A method for preparing high-density secondary graphite particles by two-step granulation of natural graphite, its products and applications

By employing a two-step granulation process, ultrafine natural graphite particles are first treated with thermosetting epoxy resin, and then asphalt is added to construct a gradient composite structure. This solves the problem of high-density granulation of ultra-small diameter natural graphite particles, achieving high-density, highly conductive secondary graphite particles suitable for fast-charging lithium-ion battery anode materials.

CN123105628APending Publication Date: 2026-11-17CNBM HEILONGJIANG GRAPHITE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611409708.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively solve the problem of high-density granulation of ultra-small-diameter natural graphite particles, resulting in insufficient particle mechanical strength and an imperfect conductive network. This makes it difficult to suppress lithium plating under high-rate charging, thus limiting its application in fast-charging anode materials.

Method used

A two-step granulation process is adopted. First, natural graphite is ultra-finely pulverized by ball milling or air jet milling, and then mechanically fused and cured with thermosetting epoxy resin to form primary particles with a certain mechanical strength. Then, asphalt is added for secondary granulation to construct a gradient composite structure with an inner resin carbon skeleton and an outer asphalt carbon conductive network.

Benefits of technology

It significantly improves the tap density and formability of the particles, forming regular spherical high-density secondary graphite particles with excellent mechanical strength, perfect conductive network, good cycle stability, and can achieve excellent fast charging performance without lithium plating under 6C charging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105628A_ABST
    Figure CN123105628A_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing high-density secondary graphite particles using a two-step granulation process for natural graphite, along with the resulting products and applications, belonging to the technical field of graphite anode materials for lithium-ion batteries. To address the problem of extremely low particle density in traditional granulation of ultra-small-particle-size natural graphite with a D50 of 1-3 μm, this invention provides a method for preparing high-density secondary graphite particles using a two-step granulation process. Natural graphite is used as raw material, and after ultrafine grinding and shaping to obtain powder with a D50 of 1-3 μm, it is mechanically fused with a binder and solidified to obtain primary particles with a D50 of 5-8 μm. Then, asphalt is added, and the mixture is granulated in an inert atmosphere at a staged heating temperature of 600-800℃ for 2-8 hours to obtain secondary particles with a D50 of 10-18 μm and a tap density of not less than 1.05 g / cm³. 3 The particles are regular and spherical with uniform particle size distribution and high mechanical strength. They are not easily broken during subsequent graphitization and electrode preparation, and can be used as a high-quality graphitization precursor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of graphite anode material technology for lithium-ion batteries, and particularly relates to a method for preparing high-density secondary graphite particles by two-step granulation of natural graphite, as well as its products and applications. Background Technology

[0002] With the increasing demand for fast charging in electric vehicles, small-particle-size natural graphite has attracted widespread attention due to its shorter lithium-ion diffusion path. However, when the particle size of natural graphite is reduced to D50 of 1~3μm, the specific surface area of ​​the particles increases dramatically, making it difficult for binders to uniformly coat the particles. Traditional one-step asphalt thermal granulation processes cannot effectively aggregate ultrafine particles, resulting in extremely low bulk density, with a tap density typically only reaching 0.65g / cm³. 3 The limited availability of ultrafine natural graphite severely restricts its application in the field of fast-charging negative electrodes.

[0003] Existing one-step granulation methods cannot allow for the designed control of the internal structure of the particles, resulting in secondary particles with a single structure that makes it difficult to simultaneously achieve both mechanical strength and electrochemical performance. For ultra-small particle size natural graphite, a single pitch-bonded system cannot simultaneously achieve the firm aggregation of particles and the construction of a surface conductive network during the granulation process, leading to easy breakage of particles during subsequent graphitization and electrode preparation, and insufficient stability of the cycle structure.

[0004] Furthermore, existing ultrafine natural graphite fast-charging anode solutions struggle to suppress lithium plating on the electrode surface under high-rate charging conditions of 6C and above, posing a safety risk. While ultrafine particles shorten the lithium-ion diffusion path, the uneven distribution of pores and imperfect conductive network within the granulated particles lead to a mismatch between the lithium-ion insertion rate and charge transfer rate during high-rate charging, easily causing lithium plating on the anode surface and limiting the performance of ultra-fast charging.

[0005] Therefore, how to effectively granulate ultra-small diameter natural graphite particles, construct high-density secondary particles with gradient internal structures, balance high compaction density and particle mechanical strength, and lay the structural foundation for achieving lithium-free electrode plates under 6C charging after graphitization has become a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] To address the problem of extremely low granulation density in traditional methods for producing ultra-small natural graphite with a D50 of 1~3μm, this invention provides a method for preparing high-density secondary graphite particles through a two-step granulation process, along with the resulting products and applications.

[0007] The technical solution of the present invention:

[0008] A two-step granulation method for preparing high-density secondary graphite particles from natural graphite includes the following steps:

[0009] Step 1: Using natural graphite as raw material, it is ultra-finely pulverized by ball milling or air jet milling, and mechanical particle shaping is combined to trim the particle edges and eliminate flaky debris, so as to obtain ultra-fine natural graphite particle powder with uniform particle size, regular morphology and D50 of 1~3μm.

[0010] Step 2: At room temperature of 15~35℃, 85%~97% of the ultrafine natural graphite powder obtained in Step 1 is mechanically fused with 3%~15% of the binder to obtain primary particles with a D50 of 5~8μm. The primary particles are then cured at 100~200℃.

[0011] Step 3: Add asphalt to the cured primary granules, wherein the mass of the asphalt is 15% to 30% of the mass of the cured primary granules; place the uniformly mixed material in a horizontal reactor and perform secondary granulation under an argon or nitrogen atmosphere, gradually increasing the temperature to the target temperature of 600 to 800°C at a heating rate of 1 to 10°C / min, and holding at the target temperature until the end of secondary granulation, while simultaneously completing the carbonization and shaping of the asphalt; the total time for secondary granulation, including the heating time, is 2 to 8 hours, resulting in high-density graphite secondary granules with a D50 of 10 to 18 μm.

[0012] Furthermore, the adhesive used in step two is a thermosetting epoxy resin, which does not contain a curing agent and has a curing temperature of 100~200℃.

[0013] Furthermore, in step two, the rotation speed of the fusion treatment is 500~3000 rpm, and the fusion treatment time is 1~2 h; the heating rate of the curing treatment is 1~10℃ / min, and the curing time is 1~5 h.

[0014] Furthermore, the asphalt described in step three is coal tar pitch, petroleum asphalt, or mesophase asphalt, with a softening point of 60~120℃, a coking value of 40%~70%, a quinoline insoluble content of ≤1%, and a particle size of 5~8μm.

[0015] Furthermore, during the heating and heat preservation process of the secondary granulation in step three, the reactor continues to rotate, with a reactor speed of 10~30 rpm and an equipment axis tilt angle of 3°~8°.

[0016] Furthermore, in step three, the temperature is increased in stages from room temperature to 300℃ and held for 0.5~2 hours, then increased to 600℃ and held until the second granulation is completed.

[0017] Alternatively, the temperature can be raised from room temperature to 300℃ and held for 0.5 to 2 hours, then raised to 600℃ and held for 0.5 to 2 hours, and then raised to the target temperature and held until the secondary granulation is completed.

[0018] Furthermore, the heating rate in step three is 3~5℃ / min for the staged heating.

[0019] Furthermore, the process includes a fourth post-processing step: the secondary particles obtained in step three are broken down and deagglomerated, then sieved through a 150-325 mesh vibrating screen, and the undersize material is collected.

[0020] A high-density secondary graphite particle prepared by the method provided by the present invention has a gradient composite structure with ultrafine natural graphite primary particles as the core, inner resin carbon as the bonding skeleton, and outer pitch carbon as the coating layer.

[0021] The application of the high-density secondary graphite particles prepared by this invention as a graphitization precursor in the preparation of anode materials for fast-charging lithium-ion batteries.

[0022] The beneficial effects of this invention are:

[0023] This application employs a two-step granulation process. First, ultrafine natural graphite particles are mechanically fused and bonded using thermosetting epoxy resin. A subsequent curing treatment imparts sufficient mechanical strength to the particles, overcoming the technical bottlenecks of poor flowability of ultrafine particles and difficulty in uniformly coating the binder. This significantly improves granulation density and particle formability. Next, asphalt is added for high-temperature rolling granulation. During heating and heat preservation, the asphalt gradually softens and coats the particles, simultaneously completing carbonization and shaping during the target temperature heat preservation stage. The final product has a D50 of 10~18μm and a tap density of not less than 1.05g / cm³. 3 The high-density secondary graphite particles have regular spherical morphology and uniform particle size distribution, and can be used as graphitization precursors.

[0024] This application utilizes a sequential design of resin curing and pitch spheroidization to construct a gradient composite carbon structure. The inner layer of resin carbon provides skeletal strength, while the outer layer of pitch carbon provides conductivity and interfacial compatibility. This structure makes the secondary particles less prone to breakage during subsequent graphitization and electrode fabrication, exhibiting excellent mechanical strength. Simultaneously, the outer pitch carbon improves the conductive network on the particle surface and its interfacial compatibility with the electrolyte. Furthermore, because the base particles are ultrafine natural graphite, the lithium-ion diffusion path is short, the absolute change in particle volume is small, and the internal stress is low, making them less prone to breakage. Stable conductive connections are formed between the particles through the resin carbon and pitch carbon skeletons, resulting in good cycle stability and laying a structural foundation for excellent fast-charging performance after graphitization. After graphitization, the resulting anode material exhibits an initial discharge specific capacity of no less than 355 mAh / g and an initial coulombic efficiency of no less than 92%. No lithium plating is observed on the electrode at a 6C charging rate, demonstrating promising prospects for ultra-fast charging applications. Attached Figure Description

[0025] Figure 1 This is a particle size distribution curve of the ultrafine graphite powder used in Example 1.

[0026] Figure 2 The particle size distribution curve of the primary particles obtained in Example 1 is shown.

[0027] Figure 3 This is a particle size distribution curve of the secondary particles obtained in Example 1. Detailed Implementation

[0028] The technical solution of the present invention will be further described below with reference to embodiments, but it is not limited thereto. Any modifications or equivalent substitutions to the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be covered within the protection scope of the present invention. In the following embodiments, the process equipment or apparatus not specifically specified are all conventional equipment or apparatus in the art. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commercially available; unless otherwise specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.

[0029] Example 1

[0030] This embodiment provides a two-step granulation method for preparing high-density secondary graphite particles from natural graphite, including the following steps:

[0031] Step 1: Using natural flake graphite as raw material, the material is ultra-finely pulverized by ball milling and mechanically shaped to trim the edges and corners of the particles and eliminate flaky debris, resulting in ultra-fine natural graphite particle powder with uniform particle size, regular morphology, and D50 of 2μm.

[0032] Step 2: Using bisphenol A type epoxy resin as the thermosetting epoxy resin, with an epoxy value of 0.40~0.55 eq / 100g and a viscosity of 5000~20000 mPa·s at 25℃. The bisphenol A type epoxy resin does not contain a curing agent and undergoes a cross-linking curing reaction at 100~200℃.

[0033] At room temperature of 25℃, 92.6% by mass of the ultrafine natural graphite powder obtained in step one and 7.4% by mass of thermosetting epoxy resin were added to a fusion machine (VS-1000) for mechanical fusion treatment. The fusion machine speed was 1500 rpm and the fusion treatment time was 1.5 h, resulting in primary particles with a D50 of approximately 6 μm. Subsequently, the particles were cured at 150℃ for 2 h at a curing rate of 5℃ / min, resulting in primary particles with a certain mechanical strength.

[0034] Step 3: Weigh 20% of the mass of the solidified coal tar pitch particles. The coal tar pitch has a softening point of 80℃, a coking value of 55%, a quinoline insoluble content of ≤1%, and a particle size of 5~8μm.

[0035] Coal tar pitch was added to the solidified primary granules, mixed thoroughly, and then placed in a horizontal reactor for secondary granulation under an argon protective atmosphere. During the secondary granulation process, the reactor rotated continuously at a speed of 15 rpm, with the equipment axis tilted at 5°. The temperature was increased from room temperature to 300°C at a rate of 5°C / min and held for 1 hour, then increased to 600°C and held for 1 hour, and finally increased to 700°C and held until the secondary granulation was completed. The total secondary granulation time, including the heating time, was 4 hours, simultaneously completing the carbonization and shaping of the asphalt to obtain high-density graphite secondary granules.

[0036] Step 4: The obtained secondary particles are broken down and deagglomerated, then sieved through a 325-mesh vibrating screen. The undersize material is collected to obtain the finished product. This process does not require demagnetization treatment or asphalt carbon coating modification.

[0037] The ultrafine natural graphite powder obtained in step one, the primary particles obtained in step two, and the high-density secondary graphite particles obtained in step three of this embodiment were used to determine the particle size distribution according to GB / T 19077 "Particle Size Analysis - Laser Diffraction Method". The particle size distribution curves are shown below. Figure 1 , Figure 2 and Figure 3 As shown, the D10 of ultrafine natural graphite powder is 0.546 μm, D50 is 1.734 μm, and D90 is 5.955 μm; the D10 of primary particles is 3.431 μm, D50 is 6.228 μm, and D90 is 11.14 μm; and the D10 of high-density secondary graphite particles is 5.609 μm, D50 is 11.35 μm, and D90 is 19.78 μm. These results show that as the granulation process progresses, the particle D50 increases from 1–3 μm in the raw material to 5–8 μm in primary particles, and then to 10–18 μm in secondary particles, exhibiting a uniform particle size distribution.

[0038] The tap density of the secondary particles was determined in accordance with GB / T 5162 "Determination of tap density of metal powders", and the tap density was not less than 1.05 g / cm3. The particle morphology was observed by scanning electron microscopy, showing that the secondary particles were regular and spherical.

[0039] The high-density graphite secondary particles prepared in this embodiment were graphitized at 2600℃ and used as the negative electrode active material. The electrochemical performance of the coin cell was tested in accordance with GB / T 24533 "Graphite Anode Materials for Lithium-ion Batteries". The measured first discharge specific capacity was not less than 355mAh / g and the first coulombic efficiency was not less than 93%. The graphitized material was then used to prepare the electrode sheet and assembled into a soft-pack battery. The lithium plating test was performed at a 6C charging rate, and the results showed that there was no lithium plating on the electrode sheet.

[0040] Example 2

[0041] This embodiment provides a two-step granulation method for preparing high-density secondary graphite particles from natural graphite, including the following steps:

[0042] Step 1: Using natural flake graphite as raw material, ultrafine grinding is carried out by air jet mill, and mechanical particle shaping treatment is combined to trim the particle edges and eliminate flaky debris, so as to obtain ultrafine natural graphite particle powder with uniform particle size, regular morphology and D50 of 1.5μm.

[0043] Step 2: Using bisphenol A type epoxy resin as the thermosetting epoxy resin, with an epoxy value of 0.40~0.55 eq / 100g and a viscosity of 5000~20000 mPa·s at 25℃. The bisphenol A type epoxy resin does not contain a curing agent and undergoes a cross-linking curing reaction at 100~200℃.

[0044] At room temperature of 25℃, 87% by mass of the ultrafine natural graphite powder obtained in step one and 13% by mass of thermosetting epoxy resin were added to a fusion machine (VS-1000) for mechanical fusion treatment. The fusion machine speed was 2000 rpm and the fusion treatment time was 2 hours, resulting in primary particles with a D50 of approximately 5.5 μm. Subsequently, the particles were cured at 180℃ for 3 hours with a curing temperature rise rate of 5℃ / min, resulting in primary particles with a certain mechanical strength.

[0045] Step 3: Weigh 25% of the mass of the petroleum asphalt after curing. The softening point of the petroleum asphalt is 100℃, the coking value is 60%, the quinoline insoluble content is ≤1%, and the particle size is 5~8μm.

[0046] Petroleum asphalt was added to the cured primary granules, mixed thoroughly, and then placed in a horizontal reactor for secondary granulation under a nitrogen protective atmosphere. During the secondary granulation process, the reactor rotated continuously at a speed of 20 rpm, with the equipment axis tilted at 5°. The temperature was increased from room temperature to 300°C at a rate of 5°C / min and held for 1 hour, then increased to 600°C and held for 1 hour, and finally increased to 750°C and held until the secondary granulation was completed. The total secondary granulation time, including the heating time, was 5 hours, simultaneously completing the carbonization and shaping of the asphalt to obtain high-density graphite secondary granules.

[0047] Step 4: The obtained secondary particles are broken down and deagglomerated, then sieved through a 325-mesh vibrating screen. The undersize material is collected to obtain the finished product. This process does not require demagnetization treatment or asphalt carbon coating modification.

[0048] The high-density graphite secondary particles were tested using the same method as in Example 1. The D50 of the high-density graphite secondary particles obtained in this example was found to be approximately 12 μm, and the tap density was not less than 1.05 g / cm³. 3 The secondary particles have a regular spherical shape and high sphericity.

[0049] The high-density graphite secondary particles prepared in this embodiment were graphitized at 2800℃ and used as the negative electrode active material. The coin cells were assembled according to GB / T 24533 "Graphite Anode Materials for Lithium-ion Batteries" and the electrochemical performance was tested. The lithium plating test was carried out at a 6C charging rate. The results showed that there was no lithium plating on the electrode and the fast charging performance was comparable to that of Example 1.

[0050] Example 3

[0051] This embodiment provides a two-step granulation method for preparing high-density secondary graphite particles from natural graphite, including the following steps:

[0052] Step 1: Using natural flake graphite as raw material, the material is ultra-finely pulverized by ball milling and mechanically shaped to trim the edges and corners of the particles and eliminate flaky debris, resulting in ultra-fine natural graphite particle powder with uniform particle size, regular morphology, and D50 of 3μm.

[0053] Step 2: Using bisphenol A type epoxy resin as the thermosetting epoxy resin, with an epoxy value of 0.40~0.55 eq / 100g and a viscosity of 5000~20000 mPa·s at 25℃. The bisphenol A type epoxy resin does not contain a curing agent and undergoes a cross-linking curing reaction at 100~200℃.

[0054] At room temperature of 20℃, 95% by mass of the ultrafine natural graphite powder obtained in step one and 5% by mass of thermosetting epoxy resin were added to a fusion machine (VS-1000) for mechanical fusion treatment. The fusion machine speed was 1000 rpm and the fusion treatment time was 1 h, resulting in primary particles with a D50 of approximately 7 μm. Subsequently, the particles were cured at 120℃ for 2 h with a curing temperature rise rate of 3℃ / min, resulting in primary particles with a certain mechanical strength.

[0055] Step 3: Weigh out 15% of the mass of the mesophase asphalt after curing. The softening point of the mesophase asphalt is 120℃, the coking value is 70%, the quinoline insoluble content is ≤1%, and the particle size is 5~8μm.

[0056] Mesophase asphalt was added to the cured primary granules, mixed thoroughly, and then placed in a horizontal reactor for secondary granulation under an argon protective atmosphere. During the secondary granulation process, the reactor rotated continuously at a speed of 10 rpm, with the equipment axis tilted at 3°. The temperature was increased from room temperature to 300°C at a rate of 3°C / min and held for 0.5 hours, then increased to 600°C and held for 0.5 hours, and finally increased to 650°C and held until the secondary granulation was completed. The total secondary granulation time, including the heating time, was 3 hours, during which the asphalt carbonization and shaping were simultaneously completed, resulting in high-density graphite secondary granules.

[0057] Step 4: The obtained secondary particles are broken down and deagglomerated, then sieved through a 325-mesh vibrating screen. The undersize material is collected to obtain the finished product. This process does not require demagnetization treatment or asphalt carbon coating modification.

[0058] The high-density graphite secondary particles were tested using the same method as in Example 1. The D50 of the high-density graphite secondary particles obtained in this example was found to be approximately 16 μm, and the secondary particles had a regular spherical morphology. Due to the lower amount of asphalt used in this example, the tapped density was slightly lower than 1.05 g / cm³. 3 However, it can still be used as a graphitization precursor.

[0059] The high-density graphite secondary particles prepared in this embodiment were graphitized at 2200℃ and used as negative electrode active materials. Coin cells were assembled according to GB / T 24533 "Graphite Anode Materials for Lithium-ion Batteries" and their electrochemical performance was tested. Lithium plating was tested at a 6C charging rate, and the results showed that no lithium plating occurred on the electrode.

[0060] Comparative Example 1

[0061] This comparative example provides a method for preparing secondary graphite particles by one-step granulation of ultra-small particle size natural graphite, including the following steps:

[0062] Step 1: Using natural flake graphite as raw material, the material is ultra-finely pulverized by ball milling and mechanically shaped to obtain ultra-fine natural graphite particle powder with uniform particle size, regular morphology, and D50 of 2μm.

[0063] Step 2: Weigh out 20% of the mass of ultrafine natural graphite powder in coal tar pitch. The coal tar pitch has a softening point of 80℃, a coking value of 55%, a quinoline insoluble content of ≤1%, and a particle size of 5~8μm.

[0064] Ultrafine natural graphite powder was directly mixed with coal tar pitch and then placed in a horizontal reactor. One-step granulation was carried out under an argon protective atmosphere. During the granulation process, the reactor rotated continuously at a speed of 15 rpm and the axis of the equipment was tilted at 5°. The temperature was increased from room temperature to 700°C at a heating rate of 5°C / min and then held until the granulation was completed. The total granulation time was 4 hours, and secondary graphite particles were obtained.

[0065] Step 3: Disperse and deagglomerate the obtained secondary particles, then sieve them through a 325-mesh vibrating screen, and collect the sieved material to obtain the finished product.

[0066] The obtained secondary graphite particles were tested using the same method as in Example 1. The results showed that the secondary graphite particles obtained in this comparative example had a wide D50 distribution and a tap density of only 0.65 g / cm³. The particles had poor dispersibility and irregular morphology.

[0067] The graphite secondary particles prepared in this comparative example were graphitized at 2600℃ and used as the negative electrode active material. A coin cell was assembled according to GB / T 24533 "Graphite Anode Materials for Lithium-ion Batteries" for electrochemical performance testing. Lithium plating tests were conducted at a 6C charging rate, and the results showed severe lithium plating on the electrode. This is because the tap density of the secondary particles obtained by one-step granulation was only 0.65 g / cm³. 3 The original particles had poor dispersion and irregular morphology, uneven pore distribution within the electrode, and an imperfect conductive network, resulting in high charge transfer resistance. During 6C fast charging, the lithium-ion insertion rate could not keep up with the current demand, causing the surface lithium concentration to rise rapidly and reach the lithium deposition potential. Simultaneously, the particles lacked mechanical strength, making them prone to breakage during cycling and exposing fresh surfaces, further exacerbating localized lithium deposition. In contrast, this application constructs regular spherical, high-density secondary particles with a complete conductive network through a two-step granulation process, matching the lithium-ion insertion rate with the charge transfer rate, thus preventing lithium deposition on the electrode during 6C charging.

[0068] Comparative Example 2

[0069] This comparative example provides a method for preparing secondary graphite particles by granulating ultra-small particle size natural graphite using phenolic resin instead of epoxy resin without curing treatment, comprising the following steps:

[0070] Step 1: Using natural flake graphite as raw material, the material is ultra-finely pulverized by ball milling and mechanically shaped to obtain ultra-fine natural graphite particle powder with uniform particle size, regular morphology, and D50 of 2μm.

[0071] Step 2: Using thermosetting phenolic resin (Resol type, A-stage phenolic resin) as the adhesive, with a softening point of 60~75℃, without adding a curing agent, a cross-linking curing reaction occurs at 100~200℃.

[0072] At room temperature of 25℃, 92% by mass of the ultrafine natural graphite powder obtained in step one and 8% by mass of thermosetting phenolic resin were added to a fusion machine (VS-1000) for mechanical fusion treatment. The fusion machine speed was 1500 rpm and the fusion treatment time was 1.5 h, resulting in primary particles with a D50 of approximately 6 μm. No curing treatment was performed in this step.

[0073] Step 3: Weigh out 20% of the mass of the coal tar pitch. The softening point of the coal tar pitch is 80℃, the coking value is 55%, the quinoline insoluble content is ≤1%, and the particle size is 5~8μm.

[0074] Coal tar pitch was added to the uncured primary granules, mixed thoroughly, and then placed in a horizontal reactor for secondary granulation under an argon protective atmosphere. During the secondary granulation process, the reactor rotated continuously at a speed of 15 rpm, with the equipment axis tilted at 5°. The temperature was increased from room temperature to 300°C at a rate of 5°C / min and held for 1 hour, then increased to 600°C and held for 1 hour, and finally increased to 700°C and held until the secondary granulation was completed. The total secondary granulation time, including the heating time, was 4 hours.

[0075] The primary pellets disintegrated after the addition of asphalt, failing to effectively form high-density secondary particles. The resulting particles exhibited an uneven structure, a wide D50 distribution, and a low tap density. This indicates that whether or not a curing treatment is performed after the initial pelletizing step is crucial to the mechanical strength of the primary particles. Uncured primary particles lack sufficient strength and cannot withstand the rolling impact and asphalt softening and penetration during the second step of high-temperature rolling granulation, leading to the disintegration of the primary pellets. This application addresses this issue by using resin curing treatment to impart sufficient mechanical strength to the primary particles, enabling them to maintain structural integrity during the second asphalt pelletizing process and ultimately form high-density secondary particles.

[0076] This application employs a two-step approach: resin curing and pitch spheroidization. First, resin curing addresses the challenges of granulation of ultra-small-diameter natural graphite and the insufficient strength of primary particles. Then, pitch spheroidization constructs a gradient structure consisting of an inner resin carbon skeleton and an outer pitch carbon conductive network. Both steps are indispensable. Simultaneously, the short diffusion path of the ultra-small-diameter primary particles and the high-density secondary particle structure work together to achieve lithium-free electrode plating under 6C charging after graphitization.

Claims

1. A method for preparing high-density secondary graphite particles by two-step granulation of natural graphite, characterized in that, Includes the following steps: Step 1: Using natural graphite as raw material, it is ultra-finely pulverized by ball milling or air jet milling, and mechanical particle shaping is combined to trim the particle edges and eliminate flaky debris, so as to obtain ultra-fine natural graphite particle powder with uniform particle size, regular morphology and D50 of 1~3μm. Step 2: At room temperature of 15~35℃, 85%~97% of the ultrafine natural graphite powder obtained in Step 1 is mechanically fused with 3%~15% of the binder to obtain primary particles with a D50 of 5~8μm. The primary particles are then cured at 100~200℃. Step 3: Add asphalt to the cured primary granules, wherein the mass of the asphalt is 15% to 30% of the mass of the cured primary granules; place the uniformly mixed material in a horizontal reactor and perform secondary granulation under an argon or nitrogen atmosphere, gradually increasing the temperature to the target temperature of 600 to 800°C at a heating rate of 1 to 10°C / min, and holding at the target temperature until the end of secondary granulation, while simultaneously completing the carbonization and shaping of the asphalt; the total time for secondary granulation, including the heating time, is 2 to 8 hours, resulting in high-density graphite secondary granules with a D50 of 10 to 18 μm.

2. The method according to claim 1, characterized in that, The adhesive used in step two is a thermosetting epoxy resin, which does not contain a curing agent and has a curing temperature of 100~200℃.

3. The method according to claim 1 or 2, characterized in that, In step two, the rotation speed for fusion treatment is 500~3000 rpm, and the fusion treatment time is 1~2 h; the heating rate for curing treatment is 1~10℃ / min, and the curing time is 1~5 h.

4. The method according to claim 3, characterized in that, The asphalt described in step three is coal tar pitch, petroleum asphalt, or mesophase asphalt, with a softening point of 60~120℃, a coking value of 40%~70%, a quinoline insoluble content of ≤1%, and a particle size of 5~8μm.

5. The method according to claim 4, characterized in that, During the heating and heat preservation process of the secondary granulation in step three, the reactor continues to rotate, with a reactor speed of 10~30 rpm and an equipment axis tilt angle of 3°~8°.

6. The method according to claim 5, characterized in that, In step three, the temperature is gradually increased from room temperature to 300℃ and held for 0.5 to 2 hours, then increased to 600℃ and held until the second granulation is completed. Alternatively, the temperature can be raised from room temperature to 300℃ and held for 0.5 to 2 hours, then raised to 600℃ and held for 0.5 to 2 hours, and then raised to the target temperature and held until the secondary granulation is completed.

7. The method according to claim 6, characterized in that, In step three, the heating rate for the staged heating is 3~5℃ / min.

8. The method according to claim 7, characterized in that, It also includes a fourth post-processing step: the secondary particles obtained in step three are broken down and deagglomerated, and then sieved through a 150-325 mesh vibrating screen to collect the sieve material.

9. A high-density secondary graphite particle prepared by the method according to any one of claims 1 to 8, characterized in that, It has a gradient composite structure with ultrafine natural graphite primary particles as the core, inner resin carbon as the bonding skeleton, and outer pitch carbon as the coating layer.

10. The application of the high-density graphite secondary particles as a graphitization precursor in the preparation of anode materials for fast-charging lithium-ion batteries, as described in claim 9.