A core-shell structured carbon composite material and its preparation method

By controlling the nucleation and shell growth of triglyceride pyrolysis carbon deposits in stages, combined with CO2 shaping treatment, the problem of difficulty in controlling the location and extent of triglyceride pyrolysis carbon deposits was solved, achieving structural stability and pore openness of the material, making it suitable for a variety of applications.

CN123105604APending Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611312682.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to control the location and extent of coke buildup from triglyceride pyrolysis, leading to coking on reactor walls, adhesion of carbon particles, and pore blockage, resulting in poor structural repeatability.

Method used

A phased carbon source supply method is adopted, first carrying out the nucleation stage, and then the shell growth stage. By controlling the feed rate and atmosphere conditions of the carbon source stream, discrete deposited nuclei are formed on the surface of porous carbon nuclei, and continuous or island-shaped deposited carbon shells are grown within a limited range, combined with CO2 selective shaping treatment.

Benefits of technology

It effectively controls the location and extent of carbon buildup, reduces coking on reactor walls and pore blockage, improves the structural repeatability and pore accessibility of materials, and is suitable for adsorbent materials, solid fuels and catalyst supports.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105604A_ABST
    Figure CN123105604A_ABST
Patent Text Reader

Abstract

This invention discloses a core-shell structured carbon composite material and its preparation method, belonging to the fields of biomass char materials and triglyceride thermochemical conversion technology. The invention involves carbonizing biomass and activating it with CO2 to obtain a porous carbon core; triglyceride raw material is atomized and fed into a deposition reaction zone, where a nucleation stage and a shell growth stage are sequentially implemented. During the nucleation stage, the triglyceride carbon source flux is strictly controlled at 0.02–0.30 g / (g·h), causing the carbon-containing intermediates formed by pyrolysis to preferentially discretize and nucleate on the outer surface and pores of the porous carbon core; subsequently, the carbon source flux is increased to 1.2–10 times that of the nucleation stage, transforming the deposited carbon from discrete islands into a continuous or interconnected dense outer shell. The deposition endpoint is determined based on parameters such as weight gain or pressure drop, and the composite material is obtained through controlled cooling. This method transforms traditional pyrolysis carbon deposits that lead to catalytic deactivation into a controllable carbon shell structure, achieving synergistic regulation of the core pore structure and shell density, and is suitable for preparing adsorbent materials, solid fuel precursors, and electrochemical carbon material precursors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biochar materials and thermochemical conversion technology of triglycerides, specifically relating to a core-shell structured carbon composite material and its preparation method. Background Technology

[0002] Triglycerides are widely found in vegetable oils, animal oils, and waste oils. Under high temperature, anaerobic or hypoxic environments, they can undergo chain scission, decarboxylation, decarbonylation, dehydrogenation, aromatization, and condensation reactions, forming gaseous, liquid products and solid char deposits. Activated biochar possesses well-developed pores, surface defects, and oxygen-containing functional groups, enabling it to adsorb heavy intermediates formed from triglyceride cracking and promote their further cracking and aromatization. Existing research typically considers coke buildup on the surface of activated biochar as a cause of catalyst deactivation, with technical goals focusing on inhibiting coke buildup, regenerating coke from burnout, or utilizing deactivated char as fuel. Publicly available data also indicates that spherical char particles and concentric shell-like char layers can form during the rapid pyrolysis of rubber seed oil, and pyrolysis coke buildup has been observed on the surface of activated biochar. However, the aforementioned disclosures focus on explaining the morphology of the carbon deposits and the catalytic deactivation mechanism, without establishing a material preparation pathway that uses porous carbon particles as pre-formed nuclei, triglyceride cracking intermediates as the shell carbon source, and coordinates the control of shell formation through differences in carbon source flux between the nucleation and shell growth stages, the deposition endpoint, and optional selective shaping. If deposition continues under single-feed conditions, coking of the reactor wall, adhesion of carbon nuclei, excessively thick shells in certain areas, and complete blockage of pores can easily occur, resulting in poor structural repeatability of the obtained solid. Therefore, it is necessary to transform non-selective carbon deposition into a controllable preparation behavior, allowing the carbon source to first nucleate on the surface of the carbon nuclei, then grow within a confined area, and promptly terminate deposition or perform mild gasification shaping. Summary of the Invention

[0003] This invention aims to solve the problem of difficulty in controlling the location and extent of coking during triglyceride pyrolysis. This invention proposes a core-shell structured carbon composite material and its preparation method. By supplying carbon sources in stages, pyrolysis deposited carbon is directionally constructed on the surface of a porous carbon core, reducing non-target coking on the reactor wall and controlling the degree of pore blockage.

[0004] This invention provides a method for preparing a core-shell structured carbon composite material, comprising the following steps: (1) Carbonize the biochar precursor under an inert atmosphere, and then activate it under an atmosphere containing CO2 or anhydrous air to obtain a porous carbon core; (2) The porous carbon core is placed in a high-temperature deposition reaction zone with an inert or low-oxygen atmosphere, and a carbon source stream is introduced. The nucleation stage is carried out first, followed by the shell growth stage. After the deposition endpoint is reached, the carbon source stream is stopped, and the core-shell structured carbon composite material is obtained by purging with inert gas and controlled cooling. The carbon source stream includes atomized triglyceride-containing raw materials; the feed rate of the carbon source stream during the nucleation stage is controlled at 0.02-0.30 g / (g·h) per unit mass of porous carbon cores, and during the shell growth stage, the feed rate of triglycerides per unit mass of porous carbon cores is 0.05-1.50 g / (g·h), and the feed rate during the shell growth stage is 1.2-10 times that of the nucleation stage, so that the carbon-containing intermediates generated by triglyceride cracking first form discrete deposition nuclei on the outer surface and pores of the porous carbon cores, and then grow laterally through cross-linking into continuous or island-like connected deposition carbon shells.

[0005] Preferably, the biochar precursor is at least one of sawdust, bamboo shavings, rice husks, straw, sugarcane bagasse, fruit shells, hemp stalks, and lignin.

[0006] Preferably, in step (1), the carbonization temperature is 400-800 ℃ and the time is 20-240 min; the activation is carried out after carbonization, and the activation temperature is 650-800 ℃ and the time is 30-180 min. Carbonization is used to convert the biomass precursor into a stable carbon skeleton, and the subsequent activation is used to gasify and etch the carbon skeleton to form pores. The two are two sequential process stages.

[0007] Preferably, the porous carbon core has a particle size of 0.1-8 mm, a BET specific surface area of ​​200-1200 m² / g, a total pore volume of 0.10-0.80 cm³ / g, and includes micropores with a pore size of less than 2 nm.

[0008] Preferably, the triglyceride-containing raw material is at least one of rubber seed oil, hemp seed oil, jatropha oil, kitchen waste oil, animal fat, algal oil, and triglyceride concentrates obtained from the above-mentioned oils.

[0009] Preferably, the median diameter of the atomized triglyceride-containing raw material droplets is 10-100 μm; the carbon source stream also includes at least one carrier gas selected from nitrogen, argon, CO2, water vapor, and non-condensable pyrolysis gas; wherein the carrier gas fraction is 85%-95% during the nucleation stage and 70%-85% during the shell growth stage.

[0010] Preferably, the free oxygen volume fraction during the nucleation stage and the shell growth stage is less than 1%, and more preferably, the free oxygen volume fraction is less than 0.5%.

[0011] Preferably, in step (2), the temperature of the high-temperature deposition reaction zone is 600-750 ℃.

[0012] Preferably, in step (2), the nucleation stage lasts for 1-30 min and the shell growth stage lasts for 5-120 min.

[0013] Preferably, in step (2), the carbon source stream is introduced by pulse feeding, with each feeding lasting 1-30 s and the inert gas interval between two adjacent feedings being 1-120 s; the duty cycle of the nucleation stage is lower than that of the shell growth stage.

[0014] Preferably, in step (2), when the weight gain of the porous carbon core relative to the dry basis before deposition reaches 1-2%, the volume fraction of the sum of outlet hydrogen and carbon monoxide enters a stable plateau, or the bed pressure drop increases by 5-60% relative to before deposition, the deposition is considered to be completed.

[0015] Preferably, after deposition is completed and the zone is purged with inert gas, the temperature of the reaction zone is adjusted and maintained at 650-750 °C, and a composite shaping gas containing 5-100 vol.% CO2 is introduced for 1-60 min to preferentially remove clogging pores or weakly bonded, non-uniformly deposited carbon. Here, "adjustment" includes maintaining, increasing, or decreasing the temperature, depending on the reaction temperature of the previous deposition stage.

[0016] The present invention also claims protection for the preparation method of the core-shell structured carbon composite material, which is a core-shell structured carbon composite material with a porous carbon core as the core and triglyceride pyrolysis deposited carbon as the shell, specifically: a porous biochar core and a triglyceride pyrolysis deposited carbon shell layer located on the outer surface and pores of the porous biochar core, wherein the deposited carbon shell layer is a continuous or island-like interconnected structure.

[0017] Preferably, the deposited carbon shell covers more than 30% of the outer surface area of ​​the porous carbon core, and the deposited carbon shell has an amorphous carbon structure, a disordered carbon structure, or a combination of both.

[0018] The present invention also claims the use of the core-shell structured carbon composite material in adsorbent materials, solid fuel or shaped fuel precursors, electrochemical carbon material precursors, and catalyst supports.

[0019] The technical solution provided by this invention has the following beneficial effects: This invention adopts a process route of "porous carbon nucleus preconstruction - low-flux nucleation - high-flux shell growth - endpoint determination - inert purging and controlled cooling". In the low-flux nucleation stage, the instantaneous supersaturation is reduced, so that carbon-containing intermediates are preferentially captured by the defect sites and pores of the porous carbon nuclei; then the carbon source feed rate, carbon source partial pressure or pulse duty cycle are increased to promote the lateral connection and radial growth of the formed deposited nuclei; when the preset weight gain rate, exhaust gas plateau, pressure drop increase or deposition time is reached, carbon supply is stopped to reduce particle adhesion and complete pore closure caused by excessive deposition.

[0020] This invention uses CO2 for short-term selective shaping, which can preferentially gasify non-uniformly deposited carbon with high activity, blocked pores, or weak bonding, while preserving the main body of the deposited carbon shell and reopening some of the blocked pores, thereby improving the pore accessibility of the obtained material. Attached Figure Description

[0021] Figure 1 This is a process flow diagram for core-shell structured carbon composite materials.

[0022] Figure 2 The infrared image of the core-shell structured carbon composite material in Example 1 is shown in (a) for the distribution of oxygen-containing functional groups, (b) for the distribution of aliphatic functional groups, and (c) for the distribution of hydroxyl functional groups.

[0023] Figure 3 This is a Raman diagram of the core-shell structured carbon composite material of Example 1.

[0024] Figure 4 The image shows the BET results of the core-shell structured carbon composite material in Example 1. From left to right, the images are the original porous carbon core, the pre-shaping deposited sample, and the post-shaping composite material.

[0025] Figure 5 This is a schematic diagram of a core-shell structured carbon composite material. Detailed Implementation

[0026] To better understand the technical content of this invention, specific embodiments are provided below to further illustrate this invention.

[0027] Example 1 like Figure 1 A method for preparing a core-shell structured carbon composite material includes the following steps: Preparation of porous carbon cores: Waste industrial hemp stalks were selected as biochar precursors, dried at 105 °C until the moisture content was below 5%, pulverized, and sieved to obtain particles of 0.1–0.5 mm. 50 g of these particles were placed in a reactor, and the system was purged with 99.9% pure nitrogen. Under nitrogen protection, the temperature was increased to 600 °C at a rate of 15 °C / min and maintained for 60 min to complete carbonization. Subsequently, the temperature was adjusted to 700 °C, and CO2 was introduced and maintained for 100 min for activation. After activation, nitrogen was switched back and the mixture was cooled to room temperature. The porous biochar cores were obtained by sieving. The carbonization stage was used to form a stable carbon framework, while the subsequent CO2 activation stage formed surface defects and open pores through gasification etching. These two stages were performed sequentially. The actual dry weight of the obtained biochar cores was denoted as m0; their particle size, specific surface area, total pore volume, and pore size distribution were characterized by sieving and nitrogen adsorption-desorption methods, respectively. After loading 12.00g of carbon core, the initial bed pressure drop ΔP was measured to be 0.82kPa under the set nitrogen flow rate, which was used as the benchmark for judging the subsequent deposition endpoint.

[0028] Staged controlled deposition: 12.00 g of porous carbon cores were packed into the deposition reaction zone and heated to 750 ℃ ​​under a nitrogen atmosphere. Dehydrated and filtered rubber seed oil was used as the carbon source and atomized to a droplet median diameter of 70 μm. A two-stage pulse feeding method was employed: Stage 1 was the nucleation stage, with an average feed rate of 0.05 g / (g·h) per unit mass of porous carbon cores, a single feed interval of 5 s, followed by nitrogen purging for 55 s, lasting 10 min, corresponding to a theoretical oil input of 0.100 g; Stage 2 was the shell growth stage, with the average feed rate increased to 0.30 g / (g·h), a single feed interval of 15 s, followed by nitrogen purging for 15 s, lasting 45 min, corresponding to a theoretical oil input of 2.700 g. The total theoretical oil input for both stages was 2.800 g, or 0.233 g / g carbon core. After completing the two stages, the outlet H2 and CO concentrations stabilized at 6.8 vol.% and 4.1 vol.% respectively in the last 5 minutes, with fluctuations of less than 3%. The bed pressure drop increased from 0.82 kPa to 0.98 kPa, approximately 1.20 times the initial value. Rubber seed oil feeding was stopped, and the bed was purged with pure nitrogen. After cooling to room temperature, the dry basis mass m1 of the composite material before shaping was measured to be 12.240 g, and the mass of deposited carbon was 0.240 g. Calculated using η=(m1-m0) / m0×100%, the dry basis weight gain η was 2.00%, and the mass of deposited carbon accounted for 8.57% of the theoretical oil input.

[0029] CO2 selective shaping: To selectively reshape the pores that might be obscured by non-uniform carbon deposits after deposition, the reaction zone was maintained at 750 °C after stopping the feed and completing nitrogen purging. A composite reshaping gas consisting of 30 vol.% CO2 and 70 vol.% N2 was introduced and treated for 20 min; then CO2 was stopped and nitrogen cooling was switched on. After cooling, the dry basis mass (m2) of the reshaped composite material was measured to be 12.200 g. The reshaping process removed 0.040 g of weakly bonded deposited carbon, and the net weight gain relative to the original carbon core was 1.67%. This mass change indicates that the short-term CO2 treatment mainly removed the highly active non-uniform deposited carbon at the pores without causing significant loss of the continuous shell matrix.

[0030] The shell thickness of the shaped samples ranged from 0.8 to 2.5 μm, with an average thickness of 1.6 μm. Based on the proportion of the arc length of the continuous or island-like interconnected depositional layers around the particles to the total arc length of the outer perimeter, the outer surface coverage was approximately 72%. Combined with FTIR (… Figure 2 ) and Raman spectroscopy ( Figure 3 The results confirmed that the core-shell structured carbon composite material has two carbons with different chemical structures. According to the corresponding analysis, the outer layer deposit is identified as pyrolytic carbon formed by the cracking of rubber seed oil. The above-mentioned thickness, coverage and 2.00% dry basis weight gain before shaping together indicate that the obtained material has a core-shell structure composed of a porous carbon core and a surface deposited carbon shell. Figure 5 This is a schematic diagram drawn based on the above structure.

[0031] according to Figure 4 The BET specific surface areas of the original porous carbon core, the pre-deposition sample, and the post-deposition composite material, measured using nitrogen adsorption-desorption, were 648 m² / g, 512 m² / g, and 556 m² / g, respectively, with total pore volumes of 0.42 cm³ / g, 0.34 cm³ / g, and 0.37 cm³ / g, respectively. The decrease in specific surface area and total pore volume after deposition indicates that the deposited carbon covered part of the outer surface and pore openings. After CO2 shaping, these two indicators recovered to 85.8% and 88.1% of the original carbon core, respectively, consistent with the structural effect of removing the weakly bound deposited carbon at the pore openings. The higher heating value of the post-deposition composite material, measured using bomb calorimetry, was 28.605 MJ / kg, indicating that this material has the potential for application as a precursor for solid fuels or shaped fuels; its retained pore structure also provides a basis for further use as an adsorbent material or catalyst support.

[0032] Example 2 A method for preparing a core-shell structured carbon composite material includes the following steps: Preparation of porous carbon cores: Waste wood chips were selected as the biochar precursor, dried at 105 °C until the moisture content was less than 5%, pulverized, and sieved to obtain particles of 0.1–0.5 mm. 50 g of these particles were placed in a reactor, and the system was purged with 99.9% pure nitrogen. Under nitrogen protection, the temperature was raised to 400 °C and maintained for 240 min to complete carbonization. Subsequently, the temperature was raised to 650 °C, and CO2 was introduced and maintained for 180 min for activation. After activation, nitrogen was switched back to the reactor and the mixture was cooled to room temperature. The porous biochar cores were obtained by sieving, and the actual dry basis mass m0 of the obtained biochar cores was recorded.

[0033] Staged controlled deposition: 13,500 g of porous carbon cores were packed into the deposition reaction zone and heated to 600 °C under a nitrogen atmosphere. Dehydrated and filtered hemp seed oil was used as the carbon source and atomized to a droplet median diameter of 100 μm. During the nucleation stage, the average feed rate of hemp seed oil per unit mass of porous carbon cores was 0.30 g / (g·h) for 1 min. During the shell growth stage, the average feed rate of hemp seed oil per unit mass of porous carbon cores was increased to 1.50 g / (g·h) and maintained for 5 min. After both stages, feeding was stopped based on any one of the following conditions: a dry basis weight gain of 1%, outlet H2 and CO concentrations reaching a stable plateau, or bed pressure drop reaching 1.2 times the initial value ΔP. Nitrogen purging was then applied. After cooling, the dry basis mass m1 of the composite material was measured to be 13.635 g, an increase of 0.135 g relative to the 13,500 g carbon cores, corresponding to a dry basis weight gain of 1.00%. Based on the above settings, the theoretical total oil injection amount for the two stages is 1.755 g, which is 0.130 g / g carbon core, and the mass of deposited carbon accounts for 7.69% of the theoretical oil injection amount.

[0034] CO2 selective shaping: After nitrogen purging, the reaction zone was heated from 600 °C to 650 °C and maintained at a stable temperature. A composite shaping gas consisting of 5 vol.% CO2 and 95 vol.% N2 was introduced and treated for 60 min. Subsequently, CO2 was stopped and the zone was cooled under a nitrogen atmosphere. The lower CO2 volume fraction combined with the longer treatment time was used to slow down the vaporization rate and reduce the risk of excessive consumption of the shell bulk.

[0035] This embodiment uses a higher instantaneous carbon source flux and a shorter deposition time, which can quickly improve the deposition coverage on the outer surface of the carbon core. Compared with Example 1, the resulting shell is more likely to be interconnected in an island shape and have certain local thickness differences. Subsequent low-concentration CO2 long-term shaping helps to remove weakly bonded non-uniformly deposited carbon and improve pore accessibility.

[0036] The resulting material can be verified by cross-sectional SEM or TEM to show the spatial relationship between the carbon core and the outer layer of deposited carbon, and the pore accessibility before and after shaping can be evaluated by nitrogen adsorption-desorption. Based on its relatively fast carbon deposition mode, this material can be preferentially used as a precursor for solid fuels or shaped fuels, and can also be used as an adsorbent or catalyst support after the pore structure and surface chemistry are evaluated.

[0037] Example 3 A method for preparing a core-shell structured carbon composite material includes the following steps: Preparation of porous carbon cores: Waste wood chips were selected as the biochar precursor, dried at 105 °C until the moisture content was less than 5%, pulverized, and sieved to obtain particles of 0.1-0.5 mm. 50 g of these particles were placed in a reactor, and the system was purged with 99.9% pure nitrogen. The temperature was raised to 800 °C and maintained for 20 min under nitrogen protection to complete carbonization. Subsequently, CO2 was introduced, and the reactor was activated at 800 °C for 30 min. After activation, nitrogen was switched back to the reactor and the mixture was cooled to room temperature. The porous biochar cores were obtained by sieving, and the actual dry basis mass m0 of the obtained biochar cores was recorded.

[0038] Staged controlled deposition: 11,800 g of porous carbon cores were packed into the deposition reaction zone and heated to 700 °C under a nitrogen atmosphere. Dehydrated and filtered Jatropha curcas oil was used as the carbon source, which also included N2, and was atomized to a droplet median diameter of 10 μm. During the nucleation stage, the average Jatropha curcas oil feed rate per unit mass of porous carbon cores was 0.02 g / (g·h), with continuous feeding for 30 min, and the N2 carrier gas fraction was 90%. During the shell growth stage, the average Jatropha curcas oil feed rate per unit mass of porous carbon cores was 0.05 g / (g·h), with continuous feeding for 120 min, and the N2 carrier gas fraction was 80%. After both stages were completed, Jatropha curcas oil feeding was stopped and nitrogen purging was initiated when any of the following conditions were met: the dry basis weight gain reached 2%, the outlet H2 and CO concentrations reached a stable plateau, or the bed pressure drop increased by 5% relative to the initial value. After cooling, the dry basis mass m1 of the composite material was measured to be 12.036 g, which is an increase of 0.236 g relative to the 11.800 g carbon core, corresponding to a dry basis weight gain of 2.00%. According to the above settings, the theoretical total oil addition in the two stages is 1.298 g, i.e., 0.110 g / g carbon core, and the mass of deposited carbon accounts for 18.18% of the theoretical oil addition.

[0039] CO2 selective shaping: After nitrogen purging, the reaction zone was cooled from 700 °C to 650 °C and maintained at a stable temperature. 100 vol.% CO2 shaping gas was introduced and treated for 1 min. CO2 was then stopped and nitrogen cooling was immediately switched on. The combination of a high CO2 volume fraction and an extremely short treatment time was used to rapidly remove highly active, non-uniformly deposited carbon while limiting the gasification loss of the continuous shell bulk.

[0040] This embodiment employs a lower carbon source flux and a longer deposition time, controlling the dry basis weight gain at 2.0%, resulting in a lower instantaneous concentration of pyrolysis intermediates on the carbon core surface. The resulting deposited carbon layer is relatively thin, mainly distributed on the outer surface and pore area, yet still forms a core-shell structure similar to that of Example 1, with a lower tendency for complete pore closure and particle adhesion. Therefore, a dry basis weight gain of 2.0% can be considered the upper limit of the deposition endpoint range of this invention; further increasing the weight gain will increase the risk of excessively thick shells, pore occlusion, and particle bridging.

[0041] The core-shell spatial relationship of the obtained material can be observed by cross-sectional SEM or TEM, the shell continuity can be judged by Raman spectroscopy and surface elemental analysis, and the pore openness can be evaluated by nitrogen adsorption-desorption testing. This material is more suitable as an adsorbent material or catalyst support precursor that requires the preservation of pore accessibility; whether it can be used in electrochemical materials should be further evaluated based on conductivity, rate performance, and cycle stability.

[0042] Comparative Example 1 The method for preparing a core-shell structured carbon composite material in this comparative example differs from that in the previous examples in that: The only difference between this comparative example and Example 1 is that the low-throughput nucleation stage and the high-throughput shell growth stage are not set, but a constant average flux continuous feeding is used; the other reaction temperature, carbon nuclei, oil type, theoretical total oil input and total feeding time remain the same.

[0043] An equal amount of porous carbon cores used in Example 1 were loaded into the same reactor. The reaction temperature was maintained at 750 °C, and rubber seed oil was used as the carbon source. A constant average feed rate of 0.255 g / (g·h) was continuously fed for 55 min. This average feed rate was obtained by dividing the total amount of oil input in the two stages of Example 1 by the total feeding time, so that the theoretical total amount of oil input in this comparative example and Example 1 was approximately 0.233 g / g carbon core. Due to the high carbon source flux in the initial stage, the pyrolysis intermediates were more likely to simultaneously condense at the pore opening and particle contact point, resulting in excessively thick local deposition, pore opening obstruction, particle adhesion, and non-target coking on the reactor wall; the uniformity and controllability of the resulting deposition layer were lower than those in Example 1.

[0044] Example 1 differs from this comparative example only in the feeding sequence. Therefore, the difference between the two can be used to illustrate the effect of two-stage flux control: first, a low flux is used to form dispersed deposition nuclei, and then a higher flux is used to promote their connectivity. This is more conducive to controlling the shell position, reducing particle adhesion, and retaining some open pores than using a constant higher flux from the beginning.

[0045] In terms of application performance, the material obtained in this comparative example is not expected to perform as well as in adsorption, catalytic support or electrochemical precursor applications that rely on open channels and mass transfer efficiency as in Example 1. If used as a fuel precursor, its deposited carbon can still increase the fixed carbon composition, but particle adhesion and wall coking will reduce process stability and product uniformity.

[0046] Comparative Example 2 A method for preparing a core-shell structured carbon composite material includes the following steps: Preparation of porous carbon cores: Waste industrial hemp stalks were selected as biochar precursors, dried at 105 °C until the moisture content was below 5%, pulverized, and sieved to obtain particles of 0.1–0.5 mm. 50 g of these particles were placed in an activation furnace, and the system was purged with nitrogen gas of 99.9% purity. Subsequently, 100% CO2 (by volume) was introduced as an activator, and the temperature was increased to 700 °C at a rate of 15 °C / min and maintained at this temperature for 100 min. After cooling to room temperature, porous biochar cores were obtained by sieving.

[0047] Staged controlled deposition: Porous carbon cores were loaded into the deposition reaction zone and heated to 750 °C under a nitrogen atmosphere. Dehydrated and filtered rubber seed oil was selected as the carbon source. The rubber seed oil was atomized, with a median droplet diameter of 70 μm. The thermochemical cracking process of rubber seed oil exhibited significant phase reconstruction behavior, and the polycyclic aromatic hydrocarbons formed after decarbonylation and decarboxylation were precursors for the formation of deposited carbon. To transform disordered carbon deposits into ordered shells, a two-stage carbon source supply strategy was implemented: Stage 1 (nucleation stage) employed low-flux continuous feeding, with the rubber seed oil feed rate per unit mass of porous carbon cores strictly controlled at 0.05 g / (g·h) for 10 min. Under extremely low carbon source partial pressure, the mass transfer of heavy intermediates generated by cracking was controlled by internal diffusion, preferentially captured by high-energy defect sites and mesopores on the carbon core surface, forming discontinuous discrete island-like deposited nuclei. This stage avoided the instantaneous agglomeration phenomenon on the pore surface caused by instantaneous supersaturation. In Phase Two (shell growth phase), the feed rate was rapidly increased to 0.30 g / (g·h) and maintained for 45 min. High-flux carbon supply caused the deposition reaction to shift to external diffusion control. The newly formed liquid film and polycyclic aromatic hydrocarbons used the existing deposition cores as templates for lateral cross-linking and radial growth. As deep aromatization progressed, the deposited carbon gradually transformed from a discrete state into a continuous and dense carbon shell. The system monitored the H2 and CO concentrations at the reactor outlet and the bed pressure drop in real time. The kinetic endpoint was determined when the dry weight gain of the carbon core reached 15% or the bed pressure drop abruptly increased to 1.2 times ΔP. ​​The rubber seed oil feed was immediately cut off, and high-flow-rate pure nitrogen purging was switched to remove incompletely carbonized free tar. The resulting composite material was then cooled under an inert atmosphere of pure nitrogen to obtain a core-shell structured carbon composite.

[0048] Without CO2 shaping, the core shell remains intact, but blockages or weakly bonded, heterogeneous carbon deposits are not selectively removed, resulting in a lower expected number of open pores and pore accessibility compared to Example 1. This difference is more detrimental to adsorbent materials, catalyst supports, and electrochemical precursors that rely on intrapore mass transfer; however, the impact is relatively smaller for solid fuel precursors where the primary concern is fixing carbon content. Therefore, this comparative example illustrates that CO2 shaping is not a necessary prerequisite for forming a core-shell structure, but rather a preferred post-processing step to improve pore openness and material mass transfer performance.

[0049] Comparative Example 3 A method for preparing a core-shell structured carbon composite material includes the following steps: Preparation of porous carbon cores: This comparative example uses the porous biochar cores prepared in Example 1, and performs staged pulse feeding according to the conditions of Example 1. The difference is that after the nucleation stage is completed, feeding continues at the average feed rate and pulse duty cycle of the shell growth stage until the dry weight gain of the biochar core reaches 30%, then feeding is stopped and the core is purged with nitrogen. This 30% dry weight gain is significantly higher than the 1-2% range specified in this invention.

[0050] Porous carbon nuclei were packed into the deposition reaction zone and heated to 750 °C under a nitrogen atmosphere. Dehydrated and filtered rubber seed oil was used as the carbon source and atomized to a droplet median diameter of 70 μm. The average feed rate for the nucleation stage was 0.05 g / (g·h), with a single feed interval of 5 s and a nitrogen gas interval of 55 s, lasting for 10 min. The average feed rate for the shell growth stage was 0.30 g / (g·h), with a single feed interval of 15 s and a nitrogen gas interval of 15 s, and the feed was extended until the measured dry basis weight gain reached 30%. After reaching the endpoint, the rubber seed oil feed was stopped and the mixture was purged with nitrogen.

[0051] CO2 selective shaping: After stopping the feed and completing nitrogen purging, the reaction zone was maintained at 750 °C, and a composite shaping gas consisting of 30 vol.% CO2 and 70 vol.% N2 was introduced for 20 min; then CO2 was stopped and nitrogen cooling was switched on. The shaping conditions were the same as in Example 1 to compare the effects of different deposition endpoints on the final structure.

[0052] Compared to Example 1, where deposition ceased at a 2% dry-basis weight gain, this comparative example extended high-throughput shell growth to 30%, a endpoint significantly exceeding the 1-2% range defined in this invention. The resulting deposited carbon outer layer was noticeably thicker and locally uneven, exhibiting pore occlusion, bridging between adjacent particles, and particle adhesion. Even with subsequent CO2 shaping conditions similar to those in Example 1, it was difficult to completely eliminate the deep pore occlusion caused by excessive deposition. Therefore, the core-shell ratio, pore openness, process stability, and particle uniformity of the material obtained at a 30% weight gain were inferior to those of Examples 1 and 3, demonstrating the necessity of limiting the dry-basis weight gain to 1-2%.

[0053] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or improvement of the technology in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a core-shell structured carbon composite material, characterized in that, Includes the following steps: (1) Carbonize the biochar precursor under an inert atmosphere, and then activate it under an atmosphere containing CO2 or anhydrous air to obtain a porous carbon core; (2) The porous carbon core is placed in a high-temperature deposition reaction zone with an inert or low-oxygen atmosphere, and a carbon source stream is introduced. The nucleation stage is carried out first, followed by the shell growth stage. After the deposition endpoint is reached, the carbon source stream is stopped, and the mixture is purged with inert gas and cooled to obtain a core-shell structured carbon composite material. The carbon source stream includes atomized triglyceride-containing raw materials. The feed rate of the carbon source stream during the nucleation stage is controlled as follows: the triglyceride feed rate per unit mass of porous carbon nuclei is controlled as 0.02-0.30 g / (g·h), and the triglyceride feed rate per unit mass of porous carbon nuclei during the shell growth stage is controlled as 0.05-1.50 g / (g·h). Furthermore, the feed rate of the carbon source stream during the shell growth stage is 1.2-10 times that of the feed rate during the nucleation stage.

2. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, The biochar precursor is at least one of sawdust, bamboo shavings, rice husks, straw, sugarcane bagasse, fruit shells, hemp stalks, and lignin.

3. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, In step (1), the carbonization temperature is 400-800 ℃ and the time is 20-240 min; the activation temperature is 650-800 ℃ and the time is 30-180 min.

4. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, The triglyceride-containing raw materials are at least one of rubber seed oil, hemp seed oil, jatropha oil, kitchen waste oil, animal fats, algal oil, and triglyceride concentrates obtained from the above-mentioned oils.

5. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, The median diameter of the atomized triglyceride-containing raw material droplets is 10-100 μm; the carbon source stream also includes at least one carrier gas selected from N2, Ar, CO2, water vapor, and non-condensable pyrolysis gas; wherein the carrier gas fraction is 85%-95% during the nucleation stage and 70%-85% during the shell growth stage.

6. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, In step (2), the temperature of the high-temperature deposition reaction zone is 600-750 ℃; the nucleation stage lasts for 1-30 min, and the shell growth stage lasts for 5-120 min.

7. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, In step (2), the carbon source stream is fed by pulse feeding, with each feeding lasting 1-30s. An inert gas purging interval is set between two adjacent feedings, with an interval of 1-120s. The duty cycle of the nucleation stage is lower than that of the shell growth stage.

8. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, In step (2), when the weight gain of the porous carbon core relative to the dry basis before deposition reaches 1-2%, the volume fraction of the sum of H2 and CO at the outlet enters a stable plateau, or the bed pressure drop increases by 5-60% relative to before deposition, the deposition is considered to be complete.

9. The method for preparing the core-shell structured carbon composite material as described in claim 1, characterized in that, In step (2), during the inert gas purging, the temperature of the reaction zone is adjusted and maintained at 600-750 ℃, and a composite shaping gas containing 5-100 vol.% CO2 is introduced for treatment for 1-60 min.

10. The core-shell structured carbon composite material prepared by the method of any one of claims 1-9, characterized in that, A core-shell structured carbon composite material with a porous carbon core as the core and triglyceride pyrolysis deposited carbon as the shell.