance range.

[0023] The directional terms used in the following description refer to the directions shown in the figures and are not intended to limit the specific structure of this application. It should also be noted in the description of this application that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "joining" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0024] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0025] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B".

[0026] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0027] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0028] This invention discloses a method for preparing silicon-carbon composite anode materials in a vapor deposition reactor using silane pyrolysis and gradient chemical vapor deposition. The preparation method includes the following steps: S1. Carbon nanotubes (CNTs) are placed into a chemical vapor deposition reactor, and nitrogen (N2) is introduced to ensure complete air removal from the reactor. Silane gas (SiH4) and a chain hydrocarbon gas (one of CH4, C2H2, C2H4, C2H6, C3H6, or C3H8) are introduced, with a volume ratio of 1:1 between silane and chain hydrocarbon gas, and a flow rate of 0.5 L / min for both gases. After complete introduction of both gases, the reactor is heated to a chamber temperature of 400℃~650℃ and held at this temperature for 30 min~120 min, with the same heating and holding time for both gases. Afterwards, the reactor is cooled to room temperature, and the carbon nanotubes after chemical vapor deposition (CVD) of silicon are removed. This heating step causes silane decomposition, resulting in the vapor deposition of silicon on the surface and inside of the carbon nanotubes, forming silicon nanoparticles with a particle size of 10 nm~50 nm.

[0029] Specifically, the vapor deposition reactor can be any one of a fluidized bed, rotary kiln, vibrating bed, or fixed bed.

[0030] Specifically, the chain hydrocarbon gas is any one of methane (CH4), acetylene (C2H2), ethylene (C2H4), ethane (C2H6), propylene (C3H6), or propane (C3H8).

[0031] S2, nitrogen (N2) is continuously introduced into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min until all waste gas is discharged. Then, acetylene (C2H2) gas is introduced at a flow rate of 0.5 L / min. After the gas is completely introduced, the reactor is heated to a chamber temperature of 600℃~900℃ and held at this temperature for 30 min~90 min. Afterwards, it is cooled to room temperature, and the carbon nanotubes after CVD of silicon are removed. Through this step, acetylene undergoes high-temperature pyrolysis to form the conductive carbon outer layer; the conductive carbon outer layer coats the surface of the carbon nanotubes and silicon particles. The thickness of the conductive carbon outer layer is 10 nm, and the electronic conductivity is ≥33 mS / cm.

[0032] The second aspect of the present invention discloses a silicon-carbon composite material prepared by the above method, the silicon-carbon composite material comprising carbon nanotubes (CNTs) as a carbon skeleton, nano-silicon particles anchored to the surface and interior of the carbon nanotubes, amorphous carbon coating the surface of the carbon nanotubes and nano-silicon particles, and a gradient interface layer constructed by them.

[0033] The present invention also provides the application of the above-mentioned silicon-carbon composite anode material in the preparation of lithium-ion batteries.

[0034] In this silicon-carbon composite material, the carbon nanotube framework and the outer carbon layer together construct a three-dimensional conductive network: the inner carbon nanotubes primarily perform efficient electron transport, while the outer carbon layer plays a dual role in conducting both electrons and ions, forming a functional gradient distribution of "inner electrons, outer ions." Simultaneously, the material exhibits a significant internal rigidity and external flexibility mechanical gradient—the carbon nanotube framework has a high Young's modulus, providing rigid support; the outer carbon layer, formed by the amorphous carbon structure from acetylene cracking, is relatively soft with a low Young's modulus (<40 MPa), enabling flexible buffering of volume changes. When silicon particles expand in volume during charging and discharging, approximately 60% of the stress is first absorbed by the inner rigid framework, and the remaining stress is gradually dissipated by the outer flexible carbon layer, achieving hierarchical management and gradual attenuation of stress. This synergistic functional and mechanical gradient design from the inside out not only ensures rapid electron / ion conduction but also significantly alleviates the volume effect of silicon, thereby stabilizing the electrode structure and extending cycle life.

[0035] The gradient-characteristic interfacial interactions in this silicon-carbon composite material include: (a) the amorphous carbon outer layer formed by acetylene cracking is firmly anchored to the CNT surface and nano-silicon particles through in-situ carbon-carbon covalent bonding (the dangling bonds on the CNT surface are bonded to active carbon atoms) and Si–C chemical bonds (a local silicon carbide transition layer at the interface between the nano-silicon surface and the carbon layer); (b) during carbon layer deposition, active carbon penetrates into the gaps between CNT tubes and the surface of silicon particles, forming an interlocked carbon-carbon / carbon-silicon interpenetrating network structure through in-situ polymerization / deposition, enhancing mechanical interlocking; (c) the disordered layer structure of the outer carbon layer and the graphene layer of the CNT form a tight contact through π–π stacking and van der Waals forces. The above-mentioned multiple interfacial interactions ensure that the carbon outer layer remains completely covered during the repeated volume expansion of silicon nanoparticles, without delamination; at the same time, the sp² hybrid conductive network of the outer carbon layer works synergistically with the inner CNT framework to ensure Li + / e - Rapid transmission at the interface enables coordinated management of stress and charge under functional gradient.

[0036] The following detailed explanation, with reference to specific embodiments, will further illustrate this point.

[0037] Example 1 Step 1: Take carbon nanotubes (CNTs) (approximately 900 g) and place them into a fluidized bed. Then, introduce nitrogen (N2) at a flow rate of 0.5 L / min to ensure that all air is completely expelled from the reactor.

[0038] Step 2: Simultaneously introduce 20 L of silane gas (SiH4) and 20 L of chain hydrocarbon gas (CH4) at a flow rate of 0.5 L / min at a volume ratio of 1:1. After both gases are completely introduced, heat the reactor to bring the chamber temperature to 500℃ and maintain this temperature for 120 min. Then cool to room temperature to obtain carbon nanotubes (approximately 915 g) after chemical vapor deposition (CVD) of silicon.

[0039] Step 3: Continue to introduce nitrogen (N2) into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min to ensure that the air in the reactor is completely purged.

[0040] Step 4: Introduce 20 L of acetylene (C2H2) gas at a flow rate of 0.5 L / min. After the gas is completely introduced, heat the reactor to bring the temperature inside the chamber to 750℃ and keep it at that temperature for 90 min. Then cool it to room temperature to obtain the final silicon-carbon anode material with a three-dimensional conductive framework and stress dissipation layer, denoted as DCNT-0417-X2.

[0041] Figure 1 This is a schematic diagram of the silicon-carbon composite anode material provided in an embodiment of the present invention. As shown in the figure, carbon nanotubes are intertwined, and nano-silicon particles are uniformly deposited on the carbon nanotubes. Conductive carbon is uniformly coated on the surfaces of the carbon nanotubes and silicon particles. The carbon nanotubes form a three-dimensional carbon framework core; the nano-silicon particles loaded inside and on the surface of the three-dimensional carbon framework core are formed by in-situ pyrolysis of silane gas and chain hydrocarbon gas, providing space for lithium-ion insertion; and the carbon outer layer coating the three-dimensional carbon framework and the surface of the nano-silicon particles is formed by in-situ pyrolysis of acetylene gas, providing conductive electron channels and flexibly buffering volume changes. The carbon outer layer and the three-dimensional carbon framework together constitute a three-dimensional conductive network and a stress buffer layer. While achieving synergistic electron conduction, the mechanical gradient of inner rigidity and outer flexibility gradually alleviates the volume expansion stress of the silicon particles, thereby stabilizing the electrode structure and extending cycle life.

[0042] like Figure 1 As shown, Figure 1This is a schematic diagram of the silicon-carbon composite anode material provided in an embodiment of the present invention. As shown, the core consists of a three-dimensional carbon nanotube framework; nano-silicon particles loaded inside and on the surface of the three-dimensional carbon framework core, formed by in-situ pyrolysis of silane gas and chain hydrocarbon gas, providing space for lithium-ion insertion; and a carbon outer layer coating the surface of the three-dimensional carbon framework and nano-silicon particles, formed by in-situ pyrolysis of acetylene gas, providing conductive electron channels and flexibly buffering volume changes. The carbon outer layer and the three-dimensional carbon framework together constitute a three-dimensional conductive network and a stress buffer layer. While achieving synergistic electron conduction, the mechanical gradient of inner rigidity and outer flexibility gradually alleviates the volume expansion stress of the silicon particles, thereby stabilizing the electrode structure and extending cycle life.

[0043] Example 2 Step 1: Take carbon nanotubes (CNTs) (approximately 900 g, with a diameter of approximately 10 nm) and place them into a rotary kiln. Then, introduce nitrogen (N2) at a flow rate of 0.5 L / min to ensure that all air is completely expelled from the reactor.

[0044] Step 2: Simultaneously introduce 20 L of silane gas (SiH4) and 20 L of chain hydrocarbon gas (C2H4) at a flow rate of 0.5 L / min at a volume ratio of 1:1. After both gases are completely introduced, heat the reactor to bring the temperature inside the chamber to 400℃ and keep it at that temperature for 120 min. Then cool it to room temperature to obtain carbon nanotubes after chemical vapor deposition (CVD) of silicon.

[0045] Step 3: Continue to introduce nitrogen (N2) into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min to ensure that the air in the reactor is completely purged.

[0046] Step 4: Introduce 20 L of acetylene (C2H2) gas at a flow rate of 0.5 L / min. After the gas is completely introduced, heat the reactor to bring the temperature inside the chamber to 600℃ and keep it at that temperature for 90 min. Then cool it to room temperature to obtain the final silicon-carbon anode material with a three-dimensional conductive framework and a stress dissipation layer.

[0047] Characterization revealed that in the silicon-carbon anode material obtained in this embodiment, carbon nanotubes are intertwined, and nano-silicon particles are uniformly deposited on the carbon nanotubes with a particle size of approximately 10 nm to 50 nm. A conductive carbon outer layer is uniformly coated on the surface of the carbon nanotubes and silicon particles with a thickness of approximately 5 nm, and the electronic conductivity is approximately 35 mS / cm.

[0048] Example 3 Step 1: Take carbon nanotubes (CNTs) (approximately 900 g, with a diameter of approximately 50 nm) and place them into a vibrating bed. Then, introduce nitrogen (N2) at a flow rate of 0.5 L / min to ensure that all air is expelled from the reactor.

[0049] Step 2: Simultaneously introduce 20 L of silane gas (SiH4) and 20 L of chain hydrocarbon gas (C2H6) at a flow rate of 0.5 L / min at a volume ratio of 1:1. After both gases are completely introduced, heat the reactor to bring the temperature inside the chamber to 650℃ and keep it at that temperature for 30 min. Then cool it to room temperature to obtain carbon nanotubes after chemical vapor deposition (CVD) of silicon.

[0050] Step 3: Continue to introduce nitrogen (N2) into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min to ensure that the air in the reactor is completely purged.

[0051] Step 4: Introduce 20 L of acetylene (C2H2) gas at a flow rate of 0.5 L / min. After the gas is completely introduced, heat the reactor to bring the temperature inside the chamber to 900℃ and keep it at that temperature for 30 min. Then cool it to room temperature to obtain the final silicon-carbon anode material with a three-dimensional conductive framework and a stress dissipation layer.

[0052] Characterization revealed that in the silicon-carbon anode material obtained in this embodiment, carbon nanotubes are intertwined, and nano-silicon particles are uniformly deposited on the carbon nanotubes with a particle size of approximately 10 nm to 50 nm. A conductive carbon outer layer is uniformly coated on the surface of the carbon nanotubes and silicon particles with a thickness of approximately 20 nm, and the electronic conductivity is approximately 60 mS / cm.

[0053] Example 4 Step 1: Take carbon nanotubes (CNTs) (approximately 900 g, with a diameter of approximately 30 nm) and place them into a fixed bed. Then, introduce nitrogen (N2) at a flow rate of 0.5 L / min to ensure that all air is completely expelled from the reactor.

[0054] Step 2: Simultaneously introduce 20 L of silane gas (SiH4) and 20 L of chain hydrocarbon gas (C3H6) at a flow rate of 0.5 L / min at a volume ratio of 1. After both gases are completely introduced, heat the reactor to bring the chamber temperature to 525℃ and maintain this temperature for 75 min. Then cool it to room temperature to obtain carbon nanotubes after chemical vapor deposition (CVD) of silicon.

[0055] Step 3: Continue to introduce nitrogen (N2) into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min to ensure that the air in the reactor is completely purged.

[0056] Step 4: Introduce 20 L of acetylene (C2H2) gas at a flow rate of 0.5 L / min. After the gas is completely introduced, heat the reactor to bring the temperature inside the chamber to 750℃ and keep it at that temperature for 60 min. Then cool it to room temperature to obtain the final silicon-carbon anode material with a three-dimensional conductive framework and a stress dissipation layer.

[0057] Characterization revealed that in the silicon-carbon anode material obtained in this embodiment, carbon nanotubes are intertwined, and nano-silicon particles are uniformly deposited on the carbon nanotubes with a particle size of approximately 10 nm to 50 nm. A conductive carbon outer layer is uniformly coated on the surface of the carbon nanotubes and silicon particles with a thickness of approximately 13 nm, and the electronic conductivity is approximately 48 mS / cm.

[0058] Example 5 Step 1: Take carbon nanotubes (CNTs) (approximately 900 g, with a diameter of approximately 20 nm) and place them into a fluidized bed. Then, introduce nitrogen (N2) at a flow rate of 0.5 L / min to ensure that all air is completely expelled from the reactor.

[0059] Step 2: Simultaneously introduce 20 L of silane gas (SiH4) and 20 L of chain hydrocarbon gas (C3H8) at a flow rate of 0.5 L / min at a volume ratio of 1:1. After both gases are completely introduced, heat the reactor to bring the temperature inside the chamber to 450℃ and keep it at that temperature for 90 min. Then cool it to room temperature to obtain carbon nanotubes after chemical vapor deposition (CVD) of silicon.

[0060] Step 3: Continue to introduce nitrogen (N2) into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min to ensure that the air in the reactor is completely purged.

[0061] Step 4: Introduce 20 L of acetylene (C2H2) gas at a flow rate of 0.5 L / min. After the gas is completely introduced, heat the reactor to bring the temperature inside the chamber to 850℃ and keep it at that temperature for 45 min. Then cool it to room temperature to obtain the final silicon-carbon anode material with a three-dimensional conductive framework and stress dissipation layer.

[0062] Characterization revealed that in the silicon-carbon anode material obtained in this embodiment, carbon nanotubes are intertwined, and nano-silicon particles are uniformly deposited on the carbon nanotubes with a particle size of approximately 10 nm to 50 nm. A conductive carbon outer layer is uniformly coated on the surface of the carbon nanotubes and silicon particles with a thickness of approximately 8 nm, and the electronic conductivity is approximately 38 mS / cm.

[0063] Example 6 Step 1: Take carbon nanotubes (CNTs) (approximately 900 g, with a diameter of approximately 40 nm) and place them into a rotary kiln. Then, introduce nitrogen (N2) at a flow rate of 0.5 L / min to ensure that all air is completely expelled from the reactor.

[0064] Step 2: Simultaneously introduce 20 L of silane gas (SiH4) and 20 L of chain hydrocarbon gas acetylene (C2H2) at a flow rate of 0.5 L / min at a volume ratio of 1:1. After both gases are completely introduced, heat the reactor to bring the temperature inside the chamber to 600℃ and keep it at that temperature for 60 min. Then cool it to room temperature to obtain carbon nanotubes after chemical vapor deposition (CVD) of silicon.

[0065] Step 3: Continue to introduce nitrogen (N2) into the reactor after chemical vapor deposition (CVD) of silicon at a flow rate of 0.5 L / min to ensure that the air in the reactor is completely purged.

[0066] Step 4: Introduce 20 L of acetylene (C2H2) gas at a flow rate of 0.5 L / min. After the gas is completely introduced, heat the reactor to bring the temperature inside the chamber to 800℃ and keep it at that temperature for 75 min. Then cool it to room temperature to obtain the final silicon-carbon anode material with a three-dimensional conductive framework and a stress dissipation layer.

[0067] Characterization revealed that in the silicon-carbon anode material obtained in this embodiment, carbon nanotubes are intertwined, and nano-silicon particles are uniformly deposited on the carbon nanotubes with a particle size of approximately 10 nm to 50 nm. A conductive carbon outer layer is uniformly coated on the surface of the carbon nanotubes and silicon particles with a thickness of approximately 16 nm, and the electronic conductivity is approximately 52 mS / cm.

[0068] Comparative Example 1 The carbon nanotubes were replaced with porous carbon materials, and steps 1, 2, 3, and 4 were performed. This was designated as TL-1126.

[0069] Comparative Example 2 In step 2, only silane gas is introduced at a flow rate of 0.5 L / min, and the rest of the steps are the same. This is referred to as DCNT-0417.

[0070] The materials obtained in Example 1 and Comparative Example 2 were characterized using transmission electron microscopy (TEM) to obtain their images and corresponding carbon (C) and silicon (Si) elemental mapping distributions, as shown below. Figure 2 As shown in the image of Comparative Example 2, it can be observed that the silicon particles exhibit obvious agglomeration, with large particle sizes and extremely uneven distribution. The C element coating layer also appears relatively loose and uneven in thickness. In contrast, the material of Example 1 exhibits extremely excellent microscopic uniformity. The silicon particles are uniformly embedded in the carbon framework at extremely fine nanoscale sizes, without any obvious agglomeration. Furthermore, the distributions of C and Si elements are highly overlapping, indicating that the carbon coating layer is dense and tightly bonded to the silicon particles. This highly ordered "carbon-coated silicon" structure not only ensures that each silicon particle is effectively protected by the carbon layer but also constructs a continuous and stable electron transport network, significantly reducing the probability of interfacial side reactions.

[0071] Performance Testing and Results The materials obtained in Example 1 and Comparative Examples 1 and 2 were used in a sulfide all-solid-state battery. The preparation process of this battery includes the following steps: Step 1: In a mushroom-shaped container, add 160 mg of DCNT-0417-X2 / DCNT-0417 / TL-1126, 30 mg of Li6PS5Cl sulfide solid electrolyte, 4 mg of vapor-deposited carbon nanofibers (VGCF), and 60 mg of SEBS binder (10% by mass) in a mass ratio of 8:1.5:0.2:0.3. Then add 190 mg of ultra-dry p-xylene, bringing the total mass fraction of DCNT-0417-X2 / DCNT-0417 / TL-1126, Li6PS5Cl sulfide solid electrolyte, vapor-deposited carbon nanofibers, and SEBS binder in the slurry to 45%. Seal the mushroom-shaped container with sealing adhesive and ball mill it in a planetary ball mill at 350 rpm for 1 hour to ensure thorough mixing and obtain a uniformly dispersed negative electrode slurry. In an argon-filled glove box, use an automatic coating agent to coat the slurry onto a copper foil current collector to a thickness of 100 mm. The coating was applied to a diameter of μm, and then the solvent was completely evaporated in a vacuum oven. The coated material was then cut into electrode sheets with a diameter of 12 mm, ultimately yielding a composite silicon-carbon anode of DCNT-0417-X2 / DCNT-0417 / TL-1126. Step 2: Assemble the sulfide all-solid-state battery in an argon-filled glove box. First, weigh 100 mg of sulfide solid electrolyte Li6PS5Cl (LPSC) and grind it twice in a mortar. Spread the ground powder in a mold, then press the solid electrolyte at 175 MPa for 1 min to obtain a solid electrolyte sheet. Then, place the prepared negative electrode sheet into one side of the solid electrolyte sheet in the mold, ensuring the active material is in contact with the solid electrolyte. Pour 30 mg of positive electrode powder into the other side of the solid electrolyte sheet in the mold, press at 175 MPa for 1 min, then increase the pressure to 350 MPa and hold for 5 min. After holding the pressure, slowly depressurize to 30 MPa and tighten the screws. The sulfide all-solid-state battery assembly is now complete.

[0072] Then, electrochemical performance comparison tests were conducted.

[0073] Testing Procedure: The formed sulfide all-solid-state full cells were tested using a Newway test bench at the same current to measure their charge and discharge capacities, and then the initial efficiency was calculated. Next, the cycle performance was tested at 1C.

[0074] like Figure 3As shown, the solid-state battery assembled in Example 1 exhibits significant advantages. Its capacity retention curve is extremely flat, showing almost no degradation from the initial stage to 300 cycles, consistently maintaining a high level close to 100%, far superior to the solid-state batteries assembled in Comparative Examples 1 and 2. The latter two rapidly dropped below 90% in the first 100 cycles and accelerated their degradation after 150 cycles, ultimately retaining only about 85%. Example 1, with its ultra-long cycle life, excellent capacity retention, and extremely low degradation rate, demonstrates its extremely high structural stability and anti-aging capabilities, making it highly suitable for high-performance energy storage applications with stringent long-term stability requirements.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a silicon-carbon composite negative electrode material based on silane cleavage and gradient chemical vapor deposition, characterized in that, Includes the following steps: S1, carbon nanotubes are placed in a vapor deposition reactor, and silane gas and chain hydrocarbon gas are introduced and heated at the same time, so that the active carbon free radicals generated by the cracking of the chain hydrocarbons form heterogeneous nucleation sites on the surface of carbon nanotubes, inducing silicon atoms to be directionally deposited on the surface and inside of carbon nanotubes as nano-silicon particles, forming carbon nanotubes with silicon nanoparticles attached to the surface. S2, acetylene gas is introduced into the vapor deposition reactor and heated to decompose it, thereby coating the carbon nanotubes and silicon particles with a conductive carbon outer layer to obtain a silicon-carbon composite anode material.

2. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, In S1, the vapor deposition reactor includes any one of fluidized bed, rotary kiln, vibrating bed, and fixed bed.

3. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, In S1, the chain hydrocarbon gas is any one of methane, acetylene, ethylene, ethane, propylene, and propane.

4. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, S1, after the carbon nanotubes are placed in the vapor deposition reactor, nitrogen gas is introduced to purge the air.

5. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, In S1, the diameter of the carbon nanotubes is 10nm~50nm.

6. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, In S1, the volume ratio of the silane gas to the chain hydrocarbon gas is 1:1, and the flow rates of both the silane gas and the chain hydrocarbon gas are 0.5 L / min.

7. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, In S1, the silane pyrolysis heating temperature is 400℃~650℃, and the heating time is 30 min~120 min.

8. The method for preparing a silicon-carbon composite anode material according to claim 1, characterized in that, In S2, the acetylene cracking heating temperature is 600℃~900℃, and the heating time is 30 min~90 min.

9. A silicon-carbon composite anode material prepared by any one of claims 1-8, characterized in that, include: Three-dimensional framework of carbon nanotubes; Nanoscale silicon particles deposited on the surface and inside of carbon nanotubes, the silicon particles being formed by the high-temperature pyrolysis of silane; A conductive carbon outer layer coating the surface of carbon nanotubes and silicon particles; The carbon nanotube three-dimensional framework and the conductive carbon outer layer together construct a three-dimensional conductive network.

10. The silicon-carbon composite anode material according to claim 9, characterized in that, The inner layer of silicon particles has a particle size of 10 nm to 50 nm; the outer layer of conductive carbon has a thickness of 5 nm to 20 nm and an electronic conductivity of ≥33 mS / cm.