A novel in-situ composite nano-tungsten carbide with a carbon source and its preparation method
By using water-soluble starch as a carbon source, combined with spray drying, low-temperature pre-carbonization, and high-temperature reducing atmosphere treatment, the problems of uneven mixing and agglomeration of carbon and tungsten sources were solved, and high-purity nano-tungsten carbide materials were prepared, which are suitable for industrial applications.
Patent Information
- Application Number
- CN202611525977.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, it is difficult to uniformly mix carbon and tungsten sources, tungsten carbide particles tend to agglomerate and grow, and it is difficult to balance the purity of the product phase with the synergy of the carbon matrix, resulting in poor performance of nano-tungsten carbide materials.
Water-soluble starch was used as a novel carbon source. It was dissolved with tungsten source compounds in a stoichiometric ratio and then spray-dried and granulated. After low-temperature pre-carbonization in an inert atmosphere and high-temperature carbonization in a reducing atmosphere, nano-tungsten carbide was generated. Subsequently, it was mechanically ground and acid-washed to remove impurities.
The method achieves uniform dispersion and high purity of tungsten-carbon composite materials, with tungsten carbide grains uniformly embedded in the amorphous carbon matrix. The total impurity content of the product is less than 0.5%, making it suitable for industrial production.
Smart Images

Figure CN123105642A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of tungsten carbide technology, and in particular to a novel in-situ composite nano-tungsten carbide with a carbon source and its preparation method. Background Technology
[0002] Tungsten carbide possesses high hardness, good thermal stability, and chemical stability, making it widely used in cemented carbide, wear-resistant coatings, and electrocatalysis. Nano-sizing tungsten carbide and in-situ compositing it with a carbon matrix can further enhance the material's specific surface area and electrical conductivity, expanding its applications in emerging fields such as energy storage and conversion. Currently, the main method for preparing nano-tungsten carbide / carbon composites involves mixing a tungsten source with a solid carbon source (such as activated carbon, carbon black, or graphite) through physical methods like ball milling, followed by a carbonization reaction under a high-temperature reducing atmosphere. However, this method suffers from poor mixing uniformity between the tungsten and carbon sources, incomplete carbonization, and a tendency for tungsten carbide grains to agglomerate and grow in the product. Furthermore, physical mixing makes it difficult to achieve uniform embedding and dispersion of tungsten carbide within the carbon matrix.
[0003] To address the aforementioned issues, existing technologies employ soluble organic compounds (such as glucose, sucrose, phenolic resin, etc.) as carbon sources. These compounds are mixed with a tungsten source to form a solution, which is then dried to obtain a precursor, followed by high-temperature carbonization.
[0004] However, small-molecule sugars such as glucose and sucrose are prone to melting and coking during spray drying, leading to equipment blockage and failure to obtain powder products. Although phenolic resins have a high residual carbon rate after pyrolysis, their curing process is complex, the operating window is narrow, and the introduced impurities are difficult to completely remove in subsequent purification. In addition, the feed ratio of tungsten to carbon source in existing methods lacks reasonable design. Too low a carbon content results in incomplete carbonization of tungsten, generating W2C or elemental tungsten impurities, while too high a carbon content reduces the overall purity of the product. Neither approach can achieve a synergistic composite of high-purity nano-tungsten carbide and an appropriate amount of amorphous carbon matrix. Summary of the Invention
[0005] The purpose of this invention is to provide a novel in-situ composite nano-tungsten carbide with a carbon source and its preparation method, which solves the problems in the prior art of the difficulty in uniformly mixing carbon and tungsten sources, the easy agglomeration and growth of tungsten carbide particles, and the difficulty in achieving both product phase purity and synergy with the carbon matrix.
[0006] To achieve the above objectives, this invention provides a novel in-situ composite nano-tungsten carbide preparation method using a carbon source, comprising the following steps: The tungsten source compound and the novel carbon source were added to the solvent in a stoichiometric ratio and stirred until completely dissolved to obtain a clear and homogeneous mixed precursor solution. The obtained mixed precursor solution was dried and granulated to obtain tungsten-carbon composite precursor powder with uniform particle size. The obtained composite precursor powder was placed in a reactor, an inert protective atmosphere was introduced, the temperature was raised to the pre-carbonization temperature and then held to allow the carbon source to undergo preliminary pyrolysis and carbonization, thus obtaining the pre-carbonized intermediate powder. The atmosphere inside the reactor is switched to a reducing atmosphere, and the temperature is raised to the carbonization temperature and held, so that the tungsten component completes the reduction reaction and subsequent carbonization reaction in situ in the carbon matrix, generating nano-tungsten carbide composite crude product. After the reaction is complete, heating is stopped, and the mixture is cooled to room temperature under a protective atmosphere. The crude composite product is then removed and mechanically ground to obtain the pre-treated powder. The pre-treated powder was acid-washed to remove impurities, washed with water until neutral, and then dried to obtain in-situ composite nano-tungsten carbide finished product.
[0007] The method specifically includes adding a tungsten source compound and a novel carbon source to a solvent in a stoichiometric ratio, stirring until completely dissolved, and obtaining a clear, homogeneous mixed precursor solution. According to the molar ratio of tungsten to carbon of 1:3~6, weigh out the tungsten source compound and the novel carbon source respectively; The tungsten source compound was added to deionized water and stirred at 30-50°C for 20-40 minutes until completely dissolved, to obtain a tungsten salt solution with a mass fraction of 10%-25%. The weighed novel carbon source was added to the tungsten salt solution and stirred continuously for 30-60 minutes until completely dissolved, resulting in a clear and homogeneous mixed precursor solution.
[0008] The tungsten source compound is any one of ammonium metatungstate, ammonium paratungstate, or sodium tungstate; the novel carbon source is water-soluble starch; and the solvent is deionized water.
[0009] In the process of drying and granulating the obtained mixed precursor solution: Spray drying was used for drying and granulation. The inlet air temperature was 180~220℃, the outlet air temperature was 80~100℃, the feed flow rate was 5~15mL / min, and the atomization pressure was 0.2~0.4MPa. The average particle size of the resulting tungsten-carbon composite precursor powder was 10~50μm.
[0010] The method specifically includes the following steps: placing the obtained composite precursor powder in a reactor, introducing an inert protective atmosphere, heating to the pre-carbonization temperature, and then holding at that temperature. The tungsten-carbon composite precursor powder was spread evenly in the corundum boat and placed in the constant temperature zone of the tubular reactor. After sealing the furnace, the pressure inside the furnace was evacuated to ≤10Pa. Then, high-purity argon gas was introduced to atmospheric pressure. The evacuation-gas-introduction operation was repeated 2-3 times. The temperature was increased from room temperature to 250-500℃ at a heating rate of 3-10℃ / min, and held for 1-4 hours to complete the low-temperature pre-carbonization and obtain the pre-carbonized intermediate powder. Throughout the pre-carbonization process, the flow rate of high-purity argon gas in the furnace is maintained at 100~200 mL / min.
[0011] The method specifically includes the following steps: Switching to a reducing atmosphere inside the reactor, continuing to heat to the carbonization temperature, and holding at that temperature. After the pre-carbonization and heat preservation are completed, the atmosphere inside the furnace is switched to a hydrogen-argon mixed reducing atmosphere or a carbon monoxide-argon mixed reducing atmosphere, and the total gas flow rate is maintained at 150~250mL / min. Continue heating to 1000-1500℃ at a heating rate of 2-8℃ / min, and hold for 1-6 hours to reduce tungsten oxide in situ to elemental tungsten in the carbon matrix, and then react with the carbon matrix to form tungsten carbide. After the heat preservation reaction is completed, the reducing atmosphere is stopped and the protection is switched back to high-purity argon.
[0012] In the hydrogen-argon mixed reducing atmosphere, the volume percentage of hydrogen is 10% to 30%, and the remainder is high-purity argon. In the carbon monoxide-argon mixed reducing atmosphere, the volume percentage of carbon monoxide is 10% to 30%, and the remainder is high-purity argon.
[0013] The present invention also includes a novel in-situ carbon source composite nano-tungsten carbide, which is prepared by the aforementioned novel in-situ carbon source composite nano-tungsten carbide preparation method.
[0014] This invention discloses a novel carbon source in-situ composite nano-tungsten carbide and its preparation method. Water-soluble starch is used as a novel carbon source, and ammonium metatungstate is used as a tungsten source. A homogeneous precursor solution is prepared by mixing tungsten and carbon in a molar ratio of 1:3 to 6. The tungsten-carbon composite precursor powder is obtained by spray drying and granulation. Then, it is subjected to low-temperature pre-carbonization in an inert atmosphere and high-temperature in-situ carbonization in a reducing atmosphere, so that the tungsten carbide grains nucleate and grow in situ in an amorphous carbon matrix. Finally, the finished product is obtained by grinding, acid washing and drying. This invention uses water-soluble starch to avoid the melting and coking problem during the spray drying of small molecule sugars. Its pure carbon, hydrogen, and oxygen composition ensures that the total impurity content of the product is ≤0.5%. The liquid-phase molecular-level mixing and in-situ carbonization process realizes the uniform embedding and dispersion of tungsten carbide grains (20~80nm) in an amorphous carbon matrix. The carbon content of the product is 5%~15%. It overcomes the defects of traditional methods, such as uneven mixing of tungsten source and carbon source, easy agglomeration of particles, and unreasonable carbon ratio leading to the formation of impurity phases. The process is simple and suitable for industrial production. Attached Figure Description
[0015] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0016] Figure 1This is a flowchart of the preparation method of the novel in-situ composite nano-tungsten carbide using a carbon source according to the present invention. Detailed Implementation
[0017] The embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.
[0018] This invention provides a novel in-situ composite nano-tungsten carbide preparation method using a carbon source, comprising the following steps: S1: Add the tungsten source compound and the novel carbon source to the solvent in a stoichiometric ratio, stir until completely dissolved, and obtain a clear and homogeneous mixed precursor solution.
[0019] Specifically, S11: Weigh out the tungsten source compound and the novel carbon source according to the molar ratio of tungsten to carbon of 1:3~6; S12: Add the tungsten source compound to deionized water and stir at 30~50℃ for 20~40 min until completely dissolved to obtain a tungsten salt solution with a mass fraction of 10%~25%; S13: Add the weighed novel carbon source to the tungsten salt solution and stir continuously for 30-60 minutes until completely dissolved to obtain a clear and homogeneous mixed precursor solution.
[0020] The tungsten source compound is any one of ammonium metatungstate, ammonium paratungstate, or sodium tungstate; the novel carbon source is water-soluble starch; and the solvent is deionized water.
[0021] In this embodiment, the water-soluble starch is a soluble starch derived from corn or potato, with a molecular weight ranging from tens of thousands to millions of Daltons, exhibiting good water solubility and film-forming properties. During spray drying, the water-soluble starch does not undergo melting or coking, ensuring a stable powder product. Furthermore, the abundant hydroxyl groups on its molecular chain can form hydrogen bonds with the tungsten source, facilitating the uniform anchoring of tungsten ions at the carbon source molecular level. Moreover, the water-soluble starch is a pure carbon-hydrogen-oxygen natural polymer; after high-temperature pyrolysis, the products are only amorphous carbon and water vapor, without introducing impurities such as sulfur, nitrogen, or metals into the system, thus ensuring the high purity of the product.
[0022] S2: The obtained mixed precursor solution is dried and granulated to obtain tungsten-carbon composite precursor powder with uniform particle size.
[0023] Specifically, spray drying is used for drying and granulation, with an inlet air temperature of 180~220℃, an outlet air temperature of 80~100℃, a feed flow rate of 5~15mL / min, and an atomization pressure of 0.2~0.4MPa; the average particle size of the resulting tungsten-carbon composite precursor powder is 10~50μm.
[0024] In this embodiment, the inlet air temperature for spray drying needs to be higher than the boiling point of water and lower than the thermal decomposition initiation temperature of starch to ensure rapid evaporation of moisture while avoiding premature pyrolysis of the carbon source. The outlet air temperature reflects the degree of completion of droplet drying. An outlet air temperature of 80~100℃ ensures that the powder moisture content is less than 3% to prevent sticking to the wall. The coordinated control of feed flow rate and atomization pressure determines the droplet size and particle size distribution. A low feed flow rate of 5~15mL / min combined with an atomization pressure of 0.2~0.4MPa can obtain spherical precursor powder with a particle size of 10~50μm. This particle size range ensures uniform heating of the powder in the subsequent tubular furnace reaction and avoids the loss of excessively fine powder due to dispersion in the airflow.
[0025] S3: Place the obtained composite precursor powder in a reactor, introduce an inert protective atmosphere, heat to the pre-carbonization temperature and hold for a period of time to allow the carbon source to undergo preliminary pyrolysis and carbonization, thereby obtaining the pre-carbonized intermediate powder.
[0026] Specifically, S31: Spread the tungsten-carbon composite precursor powder evenly in the corundum boat, place it in the constant temperature zone of the tubular reactor, seal the furnace body, evacuate to the furnace pressure ≤10Pa, then introduce high-purity argon to atmospheric pressure, and repeat the evacuation-ventilation operation 2~3 times. S32: Heat from room temperature to 250-500℃ at a heating rate of 3-10℃ / min, and hold for 1-4 hours to complete low-temperature pre-carbonization and obtain pre-carbonized intermediate powder; S33: Maintain the flow rate of high-purity argon gas in the furnace at 100~200mL / min throughout the pre-carbonization process.
[0027] In this embodiment, the purpose of the vacuum-ventilation cycle is to fully replace and remove the residual air (especially oxygen) in the furnace, preventing the carbon source from being oxidized and consumed during subsequent heating. The pre-carbonization temperature range of 250~500℃ covers the main pyrolysis stages of water-soluble starch: 250~350℃ is the dehydroxylation and condensation reaction of starch molecular chains, generating unsaturated carbon skeletons and releasing small molecule gases such as H2O and CO2; 350~500℃ is the further aromatization of carbon skeletons, forming reactive amorphous carbon; the heating rate of 3~10℃ / min avoids powder cracking or bubbling due to concentrated release of pyrolysis gases, and holding the temperature for 1~4h ensures the full progress of the pyrolysis reaction; after pre-carbonization, the tungsten source (ammonium metatungstate) decomposes into WO3 in this temperature range, which is uniformly distributed in the pyrolytic carbon matrix, providing reactants for subsequent high-temperature carbonization.
[0028] S4: Switch the atmosphere inside the reactor to a reducing atmosphere, continue to heat to the carbonization temperature and hold the temperature, so that the tungsten component completes the reduction reaction and subsequent carbonization reaction in situ in the carbon matrix, generating nano-tungsten carbide composite crude product.
[0029] Specifically, S41: After the pre-carbonization and heat preservation are completed, the atmosphere inside the furnace is switched to a hydrogen-argon mixed reducing atmosphere or a carbon monoxide-argon mixed reducing atmosphere, and the total gas flow rate is maintained at 150~250mL / min. S42: Continue heating to 1000~1500℃ at a heating rate of 2~8℃ / min, hold for 1~6h, so that tungsten oxide is reduced to elemental tungsten in situ in the carbon matrix, and then reacts with the carbon matrix to form tungsten carbide. S43: After the heat preservation reaction is completed, stop the introduction of the reducing atmosphere and switch back to high-purity argon gas protection.
[0030] In the hydrogen-argon mixed reducing atmosphere, the volume percentage of hydrogen is 10% to 30%, and the remainder is high-purity argon. In the carbon monoxide-argon mixed reducing atmosphere, the volume percentage of carbon monoxide is 10% to 30%, and the remainder is high-purity argon.
[0031] In this embodiment, hydrogen or carbon monoxide is used as a reducing component, with a volume percentage of 10% to 30%. Too low a concentration of reducing component will reduce the reduction rate, while too high a concentration of reducing component will increase safety risks and costs. The carbonization temperature of 1000 to 1500°C is selected based on the following considerations: below 1000°C, the reduction rate of WO3 is slow and the carbonization reaction is incomplete, which easily leads to the formation of low-order tungsten carbide phase; 1500°C is the upper limit temperature, above which the tungsten carbide grains grow significantly and energy consumption increases; a heating rate of 2 to 8°C / min is conducive to the full reduction of WO3 to metallic W before reacting with carbon to form WC, avoiding the formation of W2C impurity phase due to incomplete reduction of WO3 before entering the carbonization stage caused by excessively rapid heating. The reaction process of high-temperature carbonization is as follows: WO3 is first reduced to WO2 by H2 or CO, and further reduced to W. The newly generated active W atoms react with neighboring carbon atoms to form WC crystal nuclei. As the holding time increases, the WC crystal nuclei grow to a limited size under the spatial confinement of the carbon matrix, forming fine grains of 20~80nm.
[0032] S5: After the reaction is complete, stop heating, cool to room temperature under a protective atmosphere, take out the composite crude product and mechanically grind it to obtain the pre-treated powder.
[0033] Specifically, the mechanical grinding is a planetary ball mill with a ball-to-material ratio of (5~10):1 and a grinding time of 10~30 min. The D50 particle size of the pre-treated powder after grinding is ≤5μm.
[0034] In this embodiment, after the reaction is completed, the product is naturally cooled to room temperature under a protective atmosphere to prevent oxidation of the high-temperature product upon contact with air. The ball-to-material ratio of 5~10:1 in the planetary ball mill ensures grinding efficiency. If the ball-to-material ratio is too low, the grinding will be insufficient, and if it is too high, wear impurities from the grinding jar and grinding balls may be introduced. A grinding time of 10~30min is a moderately short grinding time, the purpose of which is to break up the loose agglomerates formed by high-temperature sintering, while avoiding excessive grinding that would cause tungsten carbide grains to fall off from the carbon matrix or introduce too many impurities. The pre-treated powder with a D50 particle size ≤5μm after grinding is beneficial for the full dissolution of impurities in the subsequent acid washing process.
[0035] S6: The pre-treated powder is acid-washed to remove impurities, washed with water until neutral, and then dried to obtain the in-situ composite nano tungsten carbide product.
[0036] Specifically, the pickling process uses 5% to 10% dilute hydrochloric acid at a temperature of 40 to 60°C for 1 to 2 hours; after washing with water until the pH of the filtrate is 6 to 8, it is dried in a vacuum environment at 60 to 80°C for 8 to 12 hours.
[0037] In this embodiment, the main purpose of acid washing with dilute hydrochloric acid is to remove trace amounts of residual WO3 (parts that are not completely reduced or carbonized) and trace impurity ions introduced by the tungsten source from the pre-treated powder. 5%~10% dilute hydrochloric acid can effectively dissolve WO3 to form soluble tungsten oxychloride complexes under heating conditions of 40~60℃, but it has no corrosive effect on tungsten carbide and carbon matrix, thus achieving selective impurity removal. Washing with water to a pH of 6~8 ensures the complete removal of free acid and chloride ions, preventing residual acid from affecting the product performance. The vacuum drying temperature of 60~80℃ is lower than the oxidation temperature of the carbon matrix, and the vacuum environment avoids oxidation during the drying process. The drying time of 8~12h ensures that the product moisture content is less than 0.5%.
[0038] The present invention discloses a method for preparing a novel in-situ composite nano-tungsten carbide using a novel carbon source. Water-soluble starch is used as the carbon source, leveraging its excellent water solubility, non-melting and non-coking properties, and pure carbon, hydrogen, and oxygen elemental composition. It is uniformly mixed with the tungsten source at the molecular level in the liquid phase, and then spray-dried to obtain a homogeneous tungsten-carbon composite precursor powder. Low-temperature pre-carbonization in an inert atmosphere allows the starch to be fully pyrolyzed into reactive amorphous carbon, while the tungsten source decomposes in situ into WO3 uniformly distributed within the carbon matrix. Subsequently, a reducing agent is used. High-temperature in-situ carbonization is carried out in an atmosphere, where WO3 is converted into metallic tungsten under the synergistic reduction of hydrogen / carbon monoxide and the carbon matrix. It then reacts with neighboring carbon atoms to form WC crystal nuclei. Under the spatial confinement of the carbon matrix, the grain size is suppressed to 20~80nm, forming a composite structure in which tungsten carbide particles are uniformly embedded in the amorphous carbon matrix. The agglomerates are then dispersed by short-time ball milling, and residual WO3 and trace impurities are selectively dissolved by dilute hydrochloric acid. The final product has a carbon content of 5%~15% and a total impurity content of ≤0.5%.
[0039] The present invention also includes a novel carbon source in-situ composite nano-tungsten carbide, which is prepared by the aforementioned method for preparing the novel carbon source in-situ composite nano-tungsten carbide.
[0040] The above-disclosed embodiments are merely one or more preferred embodiments of this application and should not be construed as limiting the scope of this application. Those skilled in the art can understand that all or part of the processes for implementing the above embodiments and equivalent changes made in accordance with the claims of this application still fall within the scope of this application.
Claims
1. A novel method for preparing in-situ composite nano-tungsten carbide using a carbon source, characterized in that, Includes the following steps: The tungsten source compound and the novel carbon source were added to the solvent in a stoichiometric ratio and stirred until completely dissolved to obtain a clear and homogeneous mixed precursor solution. The obtained mixed precursor solution was dried and granulated to obtain tungsten-carbon composite precursor powder with uniform particle size. The obtained composite precursor powder was placed in a reactor, an inert protective atmosphere was introduced, the temperature was raised to the pre-carbonization temperature and then held to allow the carbon source to undergo preliminary pyrolysis and carbonization, thus obtaining the pre-carbonized intermediate powder. The atmosphere inside the reactor is switched to a reducing atmosphere, and the temperature is raised to the carbonization temperature and held, so that the tungsten component completes the reduction reaction and subsequent carbonization reaction in situ in the carbon matrix, generating nano-tungsten carbide composite crude product. After the reaction is complete, heating is stopped, and the mixture is cooled to room temperature under a protective atmosphere. The crude composite product is then removed and mechanically ground to obtain the pre-treated powder. The pre-treated powder was acid-washed to remove impurities, washed with water until neutral, and then dried to obtain in-situ composite nano-tungsten carbide finished product.
2. The method for preparing novel in-situ composite nano-tungsten carbide using a novel carbon source as described in claim 1, characterized in that, The method specifically includes adding a tungsten source compound and a novel carbon source to a solvent in a stoichiometric ratio, stirring until completely dissolved, and obtaining a clear, homogeneous mixed precursor solution. According to the molar ratio of tungsten to carbon of 1:3~6, weigh out the tungsten source compound and the novel carbon source respectively; The tungsten source compound was added to deionized water and stirred at 30-50°C for 20-40 minutes until completely dissolved, to obtain a tungsten salt solution with a mass fraction of 10%-25%. The weighed novel carbon source was added to the tungsten salt solution and stirred continuously for 30-60 minutes until completely dissolved, resulting in a clear and homogeneous mixed precursor solution.
3. The method for preparing novel in-situ composite nano-tungsten carbide using a novel carbon source as described in claim 2, characterized in that, The tungsten source compound is any one of ammonium metatungstate, ammonium paratungstate, or sodium tungstate; the novel carbon source is water-soluble starch; and the solvent is deionized water.
4. The method for preparing novel in-situ composite nano-tungsten carbide using a novel carbon source as described in claim 1, characterized in that, In the drying and granulation process of the obtained mixed precursor solution: Spray drying was used for drying and granulation. The inlet air temperature was 180~220℃, the outlet air temperature was 80~100℃, the feed flow rate was 5~15mL / min, and the atomization pressure was 0.2~0.4MPa. The average particle size of the resulting tungsten-carbon composite precursor powder was 10~50μm.
5. The method for preparing novel in-situ composite nano-tungsten carbide using a novel carbon source as described in claim 1, characterized in that, The method specifically includes placing the obtained composite precursor powder in a reactor, introducing an inert protective atmosphere, heating to the pre-carbonization temperature, and then holding at that temperature. The tungsten-carbon composite precursor powder was spread evenly in the corundum boat and placed in the constant temperature zone of the tubular reactor. After sealing the furnace, the pressure inside the furnace was evacuated to ≤10Pa. Then, high-purity argon gas was introduced to atmospheric pressure. The evacuation-gas-introduction operation was repeated 2-3 times. The temperature was increased from room temperature to 250-500℃ at a heating rate of 3-10℃ / min, and held for 1-4 hours to complete the low-temperature pre-carbonization and obtain the pre-carbonized intermediate powder. Throughout the pre-carbonization process, the flow rate of high-purity argon gas in the furnace is maintained at 100~200 mL / min.
6. The method for preparing novel in-situ composite nano-tungsten carbide using a novel carbon source as described in claim 1, characterized in that, The method specifically includes switching the atmosphere inside the reactor to a reducing atmosphere, continuing to heat to the carbonization temperature and holding at that temperature. After the pre-carbonization and heat preservation are completed, the atmosphere inside the furnace is switched to a hydrogen-argon mixed reducing atmosphere or a carbon monoxide-argon mixed reducing atmosphere, and the total gas flow rate is maintained at 150~250mL / min. Continue heating to 1000-1500℃ at a heating rate of 2-8℃ / min, and hold for 1-6 hours to reduce tungsten oxide in situ to elemental tungsten in the carbon matrix, and then react with the carbon matrix to form tungsten carbide. After the heat preservation reaction is completed, the reducing atmosphere is stopped and the protection is switched back to high-purity argon.
7. The method for preparing novel in-situ composite nano-tungsten carbide using a novel carbon source as described in claim 6, characterized in that, In the hydrogen-argon mixed reducing atmosphere, the volume percentage of hydrogen is 10% to 30%, and the remainder is high-purity argon. In the carbon monoxide-argon mixed reducing atmosphere, the volume percentage of carbon monoxide is 10% to 30%, and the remainder is high-purity argon.
8. A novel in-situ composite nano-tungsten carbide with a carbon source, characterized in that, It is prepared by the method described in any one of claims 1-7.